Marine atmosphere corrosion resistant hot-rolled H-shaped steel and manufacturing method thereof
By adding vanadium nitrogen alloy and appropriate amount of Cu, Ni, Cr elements to the H-shaped steel for marine engineering, and selecting the addition of trace Ce, combined with high-temperature final rolling and temperature-controlled rolling technology, the corrosion problem of H-shaped steel in the marine environment is solved, and the High strength, low temperature toughness and economical production resistance to marine atmospheric corrosion.
Patent Information
- Application Number
- CN202410975040.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-07-19
AI Technical Summary
In the prior art, H-shaped steel for marine engineering is prone to electrochemical corrosion in marine environments, resulting in a decrease in strength and a shortened service life. The added precious alloy elements increase production costs and corrosion rates, making it difficult to meet high-strength and low-temperature toughness at the same time. and the demand for resistance to marine atmospheric corrosion.
Through reasonable chemical composition design, add vanadium nitrogen alloy and appropriate amounts of Cu, Ni, and Cr elements, and select and add trace Ce elements according to needs to control chemical composition such as C: 0.07-0.12%, Si+Mn: 0.80-1.2%, Ni +Cu:0.30-0.60%, Cr:0.40-0.70%, V:0.03-0.045%, to improve the marine atmospheric corrosion resistance of hot-rolled H-shaped steel, and adopt high-temperature final rolling and temperature-controlled rolling technology to reduce production costs .
It significantly improves the corrosion resistance of hot-rolled H-shaped steel in marine atmospheric environments, reduces alloy costs, and does not require further heat treatment, reduces production processes and costs, and improves the strength and toughness of steel, with corrosion rate lower than that of Q355B steel. 35%.
Smart Images

Figure CN119020689A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of H-beam production, and particularly relates to a hot-rolled H-beam resistant to marine atmospheric corrosion and a manufacturing method thereof. Background Art
[0002] The development and utilization of the ocean cannot be separated from the development and application of high-strength steel. The demand for marine engineering steel will continue to expand, and the research and development of marine engineering steel has become a focus of widespread attention. However, due to the complexity and variability of the marine environment, marine engineering steel will be affected by marine environmental factors during service, and electrochemical corrosion will occur, resulting in corrosion cracking of steel and reduction of mechanical properties, which will shorten the service life of marine equipment.
[0003] As the steel environment for marine engineering develops towards high-cold polar regions and humid and harsh seas, there is a higher demand for the strength, toughness and marine environmental corrosion resistance of H-beams for marine engineering. Therefore, it has become an inevitable trend to produce an H-beam that is resistant to marine atmospheric corrosion.
[0004] After searching, Chinese patent CN 113528970 A discloses a low compression ratio yield strength 355MPa grade heavy hot-rolled H-beam and its production method and application. The hot-rolled H-beam includes the following chemical components in weight percentage: C: 0.13~0.20%, Si: 0.15~0.40%, Mn: 1.10~1.50%, P: ≤0.035%, S: ≤0.035%, V: 0.030~0.060%, B: 0.0008% ~0.0015%, Nb: 0.02~0.05%, N: 0.015~0.020%, 3.5≤(Nb+V) / N≤5.5, Als: ≤0.005%, and the rest is Fe and unavoidable impurities. The obtained hot-rolled H-shaped steel has good mechanical properties, with yield strength ≥355MPa, tensile strength ≥570MPa, elongation ≥20%, and 0°C longitudinal V-shaped impact energy KV2 ≥85J. The hot-rolled H-shaped steel provided by the prior art has a high carbon content and is added with B element, and its welding performance and low-temperature impact toughness are poor. Due to the addition of more Mn elements, the degree of internal segregation of the steel plate is increased, and the low-temperature toughness and corrosion resistance of the steel plate are reduced. It does not explain the corrosion resistance.
[0005] Chinese patent CN 101760704 A discloses an economical high-strength and high-weathering hot-rolled H-shaped steel containing vanadium and nitrogen and a rolling method thereof, wherein the H-shaped steel comprises the following chemical components in weight percentage: C: 0.07-0.12%, Si: 0.30-0.55%, Mn: 1.30-1.55%, P≤0.045%, S: ≤0.010%, Cr: 0.20-0.30%, Ni: 0.15-0.30%, Cu: 0.25-0.35%, V: 0.010~0.015%, N: 0.10~0.015%, Alt: 0.006-0.03%, and the rest is Fe and unavoidable impurities. This prior art is similar to the present invention, and both are obtained by adding an appropriate amount of vanadium-nitrogen alloy to obtain economical weathering steel. However, due to the high content of added Mn, the marine atmospheric corrosion resistance deteriorates sharply, and the corrosion rate is 2.49~2.53g / m 2 ∙h, which is 55% of the corrosion rate of Q345B steel and has poor corrosion performance.
[0006] Chinese patent CN 106947913 A discloses a high-strength and high-toughness hot-rolled weathering steel plate and a preparation method thereof, wherein the hot-rolled weathering steel plate comprises the following chemical components in weight percentage: C: 0.05%~0.10%, Si: 0.10%~0.50%, Mn: 1.00%~1.30%, P: ≤0.015%, S: ≤0.010%, Cr: 0.30%~0.70%, Ni: 0.10%~0.40%, Cu: 0.25%~0.50%, Al: 0.020%~0.050%, Nb: 0.01%~0.04%, Ti: 0.010%~0.030%, and the rest is Fe and unavoidable impurities. Based on the traditional hot rolling production line, the existing technology has developed a high-strength and high-toughness hot-rolled weathering steel plate suitable for thick specifications, with a yield strength of 450-500MPa, a tensile strength ≥550MPa, an elongation of 25.0%-30.0%, and a longitudinal impact force of >300J at -60°C. However, this product is a steel plate produced from continuous casting billets, which is very different from the H-beam produced from special-shaped billets in terms of process. Moreover, due to the high content of added Mn, the marine atmospheric corrosion resistance deteriorates sharply, and the average corrosion rate in the marine environment is 2.22~2.48g / m 2 ∙h, the corrosion rate of Q345B steel is only 55%.
[0007] Chinese patent CN112795844 A discloses a low-carbon Cr-Ni high-strength corrosion-resistant steel and its preparation method, wherein the corrosion-resistant steel comprises the following chemical components by weight percentage: C: 0.01-0.03%, Si: 0.1-0.5%, Mn: 0.5-1.0%, Ni: 1.0-2.0%, Cr: 3.0-10.0%, Cu: 0.2-0.5%, N: 0.02-0.06%, P: 0.04-0.1%, S: ≤ 0.005%, and the rest is Fe and unavoidable impurities. The corrosion rate of the material in the marine environment is 2.19-3.08 g / m 2 ∙h. The steel of the prior art contains a large amount of precious alloy elements such as Cu, Ni, and Cr, 4.2%≤Cu+Ni+Cr≤12.5%, and the alloy cost is high; the P content in the steel is high, which will deteriorate the welding performance and toughness and plasticity of the steel, especially reduce the low-temperature impact toughness of the steel, but the low-temperature toughness is not mentioned.
[0008] Chinese patent CN 105886961 A discloses a high-performance hot-rolled H-beam resistant to marine atmospheric corrosion and a preparation method thereof, wherein the H-beam comprises the following chemical components in weight percentage: C: 0.015-0.075%, Si: 0.20-0.65%, Mn: 0.40-1.60%, P: ≤0.025%, S: ≤0.010%, Mo: 0.20-0.70%, Cu: 0.30-1.20%, Ni: 0.90-3.50%, Sb: 0.035-0.10%, Nb: 0.015-0.100%, Ti: 0.010-0.050%, Al: 0.015-0.100%, and the rest is Fe and unavoidable impurities. The H-beam provided by the prior art has good toughness and plasticity, and has excellent marine atmospheric corrosion resistance and excellent welding performance. However, more precious alloy elements such as Cu, Ni, and Mo are added, 1.43%≤Cu+Ni+Mo+Sb+Nb+Ti≤5.65%, and the alloy cost is high.
[0009] Chinese patent CN 108396228 A discloses a high-weathering hot-rolled H-beam with a yield strength of 450MPa and a heat treatment process thereof, wherein the high-weathering hot-rolled H-beam comprises the following chemical components in weight percentage: C: 0.06-0.10%, Si: 0.20-0.40%, Mn: 0.40-0.70%, P≤0.035%, S: ≤0.010%, Cr: 2.00-3.50%, Ni: 0.30-0.50%, Cu: 0.30-0.50%, V: 0.015~0.035%, Alt: 0.02-0.04%, and the rest is Fe and unavoidable impurities. The high-weathering hot-rolled H-beam obtained by the heat treatment process in the prior art has a yield strength of ≥480MPa, a tensile strength of ≥600MPa, an elongation after fracture of ≥20%, and a -40℃ KV2 impact toughness of ≥65J. However, the Cr content in H-beam reaches 2.00-3.50%, and 2.61%≤Cu+Ni+Cr+V≤4.53%, which increases the alloy cost and increases the rolling pressure of hot rolling. At the same time, the use of heat treatment process increases the production cost.
[0010] In the prior art, the Mn content in weather-resistant hot-rolled H-beam is relatively high, which easily increases the degree of internal segregation of the steel plate, reduces the low-temperature toughness and marine atmospheric corrosion resistance of the steel plate; due to the micro-battery effect of cementite and ferrite in pearlite, the corrosion rate is relatively high; adding more precious alloys will increase the production cost of steel; at the same time, some alloy elements (Mo, Nb) lead to the formation of bainite or MA structure, which requires further heat treatment after hot rolling, which will further increase the production cost of hot-rolled H-beam. Therefore, it is necessary to provide a hot-rolled H-beam resistant to marine atmospheric corrosion in order to develop weather-resistant hot-rolled H-beam with reasonable cost and excellent performance. Summary of the invention
[0011] The present invention provides a hot-rolled H-shaped steel resistant to marine atmospheric corrosion and a manufacturing method thereof. Through reasonable chemical composition design, vanadium-nitrogen alloy and appropriate amounts of Cu, Ni and Cr elements are added, and a trace amount of Ce element is selectively added as needed, thereby greatly improving the corrosion resistance of the hot-rolled H-shaped steel in a marine atmospheric environment.
[0012] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0013] The hot-rolled H-shaped steel of the present invention has the following chemical components by mass ratio: C: 0.07-0.12%, Si+Mn: 0.80-1.2%, Ni+Cu: 0.30-0.60%, 0.8<Ni / Cu<1.25, Cr: 0.40-0.70%, V: 0.03-0.045%, 2.5≤V / N≤3.5, Ca: 0.001-0.002%, P≤0.020%, S≤0.005%, O≤40ppm, and the rest are Fe and unavoidable impurity elements. The carbon equivalent CEQ of the steel is 0.39-0.45%.
[0014] Preferably, the chemical composition further comprises Al<0.03%, Ce≤0.03%, and 0.6≤Ce / (S+O)≤4.5.
[0015] The present invention also provides a method for preparing the hot-rolled H-beam, comprising the following steps: heating the steel billet melted and cast with the above chemical composition to 1180-1230°C and then hot rolling, the final rolling temperature is 850-1000°C, cooling to 600-750°C at 2.5-30°C / s after rolling, and then air cooling to room temperature. Since the hot-rolled H-beam is suitable for high-temperature final rolling and temperature-controlled rolling, air cooling can meet the performance control requirements. If temperature-controlled rolling and controlled cooling after rolling are adopted, the strength and toughness of the steel are higher.
[0016] Preferably, the yield strength of the hot-rolled H-beam is 360-420MPa, the tensile strength is 490-570MPa, the elongation is >30%, and the impact energy at -20°C is >120J; in the marine atmospheric environment, the corrosion rate of the H-beam is ≤35%×the corrosion rate of Q355B steel, and the electrode potential of the steel after corrosion is -0.40~-0.53V.
[0017] Preferably, the room temperature structure of the hot-rolled H-beam is ferrite and a small amount of pearlite.
[0018] The hot-rolled H-shaped steel has been in service for a long time in a marine atmosphere environment, and the formed corrosion rust layer has a low elastic modulus and good adhesion. It can be used as a structure that bears dynamic loads such as coastal building structures, coastal bridges, offshore oil drilling platforms, etc., and can also be used in cold areas below -20°C.
[0019] The role of each element in the present invention is analyzed as follows:
[0020] Carbon element C: Carbon element is a basic element in steel and plays a very important role in improving the strength of steel. However, too high carbon content will be detrimental to the atmospheric corrosion resistance of steel. At the same time, carbon has an impact on the welding performance, cold brittleness performance and stamping performance of steel. Therefore, in the present invention, the carbon mass percentage is controlled at 0.08-0.12%.
[0021] Silicon element Si: Si element can play a role in solid solution strengthening in steel, and can be used as a reducing agent and deoxidizer during the smelting process. Si element can also improve the marine atmospheric corrosion resistance of steel. When Si is used in combination with Cu, P, and Cr elements, it can effectively improve the marine atmospheric corrosion resistance of steel. However, too high Si content will reduce the low temperature toughness and welding performance of steel.
[0022] Manganese element Mn: Manganese element is a solid solution strengthening element in steel. Adding an appropriate amount of Mn element to steel is beneficial to improving the strength of the steel plate and the hardenability of the steel. However, a higher Mn content will increase the degree of internal segregation of the steel plate, reduce the uniformity of the mechanical properties and low-temperature toughness of the steel plate, and will also have an adverse effect on the formability of the steel. Secondly, when the Mn content is relatively high, the marine atmospheric corrosion resistance of the steel plate will deteriorate sharply. Therefore, in the present invention, the mass percentage of Mn+Si is controlled at 0.80-1.20%.
[0023] Nickel: Nickel is a relatively stable element. Adding Ni oxide to steel can improve cation selectivity and prevent Cl - The diffusion of ions can significantly improve the corrosion resistance of steel in marine atmospheric environments, and can also effectively improve the strength and toughness of steel. Therefore, theoretically, the higher the Ni content in steel is within a certain range, the better. However, Ni is a very expensive alloy element, and from the perspective of low-cost mass production, the Ni content should be controlled.
[0024] Copper element Cu: Copper is the most important alloy element for improving atmospheric corrosion resistance. In order to improve atmospheric corrosion resistance and reduce the hot working sensitivity of Cu-containing steel, it is necessary to use it in combination with Ni element to improve the hot cracking problem. However, adding too high a content of Cu is prone to copper brittleness and deteriorate the surface properties of the steel. Therefore, in the present invention, the mass percentage of Cu+Ni is controlled at 0.30-0.60%, and Ni / Cu: 0.8-1.25.
[0025] Chromium Cr: Chromium can form a dense oxide film on the steel surface, improve the passivation ability of the steel, slow down the growth of the rust layer, and improve the steel's resistance to marine atmospheric corrosion; at the same time, chromium is a solid solution strengthening element that can enhance the hardenability of steel and delay the austenite-ferrite transformation. Chromium is a carbide-forming element. A high Cr content will cause Cr to form M with C. 23 C7 carbides reduce the corrosion resistance of the Cr element and may also reduce the toughness and welding performance of the steel. Therefore, in the present invention, the mass percentage of Cr is controlled to be 0.40-0.70%.
[0026] Vanadium, nitrogen elements V, N: The addition of nitrogen promotes the precipitation rate of V in the alloy system, significantly increases the volume fraction of V (C, N) particles precipitated, and increases the precipitation strengthening effect of vanadium; vanadium is a strong carbide-forming element, and has a strong binding ability with C and N. It can precipitate small and dispersed VN or V (C, N) particles in the γ phase, thereby achieving a fine grain strengthening effect, greatly improving the strength and toughness of the steel. At the same time, V, as a corrosion-resistant alloying element, can increase the self-corrosion potential of steel after addition, which is beneficial to the steel's resistance to marine atmospheric corrosion. However, the unit price of vanadium alloy is relatively high, and excessive addition will increase production costs. Vanadium-nitrogen alloy brings N elements into molten steel, which may further absorb or lose nitrogen during the smelting process. In order to better achieve the precipitation strengthening and fine grain strengthening effects of vanadium, the vanadium-nitrogen ratio should be controlled. Therefore, in the present invention, the mass percentage of V is controlled at 0.030-0.045%, and 2.5≤V / N≤3.5. This ensures that the vanadium-nitrogen ratio is within a certain range, maximizing the strengthening effect of vanadium and nitrogen elements in steel.
[0027] Aluminum element Al: Aluminum element is a strong deoxidizing element and can be used to remove oxygen from molten steel. At the same time, unremoved Al2O3 inclusions in the molten steel will cause local corrosion of the matrix around the steel inclusions. Large-sized Al2O3 inclusions will also reduce the toughness of the steel. At the same time, aluminum can also inhibit nitrogen from dissolving in ferrite, forming AlN to inhibit grain coarsening. However, AlN is easy to aggregate and grow in molten steel, increasing crack sensitivity and prone to cracks on the surface. At the same time, too much Al in the steel occupies the N element, reducing the number of second phase particles such as V (C, N) in the steel, weakening the effect of the V element. Therefore, in the present invention, the mass percentage of Al is controlled at 0.02-0.04%.
[0028] Rare earth element Ce: Rare earth elements are extremely active elements, and are strong deoxidizers and desulfurizers. They mainly purify steel and form inclusions such as CeO2, Ce2O2S or CeAlO3. At the same time, the fine oxides formed by rare earth element Ce promote the precipitation of Nb and V, which can refine the grains and change the state of inclusions in steel. The corrosion products formed by rare earth inclusions (CeO2, Ce2O2S or CeAlO3) during the corrosion process are alkaline and take precedence over the matrix corrosion, reducing the corrosion source points, thereby improving the atmospheric corrosion resistance of steel. Secondly, the rare earth elements dissolved in steel will change the mechanical properties of the rust layer after corrosion, reduce the elastic modulus of the rust layer, stabilize the structure of the rust layer, and have good adhesion, thereby improving the anti-corrosion effect of the rust layer. Thirdly, Ce can reduce aluminum oxides in molten steel to avoid the influence of aluminum oxide inclusions on plasticity and toughness. In addition, rare earth elements can modify inclusions, spheroidize, refine and evenly distribute carbides, sulfides, etc., and improve the plasticity and toughness of steel. Therefore, in the present invention, the mass percentage of rare earth element Ce is controlled to be ≤0.03%, and the mass ratio of Ce / (S+O) is controlled to be within the range of 0.6≤Ce / (S+O)≤4.5 according to the content of S and O impurity elements in the steel.
[0029] Phosphorus and sulfur elements P and S: As impurity elements, they have an adverse effect on the plasticity, toughness and welding performance of steel. When P and Cu are added to steel together, a better composite effect is shown. However, adding more P elements will deteriorate the welding performance of steel, and will also deteriorate the plasticity and toughness of steel, especially drastically reduce the low-temperature impact toughness of steel; it is also prone to local segregation and form banded structure; S elements are prone to form MnS during segregation, causing welding cracks, reduced toughness and resistance to lamellar tearing. Therefore, in the present invention, the mass percentages of P and S are controlled at P≤0.020% and S≤0.005%.
[0030] The key points of the present invention are:
[0031] 1. The difference between the present invention and the prior art CN 108396228 A is that the content of the noble alloy elements is much lower than that of the prior art, which greatly reduces the alloy cost; and the present invention has lower corrosion resistance in the marine atmosphere environment and better corrosion resistance; in addition, the present invention does not require further heat treatment after rolling, which reduces the production process and reduces the production cost.
[0032] 2. Compared with the prior art CN 105886961 A, the present invention has a lower corrosion rate in a marine atmosphere environment and better corrosion resistance; and uses vanadium-nitrogen alloy instead of vanadium iron for vanadium alloying, which reduces the addition of precious alloy elements and reduces the alloy cost.
[0033] 3. Compared with the prior art CN 106947913 A, the present invention is different in that although the content of the added precious alloy elements is relatively similar, the present invention has better low-temperature toughness and formability; the corrosion rate in the marine atmospheric environment is lower and the corrosion resistance is better; and the present invention better controls the content of the Mn element, effectively improving the mechanical properties and corrosion resistance of the steel.
[0034] 4. Compared with the prior art CN 112795844 A, the present invention has higher strength, better welding performance and cold crack sensitivity; lower corrosion rate in marine atmospheric environment and better corrosion performance; from the perspective of the content of precious alloy elements, the content of the present invention is much lower than that of the prior art, and has better economy; and the present invention better controls the content of P element, further improving the welding performance and toughness of steel.
[0035] The relevant data of the present invention and the comparison information of the prior art are shown in Table 1:
[0036] Table 1
[0037]
[0038] It can be seen from the above table that in the weather-resistant steel adapted to the marine atmospheric corrosion environment, the total content of the precious alloy elements Nb+V+Ti+Ni+Cu+Cr in this application is low, which has the advantage of alloy cost; in terms of corrosion resistance, the corrosion rate is relatively low, which has a competitive advantage.
[0039] Compared with the prior art, the outstanding advantages of the present invention are:
[0040] (1) The present invention adopts a reasonable chemical composition design, adds appropriate amounts of Cu, Ni, and Cr elements, and uses vanadium-nitrogen alloy instead of vanadium iron for vanadium alloying, which significantly improves the strength of steel and improves the comprehensive properties of steel. The addition of a trace amount of rare earth element Ce can further improve the toughness and corrosion resistance of the material while ensuring high strength.
[0041] (2) The present invention proposes a method for manufacturing hot-rolled H-shaped steel resistant to marine atmospheric corrosion. After smelting, continuous casting, heating, high-temperature final rolling (950-1000°C) or controlled final rolling (850-950°C), hot-rolled H-shaped steel with required performance can be obtained. No heat treatment process is required, which effectively improves industrial production efficiency and reduces production costs.
[0042] (3) The hot-rolled H-shaped steel described in the present invention not only has high strength and toughness, but also has excellent corrosion resistance. Its yield strength is 360-420MPa, tensile strength is 490-570MPa, elongation>30%, and impact energy at -20℃>200J; the corrosion rate in the marine atmospheric environment is equivalent to less than 35% of Q355B, and the electrode potential of the steel after corrosion is -0.40~-0.53V. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0044] Figure 1 The metallographic structure of the steel of Example 1 of the present invention;
[0045] Figure 2 The figure is a line graph of the corrosion rates of six kinds of steel in the embodiments of the present invention and the comparative examples subjected to a salt spray corrosion test for 168 hours. DETAILED DESCRIPTION
[0046] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.
[0047] The present invention provides a hot-rolled H-beam resistant to marine atmospheric corrosion. The mass percentage of alloy elements of the hot-rolled H-beam, its chemical composition components are: C: 0.07-0.12%, Si+Mn: 0.80-1.2%, Ni+Cu: 0.30-0.60%, 0.8<Ni / Cu<1.25, Cr: 0.40-0.70%, V: 0.03-0.045%, 2.5≤V / N≤3.5, Ca: 0.001-0.002%, P≤0.020%, S≤0.005%, O≤40ppm, the rest are Fe and unavoidable impurity elements, carbon equivalent CEQ: 0.39-0.45%. Preferably, its chemical composition includes Al<0.03%, Ce≤0.03%, and 0.6≤Ce / (S+O)≤4.5. After hot rolling, the yield strength of H-beam is 360-420MPa, the tensile strength is 490-570MPa, the elongation is >30%, and the impact energy at -20℃ is >120J. The room temperature structure of H-beam is ferrite and a small amount of pearlite.
[0048] This will be described below with reference to specific embodiments.
[0049] Example 1
[0050] A hot-rolled H-shaped steel resistant to marine atmospheric corrosion, the alloy element content of which is as follows by mass percentage:
[0051] C: 0.12%, Si: 0.15%, Mn: 0.75%, Cr: 0.56%, Cu: 0.276%, Ni: 0.274%, V: 0.038%, N: 0.014%, Ca: 0.0015%, P: 0.0017%, S: 0.0032%, O: 0.0039%, and the rest is Fe. Carbon equivalent CEQ: 0.40%.
[0052] The smelted and cast steel billet was heated to 1230℃ and then hot rolled. The final rolling temperature was 960℃. After rolling, it was cooled to 600℃ at 12℃ / s and then air-cooled to room temperature to finally obtain a sample with a yield strength of 378MPa, a tensile strength of 537MPa, an elongation of 35%, an impact energy of 206J at -20℃, and a corrosion rate of 1.150g / m²∙h after 168h corrosion in a marine atmosphere environment.
[0053] Example 2
[0054] A hot-rolled H-beam resistant to marine atmospheric corrosion, the alloy element content of which, by mass percentage, is:
[0055] C: 0.11%, Si: 0.20%, Mn: 0.80%, Cr: 0.67%, Cu: 0.28%, Ni: 0.28%, V: 0.036%, N: 0.010%, Ca: 0.0018%, P: 0.0015%, S: 0.0048%, O: 0.0036%, and the rest is Fe. Carbon equivalent CEQ: 0.42%.
[0056] The smelted and cast steel billet was heated to 1230℃ and then hot rolled. The final rolling temperature was 880℃. After rolling, it was cooled to 600℃ at 10℃ / s and then air-cooled to room temperature to finally obtain a sample with a yield strength of 385MPa, a tensile strength of 556MPa, an elongation of 32%, an impact energy of 232J at -20℃, and a corrosion rate of 1.045g / m²∙h after 168h of corrosion in a marine atmosphere environment.
[0057] Example 3
[0058] A hot-rolled H-beam resistant to marine atmospheric corrosion, the alloy element content of which, by mass percentage, is:
[0059] C: 0.10%, Si: 0.25%, Mn: 0.65%, Cr: 0.65%, Cu: 0.22%, Ni: 0.24%, V: 0.030%, N: 0.0092%, Ca: 0.0014%, P: 0.0017%, S: 0.0045%, O: 0.0037%, Ce: 0.008%, Al: 0.023%, and the rest is Fe. Carbon equivalent CEQ: 0.43%.
[0060] The smelted and cast steel billet was heated to 1230℃ and then hot rolled. The final rolling temperature was 880℃. After rolling, it was cooled to 600℃ at 10℃ / s and then air-cooled to room temperature to finally obtain a sample with a yield strength of 396MPa, a tensile strength of 568MPa, an elongation of 36%, an impact energy of 247J at -20℃, and a corrosion rate of 0.976g / m²∙h after 168h of corrosion in a marine atmosphere environment.
[0061] Comparative Example 1
[0062] A hot-rolled H-beam resistant to marine atmospheric corrosion, the alloy element content of which, by mass percentage, is:
[0063] C: 0.11%, Si: 0.30%, Mn: 0.50%, Cr: 0.67%, Cu: 0.32%, Ni: 0.28%, V: 0.035%, N: 0.012%, Ca: 0.0015%, P: 0.004%, S: 0.004%, O: 0.0036%, and the rest are Fe and unavoidable impurities.
[0064] The smelted and cast steel billet was heated to 1240℃ and then hot rolled. The final rolling temperature was 940℃. After cooling to room temperature after rolling, it was reheated to 550℃ and kept warm for 5h to finally obtain the sample with a yield strength of 365MPa, a tensile strength of 512MPa, an elongation of 23%, and an impact energy of 89J at -20℃.
[0065] Comparative Example 1 adopts a post-rolling annealing process, while the embodiment does not require a heat treatment process compared to Comparative Example 1, which can effectively improve industrial production efficiency and reduce production costs; the mechanical properties of the steel in the embodiment are better; and the corrosion rate of Comparative Example 1 after 168 hours of corrosion in a marine atmospheric environment is 1.46g / m²∙h, which is higher than the corrosion rate of the embodiment, and the corrosion resistance is relatively poor.
[0066] Comparative Example 2
[0067] A hot-rolled H-beam resistant to marine atmospheric corrosion, the alloy element content of which, by mass percentage, is:
[0068] C: 0.07%, Si: 0.30%, Mn: 1.00%, Cr: 0.43%, Cu: 0.25%, Ni: 0.30%, V: 0.032%, N: 0.011%, Ca: 0.0012%, P: 0.0012%, S: 0.003%, O: 0.0037%, and the rest are Fe and unavoidable impurities.
[0069] The smelted and cast steel billet was heated to 1230℃ and then hot rolled. The final rolling temperature was 880℃. After rolling, it was cooled to 600℃ at 10℃ / s and then air-cooled to room temperature to finally obtain the sample with a yield strength of 369MPa, a tensile strength of 514MPa, an elongation of 25%, and an impact energy of 73J at -20℃.
[0070] Compared with Examples 1 to 3, the Mn element content in Comparative Example 2 is increased to 1.00%, and the mechanical properties of the steel in the embodiment are better; and the corrosion rate of Comparative Example 2 after 168 hours of corrosion in the marine atmosphere environment is 1.54 g / m²∙h, which is higher than the corrosion rate of the embodiment, and the corrosion resistance is relatively poor.
[0071] Comparative Example 3
[0072] A hot-rolled H-beam resistant to marine atmospheric corrosion, the alloy element content of which, by mass percentage, is:
[0073] C: 0.09%, Si: 0.18%, Mn: 1.20%, Cr: 0.56%, Cu: 0.22%, Ni: 0.30%, V: 0.040%, N: 0.011%, Ca: 0.0010%, P: 0.015%, S: 0.004%, O: 0.0036%, and the rest are Fe and unavoidable impurities.
[0074] The smelted and cast steel billet was heated to 1230℃ and then hot rolled. The final rolling temperature was 880℃. After rolling, it was cooled to 600℃ at 10℃ / s and then air-cooled to room temperature to finally obtain a sample with a yield strength of 367MPa, a tensile strength of 509MPa, an elongation of 23%, and an impact energy of 68J at -20℃.
[0075] Compared with Comparative Example 2, the Mn element content in Comparative Example 3 is further improved, and the mechanical properties of the steel in the embodiment are better; and the corrosion rate of Comparative Example 3 after 168h of corrosion in the marine atmosphere environment is 1.73g / m²∙h, which is higher than the corrosion rate of the embodiment, and the corrosion resistance is relatively poor.
[0076] Figure 1 This is the metallographic structure of the steel of Example 1 of the present invention. It can be seen that it contains ferrite and a small amount of pearlite structure, wherein the bright polygonal grain structure is ferrite and the black area is pearlite structure. Figure 2The corrosion rate line graph of the six kinds of steel in the embodiments of the present invention and the comparative examples after a 168-hour salt spray corrosion test is shown. It can be seen that the corrosion rates of the embodiments 1, 2, and 3 for the same corrosion time under the marine atmospheric environment corrosion are all lower than the corrosion rate of the comparative example.
[0077] The mechanical properties and corrosion rates of the above-mentioned embodiments and comparative steels are compared as shown in Tables 2 and 3. It can be seen that the mechanical properties of Examples 1, 2, and 3 are better than those of the comparative examples, and the corrosion rates of Examples 1, 2, and 3 under marine atmospheric corrosion are lower than those of the comparative examples, and the corrosion rate of the H-shaped steel provided by the embodiments is much lower than that of Q355B steel, which is equivalent to less than 35% of the corrosion rate of Q355B steel.
[0078] Table 2 Comparison of mechanical properties of different steels
[0079]
[0080] Table 3 Comparison of corrosion rates of different steels after 168h corrosion
[0081]
[0082] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A hot-rolled H-beam resistant to marine atmospheric corrosion and a method for manufacturing the same, characterized in that: The chemical composition of the hot-rolled H-beam in terms of mass ratio is: C: 0.07-0.12%, Si+Mn: 0.80-1.2%, Ni+Cu: 0.30-0.60%, 0.8<Ni / Cu<1.25, Cr: 0.40-0.70%, V: 0.03-0.045%, 2.5≤V / N≤3.5, Ca: 0.001-0.002%, P≤0.020%, S≤0.005%, O≤40ppm, and the rest are Fe and unavoidable impurity elements.
2. The marine atmosphere corrosion resistant hot-rolled H-beam and the manufacturing method thereof according to claim 1, characterized in that: The carbon equivalent CEQ of the hot-rolled H-beam is 0.39-0.45%.
3. The hot-rolled H-beam resistant to marine atmospheric corrosion according to claim 1, characterized in that: Its chemical composition also contains Al<0.03%, Ce≤0.03%, and 0.6≤Ce / (S+O)≤4.
5.
4. The hot-rolled H-beam resistant to marine atmospheric corrosion according to claim 1, characterized in that: The hot-rolled H-shaped steel has a yield strength of 360-420 MPa, a tensile strength of 490-570 MPa, an elongation of >30%, and an impact energy of >120 J at -20°C.
5. The hot-rolled H-beam resistant to marine atmospheric corrosion according to claim 4, characterized in that: In a marine atmosphere environment, the corrosion rate of the H-shaped steel is ≤35%×the corrosion rate of Q355B steel, and the electrode potential of the steel after corrosion is -0.40~-0.53V.
6. The method for manufacturing hot-rolled H-beam resistant to marine atmospheric corrosion according to claim 1, characterized in that: The steel billet melted and cast with the chemical composition as claimed in claim 1 is heated to 1180-1230°C and then hot rolled, with a final rolling temperature of 850-1000°C, cooled to 600-750°C at 2.5-30°C / s after rolling, and then air-cooled to room temperature.
Citation Information
Patent Citations
High-performance hot-rolled H profile steel resisting atmosphere corrosion and preparation method thereof
CN105734406A
High-performance hot-rolled H-shape steel capable of resisting marine atmospheric environment corrosion and preparation method thereof
CN105886961A
Low-temperature-resistant corrosion-resistant H-shaped steel with yield strength of 800 MPa and preparation method thereof
CN109972042A
Easily-welded coating-free 420MPa-grade marine atmosphere corrosion-resistant steel plate and manufacturing method thereof
CN117265411A
Moisture atmospheric environment corrosion resistant cold-rolled weathering resistant steel and manufacturing method thereof
CN118222919A
Cited By
Anti-oxidation and saline-alkaline-tolerant section steel and production process thereof