A method for dissolving TaAl alloy
A method using a nitric acid-hydrofluoric acid combination with controlled heating parameters effectively dissolves TaAl alloy for ICP-OES analysis, addressing the lack of suitable dissolution methods and enabling accurate aluminum content determination.
Patent Information
- Application Number
- CN202210379044.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-12
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-04-12
AI Technical Summary
There is no effective method for dissolving TaAl alloy to prepare a sample solution suitable for inductively coupled plasma optical emission spectrometer (ICP-OES) analysis, as existing acid solutions are inadequate for complete dissolution.
A method involving a specific ratio of nitric acid to hydrofluoric acid and controlled heating parameters is used to completely dissolve TaAl alloy, forming a sample solution suitable for ICP-OES analysis.
The method ensures complete dissolution of TaAl alloy, enabling accurate determination of aluminum content using ICP-OES, thereby meeting the requirements for high-precision resistor manufacturing.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of analytical chemistry, and in particular to a dissolution method of a TaAl alloy. Background Art
[0002] TaAl alloy thin film materials play an important role in thin film integrated circuits. When the atomic ratio of Ta and Al in TaAl alloy thin film is constant, it has good stability; TaAl alloy thin film can easily form a dense oxide passivation film on the film surface through anodization, and has excellent stability in thermal aging or power aging, and can be used to manufacture high-precision, high-stability power resistors or power-type integrated resistor networks.
[0003] CN 104157632A discloses a BGA substrate multilayer interconnection structure and method based on selective aluminum anodization. The selective aluminum anodization process is used to manufacture an upper aluminum film multilayer interconnection structure and a lower aluminum substrate perforated metallization structure. Several conductive bands in a tantalum aluminum alloy film of the upper aluminum film multilayer interconnection structure are electrically connected to several conductive bands in the aluminum film respectively; two adjacent groups of tantalum aluminum alloy films are electrically connected to several conductive bands on the connecting surface of the aluminum film structure respectively; several conductive bands of the tantalum aluminum alloy film deposited on the lower aluminum substrate perforated metallization structure are electrically connected to the upper ends of several aluminum through-pillars respectively, thereby simplifying the manufacturing process of the BGA substrate, reducing the cost of the BGA substrate, and improving the stability of the interconnection structure.
[0004] CN 1997519A discloses a semiconductor substrate for a microfluid nozzle, the substrate includes a fluid injection actuator, each fluid injection actuator includes a thin film heating element and an adjacent protective layer. The thin film heating element is composed of a tantalum aluminum nitride thin film material with a nanocrystalline structure, the material mainly consists of AlN, TaN and TaAl alloy, the thin film material has a thin film resistance ranging from about 30 to 100 ohms per square, and contains about 30 to 70 atomic percent of tantalum, 10 to 40 atomic percent of aluminum and 5 to 30 atomic percent of nitrogen.
[0005] The Al content in TaAl alloy thin film is crucial for designing and manufacturing high-precision and high-stability thin film resistors. Therefore, it is necessary to accurately determine the Al content in TaAl alloy. At present, inductively coupled plasma optical emission spectrometer (ICP-OES) is generally used to detect the composition of metal materials. ICP-OES has the advantages of less interference, stable signal, simple operation, etc., and can detect most metal elements and some non-metal elements.
[0006] Before using ICP-OES for component determination, the metal material to be tested needs to be dissolved in acid solution, and then diluted to a fixed volume to obtain a sample solution for testing. Ta in TaAl alloy can be quickly dissolved in a mixed acid of hydrofluoric acid and nitric acid, and can also be dissolved in hydrofluoric acid; Al is easily dissolved by dilute sulfuric acid, nitric acid and hydrochloric acid. However, there is currently only an acid solution dissolution method for a single metal, and there is no method for dissolving TaAl alloys.
[0007] In view of the shortcomings of the prior art, it is necessary to provide a method for effectively dissolving TaAl alloy, so as to prepare a test sample that can be used for ICP-OES. Summary of the invention
[0008] The object of the present invention is to provide a method for dissolving a TaAl alloy, by adjusting a reasonable ratio of nitric acid to hydrofluoric acid and heating parameters, the TaAl alloy is completely dissolved, so that a sample solution suitable for ICP-OES can be prepared.
[0009] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0010] The present invention provides a TaAl alloy dissolution method, the dissolution method comprising the following steps:
[0011] (1) uniformly mixing the TaAl alloy and the composite acid solution to obtain a mixed solution;
[0012] (2) The mixed solution obtained in step (1) is heated and constant in volume to obtain a sample solution.
[0013] The TaAl alloy dissolution method provided by the present invention determines a composite solution of nitric acid and hydrofluoric acid as a dissolving solution in combination with the solubility degree of each element in the TaAl alloy in acid, adjusts a reasonable ratio, and controls heating parameters so that the TaAl alloy can be completely dissolved and can meet the requirements of being used as an ICP-OES sample solution.
[0014] The composite acid solution in step (1) is nitric acid and hydrofluoric acid in a volume ratio of 1:(5-7), for example, 1:5, 1:5.5, 1:6, 1:6.5 or 1:7, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0015] The ratio of nitric acid to hydrofluoric acid used in the present invention can effectively compound and dissolve TaAl alloy. If the volume ratio is too high or too low, the TaAl alloy cannot be completely dissolved and cannot meet the requirements of being used as a sample solution.
[0016] Preferably, the ratio between the mass of the TaAl alloy in step (1) and the volume of the composite acid solution is 1g:(60-80)mL, for example, it can be 1g:60mL, 1g:65mL, 1g:70mL, 1g:75mL or 1g:80mL, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0017] Preferably, the concentration of the nitric acid is 65-68wt%, for example, 65wt%, 66wt%, 67wt% or 68wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0018] Preferably, the concentration of the hydrofluoric acid is 38-42wt%, for example, 38wt%, 39wt%, 40wt%, 41wt% or 42wt%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0019] Preferably, the atomic percentage of Al in the TaAl alloy in step (1) is 49.9-50.1 at%, for example, it can be 49.9 at%, 49.95 at%, 50 at%, 50.05 at% or 50.1 at%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0020] Preferably, the mixing temperature in step (1) is 20-25°C, for example, 20°C, 21°C, 22°C, 23°C, 24°C or 25°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] Preferably, the heating temperature in step (2) is 90-110°C, for example, 90°C, 95°C, 100°C, 105°C or 110°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0022] The TaAl alloy is mixed with the composite acid solution under heating conditions. If the heating temperature is too low, the dissolution degree of the TaAl alloy is small and the TaAl alloy cannot be used as a sample solution for testing.
[0023] Preferably, the heating time in step (2) is 50-70 min, for example, 50 min, 55 min, 60 min, 65 min or 70 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0024] The TaAl alloy is mixed with the composite acid solution under heating conditions. If the heating time is too short, the TaAl alloy may not be completely dissolved. Therefore, the heating time needs to be strictly controlled.
[0025] Preferably, the heating in step (2) is carried out in a graphite heater.
[0026] Preferably, the step (2) includes an acid removal treatment before the volume fixation, and the acid removal can remove nitric acid and hydrofluoric acid as much as possible to avoid interference in the subsequent measurement process.
[0027] As a preferred technical solution of the dissolution method of the present invention, the dissolution method comprises the following steps:
[0028] (1) uniformly mixing the TaAl alloy and the composite acid solution at 20-25° C. to obtain a mixed solution;
[0029] The composite acid solution is nitric acid and hydrofluoric acid in a volume ratio of 1:(5-7); the ratio between the mass of the TaAl alloy and the volume of the composite acid solution is 1g:(60-80)mL; the concentration of the nitric acid is 65-68wt%; the concentration of the hydrofluoric acid is 38-42wt%; the atomic percentage of Al in the TaAl alloy is 49.9-50.1at%;
[0030] (2) The mixed solution obtained in step (1) is heated at 90-110° C. for 50-70 min, acid removed and constant volume is obtained to obtain a sample solution.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] The present invention provides a TaAl alloy dissolution method. Combining the dissolution characteristics of each element in the TaAl alloy in acid, a nitric acid and a hydrofluoric acid compound are determined as a dissolving solution. By adjusting the ratio of the two acids, controlling the heating temperature and time, the TaAl alloy can be completely dissolved, and the requirements for being used as an ICP-OES sample solution can be met. DETAILED DESCRIPTION
[0033] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0034] Example 1
[0035] This embodiment provides a TaAl alloy dissolution method, the dissolution method comprising the following steps:
[0036] (1) uniformly mixing the TaAl alloy and the composite acid solution at 23° C. to obtain a mixed solution;
[0037] The composite acid solution is nitric acid and hydrofluoric acid in a volume ratio of 1:6; the ratio between the mass of the TaAl alloy and the volume of the composite acid solution is 1g:70mL; the concentration of the nitric acid is 67wt%; the concentration of the hydrofluoric acid is 40wt%; the atomic percentage of Al in the TaAl alloy is 50at%;
[0038] (2) The mixed solution obtained in step (1) was heated at 100° C. for 60 min, acid removed and constant volume was obtained to obtain a sample solution.
[0039] In this embodiment, the TaAl alloy is completely dissolved in the composite acid solution. The obtained sample solution can be used for ICP-OES, and the Al content is determined to be 12.98%.
[0040] Example 2
[0041] This embodiment provides a TaAl alloy dissolution method, the dissolution method comprising the following steps:
[0042] (1) uniformly mixing the TaAl alloy and the composite acid solution at 20° C. to obtain a mixed solution;
[0043] The composite acid solution is nitric acid and hydrofluoric acid in a volume ratio of 1:5; the ratio between the mass of the TaAl alloy and the volume of the composite acid solution is 1g:60mL; the concentration of the nitric acid is 65wt%; the concentration of the hydrofluoric acid is 38wt%; the atomic percentage of Al in the TaAl alloy is 49.9at%;
[0044] (2) The mixed solution obtained in step (1) was heated at 90° C. for 50 min, acid removed and constant volume was obtained to obtain a sample solution.
[0045] In this embodiment, the TaAl alloy is completely dissolved in the composite acid solution. The obtained sample solution can be used for ICP-OES, and the Al content is determined to be 12.94%.
[0046] Example 3
[0047] This embodiment provides a TaAl alloy dissolution method, the dissolution method comprising the following steps:
[0048] (1) uniformly mixing the TaAl alloy and the composite acid solution at 25° C. to obtain a mixed solution;
[0049] The composite acid solution is nitric acid and hydrofluoric acid in a volume ratio of 1:7; the ratio between the mass of the TaAl alloy and the volume of the composite acid solution is 1g:80mL; the concentration of the nitric acid is 68wt%; the concentration of the hydrofluoric acid is 42wt%; the atomic percentage of Al in the TaAl alloy is 50.1at%;
[0050] (2) The mixed solution obtained in step (1) was heated at 110° C. for 70 min, acid removed and constant volume was obtained to obtain a sample solution.
[0051] In this embodiment, the TaAl alloy is completely dissolved in the composite acid solution. The obtained sample solution can be used for ICP-OES, and the Al content is determined to be 13.03%.
[0052] Example 4
[0053] This embodiment provides a method for dissolving a TaAl alloy, which is different from Embodiment 1 in that, except for the heating temperature being 50° C., the rest is the same as Embodiment 1.
[0054] In this embodiment, since the heating temperature is too low, the TaAl alloy cannot be completely dissolved in the composite acid solution within 60 minutes, and the obtained sample solution cannot be used for ICP-OES determination of Al content.
[0055] Example 5
[0056] This embodiment provides a method for dissolving a TaAl alloy, which is different from Embodiment 1 in that, except for the heating time being 30 minutes, the rest is the same as Embodiment 1.
[0057] In this embodiment, since the heating time is too short, the TaAl alloy cannot be completely dissolved in the composite acid solution within 30 minutes, and the obtained sample solution cannot be used for ICP-OES determination of Al content.
[0058] Comparative Example 1
[0059] This comparative example provides a method for dissolving a TaAl alloy, which is different from Example 1 in that, except that the composite acid solution is nitric acid and hydrofluoric acid in a volume ratio of 1:3, the rest is the same as Example 1.
[0060] In this comparative example, since the proportion of hydrofluoric acid in the composite acid solution is too low, the TaAl alloy cannot be completely dissolved in the composite acid solution within 60 minutes, and the obtained sample solution cannot be used for ICP-OES determination of Al content.
[0061] Comparative Example 2
[0062] This comparative example provides a method for dissolving a TaAl alloy, which is different from Example 1 in that, except that the composite acid solution is nitric acid and hydrofluoric acid in a volume ratio of 1:8, the rest is the same as Example 1.
[0063] In this comparative example, since the proportion of hydrofluoric acid in the composite acid solution is too high, the TaAl alloy cannot be completely dissolved in the composite acid solution, and the obtained sample solution cannot be used for ICP-OES determination of Al content.
[0064] Comparative Example 3
[0065] This comparative example provides a method for dissolving a TaAl alloy, which is different from Example 1 in that, except that the composite acid solution is nitric acid and hydrochloric acid in a volume ratio of 1:3, the concentration of the nitric acid is 68wt%, and the concentration of the hydrochloric acid is 38wt%, the rest is the same as Example 1.
[0066] Since Ta in TaAl alloy has extremely high corrosion resistance and does not react with aqua regia, TaAl alloy cannot be dissolved in aqua regia, and the obtained sample solution cannot be used for ICP-OES determination of Al content.
[0067] Comparative Example 4
[0068] This comparative example provides a method for dissolving a TaAl alloy, which differs from Example 1 in that there is no heating procedure in step (2), and the rest is the same as Example 1.
[0069] In this comparative example, since the mixed solution was not heated, the TaAl alloy could not be dissolved in the composite acid solution, and the obtained sample solution could not be used for ICP-OES determination of Al content.
[0070] In summary, the present invention provides a method for dissolving a TaAl alloy. Combined with the dissolution characteristics of each element in the TaAl alloy in acid, a composite of nitric acid and hydrofluoric acid is determined as a dissolving solution. By adjusting the ratio of the two acids and controlling the heating temperature and time, the TaAl alloy can be completely dissolved, which can meet the requirements of being used as an ICP-OES sample solution.
[0071] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for dissolving a TaAl alloy, characterized in that: The dissolution method comprises the following steps: (1) uniformly mixing the TaAl alloy and the composite acid solution to obtain a mixed solution; (2) The mixed solution obtained in step (1) is heated and constant in volume to obtain a sample solution; The atomic percentage of Al in the TaAl alloy in step (1) is 49.9-50.1 at %; the composite acid solution in step (1) is nitric acid and hydrofluoric acid in a volume ratio of 1:(5-7); The heating temperature in step (2) is 90-110° C. and the heating time is 50-70 min. The ratio between the mass of the TaAl alloy and the volume of the composite acid solution in step (1) is 1 g: (60-80) mL; The concentration of the nitric acid is 65-68 wt %, and the concentration of the hydrofluoric acid is 38-42 wt %.
2. The dissolution method according to claim 1, characterized in that The mixing temperature in step (1) is 20-25°C.
3. The dissolution method according to claim 1, characterized in that: The heating in step (2) is carried out in a graphite heater.
4. The dissolution method according to claim 1, characterized in that: The step (2) includes acid removal treatment before volume determination.
5. The dissolution method according to any one of claims 1 to 4, characterized in that: The dissolution method comprises the following steps: (1) uniformly mixing the TaAl alloy and the composite acid solution at 20-25° C. to obtain a mixed solution; The composite acid solution is nitric acid and hydrofluoric acid in a volume ratio of 1:(5-7); the ratio between the mass of the TaAl alloy and the volume of the composite acid solution is 1g:(60-80)mL; the concentration of the nitric acid is 65-68wt%; the concentration of the hydrofluoric acid is 38-42wt%; the atomic percentage of Al in the TaAl alloy is 49.9-50.1at%; (2) The mixed solution obtained in step (1) is heated at 90-110° C. for 50-70 min, acid removed and constant volume to obtain a sample solution.
Citation Information
Patent Citations
Ball grid array (BGA) substrate multilayer interconnection structure based on selective aluminum anodizing, and BGA substrate multilayer interconnection method based on selective aluminum anodizing
CN104157632A
Micro-fluid ejection device having high resistance heater film
CN1997519A
Method for analyzing trace boron in steel by using microwave digestion ICP-AES method
CN109270051A
Mo-w target for forming wiring, mo-w wiring thin film using the same, and liquid-crystal display device
JP2003338465A
Etching method, etching liquid and etching liquid kit to be used in said method, and semiconductor substrate product manufacturing method