Method for producing a calibrated component assembly

By using the compaction and sintering technology of powdered materials and pushing and disconnecting in the calibration tool during the manufacturing process of the component composite, the problems of dimensional stability and process complexity of the component composite in the prior art are solved. Achieved high-precision and strength component complex manufacturing.

CN114786842BActive Publication Date: 2024-10-18GKN POWDER METALLURGY ENG GMBH
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202080073742.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-19
Publication Date
2024-10-18
Estimated Expiration
2040-10-19

AI Technical Summary

Technical Problem

The existing technology is difficult to achieve high dimensional stability and has high process complexity when manufacturing component composites. Especially during the compaction and sintering process of powder metallurgy materials, it is difficult to ensure the connection stability and calibration of components.

Method used

This is achieved by producing the components as green bodies from powdered materials by compaction, sintering the joints at the contact surfaces, then pushing them axially in a calibration tool to disconnect the mating materials, and then calibrating them by compaction. High dimensional stability of the component complex.

Benefits of technology

It achieves high dimensional stability and low-complexity process of the component composite, ensures high fitting accuracy and strength of the components after calibration, and avoids the risk of cracking during sintering.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114786842B_ABST
    Figure CN114786842B_ABST
Patent Text Reader

Abstract

A method for producing a calibrated component composite (1), wherein the component composite (1) comprises at least one first component (2) with a first contact surface (3) and a second component (4) with a second contact surface (5), wherein in the component composite (1), the components (2, 4) are in contact with each other via the contact surfaces (3, 5); wherein the components (2, 4) are designed without undercuts at least with respect to an axial direction (6) and can be displaced relative to each other in the calibrated component composite (1) along the axial direction (6) and in the process along the contact surfaces (3, 5); wherein the method comprises at least the following steps: a) providing the components (2, 4) as green compacts (7, 8), b) sintering the components (2, 4) and forming at least a material-bonded connection between the components (2, 4), c) arranging the component composite (1) in a calibration tool (10); d) displacing the components (2, 4) relative to each other; e) arranging the components (2, 4) for the component composite (1) and f) calibrating the component composite (1).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for producing a calibrated component composite. The component is produced, in particular, from a powdered material by compacting to form a green compact and then by sintering to form a solid workpiece (sintered part). Such a sintered part can be further processed by re-pressing (calibration) to achieve a higher dimensional stability. Background Art

[0002] A component complex usually includes a plurality of components which must be separated from one another at least in the meantime, for example for arrangement and fastening to other components. For example, a connecting rod can be produced as a component complex, wherein the connecting rod head should be designed in two parts for fastening the connecting rod to the crankshaft.

[0003] For example, it is known to produce a composite component by first producing the composite component from a one-piece workpiece and providing a fracture notch therein. The one-piece workpiece is then fractured ("cracked") by the fracture notch, thereby producing two components which can be reassembled with corresponding other components only via individually embodied fracture surfaces.

[0004] In the production of component composites produced by powder metallurgy, it is known that the components of the component composite are each produced individually by extrusion, sintered individually and calibrated individually. Summary of the invention

[0005] The object of the present invention is to at least partially solve the problem posed with reference to the prior art. In particular, a method for producing a component composite is to be proposed, wherein the component is produced from a powdered material by compacting and sintering and, if necessary, by calibration. In this case, a high dimensional stability of the component composite is to be achieved by the method, wherein the method is to have the lowest possible complexity.

[0006] In order to achieve this object, a method having the features according to claim 1 is advantageous. Advantageous developments are the subject matter of the dependent claims. The features listed individually in the claims can be combined with one another in a technically meaningful manner and can be supplemented by the explained facts from the description and / or details from the drawings, wherein further design variants of the invention are shown.

[0007] A method for producing a calibrated component composite is proposed, wherein the component composite comprises at least a first component with a first contact surface and a second component with a second contact surface, wherein in the component composite the components are in contact with one another via the contact surfaces. The components are designed without undercuts at least with respect to the axial direction and can be displaced relative to one another in the calibrated component composite in the axial direction and in the process along the contact surfaces. The method comprises at least the following steps:

[0008] a) providing the first component and the second component as green compacts, respectively, wherein the green compacts are produced from a powdery material by compacting;

[0009] b) sintering the components and at least partially forming a material-fitting connection between the components via contact surfaces;

[0010] c) arranging the component complex in a calibration tool;

[0011] d) displacing the components relative to one another in an axial direction in a calibration tool;

[0012] e) arranging the components for forming a component assembly with contact surfaces contacting one another in a calibration tool, and

[0013] f) Calibration of the component assembly by pressing and provision of the calibrated component assembly.

[0014] The above (not definitive) division of the method steps into a) to f) should only serve as a distinction and should not impose a sequence and / or dependency. The frequency of the method steps can also be varied if necessary. It is also possible that the method steps overlap with one another at least partially in time. Very particularly preferably, method step f) takes place during step d) and / or step e). In particular, steps a) to f) are performed in the order presented.

[0015] The contact surfaces of the components extend in particular only in a plane extending parallel to the axial direction. In the arrangement of the component composite, the components contact one another via the contact surfaces. The components are designed in such a way that they can be displaced relative to one another in the axial direction, wherein the components slide on one another via the contact surfaces. For this purpose, the components are designed without undercuts, that is to say the components can be displaced relative to one another in the axial direction without restriction; that is, there are no stops against which the components can strike.

[0016] The component composite can consist of two or more components. The component is provided as a green compact according to step a). A workpiece produced by compacting powdered raw materials is referred to as a green compact.

[0017] According to step b), the components are sintered together. For this purpose, the components are positioned relative to one another, in particular in an arrangement provided by the component composite, and sintered together. In particular, during sintering, a temperature slightly below the melting temperature of the material used is used, wherein the individual particles of the powdered material are materially connected to one another via so-called sintering necks.

[0018] When the components are arranged in a component composite, the components are in contact with one another via the provided contact surfaces.

[0019] According to step c), the sintered components connected to one another via the contact surfaces are introduced as a component composite into a calibration tool.

[0020] The (known) calibration tool is in particular an extruder or can be inserted into an extruder. The component composite can be reshaped using the calibration tool. The components of the component composite are at least partially recompressed by the calibration tool and are thereby plastically deformed.

[0021] In step d), the components are displaced relative to one another in the axial direction, ie, in particular parallel to the extension of the contact surfaces. The components are displaced relative to one another by means of different components of the calibration tool (via one or more lower punches / one or more upper punches). As a result of the displacement, the connection between the contact surfaces of the components produced in step b) is disconnected.

[0022] In particular, the components are displaced in the axial direction to such an extent that the contact surfaces contacting one another still have an overlap of at least 90%, in particular at least 75%, preferably at least 25% in the axial direction (compared to an overlap of 100% of the contact surfaces in the arrangement provided for the component composite).

[0023] It is also possible to displace the components in the axial direction to such an extent that there is no longer any overlap of the contact surfaces.

[0024] Due to the breaking of the cohesive connection, the components are again separated from one another and can be moved independently of one another after being removed from the calibration tool.

[0025] In step e), the components are pushed (backwards) again and are positioned relative to one another, in particular in the arrangement provided by the component assembly. However, the arrangement of the components according to step b) and step e) can also differ from one another. In particular, the position of the components between step b) and step e) differs only in terms of the position in the axial direction.

[0026] In step f), the component or the component composite is calibrated. In this process, a re-extrusion is performed, in particular to increase the dimensional stability. In particular, a plastic deformation of the component or the component composite is performed.

[0027] The proposed method makes it possible to achieve a high dimensional stability of the component composite, since the components are aligned together (ie already joined or arranged to form the component composite) and, if necessary, plastically deformed together at the end of the method.

[0028] In particular, components of the component composite cannot be exchanged with other components of other component composites. Therefore, the components of the component composite always remain associated with one another (ie, from the time of compacting the powder to form the green compact until calibration).

[0029] In particular, before step a), the components are pressed from powdered material into a first green compact and a second green compact in a common working procedure and in a common punching tool in step a0) and joined together to form the component composite, so that the components are in contact with each other via contact surfaces. The components produced in this way are provided as a component composite in step a).

[0030] In particular, the first component is pressed into a corresponding green compact in a first working space of the punching tool and the second component is pressed into a second working space of the tool. Here, at least one green compact is moved in an axial direction relative to the corresponding other working space (or relative to the green compact that has been produced by pressing) for forming the component composite.

[0031] The (known) punching tool comprises in particular one or more lower punches and one or more upper punches as well as a die and, if necessary, one or more punches.

[0032] In particular, two components are already present as green compacts before the transfer for forming the component composite, ie two powdery materials are already compacted in the respective working spaces to form respective green compacts.

[0033] In particular, the pressing of the respective green compacts can be carried out simultaneously or in parallel with one another in terms of time. The pressing of the respective green compacts can also be carried out in a time-staggered manner relative to one another. In particular, the displacement of the green compacts or the working space can also be carried out simultaneously with the pressing of the material into the respective green compacts, in parallel with one another in terms of time, or in a time-staggered manner.

[0034] In particular, the working spaces are arranged offset relative to one another in the axial direction, so that the components (or the working spaces or the powdered material) do not come into contact with one another during the compacting of at least one component to form a green compact.

[0035] Preferably, at least one green compact is produced before the two working spaces (or the powdered materials contained therein) are pushed or brought into contact. Thus, mixing of the powdered materials can be substantially prevented. In particular, a boundary surface (later contact surface) extending parallel to the axial direction can be maintained or achieved between the green compacts, so that a later separation of the components along the contact surface can be achieved or ensured during calibration.

[0036] In particular, the green bodies are joined to one another in step a0) with a transition fit or even with an interference fit. The interference fit includes, in particular, a slight overlap of the components in a direction transverse to the axial direction. The transition fit may also allow a gap between the components in a direction transverse to the axial direction, if necessary. Due to the interference fit, the components are joined to one another only under the application of a pressing force, i.e. pushed into the arrangement of the components provided for the component composite. This fit makes it possible for the components to be handled and transported together as a composite.

[0037] Such a method for producing a component composite from a green compact is known, for example, from WO 2011 / 035862 A1, which method comprises pressing a powdery material into a green compact, moving the green compacts relative to one another while forming an interference fit, and thus producing the component composite.

[0038] It is accordingly stated there that the partial green compacts are first extruded individually in the (extrusion-) tool, then gathered and subsequently joined. Here, the separated parts of the powdery substance are extruded into two separate partial green compacts in the tool and gathered in the tool in the subsequent working step. Here, "extruding individually" can mean that the parts of the powdery substance are so spaced apart from each other in the tool that two separate, mutually spaced working spaces are formed in the tool, wherein the individual green compacts then referred to as partial green compacts are manufactured. Here, it is also possible that during the extrusion of the partial green compacts, the dies of the adjacent working spaces form working spaces for the corresponding other stamping parts or partial green compacts. Here, the die arranged in the middle of the tool can form a cavity in the first working space for the first partial green compact, while the die for the outside of the first partial green compact forms the working space for the outside of the second partial green compact, which is formed by means of the die in the middle. The embodiment is not limited to the two partial green compacts being pressed only individually; rather, it is also possible to first press a partial green compact in a first separate, spaced-apart working space and transfer this partial green compact into a second working space for a second partial green compact. The first partial green compact is then held in its working space during the pressing of the second partial green compact, so that the first partial green compact is then joined to the formed second partial green compact. The joining of the first and second partial green compacts is thus postponed in the working phase of the tool in which the second partial green compact is pressed.

[0039] The method present here particularly utilizes the high fitting accuracy of the green compacts of the calibrated component complexes manufactured in this way later. The sintered component has the risk of cracking at the cross-sectional transition not only during the actual compression but also during demolding and subsequent manipulation, mainly due to the density inhomogeneity and / or axial and radial stresses in the tool. The risk of cracking caused at the cross-sectional transition due to the stress in the green compact (which occurs during the punching process) is avoided by the method known from WO 2011 / 035862 A1, because at least two partial green compacts are compressed and subsequently joined in the working procedure without interfering effects on the cross-sectional transition independently of each other. In particular, a particularly preferred fitting accuracy is achieved between the partial green compacts to be joined. If the green compact (i.e. the green compact constituting the component complex) is sintered after demolding from the punching tool (and after the other processing steps of the green compact if necessary), the high fitting accuracy of the green compacts to each other leads to sintering at the contact surface of the green compact. The strength of sintering can be affected by the fitting accuracy. Less sintering can be expected in the case of a transition fit than in the case of an interference fit.

[0040] In particular, after the component composite has been formed in step a0), the component is provided as a component composite in step a) and sintered as a component composite in step b).

[0041] In particular, the green compacts are no longer separated from each other before being placed in the calibration tool. Therefore, the high fit accuracy of the component composite (in the state of the joined green compacts and in the state of the sintered workpiece) can be used for calibration or for using the components later as a component composite.

[0042] In particular, the first component and the second component are produced from the same powdered material.

[0043] Furthermore, a component composite is proposed, which is produced by the described method. The calibrated component composite comprises at least a first component with a first contact surface and a second component with a second contact surface, wherein in the component composite the components are in contact with one another via the contact surfaces. The components are designed without undercuts at least with respect to the axial direction and can be displaced relative to one another in the calibrated component composite at least in the axial direction and in this case along the contact surfaces.

[0044] In particular, the components can be moved relative to each other only in the axial direction for separation or for producing a component composite. In particular, a geometry is therefore provided on the components, which geometry causes a positive connection of the components relative to the radial direction and / or the circumferential direction.

[0045] In particular, the components can additionally be moved relative to one another in a radial direction for separation or for producing a component composite. In particular, a geometric structure is therefore provided on the components, which geometry results in a form-fitting connection of the components relative to other radial and / or circumferential directions. In particular, there can be a minimal undercut relative to the radial direction, which can be overcome by elastic deformation, so that a radial connection can be achieved.

[0046] In particular, the component composite is of annular design, wherein each component forms a ring segment extending in the circumferential direction.

[0047] In particular, the components are designed identically to one another (or alternatively differently from one another) with regard to the geometrical embodiment.

[0048] The component composite produced in this way can be produced with high dimensional stability, wherein the components for the component composite can be preassembled for further use.

[0049] The embodiments for the method can in particular be transferred to the component composite and vice versa.

[0050] It should be noted as a precaution that the numbers used here ("first", "second", ...) are primarily (only) used to distinguish between a plurality of identical subjects, dimensions or processes, i.e., in particular, a correlation and / or sequence of these subjects, dimensions or processes relative to one another is not necessarily predetermined. If a correlation and / or sequence is required, this is explicitly stated here or is obvious to a person skilled in the art when studying the specifically described design. As long as a component can exist multiple times ("at least one"), the description of one of these components can also apply to all or part of these multiple components, but this is not mandatory. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] The invention and the technical field are explained in more detail below with reference to the drawings. It should be noted that the invention should not be limited to the embodiments presented. In particular, it is also possible to extract partial aspects of the facts illustrated in the drawings and combine them with other components and insights from the present description, as long as different situations are not explicitly shown. In particular, it should be noted that the drawings and in particular the dimensional ratios shown are only schematic. Among them:

[0052] Figure 1 A known method for producing a green body is shown;

[0053] Figure 2 The component complex is shown in a view along the axial direction;

[0054] Figure 3 The stereoscopic view shows the Figure 2 A complex of components;

[0055] Figure 4 Shown according to Figure 2 A complex of components;

[0056] Figure 5 A perspective view of a system with components displaced relative to each other in the axial direction is shown. Figures 2 to 4 a composite of parts; and

[0057] Figure 6 The side view shows the Figure 4 and Figure 5 A complex of components. DETAILED DESCRIPTION

[0058] Figure 1The method known from WO 2011 / 035862 A1 is shown for producing green compacts 7, 8. Such a method for producing a component composite 1 made of green compacts 7, 8 comprises pressing a powdered material 9 into green compacts 7, 8, displacing / moving the green compacts 7, 8 relative to each other while forming an interference fit and thus producing the component composite 1.

[0059] The punching tool 11 comprises a die 16, a first upper punch 17, a second upper punch 18, a first lower punch 19 and a second lower punch 20. According to step A of the method shown, the lower punches 19, 20 are moved in the die 16 and the powdered material 9 is arranged. In step B, the upper punches 17, 18 are arranged in the die 16 and all the punches 17, 18, 19, 20 are moved relative to each other, so that the first working space 12 and the second working space 13 are formed with the material 9 separated from each other. In step C, the material 9 is pressed into the working spaces 12, 13 to produce the green compacts 7, 8. In step D, the green compacts 7, 8 are joined to each other by the movement of the punches 17, 18, 19, 20. In step E, the component composite 1 formed by the green compacts 7, 8 is ejected.

[0060] The green compacts 7, 8 are first pressed individually in the punching tool 11, then brought together and subsequently joined. In this case, the separate parts of the powdered material 9 are pressed into two separate green compacts 7, 8 in the punching tool 11 and brought together in the punching tool 11 in a subsequent working step. During the pressing of the green compacts 7, 8, the punches 17, 19 of the adjacent working spaces 12 form the working spaces 13 for the respective other green compacts 8. In this case, the punches 17, 19 arranged in the middle of the punching tool 11 can form a cavity in the second working space 13 surrounding these punches 17, 19, so that the first green compact 7 produced in the first working space 12 can be guided in this cavity during joining. The outer punches 18, 20 form the outer second working space 13 for the second green compact 8.

[0061] Figure 2 The component assembly 1 is shown in a view along the axial direction 6 . Figure 3 The three-dimensional view shows the Figure 2 Component complex 1. Figure 4 Shown according to Figure 2 Component complex 1. Figure 5 The perspective view shows the structure according to the invention with the components 2 , 4 displaced relative to one another in the axial direction 6 . Figures 2 to 4 Component complex 1. Figure 6 The side view shows the Figure 4 and Figure 5 Component complex 1. Figures 2 to 6 They are collectively described below.

[0062] The calibrated component composite 1 comprises a first component 2 with a first contact surface 3 and a second component 4 with a second contact surface 5 and a third component 21, wherein in the component composite 1, the components 2, 4, 21 are in contact with each other via the contact surfaces 3, 5. The components 2, 4, 21 are each designed identically. The components 2, 4, 21 are designed without undercuts with respect to the axial direction 6 and can be displaced relative to each other in the calibrated component composite 1 only along the axial direction 6 and here along the contact surfaces 3, 5.

[0063] A geometry is provided on the components 2, 4, 21 (here in the manner of a so-called dovetail connection) which produces a positive connection of the components 2, 4, 21 with respect to the radial direction 22 and the circumferential direction 14. The component assembly 1 is annular, wherein each component 2, 4, 21 forms a ring segment extending in the circumferential direction 14.

[0064] Within the scope of the method, in step a0), in a common working sequence and in a common punching tool 11, a powdery material 9 is pressed (see Figure 1 , steps A, B, C) produce a first green body 7 and a second green body 8 (as well as a third green body). The three green bodies 7, 8 are joined together to form the component composite 1 (see Figure 1 , step D), so that the green bodies 7, 8 (or components 2, 4, 21) are in contact with each other via the contact surfaces 3, 5. The components 2, 4, 21 produced in this way are provided in step a) as a component composite 1 (see Figure 1 , Step E and Figure 2 and Figure 3 ).

[0065] According to step a), the components 2, 4, 21 are provided as green compacts 7, 8, respectively, wherein the green compacts 7, 8 are produced from a powdered material 9 by compaction. According to step b), the components 2, 4, 21 are sintered and a material-bonded connection (e.g. Figure 2 and Figure 3 According to step c), the component composite 1 is arranged in the calibration tool 10. According to step d), the components 2, 4, 21 are displaced relative to one another in the axial direction 6 in the calibration tool 10 (see Figures 4 to 6 ; Calibration tools such as according to Figure 1 The punching tool 11 is designed; Figures 4 to 6 According to step e), the components 2, 4, 21 are arranged for forming a component composite 1 with contact surfaces 3, 5 in contact with one another in a calibration tool 10 (for example according to Figure 2 and Figure 3), and according to step f), the component assemblage 1 is calibrated by pressing and a calibrated component assemblage 1 is provided (for example according to Figure 2 and Figure 3 ).

[0066] The contact surfaces 3, 5 of the components 2, 4, 21 extend only in a plane extending parallel to the axial direction 6. The components 2, 4, 21 are designed so that they can be displaced relative to one another in the axial direction 6, wherein the components 2, 4, 21 slide on one another via the contact surfaces 3, 5. For this purpose, the components 2, 4, 21 are designed without undercuts, that is to say the components 2, 4, 21 can be displaced relative to one another in the axial direction 6 without restriction.

[0067] In step d), the components 2, 4, 21 are displaced relative to one another in the axial direction 6. The components 2, 4, 21 are moved relative to one another by means of different components of the calibration tool 10 (e.g. by means of one or more lower punches 19, 20 / one or more upper punches 17, 18; see e.g. Figure 1 ) are displaced relative to one another. As a result of the displacement, the connection between the contact surfaces 3, 5 of the components 2, 4, 21 produced in step b) is disconnected. In this case, the components 2, 4, 21 are displaced in the axial direction 6 to such an extent that, compared to the 100% overlap 23 of the contact surfaces 3, 5 in the arrangement provided for the component composite 1 (see Figure 2 and Figure 3 ), the contacting contact surfaces 3, 5 also have an overlap 23 of at least 25% in the axial direction 6 (see Figures 4 to 6 ).

[0068] In step e), components 2 , 4 , 21 are pushed (backwards) again and positioned relative to one another, in particular in the arrangement provided by component composite 1 . However, the arrangement of components 2 , 4 , 21 according to steps b) and e) can also differ from one another.

[0069] In step f), the component 2 , 4 , 21 or the component composite 1 is calibrated. In this process, re-extrusion is performed, in particular to increase dimensional stability. In particular, a plastic deformation of the component 2 , 4 , 21 or the component composite 1 is performed.

[0070] List of reference numerals:

[0071] 1 Component complex

[0072] 2 First part

[0073] 3 First contact surface

[0074] 4 Second component

[0075] 5 Second contact surface

[0076] 6 Axial direction

[0077] 7 The first green body

[0078] 8 Second green body

[0079] 9 Materials

[0080] 10 Calibration Tools

[0081] 11. Punching tools

[0082] 12 First Workspace

[0083] 13 Second Workspace

[0084] 14 Circumferential direction

[0085] 15 Extrusion direction

[0086] 16 Die

[0087] 17 First upper punch

[0088] 18 Second upper punch

[0089] 19 First lower punch

[0090] 20 Second lower punch

[0091] 21 Third Part

[0092] 22 Radial direction

[0093] 23 Overlapping portion.

Claims

1. A method for producing a calibrated component assembly (1), wherein: The component composite (1) comprises at least a first component (2) with a first contact surface (3) and a second component (4) with a second contact surface (5), wherein in the component composite (1), the components (2, 4) are in contact with each other via the contact surfaces (3, 5); wherein the components (2, 4) are designed without undercuts at least with respect to an axial direction (6) and can be displaced relative to each other in the axial direction (6) and in the process along the contact surfaces (3, 5) in a calibrated component composite (1); wherein the method comprises at least the following steps: a) providing the first component (2) and the second component (4) as green compacts (7, 8), respectively, wherein the green compacts are produced from a powdery material (9) by compacting; b) sintering the components (2, 4) and forming at least a material-bonded connection between the components (2, 4) via the contact surfaces (3, 5); c) arranging the component complex (1) in a calibration tool (10); d) displacing the components (2, 4) relative to one another in the calibration tool (10) along an axial direction (6); e) arranging the components (2, 4) for forming a component assembly (1) with contact surfaces (3, 5) contacting one another in the calibration tool (10); and f) calibrating the component assembly (1) by pressing and providing a calibrated component assembly (1).

2. The method according to claim 1, wherein: Prior to step a), the components (2, 4) are compacted from powdered material (9) into a first green compact (7) and a second green compact (8) in a common working procedure and in a common punching tool (11) in step a0) and joined together to form the component composite (1), so that the components (2, 4) are in contact with each other via the contact surfaces (3, 5); wherein the components (2, 4) are provided as a component composite (1) in step a).

3. The method according to claim 2, wherein: The first component (2) is pressed into a first working space (12) of the punching tool (11) and the second component (4) is pressed into a corresponding green body (7, 8) in a second working space (13) of the punching tool (11); wherein at least one green body (7, 8) is displaced in an axial direction (6) relative to the corresponding other working space (12, 13) in order to form the component composite (1).

4. The method according to claim 3, wherein: Prior to being moved for forming the component composite (1), the two components (2, 4) are present as green compacts (7, 8).

5. The method according to any one of the preceding claims 3 and 4, wherein: The working spaces (12, 13) are arranged offset relative to one another in the axial direction (6), so that the components (2, 4) do not contact one another during the pressing of at least one of the components (2, 4) to form a green compact (7, 8).

6. The method according to any one of the preceding claims 2 to 5, wherein: The green bodies (7, 8) are joined to one another in step a0) by forming an interference fit or a transition fit.

7. The method according to any one of the preceding claims 2 to 6, wherein: After forming the component composite (1) in step a0), the components (2, 4) are provided as a component composite (1) in step a) and are sintered in step b) to form the component composite (1).

8. The method according to any one of the preceding claims 1 to 7, wherein: The first component (2) and the second component (4) are manufactured from the same powdered material.

9. Component composite (1) produced by the method according to any one of the preceding claims, wherein: A calibrated component assembly (1) comprises at least a first component (2) with a first contact surface (3) and a second component (4) with a second contact surface (5), wherein in the component assembly (1), the components (2, 4) are in contact with one another via the contact surfaces (3, 5); wherein the components (2, 4) are designed without undercuts at least with respect to an axial direction (6) and can be displaced relative to one another in the calibrated component assembly (1) at least along the axial direction (6) and thereby along the contact surfaces (3, 5).

10. The component assembly (1) according to claim 9, wherein: The components (2, 4) are movable relative to one another only in an axial direction (6) for producing the component composite (1).

11. The component assembly (1) according to any one of the preceding claims 9 and 10, wherein: The components (2, 4) are movable relative to one another only in an axial direction (6) in order to separate the component assembly (1).

12. The component assembly (1) according to any one of the preceding claims 9 to 11, wherein: The component assembly (1) is annular, wherein each component (2, 4) forms a ring segment extending in a circumferential direction (14).

13. The component assembly (1) according to any one of the preceding claims 9 to 12, wherein: The components (2, 4) are identical to one another in terms of their geometrical design.

Citation Information

Patent Citations

  • Method for producing a green compact

    WO2011035862A1

  • Method for producing non-circular toothed belt pulleys or sprockets

    CN101534981A

  • Method for producing a green compact

    CN102762321A

  • Method for producing a composite part

    CN102770222A

  • Green compact, manufacturing method for same, and reactor core

    CN102792402A