A paper-based nano-metal material and its preparation method and use

The preparation of paper-based nanometallic materials by composite cellulose paper and nanometal wires solves the problems of insufficient conductivity and insolid nanometal particles, improves the efficiency and stability of catalytic reduction of carbon dioxide, and achieves a long-term catalytic effect.

CN114752958BActive Publication Date: 2024-11-12XIAN JIAOTONG LIVERPOOL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210383764.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-12
Publication Date
2024-11-12
Estimated Expiration
2042-04-12

AI Technical Summary

Technical Problem

The existing nanosilver catalytic materials lack electrical conductivity during the electrochemical reduction of carbon dioxide and the nanometal particles are not firm and easy to fall off, which affects the catalytic efficiency and stability.

Method used

Using composite cellulose paper and nanometal wires, paper-based nanometal materials are prepared by dispersing and drying, improving electrical conductivity and enhancing the stability of the material.

Benefits of technology

The excellent conductivity and stability of paper-based nanometallic materials are achieved, the service life is extended, and the efficiency and selectivity of catalytic reduction of carbon dioxide are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114752958B_ABST
    Figure CN114752958B_ABST
Patent Text Reader

Abstract

The present invention relates to a paper-based nano-metal material and a preparation method and use thereof. The paper-based nano-metal material comprises nano-metal wires and cellulose paper; the nano-metal wires comprise any one of nano-silver wires, nano-copper wires or nano-gold wires or a combination of at least two thereof; the cellulose in the cellulose paper comprises nano-cellulose. The paper-based nano-metal material provided by the present invention is a composite of cellulose and nano-metal wires, has excellent conductive properties, and at the same time, avoids the problem that nano-metal particles are not firm and easy to fall off, improves the stability of the material, and increases the service life of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrocatalysis, and relates to a paper-based nano-metal material, and in particular to a paper-based nano-metal material and a preparation method and application thereof. Background Art

[0002] In recent years, with the continuous use of fossil fuels in modern society, the emission of carbon dioxide has brought many environmental problems, including but not limited to climate change and environmental degradation. At the same time, due to the stability of the structure of carbon dioxide, it is difficult to reduce the carbon dioxide content in the atmosphere. Although the CO2RR method of electrochemical reduction reaction has been discovered and proven, considering the overall energy efficiency, the partial conversion method may not be suitable for widespread promotion.

[0003] CN 107185591A discloses a preparation method and application of a recyclable supported nano-silver catalytic material, and in particular relates to a preparation method of a silver nano-catalyst based on a surface functionalized cellulose paper base and its application in the cyclic catalytic conversion of environmental pollutants. The preparation method of the recyclable cellulose paper-based nano-silver catalytic material uses a cellulose paper-based material as a carrier, uses a silane coupling agent to modify the surface of the carrier with amino groups, and the amino groups on the surface of the modified carrier chelate with metal precursor ions, and then is reduced by an external reducing agent to form a cellulose paper-based nano-silver catalytic material. The cellulose paper-based silver nano-catalytic material prepared by the invention is used as a catalyst for the reduction reaction of 4-nitrophenol to 4-aminophenol, has high catalytic activity, high stability of the carrier and silver nanoparticles, is easy to recover the catalyst, has good reusability, and can maintain a high catalytic activity after continuous recycling for more than 20 times.

[0004] CN 114108026A discloses a carbon-supported thiol-coated silver nanoparticle catalyst and its preparation method and application. The present invention uses thiol molecules as anchoring agents under electrochemical reduction potential to make nano silver particles grow in situ, and the binding force between the generated nano silver and the carbon carrier is stable, thereby improving the structural stability and electron transmission performance of the catalyst. In terms of structure-activity relationship, the nanostructure of silver particles embedded on the carbon carrier is conducive to increasing the surface area of ​​the catalyst, providing abundant catalytic sites for the electrochemical reduction reaction, promoting the adsorption and desorption of the reaction gas, and improving the electrocatalytic activity of the catalyst. Experiments show that the catalyst has a high Faraday efficiency when applied to the electrochemical reduction reaction of carbon dioxide, and the catalyst can selectively convert carbon dioxide into carbon monoxide, reducing the diversity of reaction products. The preparation method of the invention is simple and reliable to operate, low in cost, and the obtained catalyst has good performance.

[0005] The method of reducing carbon dioxide with nanosilver in the above technical solution is a cellulose-loaded nanosilver particle and a carbon paper-based nanosilver particle reduction method, which is limited by the conductivity of carbon paper and silver particles, which makes it difficult to improve the conductivity of the prepared catalytic material. On the other hand, the second method generally uses a drop casting method to fix silver nanoparticles on carbon paper. This method makes the particles attached to the surface of carbon paper unstable and fall off during use, which is not conducive to long-term catalytic experiments. At the same time, the drop casting method is difficult to ensure the uniform distribution of catalytic particles. The aggregation of nanomaterials is likely to destroy the loose and porous three-dimensional structure of the catalytic material, resulting in a reduction in the contact area when the gas passes through, affecting the catalytic efficiency.

[0006] Therefore, how to improve the process of reducing carbon dioxide with nanosilver and invent a nanosilver catalytic material that is simple to operate, cost-effective, can be mass-produced, and has excellent conductivity and stability is an urgent problem to be solved in the field of carbon dioxide catalytic reduction technology. Summary of the invention

[0007] In view of the problems existing in the prior art, the present invention provides a paper-based nano-metal material and a preparation method and use thereof. By fixing nano-metal wires on cellulose paper, the problem of nano-metal particles being loose and easy to fall off is avoided, the stability is improved, the service life of the catalytic material is increased, and at the same time, the conductivity is improved.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a paper-based nanometal material, wherein the paper-based nanometal material comprises nanometal wires and cellulose paper;

[0010] The nanometal wires include any one of nanosilver wires, nanocopper wires or nanogold wires, or a combination of at least two thereof;

[0011] The cellulose in the cellulose paper includes nanocellulose.

[0012] The paper-based nano-metal material provided by the present invention has excellent electrical conductivity by compounding cellulose paper and nano-metal wires, and at the same time avoids the problem that the nano-metal particles are not firm and easy to fall off, thereby improving the stability of the material and increasing the service life of the material.

[0013] Preferably, the mass of the nanometal wire is 0.2 to 2 times that of the cellulose paper, for example, 0.2, 0.5, 1, 1.5, 1.8 or 2 times, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0014] Preferably, the cellulose in the cellulose paper comprises cellulose and / or cellulose derivatives.

[0015] Preferably, the cellulose derivative comprises carboxycellulose.

[0016] Preferably, the thickness of the paper-based nanometal material is 10 μm to 0.1 mm, for example, 10 μm, 20 μm, 50 μm, 80 μm or 0.1 mm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0017] Preferably, the lateral diameter of the nanometal wire is 30 to 150 nm, for example, it can be 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, 70 nm, 80 nm, 100 nm, 120 nm or 150 nm, but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable, preferably 50 to 100 nm.

[0018] In a second aspect, the present invention provides a method for preparing the paper-based nano-metal material according to the first aspect, the preparation method comprising the following steps:

[0019] (1) fragmenting cellulose paper and dispersing the fragments in a solvent to obtain a cellulose paper dispersion;

[0020] (2) dispersing the nanometal wires in a solvent to obtain a nanometal wire dispersion;

[0021] (3) Mixing and dispersing the cellulose paper dispersion obtained in step (1) and the nanometal wire dispersion obtained in step (2), and performing drying and pressing to obtain the paper-based nanometal material.

[0022] The preparation method provided by the invention is simple and quick, and is beneficial for providing a good catalytic material for industrial carbon dioxide capture and catalysis.

[0023] Preferably, the solvent in step (1) comprises water and / or ethanol.

[0024] Preferably, the dispersing method in step (1) includes emulsification dispersion.

[0025] Preferably, the solvent in step (2) comprises ethanol.

[0026] Preferably, the dispersion method in step (2) includes emulsification dispersion.

[0027] Preferably, the dispersion in step (3) includes emulsification dispersion and / or stirring dispersion.

[0028] Preferably, the emulsification dispersion time is 2 to 4 hours, for example, 2 hours, 2.5 hours, 3 hours, 3.5 hours or 4 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0029] Preferably, the stirring and dispersing time is 10 to 14 hours, for example, 10 hours, 10.5 hours, 11 hours, 12 hours, 13 hours or 14 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0030] Preferably, the drying in step (3) comprises vacuum drying.

[0031] Preferably, the drying time in step (3) is more than 12 hours, for example, it can be 12 hours, 14 hours, 16 hours, 17 hours, 18 hours or 20 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0032] Preferably, the drying temperature in step (3) is 30-40°C, for example, 30°C, 32°C, 34°C, 36°C, 38°C or 40°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0033] Preferably, the nanometal wires in step (2) include any one of nanosilver wires, nanocopper wires or nanogold wires, or a combination of at least two of them.

[0034] As a preferred technical solution, the present invention provides a method for preparing nano silver wires, the preparation method comprising:

[0035] (a) mixing a silver salt and a capping agent in a solvent to obtain a silver salt solution;

[0036] (b) mixing the impurity-removing agent in a solvent and heating to obtain an impurity-removing solution;

[0037] (c) mixing and heating the silver salt solution obtained in step (a) and the impurity removal solution obtained in step (b), and washing by centrifugation to obtain the nano silver wire.

[0038] Preferably, the end-capping agent in step (a) comprises polyvinyl pyrrolidone.

[0039] Preferably, the solvent in step (a) comprises ethylene glycol.

[0040] Preferably, in the silver salt solution of step (a), the concentration of silver salt is 0.005-0.02 g / mL, for example, 0.005 g / mL, 0.008 g / mL, 0.01 g / mL, 0.15 g / mL or 0.02 g / mL, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0041] Preferably, in the silver salt solution of step (a), the concentration of the capping agent is 0.01 to 0.04 g / mL, for example, 0.01 g / mL, 0.015 g / mL, 0.02 g / mL, 0.03 g / mL or 0.04 g / mL, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0042] Preferably, the impurity remover in step (b) comprises copper salt and / or iron salt.

[0043] Preferably, the solvent in step (b) comprises ethylene glycol.

[0044] Preferably, the volume ratio of the silver salt solution obtained in step (a) to the impurity removal solution obtained in step (b) is (1-1.5):1, for example, it can be 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1 or 1.5:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] Preferably, the heating temperature in step (c) is 140-160°C, for example, 140°C, 145°C, 150°C, 155°C or 160°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0046] Preferably, the heating time in step (c) is 30 to 120 min, for example, 30 min, 50 min, 70 min, 90 min, 110 min or 120 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0047] Exemplarily, the present invention provides a method for preparing nano copper wires, the preparation method comprising the following steps:

[0048] Copper chloride, anhydrous glucose, hydroxylamine solution and deionized water were mixed, stirred evenly, and heated in an oil bath at 120° C. for 3 hours to obtain the nano copper wire.

[0049] As a preferred technical solution of the preparation method described in the second aspect of the present invention, the preparation method comprises the following steps:

[0050] (1) After cellulose paper is fragmented, it is emulsified and dispersed in a solvent to obtain a cellulose paper dispersion; the solvent includes water and / or ethanol;

[0051] (2) emulsifying and dispersing the nanometal wires in ethanol to obtain a nanometal wire dispersion;

[0052] (3) Mixing the cellulose paper dispersion obtained in step (1) and the nanometal wire dispersion obtained in step (2), emulsifying and dispersing for 2 to 4 hours, stirring and dispersing for 10 to 14 hours, and vacuum drying at a temperature of 30 to 40° C. for more than 12 hours to obtain the paper-based nanometal material.

[0053] In a third aspect, the present invention provides a use of the paper-based nano-metal material according to the first aspect, wherein the paper-based nano-metal material is used for catalytic reduction of carbon dioxide.

[0054] According to the above technical scheme, the beneficial effects of the present invention are as follows:

[0055] (1) The paper-based nano-metal material provided by the present invention has excellent conductive properties by composite cellulose paper and nano-metal wires. At the same time, it avoids the problem that the nano-metal particles are not firm and easy to fall off, thereby improving the stability of the material and increasing the service life of the material.

[0056] (2) The preparation method provided by the present invention is simple and quick, which is conducive to providing a good catalytic material for industrial carbon dioxide capture and catalysis. The material can not only convert carbon dioxide gas into fuel, but also create a storage for unstable and intermittent renewable energy. By using renewable energy, these conversion technologies are expected to recycle carbon dioxide, improve the modern human carbon cycle, and permanently stabilize the carbon dioxide content in the atmosphere. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 3 is a scanning electron microscope image of the silver nanowire described in Example 1 of the present invention. DETAILED DESCRIPTION

[0058] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0059] Example 1

[0060] The invention provides a paper-based nano-metal material, which comprises nano-silver wires and cellulose paper. In terms of mass percentage, the mass of the nano-silver wires is 1 times the mass of the cellulose paper. The thickness of the paper-based nano-metal material is 50 μm.

[0061] The preparation method of the paper-based nano-metal material comprises the following steps:

[0062] (1) Nanocellulose paper (Whatman No. 1) is fragmented and then emulsified and dispersed in ethanol to obtain a cellulose paper dispersion;

[0063] (2) emulsifying and dispersing the nanosilver wires in ethanol to obtain a nanometal wire dispersion;

[0064] (3) Mixing the cellulose paper dispersion obtained in step (1) and the nanometal wire dispersion obtained in step (2), emulsifying and dispersing for 3 hours, stirring and dispersing for 12 hours, and vacuum drying at 35° C. for 13 hours to obtain the paper-based nanometal material.

[0065] The lateral diameter of the silver nanowire is 40 nm, and the scanning electron microscope image is as follows Figure 1 shown.

[0066] The preparation method of the nano silver wire is as follows:

[0067] (a) mixing silver nitrate and polyvinyl pyrrolidone (molecular weight of 58000) in ethylene glycol to obtain a silver salt solution; in the silver salt solution, the concentration of the silver salt is 0.01 g / mL, and the concentration of the polyvinyl pyrrolidone is 0.02 g / mL;

[0068] (b) mixing cupric chloride with ethylene glycol and heating at 160° C. to obtain a decontamination solution, wherein the concentration of cupric chloride in the decontamination solution is 0.6 mM;

[0069] (c) mixing and heating the silver salt solution obtained in step (a) and the impurity removal solution obtained in step (b) at a volume ratio of 1.2:1 at a heating temperature of 160° C. for 90 min, and centrifuging and washing to obtain the nano silver wire.

[0070] Example 2

[0071] The invention provides a paper-based nano-metal material, which comprises nano-silver wire and bacterial cellulose paper. The mass of the nano-silver wire is 0.2 times the mass of the bacterial cellulose paper. The thickness of the paper-based nano-metal material is 10 μm.

[0072] The preparation method of the paper-based nano-metal material comprises the following steps:

[0073] (1) fragmenting the carboxycellulose paper, emulsifying and dispersing the fragments in ethanol to obtain a cellulose paper dispersion;

[0074] (2) emulsifying and dispersing the nanosilver wires in ethanol to obtain a nanometal wire dispersion;

[0075] (3) Mixing the cellulose paper dispersion obtained in step (1) and the nanometal wire dispersion obtained in step (2), emulsifying and dispersing for 2 hours, stirring and dispersing for 14 hours, and vacuum drying at 30° C. for 20 hours to obtain the paper-based nanometal material.

[0076] The lateral diameter of the silver nanowire is 30 nm, and the preparation method is as follows:

[0077] (a) mixing silver nitrate and polyvinyl pyrrolidone (molecular weight 59000) in ethylene glycol to obtain a silver salt solution; in the silver salt solution, the concentration of the silver salt is 0.005 g / mL, and the concentration of the polyvinyl pyrrolidone is 0.01 g / mL;

[0078] (b) mixing cupric chloride with ethylene glycol and heating at 160° C. to obtain a decontamination solution, wherein the concentration of cupric chloride in the decontamination solution is 0.4 mM;

[0079] (c) mixing and heating the silver salt solution obtained in step (a) and the impurity removal solution obtained in step (b) in a volume ratio of 1:1 at a heating temperature of 140° C. for 120 min, and centrifuging and washing to obtain the nano silver wire.

[0080] Example 3

[0081] The invention provides a paper-based nano-metal material, which comprises nano-silver wires and carboxyl cellulose paper. The mass of the nano-silver wires is twice that of the carboxyl cellulose paper. The thickness of the paper-based nano-metal material is 0.1 mm.

[0082] The preparation method of the paper-based nano-metal material comprises the following steps:

[0083] (1) After the nanocellulose paper is fragmented, it is emulsified and dispersed in ethanol to obtain a cellulose dispersion;

[0084] (2) emulsifying and dispersing the nanosilver wires in ethanol to obtain a nanometal wire dispersion;

[0085] (3) Mixing the cellulose paper dispersion obtained in step (1) and the nanometal wire dispersion obtained in step (2), emulsifying and dispersing for 4 hours, stirring and dispersing for 10 hours, and vacuum drying at 40° C. for 12 hours to obtain the paper-based nanometal material.

[0086] The lateral diameter of the silver nanowire is 50 nm, and the preparation method is as follows:

[0087] (a) mixing silver nitrate and polyvinyl pyrrolidone (molecular weight of 57000) in ethylene glycol to obtain a silver salt solution; in the silver salt solution, the concentration of the silver salt is 0.02 g / mL, and the concentration of the polyvinyl pyrrolidone is 0.04 g / mL;

[0088] (b) mixing cupric chloride with ethylene glycol and heating at 150° C. to obtain a decontamination solution, wherein the concentration of cupric chloride in the decontamination solution is 0.8 mM;

[0089] (c) mixing and heating the silver salt solution obtained in step (a) and the impurity removal solution obtained in step (b) at a volume ratio of 1.5:1 at a heating temperature of 150° C. for 30 min, and centrifuging and washing to obtain the nano silver wire.

[0090] Example 4

[0091] The invention provides a paper-based nano-metal material, which comprises nano-copper wires and bacterial cellulose paper. The mass of the nano-copper wires is 1 times the mass of the bacterial cellulose paper. The thickness of the paper-based nano-metal material is 50 μm.

[0092] The preparation method of the paper-based nano-metal material comprises the following steps:

[0093] (1) fragmenting the carboxycellulose paper, emulsifying and dispersing the fragments in ethanol to obtain a cellulose paper dispersion;

[0094] (2) emulsifying and dispersing the nano copper wires in ethanol to obtain a nano metal wire dispersion;

[0095] (3) Mixing the cellulose paper dispersion obtained in step (1) and the nanometal wire dispersion obtained in step (2), emulsifying and dispersing for 3 hours, stirring and dispersing for 12 hours, and vacuum drying at 35° C. for 13 hours to obtain the paper-based nanometal material.

[0096] Example 5

[0097] The invention provides a paper-based nano-metal material, which comprises nano-gold wires and bacterial cellulose paper. The mass of the nano-copper wires is 1 times the mass of the bacterial cellulose paper. The thickness of the paper-based nano-metal material is 50 μm.

[0098] The preparation method of the paper-based nano-metal material comprises the following steps:

[0099] (1) After cellulose paper is fragmented, it is emulsified and dispersed in ethanol to obtain a cellulose paper dispersion;

[0100] (2) emulsifying and dispersing the gold nanowires in ethanol to obtain a nanometal wire dispersion;

[0101] (3) Mixing the cellulose paper dispersion obtained in step (1) and the nanometal wire dispersion obtained in step (2), emulsifying and dispersing for 3 hours, stirring and dispersing for 12 hours, and vacuum drying at 35° C. for 13 hours to obtain the paper-based nanometal material.

[0102] Example 6

[0103] This embodiment provides a paper-based nano-metal material, which is the same as that of Embodiment 1 except that the mass of the nano-silver wire is 0.1 times the mass of the cellulose paper.

[0104] Example 7

[0105] This embodiment provides a paper-based nanometal material, which is the same as that of Embodiment 1 except that the mass of the nanosilver wire is 2.5 times that of the cellulose paper.

[0106] Example 8

[0107] This embodiment provides a paper-based nanometal material, which is the same as that of Embodiment 1 except that the transverse diameter of the nanosilver wire is 100 nm.

[0108] Example 9

[0109] This embodiment provides a paper-based nanometal material, which is the same as that of Embodiment 1 except that the transverse diameter of the nanosilver wire is 150 nm.

[0110] Comparative Example 1

[0111] This comparative example provides a paper-based nano-metal material, which is prepared according to the method provided in CN107185591A.

[0112] Comparative Example 2

[0113] This comparative example provides a nanometal wire material, wherein the lateral diameter of the nanosilver wire is 40 nm.

[0114] The preparation method of the nano silver wire is as follows:

[0115] (a) mixing silver nitrate and polyvinyl pyrrolidone (molecular weight of 58000) in ethylene glycol to obtain a silver salt solution; in the silver salt solution, the concentration of the silver salt is 0.01 g / mL, and the concentration of the polyvinyl pyrrolidone is 0.02 g / mL;

[0116] (b) mixing cupric chloride with ethylene glycol and heating at 160° C. to obtain a decontamination solution, wherein the concentration of cupric chloride in the decontamination solution is 0.6 mM;

[0117] (c) mixing and heating the silver salt solution obtained in step (a) and the impurity removal solution obtained in step (b) at a heating temperature of 160° C. for a heating time of 90 min, and centrifuging and washing to obtain the nano silver wire.

[0118] Comparative Example 3

[0119] This comparative example provides a paper-based material, wherein the paper-based material is cellulose paper.

[0120] The above materials were used in electrochemical experiments in a gas-tight H-type cell with a standard three-electrode system. 2) will be used as the working electrode. A saturated calomel reference electrode (SCE) will be placed in the cathode region with the working electrode. The counter electrode (graphite) will be in the anode compartment. A proton exchange membrane (Nafion-117) is used to separate the anode and cathode regions. The two compartments will be filled with 25 mL of pre-saturated KHCO3 and CO2. CO2 is passed near the working electrode at a flow rate of 20 sccm. The outlet of the electrode is connected to the GC. The correct voltage is selected using LSV, and the resistance of the nanowire material is tested to represent its conductivity. The CO generated by the reaction is detected by CO (area external standard method). The reaction time represents the stability of the nanowire material. The CO selectivity of the reaction is calculated by the Faraday efficiency.

[0121] Table 1

[0122] Test No. Electrical conductivity stability <![CDATA[Catalytic reduction effect of CO2]]> Example 1 <![CDATA[9.3mΩ.cm 2 ]]> 100h 92.6% Example 2 <![CDATA[6mΩ.cm 2 ]]> 26h 93.8% Example 3 <![CDATA[8mΩ.cm 2 ]]> 50h 97.1% Example 4 <![CDATA[5.9mΩ.cm 2 ]]> 5h 76% Example 5 <![CDATA[11.3mΩ.cm 2 ]]> 7h 90% Example 6 <![CDATA[11.4mΩ.cm 2 ]]> 65h 87% Example 7 <![CDATA[8.1mΩ.cm 2 ]]> 4h 77.1% Example 8 <![CDATA[8.2mΩ.cm 2 ]]> 34h 77.6% Example 9 <![CDATA[7.9mΩ.cm 2 ]]> 32h 64% Comparative Example 1 <![CDATA[6.2mΩ.cm 2 ]]> 12h 22% Comparative Example 2 <![CDATA[8.9mΩ.cm 2 ]]> 18h 21% Comparative Example 3 <![CDATA[10.0MΩ.cm 2 ]]> --- 0.3%

[0123] From the data in Table 1, we can draw the following conclusions:

[0124] (1) It can be seen from Examples 1-5 that the paper-based nano-metal material provided by the present invention has excellent conductive properties by composite cellulose paper and nano-metal wires. At the same time, it avoids the problem that the nano-metal particles are not firm and easy to fall off, thereby improving the stability of the material and increasing the service life of the material.

[0125] (2) Comparison of Examples 6 and 7 with Example 1 shows that when the mass ratio of nanometal wires to cellulose paper is not within the preferred range provided by the invention, the conductivity of the paper-based nanometal material is poor, the stability is low and the catalytic reduction effect is unsatisfactory.

[0126] (3) Comparison of Examples 8 and 9 with Example 1 shows that when the transverse diameter of the nanometal wire is not within the preferred range provided by the present invention, the conductivity of the paper-based nanometal material is poor, the stability is low and the catalytic reduction effect is not ideal.

[0127] (4) From the comparison between Comparative Example 1 and Example 1, it can be seen that when nano-metal particles are composited on cellulose paper, the conductivity of the paper-based nano-metal material is poor, the stability is low and the catalytic reduction effect is not ideal.

[0128] (5) From the comparison between Comparative Examples 2 and 3 and Example 1, it can be seen that when the cellulose paper and the nano-metal wires are not composited, the conductivity is poor, the stability is low and the catalytic reduction effect is not ideal.

[0129] In summary, the paper-based nano-metal material provided by the present invention has excellent conductive properties by composite cellulose paper and nano-metal wires. At the same time, it avoids the problem that the nano-metal particles are not firm and easy to fall off, improves the stability of the material, and increases the service life of the material.

[0130] The present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a paper-based nano-metal material for catalytic reduction of carbon dioxide, characterized in that: The preparation method comprises the following steps: (1) After cellulose paper is fragmented, it is dispersed in a solvent to obtain a cellulose paper dispersion; the dispersion method in step (1) includes emulsification dispersion; (2) dispersing the nanometal wires in a solvent to obtain a nanometal wire dispersion; the dispersion method in step (2) includes emulsification dispersion; (3) mixing and dispersing the cellulose paper dispersion obtained in step (1) and the nanometal wire dispersion obtained in step (2), and drying and pressing to obtain the paper-based nanometal material; The paper-based nanometal material comprises nanometal wires and cellulose paper; The nanometal wires include any one of nanosilver wires, nanocopper wires or nanogold wires, or a combination of at least two thereof; The cellulose in the cellulose paper includes nanocellulose; The mass of the nano metal wire is 0.2 to 2 times that of the cellulose paper; The thickness of the paper-based nano-metal material is 10 μm to 0.1 mm; The transverse diameter of the nano metal wire is 30-150 nm.

2. The preparation method according to claim 1, characterized in that: The cellulose in the cellulose paper includes cellulose and / or cellulose derivatives.

3. The preparation method according to claim 2, characterized in that: The cellulose derivatives include carboxycellulose.

4. The preparation method according to claim 1, characterized in that: The transverse diameter of the nano metal wire is 50-100 nm.

5. The preparation method according to claim 1, characterized in that: The solvent in step (1) includes water and / or ethanol.

6. The preparation method according to claim 1, characterized in that: The solvent in step (2) includes ethanol.

7. The preparation method according to claim 1, characterized in that: The dispersion in step (3) includes emulsification dispersion and / or stirring dispersion.

8. The preparation method according to claim 7, characterized in that: The emulsification and dispersion time in step (3) is 2 to 4 hours.

9. The preparation method according to claim 7, characterized in that: The stirring and dispersing time is 10 to 14 hours.

10. The preparation method according to claim 1, characterized in that: The drying in step (3) includes vacuum drying.

11. The preparation method according to claim 1, characterized in that: The drying time in step (3) is more than 12 hours.

12. The preparation method according to claim 1, characterized in that: The drying temperature in step (3) is 30-40°C.

13. The preparation method according to claim 1, characterized in that: The preparation method of the nano silver wire comprises: (a) mixing a silver salt and a capping agent in a solvent to obtain a silver salt solution; (b) mixing the impurity-removing agent in a solvent and heating to obtain an impurity-removing solution; (c) mixing and heating the silver salt solution obtained in step (a) and the impurity removal solution obtained in step (b), and washing by centrifugation to obtain the nano silver wire.

14. The preparation method according to claim 13, characterized in that: The end-capping agent in step (a) includes polyvinyl pyrrolidone.

15. The preparation method according to claim 13, characterized in that: In the silver salt solution of step (a), the concentration of silver salt is 0.005-0.02 g / mL.

16. The preparation method according to claim 13, characterized in that: In the silver salt solution of step (a), the concentration of the capping agent is 0.01 to 0.04 g / mL.

17. The preparation method according to claim 13, characterized in that: The impurity remover in step (b) comprises copper salt and / or iron salt.

18. The preparation method according to claim 13, characterized in that: The volume ratio of the silver salt solution obtained in step (a) to the impurity removal solution obtained in step (b) is (1-1.5):

1.

19. The preparation method according to claim 13, characterized in that: The heating temperature in step (c) is 140-160°C.

20. The preparation method according to claim 13, characterized in that: The heating time in step (c) is 30 to 120 minutes.

21. The preparation method according to claim 1, characterized in that: The preparation method comprises the following steps: (1) After cellulose paper is fragmented, it is emulsified and dispersed in a solvent to obtain a cellulose paper dispersion; the solvent includes water and / or ethanol; (2) emulsifying and dispersing the nanometal wires in ethanol to obtain a nanometal wire dispersion; (3) Mixing the cellulose paper dispersion obtained in step (1) and the nanometal wire dispersion obtained in step (2), emulsifying and dispersing for 2 to 4 hours, stirring and dispersing for 10 to 14 hours, and vacuum drying at a temperature of 30 to 40° C. for more than 12 hours to obtain the paper-based nanometal material.

22. Use of the paper-based nano-metal material prepared by the preparation method according to any one of claims 1 to 21, characterized in that: The paper-based nano metal material is used for catalytic reduction of carbon dioxide.