Mould repairing method and mould
By using an end mill that is smaller than when the mold is newly made for repair, and selecting an appropriate diameter based on rotational vibration, the high-precision problem of on-site repair of the concave and convex forming surface of the mold is solved, and high-precision repair and aesthetic protection of the luster pattern are achieved.
Patent Information
- Application Number
- CN201980103314.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-10-31
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-10-31
AI Technical Summary
It is difficult to repair the concave and convex molding surface of the mold with high precision on-site with the existing technology. Especially for decorations with glossy patterns on the surface, repairing can easily lead to the problem that the glossy pattern is not clear.
Use an end mill with a smaller diameter than when the mold is newly made for repair, and select an appropriate diameter based on the rotational vibration of the end mill spindle to reduce cutting accuracy and overcutting. Use a small diameter end mill when repairing to suppress rotation. Inaccurate cutting due to vibration.
It achieves high-precision repair of concave and convex molding surfaces, avoids deterioration of the aesthetics of the luster pattern, and can quickly and accurately repair molds made in Japan at overseas sites, even without a high-precision processing machine.
Smart Images

Figure CN114845824B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a mold repairing method and a mold, and in particular to regeneration of a concavo-convex molding surface in a mold. Background Art
[0002] For example, Patent Document 1 discloses a surface repair method for a stamping die that repairs a damaged portion generated on the flat surface of the die. Specifically, first, for a concave damaged portion of the stamping die that exists on the flat surface, a hole is opened in an area wider than the damaged portion, thereby forming a processed hole on the flat surface. Next, the processed hole is blocked by driving a driven component into the processed hole. In addition, the flat surface of the die is regenerated by cutting the driven component (protrusion) protruding from the flat surface using a grinder or the like. In addition, although it does not involve a mold repair method, Patent Document 2 discloses a mold cutting method that makes a high-precision mold by making the cutting resistance constant relative to the feed direction of the end mill and making the cutting resistance equal when the end mill reciprocates.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2017-47447
[0006] Patent Document 2: Japanese Patent Application Laid-Open No. 11-347823 Summary of the invention
[0007] Problems to be solved by the invention
[0008] In recent years, most molds produced in Japan are used in factories overseas, including in developing countries. In the case where defects or other damage occur on the surface of the mold due to on-site use, it is not realistic to transfer it to Japan for repair from the perspective of cost and speed, and the repair must usually be performed quickly on site. However, when repairing using a processing machine that exists on site, even if an end mill with the same diameter as the end mill when the mold was newly made is used, it is sometimes impossible to repair the forming surface of the mold with high precision. This problem is particularly prominent in molded products whose surfaces are decorated with colorful patterns such as diamond block patterns and honeycomb patterns, and the colorful pattern may be unclear to the extent that it can be visually seen at the repaired part.
[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to repair a concavo-convex molding surface in a mold with high accuracy.
[0010] Means used to solve problems
[0011] In order to solve this problem, the first invention provides a mold repair method including a first step and a second step. In the first step, a damaged portion generated on a concave-convex molding surface in the mold is filled with a repair material. In the second step, a second end mill having a smaller diameter than a first end mill used when a new mold is made is used to cut the surface raised by the repair material, thereby regenerating the concave-convex molding surface.
[0012] Here, in the first invention, the second step may include the following steps: measuring the rotational vibration of the spindle on which the second end mill is installed; and selecting the diameter of the second end mill according to the measured rotational vibration. Alternatively, the second step may include the following steps: measuring the rotational vibration of the spindle on which the second end mill is installed; and allowing the use of the second end mill when the measured rotational vibration is below a predetermined threshold. At this time, the second step may also include the following steps: not allowing the use of the second end mill when the measured rotational vibration is greater than a predetermined threshold. In addition, in the first invention, it is preferred that the above-mentioned concave-convex molding surface has a concave-convex pattern, and the concave-convex pattern is used to decorate the surface of the molded product with a colorful pattern.
[0013] The second invention provides a mold having a concavo-convex forming surface. The mold has a non-repaired area where the forming surface is not repaired and a repaired area including a portion where damage on the forming surface is repaired. Here, the tool trajectory shape in the surface of the repaired area is smaller than the tool trajectory shape in the surface of the non-repaired area.
[0014] The third invention provides a mold having a concavo-convex molding surface. The mold has a non-repaired area where the molding surface is not repaired and a repaired area including a portion where damage on the molding surface is repaired. Here, the surface roughness in the repaired area is smaller than the surface roughness in the non-repaired area.
[0015] Effects of the Invention
[0016] According to the first invention, when repairing a mold, a second end mill having a smaller diameter than the first end mill used when the mold is newly made is used. Generally, the larger the rotational vibration of the spindle to which the end mill is mounted, the larger the apparent diameter of the end mill becomes. However, if the increase is anticipated and a second end mill with a smaller diameter is used, the reduction in cutting accuracy caused by the rotational vibration can be reduced. As a result, when repairing, even if a processing machine having a larger rotational vibration than when the mold is newly made is used, excessive cutting of the surface can be suppressed, so that the concave and convex forming surface can be repaired with high precision.
[0017] Furthermore, according to the second invention and the third invention, it is possible to verify whether the mold has been repaired by the repair method according to the first invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is the appearance of the mold.
[0019] Figure 2 It is a cross-sectional view of a mold having a damaged portion.
[0020] Figure 3 This is a diagram showing the process of filling the damaged portion with a repair material.
[0021] Figure 4 This is a diagram showing a cutting process using an end mill.
[0022] Figure 5 This is an explanatory diagram of the case where repair is performed using an end mill having the same diameter as that used when the die was newly manufactured.
[0023] Figure 6 This is an explanatory diagram of the case where repair is performed using an end mill having a smaller diameter than when the die was newly manufactured.
[0024] Figure 7 This is an enlarged photograph showing the state of the molding surface in the mold. DETAILED DESCRIPTION
[0025] Figure 1 1 is an appearance diagram of the mold involved in this embodiment. The mold 1 is used to form a plastic molded product, etc., after the surface is decorated with a colorful pattern such as a diamond block pattern or a honeycomb pattern. A concave-convex pattern is formed on the molding surface 1a of the mold 1 by inverting the concave-convex on the molded product side where the colorful pattern appears.
[0026] When the die 1 is installed in the punching device or removed, or when the removed die 1 is transported, if an object accidentally hits the die 1, such as Figure 2 As shown, the uneven molding surface 1a is damaged, and sometimes a locally sunken damaged portion 1b is generated. In this case, in order to avoid delaying the production line of the factory, the damaged mold 1 needs to be repaired quickly on site.
[0027] As a repair operation of the mold 1, first, Figure 3 As shown, the damaged portion 1b formed on the molding surface 1a is filled with the repair material 2. As a result, the surface containing the repair material 2 is raised from the surrounding area.
[0028] Then, if Figure 4 As shown, the surface raised by the repair material 2 is cut by the end mill 3, so that the raised surface and the surrounding surface become the same plane. In this way, the forming surface 1b is regenerated. Here, the diameter R1 of the end mill 3 used when repairing the mold 1 is smaller than the diameter R2 of the end mill used when the mold 1 is newly made.
[0029] like Figure 5As shown, consider the case where the diameter of the end mill used when the mold 1 is newly made is R2, and the end mill 3' with the same diameter is used for repair. Since there is a rotational vibration α on the main shaft of the processing machine on which the end mill 3' is installed, the apparent diameter of the end mill 3' when rotating is R2+α. In the case of repairing using a processing machine with a larger rotational vibration than when the mold 1 is newly made, in the worst case, the rotational vibration produces a difference of α. As a result, in the worst case, the contour of the forming surface 1a formed by the ball mill with a diameter of R2 when newly made is cut using a ball mill with a larger diameter (R2+α), thereby over-cutting area A of the forming surface 1b. Such over-cutting will also be truly reflected in the glossy pattern of the molded product to which the concave-convex pattern of the forming surface 1b is transferred, resulting in a deterioration in aesthetics, and is therefore not preferred.
[0030] In contrast, if Figure 6 As shown in FIG. 1 , consider the case where the end mill 3 with a diameter smaller than R1 and a diameter of R2 used when the mold 1 is newly manufactured is used for repair. In this case, due to the rotational vibration of the spindle, the apparent diameter of the end mill 3 becomes R1+α, but if it is less than R2, the above-mentioned overcutting problem will not occur. That is, if the end mill 3 with a smaller diameter than the new mold 1 is used based on the expected rotational vibration α, the overcutting of the forming surface 2 can be effectively suppressed.
[0031] The following two specific measures can be considered for repairing the mold 1. First, after measuring the rotational vibration α of the spindle on which the end mill 3 is mounted using a measuring instrument, the diameter of the end mill 3 is selected based on the rotational vibration α. For example, the larger the rotational vibration α, the smaller the diameter of the end mill 3 is selected.
[0032] Second, when the rotational vibration α measured by the measuring instrument is below a predetermined threshold value (R2~R1), the use of the end mill 3 with a diameter of R1 is allowed. When it is greater than the predetermined threshold value (R2~R1), the use of the end mill 3 with a diameter of R1 is not allowed (prohibited).
[0033] Figure 7 This is an enlarged photograph showing the state of the forming surface 1a in the mold 1. Generally, when the forming surface 1a is processed by cutting with an end mill, a spiral cutting mark (tool path shape) is generated from the tool path. As a characteristic, there is a tendency that the smaller the diameter of the end mill, the smaller the tool path shape, and the smaller the surface roughness of the forming surface 1a.
[0034] According to this characteristic, by comparing the states of the non-repaired area and the repaired area in the forming surface 1a, it is possible to determine whether the mold has been repaired by the above-mentioned repair method. The non-repaired area is an area where the forming surface 1a has not been repaired, and the repaired area is an area including the part where the damage on the forming surface 1a has been repaired (including the surrounding of the damaged part). Specifically, the tool trajectory shape generated by the surface of the repaired area is smaller than the tool trajectory shape generated by the surface of the non-repaired area, so such a state occurs, and it can be determined that the mold has been repaired by the present repair method. In addition, the roughness of the surface in the repaired area is smaller than the roughness of the surface in the non-repaired area, so such a state occurs, and it can be determined that the mold has been repaired by the present repair method.
[0035] Thus, according to the present embodiment, when repairing the mold 1, an end mill 3 having a smaller diameter than that used when the mold 1 was newly manufactured is used. Generally, the larger the rotational vibration of the spindle to which the end mill 3 is mounted, the larger the apparent diameter of the end mill 3 becomes. However, if the end mill 3 having a smaller diameter is used in anticipation of this increase, the reduction in cutting accuracy caused by the rotational vibration can be reduced. As a result, when repairing, even if a processing machine having a larger rotational vibration than that when the mold 1 was newly manufactured is used, excessive cutting of the surface can be suppressed, so that the concavo-convex molding surface 1b can be repaired with high precision.
[0036] Furthermore, according to the present embodiment, even in the case of a molded product whose surface is decorated with a graphic pattern of a bright pattern such as a diamond block pattern or a honeycomb pattern, the blurriness of the bright pattern caused by repair can be effectively eliminated.
[0037] Furthermore, according to the present embodiment, when a mold produced in Japan is repaired at an overseas site, even if there is no high-precision processing machine like that in Japan, it can be widely used as a method of repairing quickly and with high precision.
[0038] It should be noted that, in the above-mentioned embodiment, the repair of the molding surface 1b having a concave-convex pattern for decorating the surface of the molded product with a colorful pattern is described as an example, but the present invention is not limited to this and can be widely applied to the repair of molds having concave-convex molding surfaces.
[0039] Description of Reference Numerals
[0040] 1: Mould;
[0041] 1a: forming surface;
[0042] 1b: injured part;
[0043] 2: Repair materials;
[0044] 3, 3': End mill.
Claims
1. A method for repairing a mold, characterized in that: The mold repair method includes the following steps: The first step is to fill the damaged part generated on the concavo-convex molding surface of the mold with a repair material, The second step is to cut the surface raised by the repair material using a second end mill whose diameter is smaller than that of the first end mill used when the mold is newly made to produce a tool trajectory shape on the uneven forming surface in order to foresee an increase in apparent diameter caused by the rotational vibration of the spindle of the processing machine, and which produces a tool trajectory shape on the repaired surface on the uneven forming surface, thereby regenerating the uneven forming surface.
2. The mold repair method according to claim 1, characterized in that: The second step comprises the following steps: measuring the rotational vibration of a spindle to which the second end mill is mounted; and The diameter of the second end mill is selected based on the measured rotational vibration.
3. The mold repair method according to claim 1, characterized in that: The second step comprises the following steps: measuring the rotational vibration of a spindle to which the second end mill is mounted; and When the measured rotational vibration is equal to or less than a predetermined threshold value, use of the second end mill is permitted.
4. The mold repair method according to claim 3, characterized in that: The mold repair method includes the following steps: when the measured rotational vibration is greater than a predetermined threshold, the second end mill is not allowed to be used.
5. The mold repair method according to any one of claims 1 to 4, characterized in that: The concavo-convex molding surface has a concavo-convex pattern for decorating the surface of the molded product with a colorful pattern.
6. A mold, characterized in that: The mold having a concave-convex molding surface has: a non-repaired area where the repair of the forming surface is not performed; and a repaired area including a portion where the damage on the forming surface is repaired, The tool trajectory shape in the surface of the repairing area is smaller than the tool trajectory shape in the surface of the non-repairing area.
Citation Information
Patent Citations
Cutting method for metal mold
JP1999347823A
Surface repair method of press die
JP2017047447A
Orbital end mill
CN101534989A
Soldering method of ingot mould
CN102069269A
Method for repairing reinforcing pit on planar profile of die
CN102581545A