Preparation method and application of high biomass-based polyimine self-healing polymer
By using natural vegetable oils and bio-based polyaldehydes to prepare high-biomass-based polyimine self-healing polymers, using imine bonds to achieve room temperature self-healing and reprocessing, the environmental protection problems based on petrochemical-based materials in the prior art are solved. It has achieved efficient and low-cost self-healing polymer development, which is in line with the concept of sustainable development.
Patent Information
- Application Number
- CN202210546302.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-05-18
AI Technical Summary
The development of existing self-healing polymer materials mainly relies on petrochemical-based chemicals, lacking high-efficiency, low-temperature self-healing and reprocessable materials based on natural renewable biomass, making it difficult to meet the needs of green environmental protection and sustainable development.
Using natural renewable vegetable oils and bio-based polyaldehydes as raw materials, high biomass-based polyimine self-healing polymers are prepared through imine bond cross-polymerization to achieve room temperature self-healing, reprocessing and flame retardant properties. And the process is simple and the cost is low.
It achieves efficient adhesion, room temperature self-healing, reprocessable and recycling of multifunctional high-biocontent thermoset polyimine polymer, which broadens the application range, conforms to the concept of green environmental protection, and reduces production costs.
Smart Images

Figure CN114805718B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of polymer material preparation, and specifically is a preparation method and application of a high biomass-based polyimide self-healing polymer Background Art
[0002] Polymer materials are widely used in aviation, aerospace, electronics, machinery and other technical fields due to their excellent performance. However, materials will inevitably be damaged during use, among which microcracks are the main form of microscopic damage to materials, which will lead to a decrease in the mechanical properties of materials and a reduction in service life. As a novel intelligent structural functional material, self-healing polymer materials provide a new method for preventing potential hazards by realizing self-healing of microcracks, and have great development prospects and application value in some important engineering and cutting-edge technology fields. Self-healing polymers can self-repair microcracks inside materials by imitating the mechanism of self-repair of biological damage, avoiding further damage to materials and extending the service life of materials. In 2010, the American Society of Manufacturing Engineering believed that smart polymers with self-healing functions (containing self-healing agents) were one of the eight innovative technologies that changed the face of the industry. As a general polymer material, polymer adhesives are also sensitive to damage and have a strong demand for self-healing properties. Therefore, in recent years, self-healing adhesives that can self-heal and repair damaged joints have received great attention.
[0003] At present, highly biomass-based self-healing polymer materials based on dynamic reversible bonds have been reported. For example, the prior art CN110423334A discloses a fully bio-based polymer material based on ester bond cross-linking, which can perform crack self-healing, reprocessing and shape memory; however, due to the high activation energy of the ester bond, the self-healing and reprocessing of the material requires catalyst catalysis and a higher temperature of 180 to 200 ° C. The Schiff base bond selected in the present invention is a highly active reversible covalent bond. Compared with other dynamic covalent bonds (such as ester bonds, disulfide bonds, etc.), imine has many characteristics such as simple synthesis, rich raw material selection, acid-base responsiveness, water sensitivity, and the ability to undergo exchange reactions at room temperature. It has been introduced into various polymers to construct dynamic networks, so that polymers can obtain crack self-healing, reprocessing and diversified recycling.
[0004] At present, the development of most self-healing polymer materials is based on petrochemical-based chemicals as raw materials. For the sake of green environmental protection, it is of great significance to use natural, renewable and non-toxic biomass raw materials to prepare self-healing polymer materials. At the same time, the development of high-biomass-based self-healing polymer materials not only conforms to the concept of sustainable development, but also provides a new way for the high-value utilization of related biomass resources, and promotes the refinement and functionalization of biomass resources. Summary of the invention
[0005] Technical problem to be solved: The present invention provides a preparation method and application of a high-biomass-based polyimine self-healing polymer, which uses natural renewable plant oils and bio-based polyaldehydes as raw materials to prepare a multifunctional high-biomass-content thermosetting polyimine polymer that combines high-efficiency adhesion, room temperature self-healing, reprocessability and recycling, and flame retardancy.
[0006] Technical solution: A high-biomass-based polyimine self-healing polymer, castor oil-based polyamine and bio-based polyaldehyde react in an organic solvent, and the solvent is removed to obtain a high-biomass-based polyimine self-healing polymer; the bio-based polyaldehyde is any one of the derivatives of vanillin, o-vanillin and 5-hydroxyfurfural; the castor oil-based polyamine is prepared by reacting acrylated castor oil and a small molecule polyamine; the acrylated castor oil is prepared by microwave reaction of castor oil, acrylic acid, a catalyst and an inhibitor.
[0007] The catalyst is p-toluenesulfonic acid, and the inhibitor is hydroquinone.
[0008] The small molecule polyamines are diethylenetriamine, 1,5-pentanediamine, ethylenediamine, hexamethylenediamine, p-phenylenediamine and p-phenylenediamine.
[0009] The derivatives of vanillin are dimerized vanillin, trivanillin phosphate, 2,4,6-trivanillin-1,3,5-triazine, divanillin-dimethylsilane or divanillin-phenyl phosphate; the derivatives of o-vanillin are dimerized o-vanillin, tri-o-vanillin phosphate, 2,4,6-tri-o-vanillin-1,3,5-triazine, di-o-vanillin-dimethylsilane or di-o-vanillin-phenyl phosphate; the derivatives of 5-hydroxyfurfural are trihydroxyfurfural phosphate, 2,4,6-trihydroxyfurfural-1,3,5-triazine, dihydroxyfurfural-dimethylsilane or dihydroxyfurfural-phenyl phosphate.
[0010] The method for preparing the high biomass-based polyimine self-healing polymer comprises the following steps:
[0011] (1) Microwave synthesis of acrylated castor oil: Castor oil, acrylic acid, a catalyst and a polymerization inhibitor are added to a microwave reaction flask for microwave reaction. After the reaction is completed, the unreacted acrylic acid is removed by washing, and the organic phase is collected, dried with a desiccant, and filtered to obtain acrylated castor oil.
[0012] (2) Synthesis of castor oil-based polyamine: Add acrylated castor oil and small molecule polyamine into a reaction vessel, react at room temperature, wash to remove unreacted small molecule polyamine, collect the organic phase, dry with a desiccant, and filter to obtain castor oil-based polyamine;
[0013] (3) Preparation of high biomass-based polyimine self-healing polymer: At room temperature, the prepared castor oil-based polyamine and bio-based polyaldehyde are dissolved in an organic solvent, with the molar ratio of the primary amino group of the castor oil-based polyamine to the aldehyde group in the bio-based polyaldehyde being 1:0.5-0.9. The mixture is stirred thoroughly until it is completely dissolved and degassed, and then poured into a polytetrafluoroethylene mold, heated and placed to evaporate the solvent, and then placed under vacuum conditions to remove trace amounts of the solvent, thereby obtaining a high biomass-based polyimine self-healing polymer.
[0014] In step (1), the molar ratio of the hydroxyl group to the carboxyl group in acrylic acid is 1:3; the amount of catalyst used is 0.7 wt.%, and the amount of inhibitor used is 0.3 wt.%.
[0015] In step (1), the reaction conditions are as follows: the microwave reaction temperature is 80 to 120° C., and the reaction is carried out for 10 to 30 minutes.
[0016] In step (2), the molar ratio of double bonds to primary amine groups in the acrylated castor oil is 1:1.1, and the reaction conditions are room temperature for 12 to 24 hours.
[0017] In step (3), the organic solvent is tetrahydrofuran, N,N-dimethylformamide or N,N-dimethylacetamide, and the degassing method is static degassing, ultrasonic degassing or centrifugal degassing.
[0018] Application of the high biomass-based polyimine self-healing polymer in adhesives.
[0019] Beneficial effects: The high-biomass-based polyimine self-healing polymer of the present invention is prepared from natural renewable plant oil esters and bio-based polyaldehydes as raw materials, and the high-biomass-based polyimine self-healing polymer is cross-linked and polymerized by dynamic covalent imine bonds. Since the imine bond is a highly active reversible covalent bond, a dynamic reaction can be achieved at a mild temperature without a catalyst. Therefore, the self-healing polymer prepared by the present invention requires a low curing temperature and a low reprocessing temperature, and a high self-healing efficiency can be achieved for the polymer at room temperature; the rich variety of polar groups and coupled aromatic rings in its structure construct a mussel foot protein-like structure, which can form a rich intermolecular interaction, so that the high-biomass-based polyimine self-healing polymer exhibits effective adhesion on different substrates. In addition, since the imine bond can be dissociated under acidic conditions, the high-biomass-based polyimine self-healing polymer has an extremely high monomer recovery rate. The high-biomass-based polyimine self-healing polymer of the present invention has high-efficiency adhesion, self-healing at room temperature, reprocessing and recycling, and has flame retardant properties, which broadens the scope of practical application. The invention uses castor oil and vanillin as raw materials, has abundant raw material sources, low production cost, and complies with the concepts of green environmental protection and sustainable development; in addition, the synthesis process is simple, operability is strong, and it is easy to implement. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The infrared spectra of the microwave-synthesized acrylated castor oil of the present invention and the castor oil-based polyamine obtained in Example 1;
[0021] Figure 2 is a schematic diagram of the structure of the bio-based polyamine of the present invention;
[0022] Figure 3 This is the hydrogen spectrum of dimer vanillin obtained in Example 1 of the present invention;
[0023] Figure 4 This is the stress-strain test curve of the self-healing polymer obtained in Example 1 of the present invention;
[0024] Figure 5 This is a graph of the adhesive shear strength of the self-healing polymer obtained in Example 1 of the present invention on different substrates;
[0025] Figure 6 The scratch self-healing diagram of the self-healing polymer obtained in Example 1 of the present invention at different temperatures;
[0026] Figure 7 This is a reprocessing diagram of the self-healing polymer obtained in Example 1 of the present invention;
[0027] Figure 8 This is a recycling and degradation diagram of the self-healing polymer obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the embodiments described are only some embodiments of the present invention, rather than all embodiments.
[0029] A method for preparing a high-biomass-based polyimine self-healing polymer: (1) Microwave synthesis of acrylated castor oil: castor oil, acrylic acid, a catalyst and an inhibitor are added to a microwave reaction flask, the molar ratio of the hydroxyl group in the castor oil to the carboxyl group in the acrylic acid is 1:3; the catalyst is p-toluenesulfonic acid, the inhibitor is hydroquinone, the amount of the catalyst is 0.7wt.%, the amount of the inhibitor is 0.3wt.%, the microwave reaction temperature is 80-120°C, and the reaction is carried out for 10-30 minutes. After the reaction is completed, the mixture is washed with deionized water until the pH is neutral to remove unreacted acrylic acid, etc., the organic phase is collected, dried with a desiccant, and filtered to obtain acrylated castor oil. (2) Synthesis of castor oil-based polyamine: acrylated castor oil and a small molecule polyamine are added to a reaction vessel, the molar ratio of the double bond in the acrylated castor oil to the primary amine group in the small molecule polyamine is 1:1.1, and the reaction is carried out at room temperature for 12-24 hours. Add deionized water to wash until the pH is neutral to remove the unreacted small molecule polyamine, collect the organic phase, dry with a desiccant, and filter to obtain castor oil-based polyamine. (3) Preparation of high biomass-based polyimine self-healing polymer: At room temperature, dissolve the prepared castor oil-based polyamine and bio-based polyaldehyde in an organic solvent, the molar ratio of the primary amino group of the castor oil-based polyamine to the aldehyde group in the bio-based polyaldehyde is 1: (0.5-0.9), stir well, and after complete dissolution and degassing, pour into a polytetrafluoroethylene mold, place at 80°C for 24 hours to evaporate the solvent, and then continue to place under vacuum conditions for 12 to 24 hours to remove trace amounts of solvent, to obtain a high biomass-based polyimine self-healing polymer.
[0030] In step (1), the molar ratio of the hydroxyl group to the carboxyl group in acrylic acid is 1:3; the catalyst is p-toluenesulfonic acid, the inhibitor is hydroquinone, the amount of the catalyst is 0.7wt.%, the amount of the inhibitor is 0.3wt.%, and the desiccant is anhydrous sodium sulfate and anhydrous magnesium sulfate.
[0031] In step (1), the reaction conditions are as follows: the microwave reaction temperature is 80 to 120° C., and the reaction is carried out for 10 to 30 minutes.
[0032] In step (2), the small molecule polyamine is diethylenetriamine, 1,5-pentanediamine, ethylenediamine, hexamethylenediamine, p-phenylenediamine, and p-phenylenediamine.
[0033] In step (2), the molar ratio of double bonds to primary amine groups in the acrylated castor oil is 1:1.1, and the reaction conditions are room temperature for 12 to 24 hours.
[0034] In step (3), the bio-based polyaldehyde is a derivative of vanillin, o-vanillin and 5-hydroxyfurfural. The derivative of vanillin is dimerized vanillin, tri-o-vanillin phosphate, 2,4,6-tri-o-vanillin-1,3,5-triazine, di-o-vanillin-dimethylsilane or di-o-vanillin-phenyl phosphate. The derivative of o-vanillin is dimerized o-vanillin, tri-o-vanillin phosphate, 2,4,6-tri-o-vanillin-1,3,5-triazine, di-o-vanillin-dimethylsilane or di-o-vanillin-phenyl phosphate. The derivative of 5-hydroxyfurfural is trihydroxyfurfural phosphate, 2,4,6-trihydroxyfurfural-1,3,5-triazine, dihydroxyfurfural-dimethylsilane or dihydroxyfurfural-phenyl phosphate, and its structure is as follows: Figure 2 shown.
[0035] In step (3), the organic solvent is tetrahydrofuran, N,N-dimethylformamide or N,N-dimethylacetamide, and the degassing method is static degassing, ultrasonic degassing or centrifugal degassing.
[0036] The preparation method produces a high-biomass-based polyimine self-healing polymer.
[0037] Application of the high biomass-based polyimine self-healing polymer in adhesives.
[0038] Example 1
[0039] (1) Synthesis of acrylated castor oil: 13.95 g (0.015 mol) of castor oil, 10.8 g (0.15 mol) of acrylic acid, 0.7 wt.% of p-toluenesulfonic acid catalyst and 0.3 wt.% of hydroquinone polymerization inhibitor were added to a 40 mL microwave reaction flask with a magnet. The microwave reaction temperature was 120° C. and the reaction was carried out for 20 minutes. After the reaction was completed, the mixture was washed with saturated saline until the pH was neutral, and water was removed with anhydrous magnesium sulfate. The mixture was filtered to obtain yellow oily liquid acrylated castor oil (ACO).
[0040] (2) Synthesis of castor oil-based polyamine: 11 g (0.01 mol) of ACO and 3.1 g (0.03 mol) of diethylenetriamine were added.
[0041] Add to a 50ml conical flask with a magnet, stir at 400rpm, and react at room temperature for 12 hours. After the reaction is completed, wash with saturated brine until the pH is neutral. Remove water with anhydrous magnesium sulfate, filter, and rotary evaporate to obtain a reddish brown viscous liquid. The measured ammonia value is 98mgKOH / g, which is close to the theoretical value (108.9mgKOH / g).
[0042] (3) Synthesis of dimeric vanillin: 15.2 g (0.1 mol) vanillin, 0.76 g (5 mmol) ferrous sulfate, 13.5 g (0.05 mol) potassium persulfate and 400 ml deionized water were added to a 500 ml conical flask with a magnet, stirred at 400 rpm / min, and stirred at 80°C for 20 minutes. The mixture was aspirated while hot, and the residue was dissolved with sodium hydroxide solution and then precipitated with dilute hydrochloric acid solution. The mixture was filtered and washed with hot water for 3 to 5 times. The product was a pale gray solid powder.
[0043] (4) Preparation of high biomass-based polyimine self-healing polymer: At room temperature, the prepared castor oil-based polyamine and dimeric vanillin are dissolved in N,N-dimethylformamide, with the molar ratio of the primary amino group of the castor oil-based polyamine to the aldehyde group in dimeric vanillin being 1:0.5-0.9. The mixture is stirred thoroughly until it is completely dissolved and degassed, and then poured into a polytetrafluoroethylene mold and placed at 80°C for 24 hours to evaporate the solvent. The mixture is then placed under vacuum for 12-24 hours to remove trace amounts of the solvent, thereby obtaining a high biomass-based polyimine self-healing polymer.
[0044] (3) The tensile strength of the material can be adjusted between 4 and 21 MPa, such as Figure 4 As shown; the bonding shear strength on the glass plate can reach up to 14.1MPa. Figure 5 As shown; after scratching the obtained self-healing polymer with a fine needle (the width of the scratch is about 67 μm), it can be observed through an optical microscope at room temperature that the scratch on the polymer surface basically disappears after 4 hours (as shown Figure 6 ), indicating that the polymer has efficient self-healing properties; the polymer that has been broken into pieces can be molded into a complete sample by keeping it at 80°C and 0.2MPa for 2 minutes, and the mechanical properties can be basically fully restored (as shown in Figure 7 200 mg DAC-0.9DV was crushed into powder and placed in a 10 mL vial containing 10 ml DMF solution. It was completely dissolved at 80 ° C for 2 h. After removing DMF, the polymer was solidified again. In addition, the polymer can be completely degraded in a 5% acetic acid aqueous solution, such as Figure 8 shown.
[0045] Example 2
[0046] (1) Synthesis of acrylated castor oil: 13.95 g (0.015 mol) of castor oil, 10.8 g (0.15 mol) of acrylic acid, 0.7 wt.% of p-toluenesulfonic acid catalyst and 0.3 wt.% of hydroquinone polymerization inhibitor were added to a 40 mL microwave reaction flask equipped with a magnet. The microwave reaction temperature was 120° C. and the reaction was carried out for 20 minutes. After the reaction was completed, the mixture was washed with saturated saline until the pH was neutral, and water was removed with anhydrous magnesium sulfate. The mixture was filtered to obtain a yellow oily liquid acrylated castor oil.
[0047] (2) Synthesis of castor oil-based polyamine: 11 g (0.01 mol) of ACO and 3.07 g (0.03 mol) of 1,5-pentanediamine were added to a 50 ml conical flask with a magnet, stirred at 400 rpm, and reacted at room temperature for 12 hours. After the reaction, the mixture was washed with saturated brine until the pH was neutral. The mixture was dehydrated with anhydrous magnesium sulfate, filtered, and evaporated to obtain a reddish brown viscous liquid. The measured ammonia value was 95 mgKOH / g, which was close to the theoretical value (108.9 mgKOH / g).
[0048] (3) Synthesis of dimeric vanillin: 10 g (66 mmol) of vanillin was dissolved in 400 ml of hot deionized water, 1 mol / L acetic acid aqueous solution was added dropwise at room temperature to make the pH ≈ 4, horseradish peroxidase (type I, 90 mg, 1000 units of activity) was added at 40°C, and then 75 ml of 3% hydrogen peroxide aqueous solution (66 mmol) was added, stirred at 400 rpm / min for 5 minutes, filtered and washed with hot water for 3 to 5 times. The product was obtained by drying in an oven at 50°C.
[0049] (4) Preparation of high biomass-based polyimine self-healing polymer: At room temperature, the prepared castor oil-based polyamine and dimeric vanillin are dissolved in N,N-dimethylformamide, with the molar ratio of the primary amino group of the castor oil-based polyamine to the aldehyde group in dimeric vanillin being 1:0.5-0.9. The mixture is stirred thoroughly until it is completely dissolved and degassed, and then poured into a polytetrafluoroethylene mold and placed at 80°C for 24 hours to evaporate the solvent. The mixture is then placed under vacuum for 12-24 hours to remove trace amounts of the solvent, thereby obtaining a high biomass-based polyimine self-healing polymer.
[0050] (3) The tensile strength of the material can be adjusted between 3 and 17 MPa; the adhesive shear strength on the glass plate can reach up to 10 MPa; after scratching the obtained self-healing polymer with a fine needle (the width of the scratch is about 75 μm), it can be observed through an optical microscope at room temperature that the scratch on the polymer surface basically disappears after 12 hours; the polymer that has been broken into pieces can be molded into a complete sample by keeping it at 80°C and 0.2 MPa for 2 minutes, and the mechanical properties can be basically fully restored; 200 mg of the polymer is crushed into powder and placed in a 10 mL vial containing 10 ml of DMF solution at 80°C for 2 hours to completely dissolve it. After removing the DMF, the polymer can be solidified again. In addition, the polymer can be completely degraded in a 5% acetic acid aqueous solution.
[0051] Example 3
[0052] (1) Synthesis of acrylated castor oil: 13.95 g (0.015 mol) of castor oil, 10.8 g (0.15 mol) of acrylic acid, 0.7 wt.% of p-toluenesulfonic acid catalyst and 0.3 wt.% of hydroquinone polymerization inhibitor were added to a 40 mL microwave reaction flask equipped with a magnet. The microwave reaction temperature was 120° C. and the reaction was carried out for 20 minutes. After the reaction was completed, the mixture was washed with saturated saline until the pH was neutral, and water was removed with anhydrous magnesium sulfate. The mixture was filtered to obtain a yellow oily liquid acrylated castor oil.
[0053] (2) Synthesis of castor oil-based polyamine: 11 g (0.01 mol) of ACO and 3.07 g (0.03 mol) of 1,5-pentanediamine were added to a 50 ml conical flask with a magnet, stirred at 400 rpm, and reacted at room temperature for 12 hours. After the reaction, the mixture was washed with saturated brine until the pH was neutral. The mixture was dehydrated with anhydrous magnesium sulfate, filtered, and evaporated to obtain a reddish brown viscous liquid. The measured ammonia value was 95 mgKOH / g, which was close to the theoretical value (108.9 mgKOH / g).
[0054] (3) Synthesis of trivanillinyl phosphate: Phosphorus oxychloride (4.05 g 0.027 mol) was added dropwise to a solution of vanillyl acetone (15 g 0.09 mol) and triethylamine (9.15 g 0.09 mol) in ethyl acetate (200 ml) at 0-5°C. After 30 minutes at 0-5°C, the reaction mixture was stirred at room temperature for 16 hours. When the reaction was complete, it was filtered and washed with hot water 3 to 5 times. The product was a white solid powder.
[0055] (4) Preparation of high biomass-based polyimine self-healing polymer: At room temperature, the prepared castor oil-based polyamine and trivanillin phosphate are dissolved in N,N-dimethylformamide, with the molar ratio of the primary amino group of the castor oil-based polyamine to the aldehyde group in the trivanillin phosphate being 1:0.5-1. The mixture is stirred thoroughly until it is completely dissolved and degassed, and then poured into a polytetrafluoroethylene mold and placed at 80°C for 24 hours to evaporate the solvent. The mixture is then placed under vacuum for 12-24 hours to remove trace amounts of the solvent, thereby obtaining a high biomass-based polyimine self-healing polymer.
[0056] (3) The tensile strength of the material can be adjusted between 5 and 20 MPa; the adhesive shear strength on the glass plate can reach up to 13.5 MPa; after scratching the obtained self-healing polymer with a fine needle (the width of the scratch is about 80 μm), it can be observed through an optical microscope at room temperature that the scratch on the polymer surface basically disappears after 9 hours; the polymer that has been broken into pieces can be molded into a complete sample by keeping it at 80°C and 0.2 MPa for 2 minutes, and the mechanical properties can be basically fully restored; 200 mg of the polymer is crushed into powder and placed in a 10 mL vial containing 10 ml of DMF solution at 80°C for 3 hours to completely dissolve it. After removing the DMF, the polymer can be solidified again. In addition, the polymer can be completely degraded in a 5% acetic acid aqueous solution.
Claims
1. A biomass-based polyimine self-healing polymer, characterized in that: The castor oil-based polyamine and the bio-based polyaldehyde react in an organic solvent, and after removing the solvent, a high-biomass-based polyimine self-healing polymer is obtained; the bio-based polyaldehyde is dimeric vanillin, tri-vanillin phosphate, 2,4,6-tri-vanillin-1,3,5-triazine, di-vanillin-dimethylsilane, di-vanillin-phenyl phosphate, dimeric o-vanillin, tri-o-vanillin phosphate, 2,4,6-tri-o-vanillin-1,3,5-triazine, di-o-vanillin-dimethylsilane or di-o-vanillin-phenyl phosphate The invention relates to any one of hydroxy furfural phosphate, trihydroxy furfural phosphate, 2,4,6-trihydroxy furfural-1,3,5-triazine, dihydroxy furfural-dimethylsilane and dihydroxy furfural-phenyl phosphate; the castor oil-based polyamine is prepared by reacting acrylated castor oil with a small molecule polyamine; the small molecule polyamine is diethylenetriamine, 1,5-pentanediamine, ethylenediamine, hexamethylenediamine, p-phenylenediamine and p-phenylenediamine; the acrylated castor oil is prepared by microwave reaction of castor oil, acrylic acid, a catalyst and an inhibitor.
2. The biomass-based polyimine self-healing polymer according to claim 1, characterized in that: The catalyst is p-toluenesulfonic acid, and the inhibitor is hydroquinone.
3. A method for preparing the biomass-based polyimine self-healing polymer according to claim 1 or 2, characterized in that: The following steps are involved: (1) Microwave synthesis of acrylated castor oil: castor oil, acrylic acid, catalyst and inhibitor are added into a microwave reaction flask for microwave reaction. After the reaction is completed, the unreacted acrylic acid is removed by washing, and the organic phase is collected, dried with a desiccant, and filtered to obtain acrylated castor oil. (2) Synthesis of castor oil-based polyamine: Add acrylated castor oil and small molecule polyamine into a reaction vessel, react at room temperature, wash to remove unreacted small molecule polyamine, collect the organic phase, dry with a desiccant, and filter to obtain castor oil-based polyamine; (3) Preparation of high biomass-based polyimine self-healing polymer: At room temperature, the prepared castor oil-based polyamine and bio-based polyaldehyde are dissolved in an organic solvent, with the molar ratio of the primary amino group of the castor oil-based polyamine to the aldehyde group in the bio-based polyaldehyde being 1:0.5-0.
9. The mixture is stirred thoroughly until it is completely dissolved and degassed, and then poured into a polytetrafluoroethylene mold, heated and placed to evaporate the solvent, and then placed under vacuum conditions to remove trace amounts of the solvent, thereby obtaining a high biomass-based polyimine self-healing polymer.
4. The method for preparing a biomass-based polyimine self-healing polymer according to claim 3, characterized in that: In step (1), the molar ratio of the hydroxyl group in the castor oil to the carboxyl group in the acrylic acid is 1:3; the amount of the catalyst is 0.7 wt.%, and the amount of the inhibitor is 0.3 wt.%.
5. The method for preparing a biomass-based polyimine self-healing polymer according to claim 3, characterized in that: In step (1), the reaction conditions are as follows: the microwave reaction temperature is 80-120° C., and the reaction is carried out for 10-30 minutes.
6. The method for preparing a biomass-based polyimine self-healing polymer according to claim 3, characterized in that: In step (2), the molar ratio of double bonds to primary amine groups in the acrylated castor oil is 1:1.1, and the reaction conditions are room temperature for 12 to 24 hours.
7. The method for preparing a biomass-based polyimine self-healing polymer according to claim 3, characterized in that: In step (3), the organic solvent is tetrahydrofuran, N,N-dimethylformamide or N,N-dimethylacetamide, and the degassing method is static degassing, ultrasonic degassing or centrifugal degassing.
8. Use of the biomass-based polyimine self-healing polymer according to claim 1 in adhesives.
Citation Information
Cited By
A reprocessable bio-based cross-linked polyamide and preparation method thereof
CN118325075B