Polyolefin composition
By using ethylene/α-olefin copolymer elastomers, alkenyl functionalized monocyclic organosiloxanes and organic peroxides in polyolefin compositions, the problem of insufficient thermal creep properties of polyolefin crosslinkers at high temperatures is solved problem, achieving high thermal stability of polyolefin compositions and improving the reliability of power cables.
Patent Information
- Application Number
- CN202080085705.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-19
- Filing Date
- 2020-12-11
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-12-11
AI Technical Summary
When existing polyolefin cross-linking agents are used at high temperatures, their thermal creep properties are insufficient, causing the insulation layer to deform or sag at high temperatures, affecting the reliability and maintenance costs of power cables.
A carrier mixture containing an ethylene/α-olefin copolymer elastomer, an effective cross-linking amount of alkenyl functionalized monocyclic organosiloxane and an organic peroxide is used to prepare a polyolefin composition with excellent thermal creep properties. Forms cross-linked polyolefin products for use in the insulation layer of power cables.
After being kept at 200°C for 15 minutes, the thermal creep of the polyolefin composition is less than 175%, which significantly improves the thermal stability of the insulation layer and the reliability of the power cable, and reduces maintenance costs.
Smart Images

Figure BDA0003684957970000251 
Figure BDA0003684957970000252 
Figure BDA0003684957970000261
Abstract
Description
[0001] Patents and patent application publications in this field include CN104277182A; US 2003 / 0166817 A1; US2015 / 0376386 A1; US 4,005,254; US 8,426,519 B2; WO 2014 / 130948 A1; WO 2018 / 200319A1; WO 2019 / 000311 A1; and WO 2019 / 000654 A1. Literature in this field includes LIU Gang et al., Study on cyclosiloxane containing vinylphenyl as crosslinking agent in polypropylene, NEW CHEMICAL MATERIALS, 2006, Vol. 34, No. 10, pp. 78-80.
[0002] Overview
[0003] Insulated electric conductors typically include a conductive core covered by an insulating layer. The conductive core may be solid or stranded (e.g., a bundle of wires). Some insulated electric conductors may also contain one or more additional elements, such as one or more semiconducting layers and / or protective sheaths (e.g., windings, tapes, or sheaths). Examples are coated metal wires and power cables, including those used in low voltage ("LV", >0 kilovolts to <5 kilovolts (kV)), medium voltage ("MV", 5kV to <69kV), high voltage ("HV", 69kV to 230kV) and extra high voltage ("EHV", >230kV) power transmission / distribution applications. Power cables may be evaluated using standard and / or IEC test methods.
[0004] WO 2018 / 200319 A1 recognizes that the operating temperature of power cables may be higher than the ambient temperature. Therefore, the wire and cable industry generally requires an insulation layer made of a networked polymer that has low elongation at high temperatures ("thermal creep") in field use.
[0005] The networked polymer is made by curing the crosslinkable polymer after extruding it as an uncured insulating layer directly onto the wire or onto the inner semiconductive layer covering the wire. The crosslinkable polymer must have a sufficiently high melt flow rate to enable it to be extruded. However, the higher the melt flow rate of the crosslinkable polymer, the higher the thermal creep of the networked polymer during field use. Various types of crosslinkable polymers / networked polymers that balance these competing property requirements are known in the industry. These crosslinkable polymers / networked polymers include crosslinkable polyolefins and their crosslinked polyolefin products (networked polymers). In the case of crosslinkable polyethylene, the melt flow rate (melt index) required by the industry is 2 grams per 10 minutes measured at 190 degrees Celsius (°C), 2.16 kilograms (kg), ASTM D1238-04, "melt index" or I2".
[0006] WO 2019 / 000654 A1 recognizes the problem of crosslinking and performance that damages previous polyolefins. Auxiliary agents can be blended with polyolefins to obtain polyolefin compositions with enhanced crosslinking ability, but conventional auxiliary agents have their limitations. For example, conventional auxiliary agents generally have limited solubility or miscibility in polyolefin compositions. This limits the maximum loading level of the auxiliary agent in the composition. The limited solubility or miscibility also causes the auxiliary agent to migrate to the surface of the composition (e.g., the surface of the pellet) undesirably, thereby limiting the storage life of the composition. Conventional auxiliary agents also bring other problems. For example, during curing, conventional auxiliary agents can produce crosslinked products with insufficient crosslinking degree. Or the composition may cure too slowly to be used in certain manufacturing operations (e.g., power cable manufacturing, injection molding, and film extrusion). Or the composition may cure prematurely (i.e., it is easy to scorch during cable extrusion, injection molding, and film extrusion). Not surprisingly, these problems limit the structure of conventional auxiliary agents that have been used with polyolefins. Typically, conventional auxiliary agents include conventional substructure groups bonded to two or more olefin crosslinking groups. Conventional substructural groups are acyclic polyvalent groups or cyclic polyvalent groups comprising a main chain or a ring, respectively, which contain carbon atoms and optionally nitrogen atoms and / or oxygen atoms in the main chain or the ring, respectively, but no silicon atoms.
[0007] This problem impairs the performance of power cables operating at higher voltages. Scorch can occur during the extrusion of the insulation layer and eventually lead to insulation failure. By using more resilient materials in the insulation layer, the time to reach such failure can be extended and thus the reliability of power transmission can be improved and maintenance costs reduced.
[0008] WO 2019 / 000654 A1 solves the problem of the insulating layer by using an auxiliary agent, which is an alkenyl functionalized monocyclic organosiloxane. Based on the total weight of the crosslinkable polyolefin composition, the crosslinkable polyolefin composition comprising an effective amount of alkenyl functionalized monocyclic organosiloxane for crosslinking can also include 0.01 wt % to 4.5 wt % (wt %) of an organic peroxide. An example with 0.50 wt % of dicumyl peroxide is disclosed. Summary of the invention
[0009] We have found that as the loading of the organic peroxide drops well below 0.50 wt%, the crosslinkable polyolefin composition may not achieve satisfactory thermal creep properties, also known as hot set performance. The more stringent global standard for power cable applications is a thermal creep of less than (<) 175% (percent) when held at 200°C for 15 minutes. If the thermal creep of the crosslinkable polyolefin composition of the insulation layer of the power cable is greater than (>) 175% after being held at 200°C for 15 minutes, the insulation layer may sag or deform during operation at high temperatures. The more the thermal creep exceeds 175%, the faster and / or more the insulation layer may sag or deform.
[0010] Although power cables may not withstand operating temperatures as high as 200°C, thermal creep testing is a reliable way for the industry to evaluate materials used for their insulation layers. In the power cable industry, a thermal creep of less than <175% passes the thermal creep test after the test sample is held at 200°C for 15 minutes. And a thermal creep of <100% after 15 minutes at 200°C is particularly desirable. Likewise, the residual elongation at room temperature should be <15% of the thermal creep value measured at 200°C.
[0011] Our technical solution to this problem includes a polyolefin composition comprising a carrier mixture and optionally one or more additives, wherein the carrier mixture comprises an ethylene / α-olefin copolymer elastomer having a melt index of 0.6 to 6.2 grams per 10 minutes (g / 10min), a crosslinking effective amount of an olefin-functionalized monocyclic organosiloxane, and 0.29 wt% to 0.44 wt% of an organic peroxide. Also included are crosslinked polyolefin products obtained by curing the polyolefin composition; methods for preparing the crosslinked polyolefin composition and using the crosslinked polyolefin composition; and articles containing the crosslinked polyolefin composition. The carrier mixture has satisfactory thermal creep. Depending on the amount and type of any optional additives, the crosslinkable polyolefin composition itself may also have satisfactory thermal creep.
[0012] The polyolefin compositions and products of the present invention are suitable for use in any application where polyolefins (including crosslinked polyolefins) are utilized, including extruded articles, coatings, films, sheets, and injection molded articles, as well as power transmission applications and other non-related applications such as containers or vehicle parts. DETAILED DESCRIPTION
[0013] The following are implementations of the technical solution, some of which are numbered for easier reference.
[0014] Aspect 1. A crosslinkable polyolefin composition comprising 100 to 30 wt% (wt%) of a carrier mixture and 0 to 70 wt% of one or more optional additives, respectively; wherein the carrier mixture is composed of 97.56 to 99.31 wt% (wt%) of (A) a polyethylene polymer, 0.40 to 2.0 wt% of an olefin-functionalized monocyclic organosiloxane, and 0.29 to 0.44 wt% of (C) an organic peroxide; wherein the (A) polyethylene polymer is selected from (A1) and (A2): (A1) an ethylene / α-olefin copolymer elastomer having a melt index of 0.6 to 6.2 grams per 10 minutes (g / 10min) and a density of 0.854 to 0.912 grams per cubic centimeter (g / cm3), according to A STMD792-13, method B, or (A2) (A1) and a blend of a low density polyethylene (LDPE), the melt index of the low density polyethylene (LDPE) being 0.8 g / 10 min to 2.5 g / 10 min, wherein the mass ratio of the weight of (A1) to the weight of (LDPE) ((A1) / (LDPE) wt / wt) of the blend is 99.9 / 0.1 to 1.0 / 3.0, alternatively 99.9 / 0.1 to 1.0 / 2.0, alternatively 99.9 / 0.1 to 1.0 / 1.0, alternatively 99.9 / 0.1 to 2.5 / 1.0, and wherein both melt indices are measured according to ASTM D1238-04 (190° C., 2.16 kg; “I2”); wherein the (B) alkenyl functionalized monocyclic organosiloxane has the formula (I): [R 1 ,R 2 SiO 2 / 2 ] n (I), wherein the subscript n is an integer greater than or equal to 3; each R 1 are independently (C2-C4)alkenyl or H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is H or methyl, and the subscript m is an integer from 1 to 4; and each R 2 are independently H, (C1-C4) alkyl, phenyl or R 1; And wherein after being kept at 200° C. for 15 minutes, the thermal creep of the carrier mixture of the crosslinkable polyolefin composition is less than 175%, as measured by the thermal creep test method (described later); Provided that the crosslinkable polyolefin composition does not contain (i.e., lacks) a phosphazene base; And provided that if the melt index (I2) of the (A1) ethylene / α-olefin copolymer elastomer is greater than 2 g / 10 min, then the amount of (C) organic peroxide is 0.35 wt % to 0.44 wt % of the carrier mixture. The total weight of ingredients (A), (B) and (C) is 100.00 wt % of the carrier mixture. The total weight of ingredients (A), (B), (C) and one or more optional additives (if any) is 100.00 wt % of the crosslinkable polyolefin composition. The crosslinkable polyolefin composition may not contain any ring-opening catalyst. In some embodiments, (A1) ethylene / α-olefin copolymer elastomer is ethylene / 1-octene copolymer elastomer or ethylene / 1-butene copolymer elastomer, alternatively (A1) is ethylene / 1-octene copolymer elastomer, alternatively (A1) is ethylene / 1-butene copolymer elastomer. In some embodiments, the thermal creep value is 23% to 145%, alternatively 23% to 87%, alternatively 23% to 82%, alternatively 24% to 45%, alternatively 24% to 29%.
[0015] Aspect 2. The crosslinkable polyolefin composition according to aspect 1, wherein the (A) polyethylene polymer is further limited by any one of limitations (i) to (vii): (i) the (A) polyethylene polymer is (A1) an ethylene / α-olefin copolymer elastomer; (ii) the (A) polyethylene polymer is the (A1) ethylene / α-olefin copolymer elastomer, and (A1) has a melt index of 0.80 g / 10 min to 5.4 g / 10 min, alternatively 0.9 g / 10 min to 5.1 g / 10 min and a density of 0.855 g / cm 3 Up to 0.912g / cm 3 , alternatively 0.855 g / cm 3 Up to 0.910g / cm 3 (iii) the (A) polyethylene polymer is the (A1) ethylene / α-olefin copolymer elastomer, and (A1) has a melt index of 0.80 g / 10 min to 5.4 g / 10 min, alternatively 1.1 g / 10 min to 5.1 g / 10 min and a density of 0.859 g / cm 3 Up to 0.890g / cm 3 , alternatively 0.861 g / cm 3 Up to 0.890g / cm 3(iv) the (A) polyethylene polymer is the (A2) blend, and (A2) is a blend of ethylene / α-olefin copolymer elastomers of any one of the restrictions (i) to (iii), and the LDPE has a melt index (I2) of 1.75 g / 10 min to 2.49 g / 10 min and a density of 0.918 g / cm 3 Up to 0.920g / cm 3 (v) the (A) polyethylene polymer is the (A2) blend, and (A2) is a blend of ethylene / α-olefin copolymer elastomers of any one of the restrictions (i) to (iii), and the LDPE has a melt index (I2) of 2.4 g / 10 min and a density of 0.920 g / cm 3 (vi) the (A) polyethylene polymer is the (A2) blend, and (A2) is a blend of ethylene / α-olefin copolymer elastomers of any one of the restrictions (i) to (iii), and the LDPE has a melt index (I2) of 1.9 g / 10 min and a density of 0.9183 g / cm 3 and (vii) the (A) polyethylene polymer is the (A2) blend, and (A2) is a blend of ethylene / α-olefin copolymer elastomers of any one of the restrictions (i) to (iii), and the LDPE has a melt index (I2) of 0.80 g / 10 min to 1.24 g / 10 min and a density of 0.917 g / cm 3 Up to 0.923g / cm 3 The (A) polyethylene polymer may be 98.2 wt% to 98.6 wt% of the carrier mixture and / or the carrier mixture may be 99.4 wt% to 99.90 wt% of the crosslinkable polyolefin composition.
[0016] Aspect 3. The crosslinkable polyolefin composition according to aspect 1 or 2, wherein the subscript n is 4, and the monocyclic organosiloxane of formula (B) (I) is described by any one of restrictions (i) to (x): (i) each R 1 is independently (C2-C3)alkenyl; and each R 2 are independently H, (C1-C2)alkyl or (C2-C3)alkenyl; (ii) each R 1 is vinyl; and each R 2 are independently (C1-C2)alkyl; (iii) each R 1 is vinyl; and each R 2 is methyl; (iv) each R 1 is allyl; and each R 2are independently (C1-C2)alkyl; (v) each R 1 is allyl; and each R 2 is methyl; (vi) each R 1 is independently H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is H or methyl, and the subscript m is an integer from 1 to 4; and each R 2 are independently H, (C1-C2)alkyl or (C2-C3)alkenyl; (vii) each R 1 is independently H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is H and the subscript m is 3; and each R 2 are independently (C1-C2)alkyl; (viii) each R 1 is independently H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is methyl and the subscript m is 3; and each R 2 is independently a (C1-C2) alkyl group; (ix) the crosslinkable polyolefin composition does not contain 24 wt% or more, alternatively does not contain 22 wt% or more, alternatively does not contain 20.0 wt% or more, alternatively does not contain 15 wt% or more, alternatively does not contain 10 wt% or more, alternatively does not contain any inorganic filler; and (x) a combination of limitation (ix) and any one of limitations (i) to (viii). In some aspects, (B) the monocyclic organosiloxane of formula (I) is 2,4,6,8-tetramethyl-2,4,6,8-tetraacetyl-cyclotetrasiloxane, "(D Vi )4”, (CAS No. 2554-06-5).
[0017] Aspect 4. The crosslinkable polyolefin composition according to any one of aspects 1 to 3, further comprising 0.01 wt% to 0.10 wt% of (D) an anti-scorch agent or 0.10 wt% to 0.30 wt% of (E) an antioxidant or a combination of (D) and (E); and wherein the embodiment of the crosslinkable polyolefin composition consisting of components (A) to (E) has a thermal creep of less than 175% after being held at 200°C for 15 minutes, as measured by the Thermal Creep Test Method. In some aspects, (D) is alpha-methylstyrene dimer (AMSD), and (E) is 4,6-bis(octylthiomethyl)-2-methyl-phenol (also known as 4,6-bis(octylthiomethyl)-o-cresol). In some embodiments of any one of aspects 1 to 6, embodiments of the crosslinkable polyolefin composition consisting of ingredients (A) to (E) also have a significant degree of crosslinking, as indicated by a MH greater than (>) 2.0 dN-m, alternatively > 2.5 dN-m, alternatively > 3.0 dN-m (e.g., 2.5 dN-m to 4.0 dN-m), as measured by the Moving Die Rheometer Test Method (described later). In some embodiments, the MH value is 2.1 dN-m to 5.4 dN-m, alternatively 2.7 dN-m to 5.1 dN-m, alternatively 2.8 dN-m to 5.1 dN-m, alternatively 3.1 dN-m to 5.1 dN-m, alternatively 3.7 dN-m to 5.1 dN-m. Inventive Examples IE1 to IE6 described later have shown that embodiments of the crosslinkable polyolefin compositions composed of components (A) to (E) are shown to have a thermal creep of less than 175% after being kept at 200° C. for 15 minutes, as measured by the thermal creep test method, and have a significant degree of crosslinking, as indicated by MH greater than (>) 2.0 dN-m, alternatively >2.5 dN-m, alternatively >3.0 dN-m (e.g., 2.5 dN-m to 4.0 dN-m), as measured by the moving die rheometer test method. In some embodiments, the MH value is as described above, and the thermal creep value is 23% to 145%, alternatively 23% to 87%, alternatively 23% to 82%, alternatively 24% to 45%, alternatively 24% to 29%.
[0018] Aspect 5. A crosslinkable polyolefin composition according to any one of Aspects 1 to 4, wherein the crosslinkable composition comprises the carrier mixture and the one or more additives; wherein the one or more additives are selected from the group consisting of additives (F) to (M): (F) filler; (G) flame retardant; (H) hindered amine stabilizer; (I) anti-tree agent; (J) methyl radical scavenger; (K) conventional auxiliary agents, (L) nucleating agent and (M) carbon black; provided that the (F) filler does not include any previously omitted filler. The total amount of one or more additives (F) to (M) can be 0.1wt% to 69wt%, alternatively 0.1wt% to 20wt%, alternatively 0.1wt% to 10wt%, alternatively 0.1wt% to 5.0wt% of the crosslinkable polyolefin composition, and the carrier mixture can be 99.9wt% to 31wt%, alternatively 99.9wt% to 80wt%, alternatively 99.9wt% to 90wt%, alternatively 99.9wt% to 95.0wt% of the crosslinkable polyolefin composition, respectively. In some aspects, the crosslinkable polyolefin composition is any one of the inventive examples IE1 to IE6 described later, alternatively any one of IE1 to IE3, IE5 and IE6.
[0019] Aspect 6. A method for preparing a crosslinkable polyolefin composition according to Aspect 1, the method comprising mixing together the amount of the (A) polyethylene polymer, the amount of the (B) monocyclic organosiloxane of formula (I), and the amount of the (C) organic peroxide to prepare the carrier mixture.
[0020] Aspect 7. A method for free radical curing a crosslinkable polyolefin composition according to any one of aspects 1 to 5 to prepare a crosslinked polyolefin product, the method comprising heating the crosslinkable polyolefin composition at a curing effective temperature in a manner to react the (A) polyethylene polymer with the (B) monocyclic organosiloxane of formula (I), thereby preparing a crosslinked polyolefin product. The crosslinked polyolefin product does not contain a phosphazene base, but instead any ring-opening catalyst and products obtained therefrom. In some aspects, the crosslinkable polyolefin composition obtained by the method is a crosslinkable polyolefin composition according to any one of aspects 1 to 5.
[0021] Aspect 8. A crosslinked polyolefin product, the crosslinked polyolefin product being made by the method according to aspect 7. In some embodiments, after being kept at 182° C. for 12 minutes in a moving die rheometer, the crosslinkable polyolefin composition allows embodiments of the crosslinked polyolefin product to have a significant degree of crosslinking, as indicated by a MH greater than (>) 2.0 dN-m, alternatively >2.5 dN-m, alternatively >3.0 dN-m. These values are a remarkable achievement in just 12 minutes. In some embodiments, the MH value is 2.1 dN-m to 5.4 dN-m, alternatively 2.7 dN-m to 5.1 dN-m, alternatively 2.8 dN-m to 5.1 dN-m, alternatively 3.1 dN-m to 5.1 dN-m, alternatively 3.7 dN-m to 5.1 dN-m.
[0022] Aspect 9. A manufactured product comprising the crosslinkable polyolefin composition according to any one of aspects 1 to 5 or the crosslinked polyolefin product according to aspect 10 in a shaped form. In some aspects, the manufactured product is selected from the group consisting of: coatings, films, sheets, extruded articles, and injection molded articles. For example, coated conductors, coatings for wires and cables for transmitting power or telecommunications, agricultural films, food packaging, garment bags, grocery bags, thick-walled bags, industrial sheets, pallets and shrink wrap, bags, buckets, freezer containers, lids, toys.
[0023] Aspect 10. A coated conductor comprising a conductive core and an insulating layer at least partially covering the conductive core, wherein at least a portion of the insulating layer comprises the crosslinkable polyolefin composition according to any one of aspects 1 to 5 or the crosslinked polyolefin product according to aspect 8. An embodiment of the conductive core may be an electric wire having a proximal end and a distal end, wherein at least one end may be free of an insulating layer.
[0024] Aspect 11. A method of transmitting electricity, the method comprising applying a voltage to the conductive core of the coated conductor according to aspect 10 to generate an electric current through the conductive core. The conductive core may be a wire having a proximal end and a distal end, and electricity may flow from one end of the wire to the other end.
[0025] The crosslinkable polyolefin composition and the crosslinked polyolefin product made therefrom may be free of telechelic polyolefin and the crosslinked polyolefin product made therefrom, respectively.Telechelic polyolefin molecules have a main chain with a terminal olefin group at each end.
[0026] In some aspects, the crosslinkable polyolefin composition is of aspect 1 or 2, wherein the subscript n is 3, and (B) the monocyclic organosiloxane of formula (I) is described by any one of limitations (i) to (x): (i) each R 1 is independently (C2-C3)alkenyl; and each R 2are independently H, (C1-C2)alkyl or (C2-C3)alkenyl; (ii) each R 1 is vinyl; and each R 2 are independently (C1-C2)alkyl; (iii) each R 1 is vinyl; and each R 2 is methyl; (iv) each R 1 is allyl; and each R 2 are independently (C1-C2)alkyl; (v) each R 1 is allyl; and each R 2 is methyl; (vi) each R 1 is independently H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is H or methyl, and the subscript m is an integer from 1 to 4; and each R 2 are independently H, (C1-C2)alkyl or (C2-C3)alkenyl; (vii) each R 1 is independently H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is H and the subscript m is 3; and each R 2 are independently (C1-C2)alkyl; (viii) each R 1 is independently H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is methyl and the subscript m is 3; and each R 2 is independently a (C1-C2) alkyl group; (ix) the crosslinkable polyolefin composition does not contain 24 wt% or more, alternatively does not contain 22 wt% or more, alternatively does not contain 20.0 wt% or more, alternatively does not contain 15 wt% or more, alternatively does not contain 10 wt% or more, alternatively does not contain an inorganic filler selected from the group consisting of: aluminum oxide, aluminum silicate, calcium silicate, magnesium silicate, silicon dioxide, titanium dioxide and mixtures thereof; and (x) a combination of limitation (ix) and any one of limitations (i) to (viii).
[0027] In some aspects, the crosslinkable polyolefin composition is of aspect 1 or 2, wherein the subscript n is 5 or 6, and (B) the monocyclic organosiloxane of formula (I) is described by any one of limitations (i) to (x): (i) each R 1 is independently (C2-C3)alkenyl; and each R 2are independently H, (C1-C2)alkyl or (C2-C3)alkenyl; (ii) each R 1 is vinyl; and each R 2 are independently (C1-C2)alkyl; (iii) each R 1 is vinyl; and each R 2 is methyl; (iv) each R 1 is allyl; and each R 2 are independently (C1-C2)alkyl; (v) each R 1 is allyl; and each R 2 is methyl; (vi) each R 1 is independently H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is H or methyl, and the subscript m is an integer from 1 to 4; and each R 2 are independently H, (C1-C2)alkyl or (C2-C3)alkenyl; (vii) each R 1 is independently H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is H and the subscript m is 3; and each R 2 are independently (C1-C2)alkyl; (viii) each R 1 is independently H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is methyl and the subscript m is 3; and each R 2 is independently a (C1-C2) alkyl group; (ix) the crosslinkable polyolefin composition does not contain 24 wt% or more, alternatively does not contain 22 wt% or more, alternatively does not contain 20.0 wt% or more, alternatively does not contain 15 wt% or more, alternatively does not contain 10 wt% or more, alternatively does not contain an inorganic filler selected from the group consisting of: aluminum oxide, aluminum silicate, calcium silicate, magnesium silicate, silicon dioxide, titanium dioxide and mixtures thereof; and (x) a combination of limitation (ix) and any one of limitations (i) to (viii).
[0028] In some aspects, the crosslinkable polyolefin composition does not contain any ring-opening catalyst. In some aspects, when the subscript n is 4, the crosslinkable polyolefin composition does not contain 24 wt% or more, alternatively does not contain 22 wt% or more, alternatively does not contain 20.0 wt% or more, alternatively does not contain 15 wt% or more, alternatively does not contain 10 wt% or more, alternatively does not contain inorganic fillers selected from the group consisting of: aluminum oxide, aluminum silicate, calcium silicate, magnesium silicate, silicon dioxide, titanium dioxide and mixtures thereof. In some aspects, n is 3, 4, 5 or 6; alternatively 3, 4 or 5; alternatively 5 or 6; alternatively 3 or 4; alternatively 3; alternatively 4; alternatively 5; alternatively 6.
[0029] The carrier mixture of the crosslinkable polyolefin composition has a thermal creep of less than 175% after being kept at 200°C for 15 minutes, alternatively a thermal creep of <100% after being kept at 200°C for 15 minutes. Depending on the amount and type of any optional additives, the crosslinkable polyolefin composition itself may also have a thermal creep of less than 175% after being kept at 200°C for 15 minutes, alternatively a thermal creep of <100% after being kept at 200°C for 15 minutes. In some embodiments, the thermal creep value is 23% to 145%, alternatively 23% to 87%, alternatively 23% to 82%, alternatively 24% to 45%, alternatively 24% to 29%. Without being bound by theory, it is believed that when the melt index (I2) of the (A1) ethylene / α-olefin copolymer elastomer is higher than 2.0 g / 10 min, the loading amount of (C) organic peroxide required for the carrier mixture to achieve a thermal creep of less than 175% after being kept at 200°C for 15 minutes is higher. This is because if the melt index (I2) of the (A1) ethylene / α-olefin copolymer elastomer is greater than 2 g / 10 min, the amount of the (C) organic peroxide is 0.35 wt% to 0.44 wt%.
[0030] In some embodiments, after being kept at 182° C. for 12 minutes in a moving die rheometer, the carrier mixture of the crosslinkable polyolefin composition causes the crosslinked polyolefin product to have a significant degree of crosslinking, as indicated by a MH greater than (>) 2.0 dN-m, alternatively > 2.5 dN-m, alternatively > 3.0 dN-m (e.g., 2.5 dN-m to 4.0 dN-m). These values are a remarkable achievement in just 12 minutes. Depending on the amount and type of any optional additives, the crosslinkable polyolefin composition itself can have a significant degree of crosslinking, as indicated by a MH greater than (>) 2.0 dN-m, alternatively > 2.5 dN-m, alternatively > 3.0 dN-m (e.g., 2.5 dN-m to 4.0 dN-m). In some embodiments, the MH value is 2.1 dN-m to 5.4 dN-m, alternatively 2.7 dN-m to 5.1 dN-m, alternatively 2.8 dN-m to 5.1 dN-m, alternatively 3.1 dN-m to 5.1 dN-m, alternatively 3.7 dN-m to 5.1 dN-m.
[0031] In some embodiments, the crosslinkable polyolefin composition further comprises one or more additives, and the type and amount of one or more optional additives (e.g., ingredients (D) and (E)) are such that the crosslinkable polyolefin composition itself may also have a thermal creep of less than 175% after being kept at 200° C. for 15 minutes, alternatively a thermal creep of <100% after being kept at 200° C. for 15 minutes. In some embodiments, the thermal creep value is 23% to 145%, alternatively 23% to 87%, alternatively 23% to 82%, alternatively 24% to 45%, alternatively 24% to 29%. In some such embodiments, the crosslinkable polyolefin composition itself may also have a significant degree of crosslinking, as indicated by MH greater than (>) 2.0 dN-m, alternatively >2.5 dN-m, alternatively >3.0 dN-m (e.g., 2.5 dN-m to 4.0 dN-m). In some embodiments, the MH value is 2.1 dN-m to 5.4 dN-m, alternatively 2.7 dN-m to 5.1 dN-m, alternatively 2.8 dN-m to 5.1 dN-m, alternatively 3.1 dN-m to 5.1 dN-m, alternatively 3.7 dN-m to 5.1 dN-m
[0032] The polyolefin composition of the present invention containing polyolefin polymer and alkenyl functionalized monocyclic organosiloxane can be cured (crosslinked) via irradiation or organic peroxide, and alkenyl functionalized monocyclic organosiloxane can not open ring.The curing reaction is carried out in a way that alkenyl functionalized monocyclic organosiloxane does not obtain polymerized siloxane (silicone polymer).Not bound by theory, it is believed that the composition of the crosslinkable polyolefin composition is selected so that during the curing period of the crosslinkable polyolefin composition, alkenyl functionalized monocyclic organosiloxane can not open ring to obtain the silanol (S-OH)-functionalized organosiloxane oligomer (straight or branched chain) of ring opening, and therefore the polymerized siloxane (silicone polymer) can not be formed in situ in the polyolefin polymer.Alkenyl functionalized monocyclic organosiloxane can not open ring at least in part, because the crosslinkable polyolefin composition does not contain a ring opening catalyst, and therefore the curing reaction is carried out in the absence of a ring opening catalyst.The ring opening catalyst excluded is known and comprises phosphazene base. Phosphazene bases have a core structure P=N, wherein the free N valences are attached to hydrogen, a hydrocarbon group, -P=N or =P-N, and the free P valences are attached to =N or -N. Examples of phosphazene bases are found in US Pat. No. 8,426,519 B2, column 9, line 29 to column 10, line 31. Other types of ring-opening catalysts are known to be excluded from crosslinkable polyolefin compositions and hence from the crosslinked polyolefin products prepared therefrom. See, for example, FO. Stark et al., Silicones, Comprehensive Organometallic Chemistry, Vol. 2, 305, Pergamon Press (1982). Examples are strong acids such as trifluoromethanesulfonic acid and its metal salts, sulfuric acid, perchloric acid and hydrochloric acid; cationic ring-opening catalysts such as metal halides; and anionic ring-opening catalysts such as organolithium, alkali metal oxides and alkali metal hydroxides. In the absence of a ring-opening catalyst, the polyolefin composition of the present invention undergoes crosslinking of the alkenyl functionalized monocyclic organosiloxane with the polyolefin polymer via free radical curing to form a crosslinked polyolefin product. The crosslinking of the present invention advantageously occurs without the alkenyl functionalized monocyclic organosiloxane ring opening even in the presence of ambient moisture. The crosslinking embodiment of the present invention avoids the deleterious effects of phosphazene bases on the level of crosslinking (degree of crosslinking or degree of crosslinking).
[0033] Unexpectedly, the inventive polyolefin compositions containing an alkenyl functionalized monocyclic organosiloxane or the inventive crosslinked polyolefin products prepared therefrom have improved hot creep properties after being held at 200°C for 15 minutes.
[0034] As used herein, the term "ring-opening catalyst" refers to a substance that initiates and / or enhances the rate of the ring-opening polymerization reaction of a cyclic siloxane monomer.
[0035] The term "ring-opening polymerization" as used herein is a type of chain growth polymerization reaction in which the reactive end of a polymer chain opens the ring of a cyclic monomer to give a longer polymer chain.
[0036] Crosslinkable polyolefin composition and its carrier mixture can be made by multiple different ways.In some respects, crosslinkable polyolefin composition and its carrier mixture can be made by the melt of (A) polyolefin polymer and the monocyclic organosiloxane of (B) formula (I) and (C) organic peroxide to obtain the embodiment of the crosslinkable polyolefin composition of carrier mixture and being composed of carrier mixture.In other respects, crosslinkable polyolefin composition and its carrier mixture can be made by the melt of (A) polyolefin polymer and the monocyclic organosiloxane of (B) formula (I) and (C) organic peroxide and any optional component (for example, any zero, one or more components (D) to (M)) to obtain the crosslinkable polyolefin composition of the admixture as component (A), (B), (C) and any optional component. In other aspects, the crosslinkable polyolefin composition and its carrier mixture can be prepared by mixing (A) a melt of a polyolefin polymer with (B) a monocyclic organosiloxane of formula (I) to obtain a premix, cooling the premix to a temperature below 100°C (e.g., 20°C to 80°C), and soaking or absorbing (C) an organic peroxide into the premix to obtain a carrier mixture and an embodiment of a crosslinkable polyolefin composition consisting of a carrier mixture. Mixing can include compounding, kneading or extrusion. In order to facilitate mixing, one or more ingredients (e.g., (B), additives (C), (D), (E), etc.) can be provided in the form of an additive masterbatch in a portion of (A).
[0037] On the other hand, the crosslinkable polyolefin composition can be prepared by contacting (B) a monocyclic organosiloxane of formula (I), (C) an organic peroxide and optionally zero, one or more of any optional ingredients (e.g., (D) an anti-scorch agent and / or (E) an antioxidant) with a non-molten form of (A) a polyolefin polymer to obtain a crosslinkable polyolefin composition as an admixture of ingredients (A), (B), (C) and any optional ingredients. The contact may comprise soaking, inhalation or injection. Ingredients (B), (C) and any optional ingredients may be independently combined by compounding, extrusion, inhalation, injection, kneading or soaking. The mixing or contacting may be carried out at a temperature of about 20° C. to 100° C. for 0.1 hour to 100 hours, for example, at 60° C. to 80° C. for 0.1 hour to 24 hours. Higher temperatures may be used for mixing or contacting provided that the (C) organic peroxide is not subjected to the higher temperature. Thereafter, if desired, the admixture may be cooled to a temperature below the decomposition temperature of the peroxide before mixing or contacting the admixture with (C) the organic peroxide. If desired, the crosslinkable polyolefin composition may be cooled to a storage temperature (e.g., 23° C.) and stored for a period of 1 hour, 1 week, 1 month, or longer.
[0038] The crosslinkable polyolefin composition may be prepared as a one-part formulation, alternatively a multi-part formulation, such as a two-part formulation, alternatively a three-part formulation. There is no inherent reason why one or more of these formulations could not include any combination of components.
[0039] The melt index is 0.6 g / 10 min to 6.2 g / 10 min and the density is 0.854 g / cm 3 Up to 0.912g / cm 3 The (A1) ethylene / α-olefin copolymer elastomer may be a single such ethylene / α-olefin copolymer elastomer or a blend of any two or more such ethylene / α-olefin copolymer elastomers.
[0040] The melt index is 0.6 g / 10 min to 6.2 g / 10 min and the density is 0.854 g / cm 3 To 0.912g / cm 3 The component (A1) of the ethylene / α-olefin elastomer copolymer may be selected from the following ENGAGE TM Ethylene / 1-octene copolymer: ENGAGE TM 8100 (I2 = 1g / 10min, density 0.870g / cm 3 )、8107(I2=1g / 10min, density is 0.870g / cm 3 ), 8200 (I2 = 5g / 10min, density is 0.870g / cm 3), 8207 (I2 = 5g / 10min, density 0.870g / cm 3 )、8452(I2=3g / 10min, density is 0.875g / cm 3 )、8003(I2=1g / 10min, density is 0.885g / cm 3 )、8440(I2=1.6g / 10min, density is 0.897g / cm 3 ), 8480 (I2 = 1g / 10min, density is 0.902g / cm 3 )、8450(I2=3g / 10min, density is 0.902g / cm 3 )、8540(I2=1g / 10min, density is 0.908g / cm 3 ) and 8842 (I2 = 1g / 10min, density 0.857g / cm 3 ), all of which were obtained from The Dow Chemical Company.
[0041] The component (A1) ethylene / α-olefin copolymer elastomer having a melt index of 0.6 g / 10 min to 6.2 g / 10 min and a density of 0.854 g / 10 min to 0.912 g / 10 min may be selected from the following ENGAGE TM Ethylene / 1-butene copolymer: ENGAGE TM 7487 (I2 = 1.2 g / 10 min, density 0.862 g / cm 3 ), 7457 (I2 = 3.6 g / 10 min, density 0.862 g / cm 3 ), 7447 (I2 = 5g / 10min, density 0.865g / cm 3 ), 7367 (I2 = 0.8 g / 10 min, density 0.874 g / cm 3 ), 7270 (I2 = 0.8 g / 10m, density 0.880 g / cm 3 ), 7277 (I2 = 0.8 g / 10 min, density 0.880 g / cm 3 ) and 7256 (I2 = 2.5 g / 10 min, density 0.885 g / cm 3 ), all of which were obtained from The Dow Chemical Company.
[0042] (A2): A blend of (A1) and a LDPE having a melt index of 1.50 to 2.49 g / 10 min, wherein the LDPE may be a single such LDPE or a blend of any two or more such LDPEs.
[0043] (A2): a blend of (A1) and a LDPE having a melt index of 1.50 g / 10 min to 2.49 g / 10 min, wherein the LDPE may be selected from the following LDPEs: LDPE-1(I2 1.9 g / 10 min and a density of 0.9183 g / cm 3 ), LDPE-2 (I 22.4g / 10min and density 0.920g / cm 3 ) and LDPE-3 (I2 1.0g / 10min and density 0.920g / cm 3 ), all of which were obtained from The Dow Chemical Company.
[0044] (A) polyolefin polymers can be made by any suitable method, many of which are well known in the art. Any conventional or later found production method for producing polyolefin polymers can be used to prepare (A). Typically, the production method comprises one or more polymerization reactions.
[0045] Ingredient (B) Monocyclic organosiloxane of formula (I): a molecule containing a monocyclic substructure consisting of silicon atoms and oxygen atoms arranged in an alternating arrangement; and an unsaturated organic group; and optionally H, a saturated or aromatic substituent; wherein there are at least two unsaturated organic groups, and each of the at least two silicon atoms in the ring substructure has at least one unsaturated organic group bonded thereto, and wherein any remaining valences of the silicon atoms after taking into account the unsaturated organic groups and the oxygen atoms are bonded to H, a saturated or aromatic substituent; or a collection of such molecules. Ingredient (B) may be a monocyclic organosiloxane consisting of a 6-membered ring (n=3), an 8-membered ring (n=4), a 10-membered ring (n=5), or a 12-membered ring (n=6). The ring substructure is composed of units of formula (I): [R 1 ,R 2 SiO 2 / 2 ] n (I), where subscripts n, R 1 and R 2 As defined previously. 1 ,R 2 SiO 2 / 2 ] unit, its R 1 Group and R 2 The unit may be simply named D using conventional organosiloxane abbreviations. R1,R2 , so that formula (I) becomes [D R1,R2 ] n . R 1 With R 2 May be the same, alternatively different.
[0046] In some aspects of the monocyclic organosiloxane of formula (I), R 1 It is vinyl and R 2 is ethyl, and (B) is D Vi,Et , wherein Vi is vinyl and Et is ethyl; alternatively, R 1 is allyl and R 2 is ethyl, and (B) is D 烯丙基,Et Alternatively, R 1 is butenyl (H2C=C(H)CH2CH2-) and R 2 is ethyl, and (B) is D 丁烯基,Et In some aspects, R 1 It is vinyl and R 2 is vinyl, and (B) is D Vi,Vi Alternatively, R 1 is allyl and R 2 is allyl, and (B) is D 烯丙基,烯丙基 Alternatively, R 1 is butenyl (H2C=C(H)CH2CH2-) and R 2 is butenyl, and (B) is D 丁烯基,丁烯基 In some aspects, R 1 It is vinyl and R 2 is phenyl, and (B) is D Vi,Ph , wherein Ph is phenyl; alternatively, R 1 is allyl and R 2 is phenyl, and (B) is D 烯丙基,Ph Alternatively, R 1 is butenyl (H2C=C(H)CH2CH2-) and R 2 is phenyl, and (B) is D 丁烯基,Ph When R 2 When it is a methyl group (CH3), the unit can be more simply named D R1 , so that formula (I) becomes [D R1 ] n In some aspects, R 1 It is vinyl and R 2 is methyl, and (B) is D Vi Alternatively, R 1 is allyl and R 2 is methyl, and (B) is D 乙烯基 Alternatively, R 1 is butenyl (H2C=C(H)CH2CH2-) and R 2 is methyl, and (B) is D 丁烯基In some embodiments, (B) is 2,4,6-trimethyl-2,4,6-trivinyl-cyclotrisiloxane, "(D Vi )3" (CAS No. 3901-77-7); 2,4,6,8-tetramethyl-2,4,6,8-tetravinyl-cyclotritetrasiloxane, "(D Vi )4" (CAS No. 2554-06-5); or a combination thereof.
[0047] In some aspects of the monocyclic organosiloxane of formula (I) (B), each R 1 is independently H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a and subscript m are as previously defined. In some aspects, R 1a is H, alternatively R 1a is methyl. In some aspects, subscript m is 1, 2, or 3; alternatively, m is 2, 3, or 4; alternatively, m is 2 or 3; alternatively, m is 1; alternatively, m is 2; alternatively, m is 3; alternatively, m is 4. In some aspects, each R 2 is independently (C1-C2)alkyl or (C2-C3)alkenyl; alternatively, each R 2 is independently (C1-C2)alkyl; alternatively, each R 2 is independently methyl.
[0048] The amount of ingredient (B) monocyclic organosiloxane of formula (I) in the crosslinkable polyolefin composition may be 0.41 wt% to 1.91 wt%, alternatively 0.8 wt% to 1.6 wt%, alternatively 1.0 wt% to 1.4 wt%, alternatively 1.15 wt% to 1.24 wt%; all based on the weight of the carrier mixture, alternatively the weight of the crosslinkable polyolefin composition.
[0049] In embodiments of the crosslinkable polyolefin composition containing (F) filler, the amount of ingredient (B) monocyclic organosiloxane of formula (I) in the crosslinkable polyolefin composition may be higher than in embodiments of the crosslinkable polyolefin composition without (F) filler.
[0050] With respect to determining the amount of ingredient (B), the presence of crosslinking can be detected by the torque increase using a moving die rheometer (MDR). In some aspects, the presence of crosslinking can be detected as solvent extraction percentage (Ext%). Ext% = W1 / Wo*100%, where W1 is the weight after extraction, Wo is the original weight before extraction, / indicates division, and * indicates multiplication. The presence of crosslinking can be detected by carbon-13 or silicon-29 nuclear magnetic resonance ( 13 C-NMR spectroscopy and / or 29Si-NMR) spectroscopy is used to detect the unsaturated organic groups (e.g., R 1 )'s carbon-carbon double bonds are absent or at reduced levels.
[0051] Ingredient (C) organic peroxide: a molecule containing carbon atoms, hydrogen atoms and two or more oxygen atoms and having at least one -OO- group, provided that when more than one -OO- group is present, each -OO- group is indirectly bonded to another -OO- group via one or more carbon atoms, or a collection of such molecules. (C) organic peroxide may be added to the crosslinkable polyolefin composition for curing, which comprises heating the crosslinkable polyolefin composition comprising ingredients (A), (B) and (C) to a temperature at or above the decomposition temperature of (C) organic peroxide. (C) organic peroxide may be of formula R O -OOR O A monoperoxide, where each R O Independently (C1-C 20 )alkyl or (C6-C 20 ) aryl. Each (C1-C 20 ) alkyl is independently unsubstituted or substituted with 1 or 2 (C6-C 12 ) aryl substituted. Each (C6-C 20 ) aryl is unsubstituted or substituted with 1 to 4 (C1-C 10 Alternatively, (C) may be of the formula R O -OOROOR O A diperoxide, wherein R is a divalent hydrocarbon group, such as (C2-C 10 ) alkylene, (C3-C 10 ) cycloalkylene or phenylene, and each R OAs defined above. (C) The organic peroxide may be bis(1,1-dimethylethyl)peroxide; bis(1,1-dimethylpropyl)peroxide; 2,5-dimethyl-2,5-bis(1,1-dimethylethylperoxy)hexane; 2,5-dimethyl-2,5-bis(1,1-dimethylethylperoxy)hexyne; 4,4-bis(1,1-dimethylethylperoxy)pentanoic acid; butyl ester; 1,1-bis(1,1-dimethylethylperoxy)-3,3,5-trimethylcyclohexane; benzoyl peroxide; tert-butyl peroxybenzoate; di-tert-amyl peroxide ( "DTAP"); bis(α-tert-butylperoxyisopropyl)benzene ("BIPB"); isopropylcumyl tert-butyl peroxide; tert-butylcumyl peroxide; di-tert-butyl peroxide; 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane; 2,5-bis(tert-butylperoxy)-2,5-dimethylhexyne-3,1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane; isopropylcumyl cumyl peroxide; butyl 4,4-di(tert-butylperoxy)valerate; or di(isopropylcumyl) peroxide; or dicumyl peroxide. (C) The organic peroxide may be dicumyl peroxide. In some aspects, only a blend of two or more (C) organic peroxides is used, for example, a 20:80 (wt / wt) blend of tert-butylcumyl peroxide and bis(tert-butylperoxyisopropyl)benzene (e.g., LUPEROX D446B, which is commercially available from Arkema). In some aspects, at least one, alternatively each (C) organic peroxide contains one -OO- group. The (C) organic peroxide may be a carrier mixture, alternatively 0.29 wt% to 0.44 wt%, alternatively 0.30 wt% to 39 wt%, alternatively 0.30 wt% to 0.37 wt% of the crosslinkable polyolefin composition.
[0052] Optional ingredient (D) scorch retarder: a molecule that inhibits premature curing, or a collection of such molecules. Examples of scorch retarders are hindered phenols; semi-hindered phenols; TEMPO; TEMPO derivatives; 1,1-diphenylethylene; 2,4-diphenyl-4-methyl-1-pentene (also known as alpha-methylstyrene dimer or AMSD); and allyl-containing compounds described in US 6277925B1, column 2, line 62 to column 3, line 46. In some aspects, the crosslinkable polyolefin composition and the crosslinked polyolefin product do not contain (D). When present, (D) scorch retarder can be 0.01 wt% to 1.5 wt%, alternatively 0.05 wt% to 1.2 wt%, alternatively 0.1 wt% to 1.0 wt% of the crosslinkable polyolefin composition.
[0053] Optional Ingredients (E) Antioxidant: An organic molecule, or a collection of such molecules, that inhibits oxidation. (E) Antioxidants are used to provide antioxidant properties to the crosslinkable polyolefin composition and / or the crosslinked polyolefin product. Examples of suitable (E) are bis(4-(1-methyl-1-phenylethyl)phenyl)amine (e.g., NAUGARD 445); 2,2'-methylene-bis(4-methyl-6-tert-butylphenol) (e.g., VANOX MBPC); 2,2'-thiobis(2-tert-butyl-5-methylphenol) (CAS No. 90-66-4; 4,4'-thiobis(2-tert-butyl-5-methylphenol) (also known as 4,4'-thiobis(6-tert-butyl-m-cresol), CAS No. 96-69-5, commercially available as LOWINOX TBM-6); 2,2'-thiobis(6-tert-butyl-4-methylphenol) (CAS No. 90-66-4, commercially available as LOWINOX TBP-6); tris[(4-tert-butyl-3-hydroxy-2,6-dimethylphenyl)methyl]-1,3,5-triazine-2,4,6-trione (e.g., CYANOX 1790); pentaerythritol tetrakis(3-(3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl)propionate (e.g., IRGANOX 1010, CAS No. 6683-19-8); 2,2'-thiodiethyl 3,5-bis(1,1-dimethylethyl)-4-hydroxyphenylpropionate (e.g., IRGANOX 1035, CAS No. 41484-35-9); distearyl thiodipropionate ("DSTDP"); dilauryl thiodipropionate (e.g., IRGANOX PS 800); stearyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (e.g., IRGANOX 1076); 2,4-bis(dodecylthiomethyl)-6-methylphenol (IRGANOX 1726); 4,6-bis(octylthiomethyl)-o-cresol (e.g., IRGANOX 1520); and 2',3-bis[[3-[3,5-di-tert-butyl-4-hydroxyphenyl]propionyl]]propionohydrazide (IRGANOX 1024). In some aspects, (E) is 4,4'-thiobis(2-tert-butyl-5-methylphenol) (also known as 4,4'-thiobis(6-tert-butyl-m-cresol); 2,2'-thiobis(6-tert-butyl-4-methylphenol; tris[(4-tert-butyl-3-hydroxy-2,6-dimethylphenyl)methyl]-1,3,5-triazine-2,4,6-trione; distearyl thiodipropionate; or dilauryl thiodipropionate; or a combination of any two or more thereof. The combination can be tris[(4-tert-butyl-3-hydroxy-2,6-dimethylphenyl)methyl]-1,3,5-triazine-2,4,6-trione and distearyl thiodipropionate. In some aspects, the crosslinkable polyolefin composition and the crosslinked polyethylene product do not contain (E).When present, (E) antioxidant may be 0.01 wt% to 1.5 wt%, alternatively 0.05 wt% to 1.2 wt%, alternatively 0.1 wt% to 1.0 wt% of the crosslinkable polyolefin composition.
[0054] Optional ingredient (F) filler: a subdivided granular solid or gel that occupies space in the host material and optionally affects the function of the host material. (F) filler can be calcined clay, organoclay or hydrophobized fumed silica, such as fillers commercially available from Cabot Corporation (Cabot Corporation) under the CAB-O-SIL trade name. (F) filler can have a flame retardant effect. In some aspects, the crosslinkable polyolefin composition and the crosslinked polyolefin product do not contain (F). When present, (F) filler can be 1wt% to 40wt% of the crosslinkable polyolefin composition, alternatively 2wt% to 30wt%, alternatively 5wt% to 20wt%.
[0055] About (F) filler, in some aspects, the crosslinkable polyolefin composition does not contain 20wt% or more, alternatively does not contain 15wt% or more, alternatively does not contain 10wt% or more, alternatively does not contain an inorganic filler selected from the group consisting of the following items: aluminum oxide, aluminum silicate, calcium silicate, magnesium silicate, silicon dioxide, titanium dioxide and their mixtures. In some aspects, the crosslinkable polyolefin composition does not contain 20wt% or more, alternatively does not contain 15wt% or more, alternatively does not contain 10wt% or more, alternatively does not contain any inorganic filler selected from the group consisting of the following items: a solid containing Al, a solid containing Ca, a solid containing Mg, a solid containing Si, a solid containing Ti and their mixtures. In some aspects, the crosslinkable polyolefin composition does not contain silsesquioxane, alternatively any siloxane except component (B). In some aspects, the crosslinkable polyolefin composition does not contain any of silsesquioxane and the inorganic filler group mentioned above. For the avoidance of doubt, the term "inorganic filler" does not include carbon black.
[0056] Optional ingredient (G) flame retardant: a molecule or substance that inhibits combustion, or a collection of such molecules. (G) can be a halogenated compound or a halogen-free compound. (G) Examples of halogenated (G) flame retardants are organic chlorides and organic bromides, examples of organic chlorides are chlorendic acid derivatives and chlorinated paraffins. Examples of organic bromides are decabromodiphenyl ether, decabromodiphenyl ethane, polymerized brominated compounds (such as brominated polystyrene), brominated carbonate oligomers, brominated epoxy oligomers, tetrabromophthalic anhydride, tetrabromobisphenol A and hexabromocyclododecane. Typically, halogenated (G) flame retardants are used together with synergists to improve their efficiency. The synergist can be antimony trioxide. Examples of halogen-free (G) flame retardants are inorganic minerals, organic nitrogen expansion compounds and phosphorus expansion compounds. Examples of inorganic minerals are aluminum hydroxide and magnesium hydroxide. Examples of phosphorus-based expanding compounds are organic phosphonic acids, phosphonates, phosphinates, phosphinate diesters, phosphinates, phosphine oxides, phosphines, phosphites, phosphates, chlorophosphazenes, phosphorus ester amides, phosphoric acid amides, phosphonic acid amides, phosphinic acid amides, melamine and its melamine derivatives including melamine polyphosphate, melamine pyrophosphate and melamine cyanurate, and mixtures of two or more of these materials. Examples include phenyl didodecyl phosphate, phenyl dineopentyl phosphate, phenyl ethylene hydrogen phosphate, phenyl-bis-3,5,5'-trimethylhexyl phosphate, ethyl diphenyl phosphate, di(p-tolyl) 2-ethylhexyl phosphate, diphenyl hydrogen phosphate, p-tolyl bis(2-ethyl-hexyl) phosphate, tricresyl phosphate, bis(2-ethylhexyl)-phenyl phosphate, tri(nonylphenyl) phosphate, phenyl methyl hydrogen phosphate, didodecyl p-tolyl phosphate, tricresyl phosphate, triphenyl phosphate, triphenyl phosphate, dibutylphenyl phosphate, 2-chloroethyl diphenyl phosphate, p-tolyl bis(2,5,5'-trimethylhexyl) phosphate, 2-ethylhexyl diphenyl phosphate, and diphenyl hydrogen phosphate. Phosphates of the type described in U.S. Pat. No. 6,404,971 are examples of phosphorus-based flame retardants. Other examples include liquid phosphates such as bisphenol A diphosphate (BAPP) (Adeka Palmarole) and / or resorcinol bis(diphenyl phosphate) (FyroflexRDP) (Supresta, ICI); solid phosphorus such as ammonium polyphosphate (APP), piperazine pyrophosphate and piperazine polyphosphate. Ammonium polyphosphate is often used with flame retardant co-additives such as melamine derivatives. Also useful is Melafine (DSM) (2,4,6-triamino-1,3,5-triazine; finely ground melamine). In some aspects, the crosslinkable polyolefin composition and the crosslinked polyolefin product do not contain (G). When present, the concentration of (G) can be 0.01 wt % to 70 wt %, alternatively 0.05 wt % to 40 wt %, alternatively 1 wt % to 20 wt % of the crosslinkable polyolefin composition.
[0057] Optional ingredient (H) hindered amine light stabilizer: a molecule containing a basic nitrogen atom bonded to at least one sterically bulky organic group and used as an inhibitor of degradation or decomposition, or a collection of such molecules. (H) is a compound having a sterically hindered amino functional group and inhibiting oxidative degradation and can also increase the shelf life of an embodiment of the crosslinkable polyolefin composition containing (C) an organic peroxide. Examples of suitable (H) are dimethyl succinate, a polymer with 4-hydroxy-2,2,6,6-tetramethyl-1-piperidin-ethanol (CAS No. 65447-77-0, commercially LOWILITE 62); and N,N'-bisformyl-N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-hexamethylenediamine (CAS No. 124172-53-8, commercially Uvinul 4050H). In some aspects, the crosslinkable polyolefin composition and the crosslinked polyolefin product do not contain (H). When present, the (H) hindered amine stabilizer may be 0.001 wt % to 1.5 wt %, alternatively 0.002 wt % to 1.2 wt %, alternatively 0.002 wt % to 1.0 wt %, alternatively 0.005 wt % to 0.5 wt %, alternatively 0.01 wt % to 0.2 wt %, alternatively 0.05 wt % to 0.1 wt % of the crosslinkable polyolefin composition.
[0058] Optional ingredient (I) Anti-treeing agent: A molecule that inhibits water treeing and / or electrical treeing, or a collection of such molecules. The anti-treeing agent can be an anti-water treeing agent or an anti-electrical treeing agent. An anti-water treeing agent is a compound that inhibits water treeing, which is a process by which polyolefins degrade when exposed to a combination of an electric field and moisture or water. An anti-electrical treeing agent (also called a voltage stabilizer) is a compound that inhibits electrical treeing, which is an electrical pre-breakdown process in solid electrical insulating materials caused by partial discharge. Electrical treeing can occur in the absence of water. Water treeing and electrical treeing are problems for cables containing coated conductors where the coating contains a polyolefin. (I) can be poly(ethylene glycol) (PEG). In some aspects, the cross-linkable polyolefin composition and the cross-linked polyethylene product do not contain (I). When present,
[0059] (I) The anti-treeing agent may be 0.01 wt % to 1.5 wt %, alternatively 0.05 wt % to 1.2 wt %, alternatively 0.1 wt % to 1.0 wt % of the crosslinkable polyolefin composition.
[0060] Optional ingredient (J) Methyl radical scavenger: a molecule reactive with methyl groups, or a collection of such molecules. (J) reacts with methyl radicals in the crosslinkable polyolefin composition or the crosslinked polyolefin product. (J) may be a "TEMPO" derivative of 2,2,6,6-tetramethyl-1-piperidinyl-N-oxyl or 1,1-diarylethene. Examples of TEMPO derivatives are 4-acryloyloxy-2,2,6,6-tetramethyl-1-piperidinyl-N-oxyl (CAS No. 21270-85-9, "acrylic TEMPO"), 4-allyloxy-2,2,6,6-tetramethyl-1-piperidinyl-N-oxyl (CAS No. 217496-13-4, "allyl TEMPO"); bis(2,2,6,6-tetramethyl-1-piperidinyl-N-oxyl) sebacate (CAS No. 217496-13-4, "allyl TEMPO"); AS No. 2516-92-9, "bis-TEMPO"); N,N-bis(acryloyl-4-amino)-2,2,6,6-tetramethyl-1-piperidinyl-N-oxyl (CAS No. 1692896-32-4, "bis-acrylamide TEMPO"); and N-acryloyl-4-amino-2,2,6,6-tetramethyl-1-piperidinyl-N-oxyl (CAS No. 21270-88-2, "mono-acrylamide TEMPO"). Examples of 1,1-diarylethenes are 1,1-diphenylethylene and α-methylstyrene. In some aspects, the crosslinkable polyolefin composition and the crosslinked polyolefin product do not contain (J). When present, the (J) methyl radical scavenger can be 0.01 wt % to 1.5 wt %, alternatively 0.05 wt % to 1.2 wt %, alternatively 0.1 wt % to 1.0 wt % of the crosslinkable polyolefin composition.
[0061] Optional ingredient (K) conventional adjuvant: a molecule containing a main chain or ring substructure and one, alternatively two or more acryl, acrylate and / or vinyl groups bonded thereto, wherein the substructure is composed of carbon atoms and optionally nitrogen atoms; or a collection of such molecules. (K) The conventional adjuvant does not contain silicon atoms. (K) The conventional adjuvant may be an acryl-functionalized conventional adjuvant as described by any one of limitations (i) to (v): (i) (K) is 2-allylphenyl allyl ether; 4-isopropenyl-2,6-dimethylphenyl allyl ether; 2,6-dimethyl-4-allylphenyl allyl ether; 2-methoxy-4-allylphenyl allyl ether; 2,2'-diallylbisphenol A; O,O'-diallylbisphenol A; or tetraallyldiallyl bisphenol A; (ii) (K) is 2,4-diphenyl-4-methyl-1-pentene or 1,3-diisopropenylbenzene; (iii) (K) is triallyl isocyanurate ("TAIC"); triallyl cyanurate ("TAC"); triallyl trimellitate ("TATM"); N,N,N',N',N",N"-hexaallyl-1,3,5-triazine-2,4,6-triamine ("HATATA"; also known as N 2 ,N 2 ,N 4 ,N 4 ,N 6 ,N 6 -hexaallyl-1,3,5-triazine-2,4,6-triamine); triallyl orthoformate; pentaerythritol triallyl ether; triallyl citrate; or triallyl aconitate; (iv) (K) is a mixture of any two acryl-functionalized adjuvants in (i). Alternatively, (K) may be an acrylate-functionalized conventional adjuvant selected from the following: trimethylolpropane triacrylate ("TMPTA"), trimethylolpropane trimethacrylate ("TMPTMA"), ethoxylated bisphenol A dimethacrylate, 1,6-hexanediol diacrylate, pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, tris(2-hydroxyethyl)isocyanurate triacrylate, and propoxylated glycerol triacrylate. Alternatively, (K) may be a vinyl-functionalized conventional adjuvant selected from polybutadiene having a 1,2-vinyl content of at least 50 wt% and trivinylcyclohexane ("TVCH"). Alternatively, (K) may be a conventional auxiliary agent described in US 5,346,961 or US 4,018,852. Alternatively, (K) may be a combination of the aforementioned conventional auxiliary agents or any two or more thereof. In some aspects, the crosslinkable polyolefin composition and the crosslinked polyolefin product do not contain (K). When present, (K) conventional auxiliary agents may be 0.01wt% to 4.5wt% of the crosslinkable polyolefin composition, alternatively 0.05wt% to 2wt%, alternatively 0.1wt% to 1wt%, alternatively 0.2wt% to 0.5wt%.
[0062] Optional ingredient (L) nucleating agent: an organic or inorganic additive that enhances the crystallization rate of a polyolefin polymer. Examples of (L) are calcium carbonate, titanium dioxide, barium sulfate, ultra-high molecular weight polyethylene, potassium hydrogen phthalate, benzoic acid compounds, sodium benzoate compounds, bicyclo[2.2.1]heptane-2,3-dicarboxylic acid disodium, zinc monoglyceride and 1,2-cyclohexanedicarboxylic acid, calcium salt: zinc stearate. In some aspects, the crosslinkable polyolefin composition and the crosslinked polyethylene product do not contain (L). When present, the concentration of (l) can be 0.01wt% to 1.5wt% of the crosslinkable polyolefin composition, alternatively 0.05wt% to 1.2wt%, alternatively 0.1wt% to 1.0wt%.
[0063] Optional component (M) carbon black: subcrystalline carbon with high surface area / volume ratio but lower than the surface area / volume ratio of activated carbon in a subdivided form. (M) example is furnace black, acetylene black, conductive carbon (for example, carbon fiber, carbon nanotube, graphene, graphite and expanded graphite sheet). In some respects, crosslinkable polyolefin composition and crosslinked polyethylene product do not contain (M). When present, (M) concentration can be 0.01wt% to 40wt% of crosslinkable polyolefin composition, alternatively 0.05wt% to 35wt%, alternatively 0.1wt% to 20wt%, alternatively 0.5wt% to 10wt%, alternatively 1wt% to 5wt%.
[0064] In addition, the crosslinkable polyolefin composition may independently further include one or more other optional additives selected from the group consisting of carrier resins, lubricants, processing aids, slip agents, plasticizers, surfactants, extender oils, acid scavengers, and metal deactivators.
[0065] The foregoing ingredients of the crosslinkable polyolefin composition are not believed to act as ring-opening catalysts for cyclic siloxanes therein. However, if any one or more of the foregoing ingredients of the crosslinkable polyolefin composition are unexpectedly found to act as ring-opening catalysts for cyclic siloxanes, such ingredients will be excluded from the crosslinkable polyolefin composition.
[0066] Crosslinked polyolefin product: A reaction product containing a networked polyolefin resin containing C—C bond crosslinks formed during the curing (crosslinking) of a crosslinkable polyolefin composition. The networked polyolefin resin may comprise a reaction product of coupling (A) macromolecules of a polyolefin polymer with (B) molecules of a monocyclic organosiloxane of formula (I) to obtain a network structure containing multivalent monocyclic organosiloxane crosslinker groups, which are linked via two or more macromolecules of (A) polyolefin polymer and one or more R bonds of molecules of (B) monocyclic organosiloxane of formula (I). 1The reaction of the group is bonded to two or more macromolecules from the polyolefin polymer (A). In some aspects, the two macromolecules of (A) can be connected through one R 1 For example, when two or more R 1 is vinyl and zero, one or more R 2 When the cross-linked polyolefin product is vinyl, the network structure may contain two or more of the formula (II): [-CH2CH2(R 2 )SiO 2 / 2 ](II) and / or formula (III): [CH3C(-)(H), (R 2 )SiO 2 / 2 ] (III) and (if present) n-2 or less (e.g., n-3) unreacted units of formula (I), wherein the subscript n is as defined for formula (I) and each "-" represents one valence of the multivalent group. When each R 2 When each R in formula (II) and (III) is independently H, (C1-C4) alkyl or phenyl in formula (I), 2 are independently H, (C1-C4)alkyl or phenyl.
[0067] The cross-linked polyolefin product may also contain solidified by-products, such as alcohol and ketone by-products of the reaction of (C) organic peroxides. When the cross-linkable polyolefin composition also contains one or more optional additives or ingredients (such as (E) antioxidants), the cross-linked polyolefin product may also contain any one or more optional additives or ingredients (such as (E)), or one or more reaction products formed by them during the cross-linkable polyolefin composition curing. The cross-linked polyolefin product may be in a separate solid form or in a continuous form. The separate solid form may include granules, pellets, powders or any two or more combinations thereof. The continuous form may be a molded part (such as an injection molded part) or an extruded part (such as a coated conductor or cable).
[0068] The cross-linked polyolefin product may be free of ring-opening catalysts and / or siloxane polymer molecules (silicone prepared by ring-opening polymerization of (B)).
[0069] Coated conductor. The coated conductor may be an insulated electrical conductor. The insulated electrical conductor may be a coated metal wire or cable, including power cables for low voltage ("LV", >0 to <5 kilovolts (kV)), medium voltage ("MV", 5kV to <69kV), high voltage ("HV", 69kV to 230kV) and extra high voltage ("EHV", >230kV) data transmission and power transmission / distribution applications. "Wire" means a single strand or monofilament of conductive material, such as a conductive metal, such as copper or aluminum. "Cable" and "power cable" are synonymous and mean an insulated electrical conductor comprising at least one wire disposed within a covering, which may be referred to as a sheath, jacket (protective outer jacket) or coating. The insulated electrical conductor may be designed and constructed for use in medium voltage, high voltage or extra high voltage applications. Examples of suitable cable designs are shown in US 5,246,783; US 6,496,629; and US 6,714,707.
[0070] The insulated electrical conductor may contain a conductor / transmission core and an outer single layer covering or an outer multi-layer covering disposed around the conductor / transmission core so as to protect the conductor / transmission core from and insulate it from the external environment. The conductor / transmission core may be composed of one or more metal wires. When the conductor / transmission core contains two or more metal wires, the metal wires may be subdivided into discrete bundles of wires. Each wire in the conductor / transmission core (whether bundled or not) may be individually coated with an insulating layer and / or the discrete bundles may be coated with an insulating layer. The single layer covering or multi-layer covering (e.g., a single layer or multi-layer coating or jacket) is primarily used to protect the conductor / transmission core from or insulate it from the external environment such as sunlight, water, heat, oxygen, other conductive materials (e.g., to prevent short circuits) and / or other corrosive materials (chemical fumes).
[0071] The single or multi-layer covering from one insulated electric conductor to the next insulated electric conductor may be configured differently depending on their respective intended use. For example, a multi-layer covering of an insulated electric conductor may be configured with the following components in order from its innermost layer to its outermost layer, observed in cross section: an inner semiconductive layer, a cross-linked polyolefin insulation layer comprising a cross-linked polyolefin product (cross-linked product of the present invention), an outer semiconductive layer, a metal shield and a protective sheath. The layers and sheath are circumferentially and coaxially (longitudinally) continuous. The metal shield (grounding) is coaxially continuous and is circumferentially continuous (layer) or discontinuous (ribbon or wire). Depending on the intended application, the multi-layer covering of an insulated optical fiber may omit the semiconductive layer and / or the metal shield. The outer semiconductive layer (when present) may be composed of a peroxide cross-linked semiconductive product that is bonded to the cross-linked polyolefin layer or may be peeled off from the cross-linked polyolefin layer.
[0072] In some aspects, a method for preparing a coated conductor includes extruding a coating layer comprising a crosslinkable polyolefin composition layer onto a conductor / transmission core to obtain a coated core, and passing the coated core through a CV device configured with suitable continuous vulcanization (CV) conditions for curing the crosslinkable polyolefin composition to obtain a coated conductor. CV conditions include temperature, atmosphere (e.g., nitrogen) and a line speed or transit time period through the CV device. Suitable CV conditions can obtain a coated conductor leaving the CV device, wherein the coated conductor contains a crosslinked polyolefin layer formed by curing a layer of a crosslinked polyolefin layer.
[0073] Conductive Conductive Methods. Conductive conductive methods of the present invention may use coated conductors of the present invention including insulated electrical conductor embodiments. Also contemplated is a method of transmitting data using coated conductors of the present invention including insulated electrical conductors.
[0074] Density is measured according to ASTM D792-13, Standard Test Methods for Density and Specific Gravity (Relative Density) of Plastics by Displacement, Method B (for testing solid plastics in liquids other than water (e.g., liquid 2-propanol)). Density is expressed in grams per cubic centimeter (g / cm 3 Report results in units of g / cc).
[0075] Thermal creep (heat setting) test method: Place the test sample (dog bone shape with the dimensions specified in ASTM 638-34; thickness <2 millimeters (mm); marking lines 20 mm apart) in an oven at 200°C and apply a force equal to 20 Newtons per square centimeter (N / cm 2 ) force. The elongation of the test sample (the distance between the marked lines) is then measured under these conditions and expressed as a percentage of the initial 20mm distance. If the distance between the marked lines widens to 40mm, the thermal creep is 100% (100*(40-20) / 20)=100%), and if it widens to 100mm, the thermal creep is 400%. With all other conditions being the same, the lower the level of crosslinking in the test sample, the greater its elongation. Conversely, the higher the level of crosslinking in the test sample, the smaller its elongation. If the level of crosslinking in the test sample is low enough, the test sample may fail by breaking, which may occur within a few minutes or even seconds of the start of its test. If the test sample is intact after 15 minutes, the weight is removed, and the test sample is then taken out of the oven and allowed to cool to room temperature. The residual elongation of the test sample after cooling is measured.
[0076] Melt index (I2) is measured according to ASTM D1238-04 (190°C, 2.16 kg), Standard Test Method for Melt Flow Rates of Thermoplastics by Extrusion Platometer, using the 190°C / 2.16 kilogram (kg) condition (formerly known as "Condition E" and also referred to as I2). The results are reported in grams eluted per 10 minutes (g / 10 min.) or equivalently decigrams per 1.0 minute (dg / 1 min.). 10.0 dg = 1.00 g.
[0077] Dynamic Die Rheometer (MDR) Test Method: ASTM D5289-12, Standard Test Method for Rubber Property—Vulcanization Using Rotorless Cure Meters. The torque of the test sample is measured using the following procedure. The test sample is heated at 182°C for 12 minutes in a dynamic die rheometer (MDR) instrument MDR2000 (Alpha Technologies) while monitoring the torque change of the oscillatory deformation of 0.5 degrees arc at 100 cpm. The lowest measured torque value is designated as "ML" and is expressed in deciNewton meters (dN-m). As curing or crosslinking proceeds, the measured torque value increases and eventually reaches a maximum torque value. At 12 minutes, the maximum or highest measured torque value is designated as "MH" and is expressed in dN-m. All other events being equal, the larger the MH torque value, the greater the degree of crosslinking.
[0078] The following data is predictive of how the crosslinkable polyolefin compositions of the present invention and the crosslinked polyolefin products of the present invention will perform when extruded and crosslinked (eg, in a CV apparatus) to form the insulation layer of a cable.
[0079] Examples
[0080] (A1)-1 Ethylene / 1-octene copolymer elastomer has a melt index of 1 g / 10 min and a density of 0.870 g / cm 3 .
[0081] (A1)-2 ethylene / 1-octene copolymer elastomer has a melt index of 5 g / 10 min and a density of 0.870 g / cm 3 .
[0082] LDPE-1: LDPE has a melt index of 1.9 g / 10 min and a density of 0.9183 g / cm 3 .
[0083] Monocyclic organosiloxane (B1): 2,4,6,8-tetramethyl-2,4,6,8-tetravinyl-cyclotetrasiloxane, "(D Vi )4" (CAS No. 2554-06-5), obtained from The Dow Chemical Company.
[0084] Organic peroxide (C1): dicumyl peroxide ("DCP"), obtained from Fangruida.
[0085] Anti-scorch agent (D1): α-methylstyrene dimer (AMSD).
[0086] Antioxidant (E1): 4,6-bis(octylthiomethyl)-2-methyl-phenol.
[0087] Inventive Examples 1 to 6 (IE1 to IE6): In separate runs, monocyclic organosiloxane (B1), organic peroxide (C1), anti-scorch agent (D1) and antioxidant (E1) were impregnated into pellets of ethylene / 1-octene copolymer elastomer (A1)-1 or (A1)-2, or into a blend of ethylene / 1-octene copolymer elastomer (A1)-1 and LDPE-1 in an oven at 80° C. for 6 hours to obtain inventive compositions IE1 to IE6 in the form of pellets. The compositions and hot creep properties are shown in Tables 1 and 2, respectively.
[0088] Comparative Examples 1 to 5 (CE1 to CE5): In separate runs, monocyclic organosiloxane (B1), organic peroxide (C1), anti-scorch agent (D1) and antioxidant (E1) were impregnated into pellets of ethylene / 1-octene copolymer elastomer (A1)-1 or (A1)-2 and / or LDPE-1 in an oven at 80° C. for 6 hours to obtain comparative compositions CE1 to CE6 in the form of pellets. The compositions and hot creep properties are shown in Tables 3 and 4, respectively.
[0089] Table 1: Compositions of IE1 to IE6. (0=0.00)
[0090]
[0091] The data in Table 1 indicate that the crosslinkable polyolefin compositions of IE1 to IE6 are examples of the crosslinkable polyolefin compositions of the present invention.
[0092] Table 2: Thermal creep properties of IE1 to IE6.
[0093]
[0094]
[0095] As indicated by the data in Table 2, after holding at 200°C for 15 minutes, the thermal creep of all the inventive crosslinkable polyolefin compositions of IE1 to IE6 was less than 175% of the maximum specification. Notably, the thermal creep values of five of the six inventive crosslinkable polyolefin compositions (i.e., IE1 to IE3, IE5, and IE6) were less than 100%.
[0096] The MDR MH data in Table 2 indicate that after 12 minutes at 182° C. in a moving die rheometer, all of the crosslinkable polyolefin compositions of the present invention result in crosslinked polyolefin products having a significant degree of crosslinking, as indicated by a MH greater than (>) 2.0 dN-m, alternatively > 2.5 dN-m, alternatively > 3.0 dN-m. These values are remarkable achievements in just 12 minutes.
[0097] Table 3: Composition of CE1 to CE5. (0=0.00)
[0098]
[0099] The data in Table 3 indicate that the comparative crosslinkable polyolefin compositions of CE1 to CE5 are not examples of the inventive crosslinkable polyolefin compositions.
[0100] Table 4: Thermal creep properties of CE1 to CE5.
[0101]
[0102] As indicated by the data in Table 4, after being held at 200°C for 15 minutes, the thermal creep of all comparative crosslinkable polyolefin compositions of CE1 to CE5 was significantly greater than 175% of the maximum specification. It is worth noting that in the thermal creep test, four of the five comparative crosslinkable polyolefin compositions (i.e., CE2 to CE5) showed specimen failure (indicated by "failure"), which means that the test specimens broke or stretched to the bottom of the oven during the test, which means that the value of thermal creep could not be obtained.
[0103] The MDR MH data in Table 4 indicate that after 12 minutes at 182°C in a moving die rheometer, all but one of the comparative crosslinkable polyolefin compositions failed to result in a crosslinked polyolefin product with a significant degree of crosslinking (i.e., failed to achieve MH>2.0 dN-m). Only CE2 had MH>2.0 dN-m (i.e., 2.9 dN-m).
Claims
1. A crosslinkable polyolefin composition comprising 100 to 30 weight percent (wt%) of a carrier mixture and 0 to 70 wt% of one or more optional additives; wherein the carrier mixture is composed of 97.56 to 99.31 weight percent (wt%) of (A) a polyethylene polymer, 0.40 to 2.0 wt% of (B) an alkenyl functionalized monocyclic organosiloxane, and 0.29 to 0.44 wt% of (C) an organic peroxide; wherein the (A) polyethylene polymer is selected from any one of (A1) or (A2): (A1) an ethylene / α-olefin copolymer elastomer having a melt index of 0.6 to 6.2 grams per 10 minutes (g / 10min) and a density of 0.854 to 0.912 grams per cubic centimeter (g / cm 3 ), measured according to ASTM D792-13, method B, or (A2) a blend of (A1) and a low density polyethylene (LDPE), wherein the melt index of the low density polyethylene (LDPE) is from 0.8 g / 10 min to 2.5 g / 10 min, wherein the mass ratio of the weight of (A1) to the weight of (LDPE) of the blend ((A1) / (LDPE) wt / wt) is from 99.9 / 0.1 to 1.0 / 3.0, and wherein both melt indices I2 are measured according to ASTM D1238-04 at 190°C and 2.16 kg; Wherein the (B) alkenyl functional monocyclic organosiloxane has the formula (I): [R 1 ,R 2 SiO 2 / 2 ] n (I), wherein the subscript n is an integer greater than or equal to 3; each R 1 are independently C2-C4 alkenyl or H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is H or methyl, and the subscript m is an integer from 1 to 4; and each R 2 are independently H, C1-C4 alkyl, phenyl or R 1 ;as well as wherein after being maintained at 200° C. for 15 minutes, the thermal creep of the carrier mixture of the crosslinkable polyolefin composition is less than 175%, as measured by the thermal creep test method; Provided that the crosslinkable polyolefin composition does not contain any ring-opening catalyst; and Provided that if the melt index (I2) of the (A1) ethylene / α-olefin copolymer elastomer is greater than 2 g / 10 min, the amount of (C) organic peroxide is 0.35 wt% to 0.44 wt%.
2. The crosslinkable polyolefin composition of claim 1, wherein the (A) polyethylene polymer is further defined by any one of limitations (i) to (vii): (i) the (A) polyethylene polymer is the (A1) ethylene / α-olefin copolymer elastomer; (ii) the (A) polyethylene polymer is the (A1) ethylene / α-olefin copolymer elastomer, and (A1) has a melt index of 0.80 g / 10 min to 5.4 g / 10 min and a density of 0.855 g / cm 3 Up to 0.912g / cm 3 Ethylene / 1-octene copolymer; (iii) the (A) polyethylene polymer is the (A1) ethylene / α-olefin copolymer elastomer, and (A1) has a melt index of 0.80 g / 10 min to 5.4 g / 10 min and a density of 0.859 g / cm 3 Up to 0.890g / cm 3 Ethylene / 1-butene copolymer; (iv) the (A) polyethylene polymer is the (A2) blend, and (A2) is a blend of ethylene / α-olefin copolymer elastomers in any one of the restrictions (i) to (iii), and the LDPE has a melt index (I2) of 1.75 g / 10 min to 2.49 g / 10 min and a density of 0.918 g / cm 3 Up to 0.920g / cm 3 LDPE; (v) the (A) polyethylene polymer is the (A2) blend, and (A2) is a blend of ethylene / α-olefin copolymer elastomers limited to any one of (i) to (iii), and the LDPE has a melt index (I2) of 2.4 g / 10 min and a density of 0.920 g / cm 3 LDPE; (vi) the (A) polyethylene polymer is the (A2) blend, and (A2) is a blend of ethylene / α-olefin copolymer elastomers limited to any one of (i) to (iii), and the LDPE has a melt index (I2) of 1.9 g / 10 min and a density of 0.9183 g / cm 3 LDPE; and (vii) the (A) polyethylene polymer is the (A2) blend, and (A2) is a blend of ethylene / α-olefin copolymer elastomers limited to any one of (i) to (iii), and the LDPE has a melt index (I2) of 0.80 g / 10 min to 1.24 g / 10 min and a density of 0.917 g / cm 3 Up to 0.923g / cm 3 of LDPE.
3. The crosslinkable polyolefin composition according to claim 1, wherein the subscript n is 4 and the monocyclic organosiloxane of formula (B) (I) is described by any one of limitations (i) to (x): (i) Each R 1 is independently C2-C3 alkenyl; and each R 2 are independently H, C1-C2 alkyl or C2-C3 alkenyl; (ii) Each R 1 is vinyl; and each R 2 are independently C1-C2 alkyl; (iii) Each R 1 is vinyl; and each R 2 It is methyl; (iv) Each R 1 is allyl; and each R 2 are independently C1-C2 alkyl; (v) Each R 1 is allyl; and each R 2 It is methyl; (vi) Each R 1 is independently H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is H or methyl, and the subscript m is an integer from 1 to 4; and each R 2 are independently H, C1-C2 alkyl or C2-C3 alkenyl; (vii) Each R 1 is independently H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is H and the subscript m is 3; and each R 2 are independently C1-C2 alkyl; (viii) Each R 1 is independently H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is methyl and the subscript m is 3; and each R 2 are independently C1-C2 alkyl; (ix) the crosslinkable polyolefin composition does not contain 24 wt% or more of any inorganic filler; and (x) A combination of restriction (ix) and any one of restrictions (i) to (viii).
4. The crosslinkable polyolefin composition according to claim 2, wherein the subscript n is 4 and the monocyclic organosiloxane of formula (B) (I) is described by any one of limitations (i) to (x): (i) Each R 1 is independently C2-C3 alkenyl; and each R 2 are independently H, C1-C2 alkyl or C2-C3 alkenyl; (ii) Each R 1 is vinyl; and each R 2 are independently C1-C2 alkyl; (iii) Each R 1 is vinyl; and each R 2 It is methyl; (iv) Each R 1 is allyl; and each R 2 are independently C1-C2 alkyl; (v) Each R 1 is allyl; and each R 2 It is methyl; (vi) Each R 1 is independently H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is H or methyl, and the subscript m is an integer from 1 to 4; and each R 2 are independently H, C1-C2 alkyl or C2-C3 alkenyl; (vii) Each R 1 is independently H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is H and the subscript m is 3; and each R 2 are independently C1-C2 alkyl; (viii) Each R 1 is independently H2C=C(R 1a )-C(=O)-O-(CH2) m -, where R 1a is methyl and the subscript m is 3; and each R 2 are independently C1-C2 alkyl; (ix) the crosslinkable polyolefin composition does not contain 24 wt% or more of any inorganic filler; and (x) A combination of restriction (ix) and any one of restrictions (i) to (viii).
5. The crosslinkable polyolefin composition according to any one of claims 1 to 4, further comprising 0.01 wt% to 0.10 wt% of (D) an anti-scorch agent or 0.10 wt% to 0.30 wt% of (E) an antioxidant or a combination of (D) and (E); and The embodiment of the crosslinkable polyolefin composition consisting of ingredients (A) to (E) has a thermal creep of less than 175% after being held at 200°C for 15 minutes as measured by the Thermal Creep Test Method.
6. The crosslinkable polyolefin composition according to any one of claims 1 to 4, wherein the crosslinkable composition comprises the carrier mixture and the one or more additives; wherein the one or more additives are selected from the group consisting of additives (F) to (M): (F) fillers; (G) flame retardants; (H) hindered amine stabilizers; (I) anti-tree agents; (J) methyl radical scavengers; (K) conventional additives, (L) nucleating agents and (M) carbon black; provided that the (F) filler does not contain any previously omitted filler.
7. A method for preparing the crosslinkable polyolefin composition according to claim 1, said method comprising mixing said amount of said (A) polyethylene polymer, said amount of said (B) monocyclic organosiloxane of formula (I) and said amount of said (C) organic peroxide together to prepare said carrier mixture.
8. A method for free radical curing a crosslinkable polyolefin composition according to any one of claims 1 to 6 to prepare a crosslinked polyolefin product, the method comprising heating the crosslinkable polyolefin composition at a curing effective temperature in a manner to react the (A) polyethylene polymer with the (B) monocyclic organosiloxane of formula (I), thereby preparing a crosslinked polyolefin product.
9. A cross-linked polyolefin product, the cross-linked polyolefin product being obtained by the method according to claim 8.
10. A manufactured product comprising the crosslinkable polyolefin composition according to any one of claims 1 to 6 or the crosslinked polyolefin product according to claim 9 in a shaped form.
11. A coated conductor comprising a conductive core and an insulating layer at least partially covering the conductive core, wherein at least a portion of the insulating layer comprises the crosslinkable polyolefin composition according to any one of claims 1 to 6 or the crosslinked polyolefin product according to claim 9.
12. A method of transmitting electricity, the method comprising applying a voltage across the conductive core of the coated conductor of claim 11 so as to produce an electric current through the conductive core.