A carbon nanofiber / carbon black composite microporous layer and preparation method thereof

By depositing carbon nanofibers in situ on the surface of carbon black to form a grape bunch structure carbon nanofiber/carbon black composite microporous layer, the problem of insufficient conductivity and durability of the microporous layer in the existing technology is solved, and high conductivity is achieved and increased porosity, suitable for large-scale production.

CN114824272BActive Publication Date: 2024-10-18GUANGDONG HYDROGEN DEV NEW MATERIAL TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210391045.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-14
Publication Date
2024-10-18
Estimated Expiration
2042-04-14

AI Technical Summary

Technical Problem

The microporous layer in the existing gas diffusion layer is composed of a single conductive carbon powder and PTFE, resulting in weak point contact between carbon powder particles and the existence of microcracks that affect the conductivity and durability. It is also difficult to effectively adjust the pore structure, limiting the performance of the fuel cell. Output performance.

Method used

Using a carbon nanofiber/carbon black composite microporous layer, carbon nanofibers are deposited in situ on the surface of carbon black through vapor phase chemical deposition to form a special grape bunch structure, increase conductive paths and porosity, and improve conductivity and pore structure. Adjustability.

Benefits of technology

Significantly improves the conductivity and porosity of the microporous layer, reduces contact resistance, reduces the ohmic polarization of the battery, improves the output performance of the fuel cell in the 0.6~0.8V range, simplifies the preparation process, and reduces the cost. Suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114824272B_ABST
    Figure CN114824272B_ABST
Patent Text Reader

Abstract

The invention discloses a carbon nanofiber / carbon black composite microporous layer and a preparation method thereof. Conductive carbon black is loaded with transition metal salt by an impregnation method, and then carbon nanofibers are generated in situ by catalysis on the surface of carbon black by gas phase chemical deposition. The obtained carbon nanofiber / carbon black composite and alcohol solvent are ball milled, and then PTFE emulsion is added for ultrasonic dispersion to obtain carbon slurry; the carbon slurry is coated on hydrophobic carbon paper, and then dried and heat treated to obtain a composite microporous layer. The microporous layer uses a special grape bunch structure formed by connecting carbon nanofibers and carbon black particles, which can not only effectively increase the conductive path of the microporous layer, increase the conductivity of the microporous layer, and reduce the contact resistance, but also effectively adjust the microporous structure so that the microporous layer maintains a high porosity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a microporous layer, in particular to a carbon nanofiber / carbon black composite microporous layer and a preparation method thereof, belonging to the technical field of fuel cell materials. Background Art

[0002] With the increasing requirements for the volume power density of proton exchange membrane fuel cell (PEMFC) stacks, the gas diffusion layer is an important component of PEMFC. Improving the mass transfer capacity of the gas diffusion layer is the key to research. The gas diffusion layer is composed of a substrate and a microporous layer. Common gas diffusion layer substrate materials include carbon fiber paper, carbon fiber woven cloth, non-woven fabric, etc., while the main materials of the microporous layer include carbon nanofibers, carbon powder, graphite powder, etc. In the operating conditions of hydrogen fuel cells, the battery efficiency is highest in the range of 0.6~0.8V. In this range, ohmic polarization has the greatest impact on battery loss. It is necessary to increase the conductivity of the gas diffusion layer as much as possible to reduce the ohmic polarization of the battery and improve the output performance of the battery. In addition, the pore structure (pore size distribution and porosity) has an impact on the output performance of the fuel cell due to the transmission of gas and water. When the diffusion layer cannot discharge liquid water in time, the liquid water will hinder the transmission of gas and combine with the catalyst site to affect the battery performance. Therefore, it is particularly important to prepare suitable carbon materials and construct suitable pore structures to improve the performance of the battery.

[0003] At present, the microporous layer in the gas diffusion layer is mainly composed of conductive carbon powder and PTFE. The types of conductive carbon powder mainly include Vulcan XC-72R, Ketjen black, acetylene black, etc. The microporous layer prepared by using a single conductive carbon powder and PTFE has microcracks that affect conductivity and durability due to point contact between carbon powder particles and weak contact force. Summary of the invention

[0004] In view of the defects of the prior art, the first object of the present invention is to provide a carbon nanofiber / carbon black composite microporous layer. The microporous layer is prepared by in-situ depositing carbon nanofibers on the surface of carbon black by vapor phase chemical deposition, and the carbon black particles are connected into a special grape bunch structure by using carbon nanofibers. This structure can not only effectively increase the conductive path of the microporous layer, increase the electrical conductivity of the microporous layer, and reduce the contact resistance, but also effectively adjust the microporous structure so that the microporous layer maintains a high porosity.

[0005] The second object of the present invention is to provide a method for preparing a carbon nanofiber / carbon black composite microporous layer, which is simple to operate, low in cost and conducive to large-scale production.

[0006] In order to achieve the above technical objectives, the present invention provides a method for preparing a carbon nanofiber / carbon black composite microporous layer, which comprises the following steps:

[0007] 1) adding conductive carbon black into a transition metal salt solution and subjecting it to ultrasonic treatment, followed by filtering and drying to obtain carbon black loaded with transition metal salt;

[0008] 2) In-situ catalytic generation of carbon nanofibers on the surface of carbon black loaded with transition metal salts by vapor phase chemical deposition to obtain a carbon nanofiber / carbon black composite;

[0009] 3) After ball milling the carbon nanofiber / carbon black composite and the alcohol solvent, PTFE emulsion is added for ultrasonic dispersion to obtain a carbon slurry;

[0010] 4) Coating the carbon slurry on the hydrophobic carbon paper, and then drying and heat treating the paper to obtain the product.

[0011] The technical solution of the present invention firstly uniformly loads transition metal salts on the surface of carbon black by an impregnation method, and in the process of chemical vapor deposition, uses transition metal ions to in-situ catalyze the generation of carbon nanofibers on the surface of carbon black particles, so as to use the generated carbon nanofibers to connect the carbon black particles to form a special grape bunch structure. The carbon nanofibers, as the skeleton connecting the carbon black particles, have good conductivity and can form a good conductive path, thereby increasing the conductivity of the composite microporous layer and reducing the contact resistance. In addition, the special grape bunch structure formed by the carbon nanofibers and carbon black can effectively adjust the pore structure, so that the composite microporous layer maintains a high porosity, thereby achieving the improvement of the conductivity of the composite microporous layer without reducing its porosity.

[0012] As a preferred solution, the transition metal salt in the transition metal salt solution is at least one of sulfate, halogen or nitrate of copper and / or cobalt, and the solvent is an alcohol solvent. The transition metal salt contained in the transition metal salt solution is a soluble salt of transition metals such as copper and cobalt, such as nitrate, chloride, sulfate, etc., and the solvent contained generally uses water or alcohol as a solvent. In order to improve the wetting performance of carbon black, an alcohol solvent is generally used, and the alcohol solvent is ethanol, methanol, etc.

[0013] As a preferred solution, the transition metal salt concentration in the transition metal salt solution is 0.01 mol / L to 1 mol / L. The transition metal salt solution affects the loading amount of the transition metal salt on the carbon black surface. If the loading amount of the transition metal salt is too small, it is difficult to form carbon nanofibers. If too much transition metal salt introduces transition metal ions, the performance of the microporous layer is affected. A further preferred transition metal salt concentration is 0.05 mol / L to 0.5 mol / L.

[0014] As a preferred solution, the process of the vapor chemical deposition is: firstly heating under the condition of introducing an inert gas, when the temperature is raised to 450°C to 600°C, introducing hydrogen for reduction for 5 to 20 minutes, and then introducing a gaseous carbon source for deposition for 5 to 20 minutes. The vapor deposition conditions can regulate the amount of carbon nanofibers generated and the size of nanocarbon fibers. The generation of an appropriate amount of carbon nanofibers with an appropriate size on the surface of carbon black is beneficial to improving the pore structure and conductivity of the microporous layer. Inert gases such as argon, etc.

[0015] As a preferred solution, the gaseous carbon source is acetylene with a flow rate of 0.05-0.20 L / min, and the hydrogen flow rate is 0.3-0.8 L / min. The gaseous carbon source is a small molecule hydrocarbon commonly used in the prior art, such as acetylene, ethylene, methane, etc., preferably acetylene with a higher carbon-to-hydrogen ratio.

[0016] As a preferred solution, the mass percentage composition of PTFE and carbon nanofiber / carbon black composite in the carbon slurry is 20-30%: 70-80%.

[0017] As a preferred solution, the mass percentage concentration of PTFE in the carbon slurry is 1-10wt%,

[0018] As a preferred solution, the heat treatment temperature is 300-400° C. and the time is 20-40 minutes.

[0019] The ultrasonic treatment involved in the present invention is a conventional treatment process to promote the uniform dispersion of the conductive carbon black, and the preferred ultrasonic treatment time is 15 to 20 minutes.

[0020] The alcohol solvent involved in the present invention can be isopropanol, which serves not only as a solvent but also as a dispersant.

[0021] In the ball milling process involved in the present invention, the ball milling conditions are as follows: the rotation speed is 100-300 r / min, the ball milling time is 40-80 min, and each working time is 5-15 min and the pause time is 5-15 min.

[0022] The coating method involved in the present invention adopts blade coating, extrusion coating or screen printing, preferably blade coating.

[0023] The coating amount of the carbon slurry on the hydrophobic carbon paper is 0.5-3 mg / cm 2 Measurement.

[0024] The conductive carbon black involved in the present invention is Vulcan XC-72R carbon powder.

[0025] The invention also provides a carbon nanofiber / carbon black composite microporous layer, which is obtained by the preparation method.

[0026] The key to the carbon nanofiber / carbon black composite microporous layer provided by the technical solution of the present invention is that a carbon nanofiber / carbon black composite is used to prepare the microporous layer. The carbon nanofiber / carbon black composite is formed by connecting carbon nanofibers and carbon black particles to form a special grape bunch structure. It uses highly conductive carbon nanofibers as a skeleton to form a good conductive path, increase the conductivity of the composite microporous layer, and reduce the contact resistance. At the same time, it uses the special grape bunch structure formed by naturally curled carbon nanofibers and carbon black to effectively adjust the pore structure, so that the composite microporous layer maintains a high porosity, thereby achieving the improvement of the conductivity of the composite microporous layer while effectively improving the porosity of the microporous layer.

[0027] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:

[0028] The technical solution of the present invention realizes uniform loading of transition metal salt catalyst on the surface of conductive carbon black through liquid phase impregnation, and then in situ catalytic generation of carbon nanofibers and carbon black particles on the carbon black surface through vapor phase chemical deposition to form a special grape bunch structure. The carbon nanofibers as conductive skeletons can not only effectively increase the conductive path in the composite microporous layer, increase the conductivity of the composite microporous layer, and reduce the contact resistance, but also can utilize the special structure of carbon nanofibers and conductive carbon black particles to increase the porosity, thereby improving the conductivity of the composite microporous layer.

[0029] The technical solution of the present invention adopts a nanofiber / conductive carbon black composite with a special "grape bunch" structure to prepare a composite microporous layer. The carbon nanofiber can organically connect carbon black particles to form a conductive mesh structure, thereby enhancing the conductivity of the composite microporous layer. The grape bunch structure can effectively adjust the pore structure and increase the porosity of the composite micropores, thereby improving the conductivity of the microporous layer while maintaining the high porosity of the microporous layer. In addition, the microporous layer prepared using the nanofiber / conductive carbon black composite has a smooth surface and significantly reduced cracks, which has obvious technical advantages over the use of ordinary conductive carbon black.

[0030] The preparation method of the composite microporous layer of the technical solution of the present invention is simple, the raw material cost is low, and the chemical vapor deposition can also be realized in a rotary furnace and a deposition furnace to achieve mass production, which can effectively improve the production efficiency and is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is the SEM image of the microporous layer of the carbon nanofiber / carbon black composite prepared in Example 1.

[0032] Figure 2 This is the TEM image of the carbon nanofiber / carbon black composite prepared in Example 1.

[0033] Figure 3This is a comparison chart of the polarization performance curves of the composite microporous layer prepared in Example 1. DETAILED DESCRIPTION

[0034] The following specific implementations are intended to further illustrate the content of the present invention in detail, rather than to limit the scope of protection of the claims of the present invention.

[0035] Example 1

[0036] (1) Weigh 2.557 g CuCl2·2H2O and 1.189 g CoCl2·6H2O and dissolve them in 100 ml of alcohol and stir them ultrasonically for 10 min. Take 3 g Vulcan XC-72R carbon powder and add it to the catalyst solution. Ultrasonic dispersion is carried out for 30 min and then filtered. The filter residue is placed in an oven for drying. After drying, the agglomerated powder is ground into powder.

[0037] (2) Take 1 g of carbon powder loaded with catalyst and place it in a tube furnace for chemical vapor deposition. Add argon gas to increase the temperature. When the temperature reaches 500°C, add hydrogen for reduction for 10 minutes, and then add acetylene for deposition for 10 minutes.

[0038] (3) Take 0.8g of the sedimentation product and add it to a ball mill for dry grinding for 10min at a speed of 200r / min. Then add 15ml of isopropanol and wet grind for 60min. After working for 10min, pause for 10min for a total of 3 cycles. After taking out the slurry, add 4g of 5% PTFE and conduct ultrasonic dispersion for 30min.

[0039] (4) Take a 5×5 cm hydrophobic treated carbon paper and fix it. Use a lithium electric scraper to evenly coat the slurry and control the loading to 1.2 mg / cm 2 After the slurry is dried, it is heat treated at 350°C for 30 minutes.

[0040] The carbon black / carbon nanofiber composite microporous layer gas diffusion layer prepared in this embodiment has greatly improved conductivity compared with the traditional carbon black microporous layer gas diffusion layer, with a plane resistivity of 4.26mΩ·cm, while the latter is 10.28mΩ·cm. At the same time, it is flat and has significantly reduced cracks, which can significantly reduce the ohmic polarization of the battery and increase the output power of the battery in the range of 0.6~0.8V.

[0041] In Example 1: Surface morphology: Figure 1 and Figure 2 They are the SEM and TEM images of the samples in the example. The diameter of the carbon nanofibers is about 100~200nm. The carbon nanofibers act as a skeleton to connect the carbon particles to form a conductive path, which greatly improves the conductivity. The plane resistivity is 4.26mΩ·cm.

[0042] Battery performance: Figure 3This is a comparison of the polarization performance curves of the samples of Examples 1 to 3 and conventional single carbon powder (replacing carbon nanofiber / carbon black composite) as the gas diffusion layer in a single cell, where the sample size is 2×2 cm 2 The reaction gases are H2 and O 2, Relative humidity 100%RH, operating temperature 80℃. The results show that the ohmic polarization of the sample is significantly reduced, which improves the performance of the battery in the range of 0.6~0.8V.

[0043] Example 2

[0044] (1) Weigh 0.15 g of CoCl2·6H2O and dissolve it in 50 ml of alcohol with ultrasonic stirring. Take 3 g of Vulcan XC-72R carbon powder and add it to the catalyst solution. After ultrasonic dispersion for 30 min, place it in an oven to dry the alcohol. After drying, the carbon powder will agglomerate and grind into powder.

[0045] The subsequent steps are consistent with those in Example 1.

[0046] Example 3

[0047] The steps of Example 3 are the same as those of Example 1, except that the deposition temperature is changed to 600° C., hydrogen is introduced for reduction for 10 minutes, and then acetylene is introduced for deposition for 10 minutes.

[0048] Comparative Example

[0049] The only difference from Example 1 is that Vulcan XC-72R is used to directly prepare the microporous layer.

[0050] The following table shows the performance data of the samples in each embodiment.

[0051]

Claims

1. A method for preparing a carbon nanofiber / carbon black composite microporous layer, Features: The following steps are involved: 1) adding conductive carbon black into a transition metal salt solution for ultrasonic dispersion treatment, filtering and drying to obtain carbon black loaded with transition metal salt; 2) In-situ catalytic generation of carbon nanofibers by vapor phase chemical deposition on the surface of carbon black loaded with transition metal salts to obtain a carbon nanofiber / carbon black composite; the process of the vapor phase chemical deposition is: firstly heating under the condition of introducing an inert gas, when the temperature is raised to 450°C to 600°C, introducing hydrogen for reduction for 5 to 20 minutes, and then introducing a gaseous carbon source for deposition for 5 to 20 minutes; the gaseous carbon source is acetylene with a flow rate of 0.05 to 0.20 L / min, and the hydrogen flow rate is 0.3 to 0.8 L / min; 3) After ball milling the carbon nanofiber / carbon black composite and the alcohol solvent, PTFE emulsion is added for ultrasonic dispersion to obtain a carbon slurry; 4) Coating the carbon slurry on the hydrophobic carbon paper, and then drying and heat treating the paper to obtain the product.

2. The method for preparing a carbon nanofiber / carbon black composite microporous layer according to claim 1, Features: The transition metal salt in the transition metal salt solution is at least one of sulfate, halogen salt or nitrate of copper and / or cobalt, and the solvent is an alcohol solvent.

3. A method for preparing a carbon nanofiber / carbon black composite microporous layer according to claim 1 or 2, Features: The transition metal salt concentration in the transition metal salt solution is 0.01-1 mol / L.

4. The method for preparing a carbon nanofiber / carbon black composite microporous layer according to claim 1, Features: The mass percentage composition of the PTFE and the carbon nanofiber / carbon black composite in the carbon slurry is 20-30%:70-80%.

5. The method for preparing a carbon nanofiber / carbon black composite microporous layer according to claim 1, Features: The mass percentage concentration of PTFE in the carbon slurry is 1-10wt%.

6. The method for preparing a carbon nanofiber / carbon black composite microporous layer according to claim 1, Features: The heat treatment temperature is 300-400° C. and the time is 20-40 minutes.

7. A carbon nanofiber / carbon black composite microporous layer, Features: Obtained by the preparation method according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Method for producing carbon nanofibers, carbon composite and method for producing same

    CN104746181A

  • Novel gas diffusion layer structure and preparation method thereof

    CN109461940A

  • Electrode for fuel cell, fuel cell comprising the same, and method for preparing the same