An inorganic-organic LED hybrid color display device and its preparation method
Through the vertical bonding and evaporation technology of inorganic-organic LED hybrid color display devices, the problem of low red light external quantum efficiency under small size of Micro-LED is solved, high efficiency and high density display effect are achieved, and production costs are reduced .
Patent Information
- Application Number
- CN202210373367.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-11
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-04-11
AI Technical Summary
The existing Micro-LED colorization technology has low red light external quantum efficiency under small sizes, making it difficult to realize high-density pixel array display, and traditional preparation solutions are difficult to meet chip manufacturing and structural requirements.
Using inorganic-organic LED hybrid color display devices, the blue and green wafers are bonded vertically and the loaded red light OLED is evaporated to improve the red light external quantum efficiency, and the process flow is simplified through the non-aligned bonding process and the evaporation process. , improve yield and density.
It significantly improves the red light external quantum efficiency and overall display device efficiency, avoids the phenomenon of light string, improves color saturation and authenticity, and reduces production costs and device size.
Smart Images

Figure CN114843317B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an LED display device and a preparation method thereof, in particular to an inorganic-organic LED hybrid color display and a preparation method thereof, belonging to the field of display technology. Background Art
[0002] LED is a common light-emitting device with a history of more than 60 years. LED can efficiently convert electrical energy into light energy. Early LEDs were often used for low-light lighting and monochrome displays. With technological advances, the size of LED components has become smaller and smaller. They are currently widely used in screen displays, medical equipment and daily lighting.
[0003] In the first 20 years of this century, the size of LEDs began to move towards the micron level, from the initial RGB three-color LED to Mini-LED (about 100μm), and now has developed to Micro LED (less than 50μm). Compared with traditional LED chips, MicroLED chips show great advantages in brightness, contrast and reliability, and are generally considered to be the core of the next generation of display technology. They have great application prospects in watches, TVs, projections, virtual reality, augmented reality, mixed reality and other fields. However, these application requirements have put forward new requirements in chip manufacturing, size, structure, yield, drive and other aspects. Traditional LED preparation solutions are difficult to match and require high integration to meet the requirements. In the field of Micro-LED, colorization is also a very big challenge. The current mainstream Micro-LED colorization technologies include: three primary colors, color conversion, prism light combination and other solutions. The colorization is basically based on three colors on the planar structure. There are challenges for further compressing the device size and performing ultra-high density pixel array display. In particular, due to the characteristics of the AlGaInP quaternary system, the size of red Micro-LEDs has entered the Micro level, especially when the size is below 15um, the external quantum efficiency is extremely low, far lower than the performance of OLED, which makes the colorization of pure inorganic Micro-LEDs challenging.
[0004] In the existing technology, there are mainly two solutions for realizing colored Micro-LED micro-display:
[0005] 1) Non-aligned bonding horizontal display: After preparing single-color Micro-LED devices separately, they are bonded and stacked multiple times to prepare Micro-LED devices of different colors, ultimately achieving a horizontal layout of red, green, and blue.
[0006] 2) Alignment bonding vertical display: Prepare red, green and blue monochrome display matrices separately, and then integrate the matrices of different colors one by one through alignment bonding to achieve vertical layout of red, green and blue colors B. However, the above solutions have failed to solve the external quantum efficiency problem of red light Micro-LED. At the 15um / 5um level, the external quantum efficiency of Micro-LED is much lower than that of traditional size LED and OLED.
[0007] Patent CN111133499A adopts a solution combining LED and OLED to improve the problem of low external quantum effect of LED at small size. Among them, blue light B is realized by LED, and green light G / red light R is realized by OLED. However, this solution adopts a horizontal layout of RGB, which loses pixel integration density to a certain extent, and poses challenges to the preparation of micro-display devices with higher resolution requirements. Summary of the invention
[0008] In response to the problems existing in the prior art, the first purpose of the present invention is to provide an inorganic-organic LED hybrid color display device. After bonding blue and green wafers in the vertical direction, the display device loads red light OLEDs by evaporation. Compared with the traditional layout method, the display device has a higher integration level, a higher pixel density, and greatly improves the external quantum efficiency of red light.
[0009] The second object of the present invention is to provide a method for preparing the above-mentioned display device, using organic red light OLED and inorganic green and blue light wafer raw materials. The inorganic green and blue light wafer raw materials adopt a non-aligned bonding process, and the red light OLED adopts a vapor deposition process. The overall process is relatively simple and easy to operate, which greatly improves the yield of the display device and effectively reduces the production cost.
[0010] In order to achieve the above technical objectives, the present invention provides an inorganic-organic LED hybrid color display device, comprising: a driving backplane (1), a first bonding film (2), a first wafer (3), a second bonding film (4), a second wafer (5), a red light OLED (6) and a metal bridge (7); three anode contacts (8) with equal spacing and parallel to each other are distributed on the driving backplane, and the first bonding film is laid on two adjacent anode contacts; when the first wafer is a green light wafer, the second wafer is a blue light wafer; when the first wafer is a blue light wafer, the second wafer is a red light OLED (6) and a metal bridge (7); The two wafers are green light wafers; the first wafer is bonded to the first bonding film, the upper surface of the first wafer is covered with an insulating layer (9), the insulating layer is provided with a second bonding film, and the second wafer is bonded to the second bonding film; the red light OLED is integrated on the anode contact point not covered by the bonding film, and a black matrix (10) is provided between the red light OLED and the first and second wafers; the first wafer, the second wafer and the red light OLED are connected to the anode contact of the driving backplane through a metal bridge; the first wafer, the second wafer and the red light OLED are connected to the cathode through the metal bridge.
[0011] The present invention adopts a vertical stacking method of blue and green wafers, which greatly reduces the component size and pixel spacing and improves the arrangement density of pixels. The second bonding film between the blue and green wafers plays the role of wafer segmentation and preventing crosstalk. In addition, the red light OLED is directly integrated on the anode contact without bonding film covering on the driving backplane, which effectively solves the problem of a sharp drop in the external quantum efficiency of red light due to size reduction, significantly improves the external quantum efficiency of red light, and further improves the overall efficiency of the display device. When the external quantum efficiency of the display device is improved, due to the setting of the bonding layer and the black matrix, the "rainbow" phenomenon caused by crosstalk is effectively avoided, making the color saturation and authenticity of the display device higher.
[0012] As a preferred solution, the driving backplane is at least one of a TFT thin film transistor, a LTPS low temperature polysilicon, a CMOS integrated circuit and a high mobility transistor.
[0013] As a preferred solution, the first bonding film is at least one of gold, nickel, tin, aluminum, copper and indium.
[0014] As a preferred solution, the second bonding film is at least one of gold, nickel, tin, aluminum, copper and indium. The first bonding film and the second bonding film not only have bonding function, but also have good electrical conductivity, reflection and heat dissipation functions to avoid damage to the wafer due to heat accumulation.
[0015] As a preferred solution, the metal bridge is at least one of gold, nickel, tin, aluminum, copper and indium.
[0016] As a preferred solution, the green light wafer comprises, from bottom to top, a wafer substrate, a buffer layer, an N-type compound semiconductor, a quantum well, a P-type compound semiconductor and a P-type ohmic contact.
[0017] As a preferred solution, the blue light wafer is composed of a wafer substrate, a buffer layer, an N-type compound semiconductor, a quantum well, a P-type compound semiconductor and a P-type ohmic contact from bottom to top. The quantum well is mainly a stack of InGaN and GaN. Normally, electrons will combine with holes to emit photons, and the presence of the quantum well can force the electrons generated in the middle layer to combine with holes and release energy in the form of a changing electric field rather than photons. The action of the electric field causes new electrons and holes to be generated in adjacent quantum dots, allowing them to combine more efficiently and emit photons.
[0018] As a preferred solution, the first wafer is a green light wafer, and the second wafer is a blue light wafer.
[0019] The reason why the present invention adopts the arrangement of the green light wafer at the bottom and the blue light wafer at the top is because it takes into account the characteristic of semiconductor optoelectronic materials that there is a correlation between the bandgap width and the wavelength. The larger the bandgap width, the shorter the emitted wavelength, and the narrow bandgap material has an absorption effect on short-wave energy, so there will be an absorption effect when the short wavelength passes through the long-wavelength material. The wavelength of green light is about 525nm, and the wavelength of blue light is 460nm. Therefore, the arrangement is carried out in a manner of gradually shortening the wavelength from bottom to top, which can effectively avoid the loss of energy caused by absorption and avoid brightness loss.
[0020] As a preferred solution, the red light OLED material is a small molecule and / or high molecule OLED organic material.
[0021] As a preferred solution, the red light OLED material is DCJTB, including: 4-dinitrile methylene-2-tert-butyl-6-(1,1,7,7-tetramethyljulolidine vinyl) pyran; (E)-4-dinitrile methylene-2-tert-butyl-6-(1,1,7,7-tetramethyljulolidine vinyl) pyran; 4-(dicyanovinyl)-2-tert-butyl-6-(1,1,7,7-tetramethyljulolidine-4-vinyl)-4H-pyran; 4-(dicyanomethyl)-2-tert-butyl-6-(1,1,7,7-tetramethyljulolidine-9-enyl)-4H-pyran; 4 -(Dicyanomethylene)-2-tert-butyl-6-(1,1,7,7-tetramethyljuronidin-4-vinyl)-4H-pyran; 2-tert-butyl-4-(dicyanomethylene)-6-[2-(1,1,7,7-tetramethyljuronidin-9-yl)vinyl]-4H-pyran; 4-(dicyanovinyl)-2-tert-butyl-6-(1,1,7,7-tetramethyljuronidin-4-vinyl)-4H-pyran (DCJTB); 4-(dicyanomethylene)-2-tert-butyl-6-(1,1,7,7-tetramethyljuronidin-4-vinyl)-4H-pyran. Using DCJTB as a red light OLED material can significantly improve the external quantum efficiency of red light. Its efficiency performance in the Micro field is higher than that of inorganic LEDs, which can effectively guarantee the efficiency and power consumption of the overall device.
[0022] The present invention also provides a method for preparing an inorganic-organic LED hybrid color display discrete device, comprising the following steps: 1) preparing a first bonding film on a driving backplane; 2) preparing a bonding film on a wafer surface of a first wafer and bonding it to the driving backplane before laying an insulating layer; 3) preparing a second bonding film on a wafer surface of a second wafer and bonding it to the insulating layer of a green light wafer; 4) exposing the N-type compound semiconductor of each wafer layer by layer; 5) vapor-depositing a red light OLED onto the driving backplane; 6) after the insulating layer covers the color display device as a whole, exposing the P-type compound semiconductor of each wafer and the cathode of the red light OLED layer by layer and interconnecting them with a common electrode to obtain.
[0023] The size of the display device prepared by the present invention is between 1 and 25um, and the size of the blue, green wafers and red OLED is less than 3μm, and the alignment bonding process has a precision error of ±1 to 2μm, which is very risky for the bonding of the RGB elements in the present invention and is difficult to meet the requirements of the yield rate. Therefore, the preparation method provided by the present invention adopts a non-aligned bonding process, and after wafer bonding, the semiconductor etching process is used to complete the bonding of the device electrode and the drive contact. Since the semiconductor etching process can be achieved at the nanometer level, the wafer bonding can be accurately achieved. The red OLED is an organic material, which is directly loaded on the anode contact of the drive backplane by evaporation, and no bonding is required. Therefore, while greatly reducing the size of the display device, the product yield is also improved, and the production cost is reduced.
[0024] As a preferred solution, in step 2), the bonding method of the green light wafer is non-aligned bonding, using at least one of thermal compression bonding, eutectic bonding and surface activated bonding.
[0025] As a preferred solution, in step 3), the bonding method of the blue light wafer is non-aligned bonding, using at least one of thermal compression bonding, eutectic bonding and surface activated bonding.
[0026] As a preferred solution, the method of exposing the N-type compound semiconductor layer by layer in step 4) is wet and / or dry etching. The device shape exposed by etching in the present invention can be a common shape such as a circle, a rectangle and a triangle. Since the etching process belongs to a semiconductor etching process, it has a great preparation accuracy for ultra-small wafers. At the same time, the bonding layer is opaque, and a graphical preparation method can be used to customize the exposure size of each wafer, thereby achieving a specific allocation of the wafer area.
[0027] As a preferred solution, in step 5), the red light OLED evaporation method is at least one of patterned electron beam, thermal evaporation, vacuum evaporation and sputtering evaporation.
[0028] As a preferred solution, the overall covering method of the insulating layer in step 6) is at least one of coating, chemical vapor deposition, atomic layer deposition and sputtering evaporation. The evaporation process can uniformly prepare nano-scale thin films, and the evaporation process can be used to accurately and uniformly load the red light OLED on the anode contact of the driving backplane, ultimately forming an inorganic blue and green wafer-organic red light OLED display device.
[0029] As a preferred solution, the insulating layer is at least one of silicon oxide, aluminum oxide, silicone oil and a silane coupling agent.
[0030] The specific process of the preparation method of an inorganic-organic LED hybrid color display device provided by the present invention is as follows: 1) preparing a first bonding film on the anode metal contact surface of a driving backplane; 2) preparing a bonding film on the wafer surface of a green light wafer, wherein the film structure includes electrical interconnections formed on the target wafer; 3) bonding the wafer surface of the entire green light wafer, and removing the wafer substrate material after bonding, which can be removed by laser stripping, chemical removal or grinding removal; 4) laying a theater layer on one side of the upper surface of the green light wafer close to the edge anode contact by introducing a dielectric, and laying a second bonding layer on the insulating layer; 5) bonding the blue light wafer to the substrate; Bonded to the second bonding layer, the bonding method is the same as the green light wafer bonding method; 6) Expose N-type compound semiconductors of different compound materials layer by layer through dry and / or wet etching, and the exposed area of the N-type compound semiconductor is controlled by a graphical method; 7) Evaporate the red light OLED onto the driving backplane, and the anode of the red light OLED directly contacts the metal contact of the driving backplane to form an anode contact; 8) Cover the front side of the insulating layer on the above-mentioned display device, and realize common-pole interconnection by graphically exposing the bonding layer of each layer of the wafer and the exposed cathode compound semiconductor, and use metal bridges to realize one-to-one connection between each light-emitting device and the anode on the driving backplane.
[0031] In the technical solution provided by the present invention, an organic red light OLED and inorganic blue and green wafers are used to form an RGB display device. In previous Micro-LEDs, inorganic quaternary red light materials are often used. This material will cause a sharp drop in external quantum efficiency as the device size decreases, far exceeding the drop in external quantum efficiency of blue and green wafers. Due to the barrel effect, the external quantum efficiency of the red light material drags down the conversion efficiency of the overall RGB display. The combination of red light OLED and blue and green LEDs can just make up for this defect. When the device size is reduced, the external quantum efficiency of red light will not drop sharply, thereby effectively improving the conversion efficiency of the overall display. In addition, through the non-aligned bonding process, while further reducing the size of the display device, the product yield is also improved, greatly reducing the preparation cost.
[0032] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0033] 1) In the inorganic-organic LED hybrid color display device provided by the present invention, the blue and green wafers adopt a stacked layout, which can achieve a higher pixel density.
[0034] 2) In the technical solution provided by the present invention, a combination of organic red light OLED and inorganic blue and green LED is adopted, which effectively eliminates the problem of a sharp drop in the external quantum efficiency of red light caused by the reduction in the size of the red light material. While effectively improving the external quantum efficiency of small-size red light materials, it also improves the overall conversion efficiency of the display device.
[0035] 3) In the technical solution provided by the present invention, non-aligned bonding is adopted to achieve precise bonding of blue and green wafers, and then the red light OLED is loaded on the driving backplane by the evaporation process to achieve direct anode contact between the red light material and the driving backplane. This preparation method not only further reduces the size of the display device but also improves the product yield, greatly reducing the preparation cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 Schematic diagram of inorganic-organic LED hybrid color display device
[0037] 1. Driving backplane 2. First bonding film 3. Green light wafer 4. Second bonding film 5. Blue light wafer 6. Red light OLED 7. Metal bridge 8. Anode contact 9. Insulation layer 10. Black matrix
[0038] Figure 2 This is a front view of the inorganic-organic LED hybrid color display device in Example 1;
[0039] Figure 3 A top view of the inorganic-organic LED hybrid color display device in Example 1;
[0040] Figure 4 This is a schematic diagram of the PCB backplane in Example 1;
[0041] Figure 5 This is a schematic side view of a green light wafer in Example 1;
[0042] Figure 6 This is a schematic side view of a blue light wafer in Example 1;
[0043] Figure 7 This is the TFT driving backplane circuit diagram in Example 2; DETAILED DESCRIPTION
[0044] The following specific examples are intended to further illustrate the present invention rather than to limit the scope of protection of the claims.
[0045] Example 1
[0046] In this embodiment, the first wafer is a green wafer, and the second wafer is a blue wafer;
[0047] Step 1: Select a PCB driving backplane, and prepare a first bonding film on the PCB driving backplane, wherein the first bonding film is: gold-tin alloy;
[0048] Step 2: Select: sapphire-based green light InGaN wafer material, prepare a P-type ohmic contact layer on the wafer surface of the green light wafer and then prepare a bonding film, the bonding film is: gold-tin alloy;
[0049] Step 3: Bond the green wafer to the PCB driver backplane using eutectic bonding, and remove the wafer substrate of the green wafer using laser stripping;
[0050] Step 4: introducing a silicon oxide insulating layer on the upper surface of the green light wafer, and then preparing a second bonding film on the silicon oxide insulating layer, wherein the second bonding film is a gold-indium alloy;
[0051] Step 5: Select blue light InGaN wafer material, prepare a P-type ohmic contact layer on the wafer surface of the blue light wafer, and then prepare a bonding film. The bonding film is a gold-indium alloy. The blue wafer is bonded to the green wafer by eutectic bonding, and laser stripping is used to remove it.
[0052] Step 6: Use semiconductor photolithography to expose the N-type compound semiconductor of blue and green wafers layer by layer, use ALD to cover the entire surface of blue and green devices with aluminum oxide insulation layer, and then use semiconductor patterning to expose the bonding layer and cathode compound semiconductor of each wafer layer by layer, use Cr / Pt / Au stacking bridge to achieve anode connection and cathode ohmic contact, and expose the red light OLED anode;
[0053] Step 7: Using electron beam evaporation process to evaporate the organic (what type of DCJTB material) red light OLED device onto the device described in step 6;
[0054] Step 8: Spin coating is used to cover the entire surface of the device with an SU8 organic insulating layer, and then semiconductor patterning is used to expose the cathode of each wafer layer by layer. ITO\Ag transparent conductive layer stacking is used to achieve cathode common electrode interconnection, and a black matrix is introduced between the red light OLED device and the blue and green devices.
[0055] A display device with a device size of 5 μm and a pixel size of 11 μm is prepared by the above method. In the display device, the external quantum efficiency of red light is 20%, the external quantum efficiency of blue light is 25%, and the external quantum efficiency of green light is 15%.
[0056] Example 2
[0057] In this embodiment, the first wafer is a green wafer, and the second wafer is a blue wafer;
[0058] Step 1: Select a TFT glass backplane and prepare a first bonding film on the TFT glass backplane, wherein the first bonding film is a gold-indium alloy;
[0059] Step 2: Select quantum well silicon-based InGaN green light wafer material, prepare a P-type ohmic contact layer on the wafer surface of the green light wafer, and then prepare a bonding film, where the bonding film is a gold-nickel alloy;
[0060] Step 3: Bond the green light wafer to the TFT glass backplane using eutectic bonding. The wafer substrate of the green light wafer is removed by grinding and thinning, and the compound layer is appropriately thinned to expose the N-type contact.
[0061] Step 4: introducing a silicon oxide insulating layer on one side of the upper surface of the green light wafer, and then preparing a second bonding film on the silicon oxide insulating layer, wherein the second bonding film is a gold-indium alloy;
[0062] Step 5: Select a silicon-based InGaN blue light wafer material, prepare a P-type ohmic contact layer on the wafer surface of the blue light wafer, and then prepare a bonding film, where the bonding film is a gold-indium alloy;
[0063] Step 6: Bond the blue epitaxial wafer with the bonding layer prepared to the green epitaxial wafer in step 4, remove the Si substrate by grinding and thinning, and use semiconductor etching to expose the N-type compound semiconductor of the blue and green wafers, and use the Cr / Pt / Au structure metal to achieve interconnection between the anode and the TFT circuit contacts below and ohmic contact with the cathode;
[0064] Step 7: using an inkjet printing process to evaporate a red light OLED device onto the device described in step 6;
[0065] Step 8: Spin coating exposure is used to cover the entire surface of the device with a black glue organic insulating layer, which serves as an insulating layer and a black matrix at the same time. Semiconductor patterning is then used to expose the cathodes of each wafer and OLED layer, and ITO\ZnO transparent conductive film stacking is used to achieve cathode common electrode interconnection;
[0066] A display device with a device size of 5 μm and a pixel size of 11.5 μm is prepared by the above method. In the display device, the external quantum efficiency of red light is 20%, the efficiency of blue light is 25%, and the efficiency of green light is 15%.
[0067] Example 3
[0068] In this embodiment, the first wafer is a blue light wafer, and the second wafer is a green light wafer;
[0069] Step 1: Select a TFT glass backplane and prepare a first bonding film on the TFT glass backplane, wherein the first bonding film is a gold-indium alloy;
[0070] Step 2: Select quantum well silicon-based InGaN blue light wafer material, prepare a P-type ohmic contact layer on the wafer surface of the blue light wafer, and then prepare a bonding film, where the bonding film is a gold-nickel alloy;
[0071] Step 3: Use eutectic bonding to bond the blue light wafer to the TFT glass backplane. The wafer substrate of the blue light wafer is removed by grinding and thinning, and the compound layer is appropriately thinned to expose the N-type contact.
[0072] Step 4: introducing a silicon oxide insulating layer on one side of the upper surface of the blue light wafer, and then preparing a second bonding film on the silicon oxide insulating layer, wherein the second bonding film is a gold-indium alloy;
[0073] Step 5: Select silicon-based InGaN green light wafer material, prepare a P-type ohmic contact layer on the wafer surface of the green light wafer, and then prepare a bonding film, where the bonding film is a gold-indium alloy;
[0074] Step 6: Bond the green epitaxial wafer with the bonding layer prepared to the blue epitaxial wafer in step 4, remove the Si substrate by grinding and thinning, and use semiconductor etching to expose the N-type compound semiconductor of the green and blue wafers, and use Cr / Pt / Au structured metal to achieve interconnection between the anode and the TFT circuit contacts below and ohmic contact with the cathode;
[0075] Step 7: using an inkjet printing process to evaporate a red light OLED device onto the device described in step 6;
[0076] Step 8: Spin coating exposure is used to cover the entire surface of the device with a black glue organic insulating layer, which serves as an insulating layer and a black matrix at the same time. Semiconductor patterning is then used to expose the cathodes of each wafer and OLED layer, and ITO\ZnO transparent conductive film stacking is used to achieve cathode common electrode interconnection;
[0077] A display device with a device size of 5.5 μm and a pixel size of 12 μm is prepared by the above method. In the display device, the external quantum efficiency of red light is 20%, the efficiency of blue light is 23%, and the efficiency of green light is 13%.
[0078] Comparative Example 1
[0079] In this comparative example, the first wafer is a green light wafer, and the second wafer is a blue light wafer;
[0080] Step 1: Select a TFT glass backplane and prepare a first bonding film on the TFT glass backplane, wherein the first bonding film is a gold-indium alloy;
[0081] Step 2: Select silicon-based InGaN green light wafer material, prepare a P-type ohmic contact layer on the wafer surface of the green light wafer, and then prepare a bonding film, where the bonding film is a gold-nickel alloy;
[0082] Step 3: Bond the green wafer to the TFT glass backplane using eutectic bonding. The wafer substrate of the green wafer is removed by grinding and thinning, and the compound layer is appropriately thinned to expose the N-type contact.
[0083] Step 4: introducing a silicon oxide insulating layer on one side of the upper surface of the green light wafer, and then preparing a second bonding film on the silicon oxide insulating layer, wherein the second bonding film is a gold-indium alloy;
[0084] Step 5: Select a silicon-based InGaN blue light wafer material, prepare a P-type ohmic contact layer on the wafer surface of the blue light wafer, and then prepare a bonding film, where the bonding film is a gold-indium alloy;
[0085] Step 6: Bond the blue epitaxial wafer with the bonding layer prepared to the green epitaxial wafer in step 4, remove the Si substrate by grinding and thinning, and use semiconductor etching to expose the N-type compound semiconductor of the blue and green wafers, and use the Cr / Pt / Au structure metal to achieve interconnection between the anode and the TFT circuit contacts below and ohmic contact with the cathode;
[0086] Step 7: using a mass transfer process to align and bond the inorganic red LED device to the device described in step 6, and complete the anode connection;
[0087] Step 8: Spin coating exposure is used to cover the entire surface of the device with a black glue organic insulating layer, which serves as an insulating layer and a black matrix at the same time. Then, semiconductor graphics are used to expose the cathode of each device, and ITO\ZnO transparent conductive film stacking is used to achieve cathode common electrode interconnection;
[0088] A display device with a device size of 7 μm and a pixel size of 15 μm is prepared by the above method. In the display device, the external quantum efficiency of red light is 12%, the efficiency of blue light is 20%, and the efficiency of green light is 12%.
[0089] Comparative Example 2
[0090] In this embodiment, the first wafer is a green wafer, and the second wafer is a blue wafer;
[0091] Step 1: Select a PCB driving backplane, and prepare a first bonding film on the PCB driving backplane, wherein the first bonding film is a gold-nickel alloy;
[0092] Step 2: Select quantum well green light wafer material, and prepare a bonding film on the wafer surface of the green light wafer, wherein the bonding film is a gold-nickel alloy;
[0093] Step 3: Bond the green wafer to the PCB driver backplane by alignment bonding, and remove the wafer substrate of the green wafer by laser stripping;
[0094] Step 4: introducing a silicon oxide insulating layer on one side of the upper surface of the green light wafer close to the edge anode contact, and then preparing a second bonding film on the silicon oxide insulating layer, wherein the second bonding film is a gold-indium alloy;
[0095] Step 5: Select quantum well blue light wafer material, prepare a bonding film on the wafer surface of the blue light wafer, the bonding film is a gold-indium alloy, and use an alignment bonding method to bond the blue wafer to the green wafer.
[0096] Step 6: Using semiconductor photolithography process to expose the N-type compound semiconductor of blue and green wafers layer by layer;
[0097] Step 7: Using an electron beam evaporation process to evaporate an organic (what type) red light OLED device onto the device described in step 6;
[0098] Step 8: Use ALD to cover the entire surface of the device with an aluminum oxide insulating layer, then use semiconductor patterning to expose the bonding layer and cathode compound semiconductor of each wafer layer by layer, use gold single-element bridging to achieve anode connection and cathode common electrode interconnection, and introduce a black matrix between the red light OLED device and the blue and green wafers.
[0099] A display device with a device size of 8 μm and a pixel size of 16 μm was prepared in the above manner. However, due to the accuracy of the alignment and bonding process, the obtained display device could not be used normally.
Claims
1. An inorganic-organic LED hybrid color display device, characterized in that: It comprises a driving backplane (1), a first bonding film (2), a first wafer (3), a second bonding film (4), a second wafer (5), a red light OLED (6) and a metal bridge (7); The driving backplane is provided with three anode contacts (8) with equal spacing and in parallel, and a first bonding film is laid on two adjacent anode contacts; When the first wafer is a green wafer, the second wafer is a blue wafer; when the first wafer is a blue wafer, the second wafer is a green wafer; A first wafer is bonded to the first bonding film, an insulating layer (9) is provided on the upper surface of the first wafer, a second bonding film is provided on the insulating layer, and a second wafer is bonded to the second bonding film; The red light OLED is integrated on an anode contact point covered by no bonding film, and a black matrix (10) is provided between the red light OLED and the first and second wafers; the first wafer, the second wafer and the red light OLED are connected to the anode contact of the driving backplane via a metal bridge; the first wafer, the second wafer and the red light OLED are connected to the cathode via the metal bridge; The manufacturing method of the display device comprises the following steps: 1) preparing a first bonding film on a driving backplane; 2) preparing a bonding film on a wafer surface of a first wafer and bonding it to the driving backplane before laying an insulating layer; 3) preparing a second bonding film on a wafer surface of a second wafer and bonding it to the insulating layer of a green wafer; 4) exposing the N-type compound semiconductor of each wafer layer by layer; 5) evaporating a red light OLED onto the driving backplane; 6) after the insulating layer covers the color display device as a whole, exposing the P-type compound semiconductor of each wafer and the cathode of the red light OLED layer by layer and interconnecting them with a common electrode, thus obtaining; In the step 2), the bonding method of the green light wafer is non-aligned bonding, using at least one of thermal compression bonding, eutectic bonding and surface activated bonding; in the step 3), the bonding method of the blue light wafer is non-aligned bonding, using at least one of thermal compression bonding, eutectic bonding and surface activated bonding.
2. The inorganic-organic LED hybrid color display device according to claim 1, characterized in that: The driving backplane is at least one of a TFT thin film transistor, an LTPS low temperature polysilicon, a CMOS integrated circuit and a high mobility transistor.
3. The inorganic-organic LED hybrid color display device according to claim 1, characterized in that: The first bonding film is at least one of gold, nickel, tin, aluminum, copper and indium; the second bonding film is at least one of gold, nickel, tin, aluminum, copper and indium.
4. The inorganic-organic LED hybrid color display device according to claim 1, characterized in that: The metal bridge is at least one of gold, nickel, tin, aluminum, copper and indium.
5. The inorganic-organic LED hybrid color display device according to claim 1, characterized in that: The green light wafer comprises, from bottom to top, a wafer substrate, a buffer layer, an N-type compound semiconductor, a quantum well, a P-type compound semiconductor and a P-type ohmic contact; the blue light wafer comprises, from bottom to top, a wafer substrate, a buffer layer, an N-type compound semiconductor, a quantum well, a P-type compound semiconductor and a P-type ohmic contact; the red light OLED material is a small molecule and / or polymer OLED organic material.
6. The inorganic-organic LED hybrid color display device according to claim 1, characterized in that: In step 4), the method of exposing the N-type compound semiconductor layer by layer is wet etching and / or dry etching.
7. The inorganic-organic LED hybrid color display device according to claim 1, characterized in that: In step 5), the red light OLED evaporation method is at least one of patterned electron beam, thermal evaporation, vacuum evaporation and sputtering evaporation.
8. The inorganic-organic LED hybrid color display device according to claim 1, characterized in that: In step 6), the overall covering method of the insulating layer is at least one of coating, chemical vapor deposition, atomic layer deposition and sputtering evaporation; the insulating layer is at least one of silicon oxide, aluminum oxide, silicone oil and silane coupling agent.