Blue-emitting ZnSe with low full width at half maximum 1-x Te x Synthesis of Alloy Nanocrystals

ZnSe 1-x Te x nanostructures with ZnS/ZnSe shells address the challenge of toxic materials in LEDs by achieving narrow emission spectra and high quantum yield, providing a safe and effective alternative for LED applications.

CN114867818BActive Publication Date: 2024-12-03SHOEI CHEM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080068876.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-08-12
Filing Date
2020-08-12
Publication Date
2024-12-03
Estimated Expiration
2040-08-12

Smart Images

  • Figure CN114867818B_ABST
    Figure CN114867818B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of nanotechnology. The present invention provides a highly luminescent nanostructure, in particular comprising ZnSe 1‑x Te x Highly luminescent nanostructures with a ZnSe core and a ZnSe and / or ZnSe shell. 1‑x Te x The nanostructure of the core and the ZnS and / or ZnSe shell layer shows low half maximum full width and high quantum yield. The present invention also provides a method for preparing the nanostructure.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] BACKGROUND OF THE INVENTION Technical Field

[0002] The present invention relates to the field of nanotechnology. The present invention provides a highly luminescent nanostructure, in particular comprising ZnSe 1- x Te x Highly luminescent nanostructures with a core and a ZnS and / or ZnSe shell. 1-x Te x The nanostructure of the core and the ZnS and / or ZnSe shell layer shows low half maximum full width and high quantum yield. The present invention also provides a method for preparing the nanostructure. Background Art

[0003] Semiconductor nanostructures can be integrated into various electronic and optical devices. The electrical and optical properties of such nanostructures vary, for example depending on their composition, shape and size. For example, the size-adjustable properties of semiconductor nanoparticles are very beneficial for applications such as light emitting diodes (LEDs), lasers and biomedical markers. Highly luminescent nanostructures are particularly ideal for such applications.

[0004] In order to realize the full potential of nanostructures in applications such as LEDs and displays, nanostructures need to meet five criteria simultaneously: narrow and symmetrical emission spectra, high photoluminescence (PL) quantum yield (QY), high optical stability, environmentally friendly materials, and low-cost large-scale production methods. Previous research on high-emissivity and color-tunable quantum dots has mostly focused on materials containing cadmium, mercury, or lead. Wang, A. et al., Nanoscale 7:2951-2959 (2015). However, there is increasing concern that toxic substances such as cadmium, mercury, or lead pose a serious threat to human health and the environment, and the EU's Restriction of Hazardous Substances Regulation prohibits any consumer electronic products containing more than trace amounts of these materials. Therefore, it is necessary to prepare materials that do not contain cadmium, mercury, and lead for the production of LEDs and displays.

[0005] Electroluminescent quantum dot light-emitting devices with a BT.2020 color gamut require blue-emitting quantum dot materials with a peak wavelength in the range of 450nm to 460nm, a full width at half maximum (FWHM) of less than 30nm, and high quantum yield. To comply, cadmium- and lead-free materials are required.

[0006] It is difficult to achieve these parameters using cadmium-free materials. As described by Ning, J. et al., Chem. Commun. 53:2626-2629 (2017), indium phosphide quantum dots grown from magic size clusters, which are the smallest imaginable nuclei, exhibit a minimum photoluminescence peak at 460 nm (with a FWHM > 50 nm and low quantum yield) and a red shift upon shell coating. As described in U.S. Patent Application No. 2017 / 0066965, ZnSe quantum dots can be fabricated with very sharp emission peaks and high quantum yields at peak wavelengths up to 435 nm, but further particle growth towards the target wavelength results in significant quantum yield losses due to poor electron-hole overlap in the giant nuclei.

[0007] There is a need to prepare nanostructured compositions having a peak emission wavelength in the range of 440 nm to 460 nm and a FWHM of less than 30 nm. SUMMARY OF THE INVENTION

[0008] The present disclosure provides nanostructures comprising a core surrounded by at least one shell, wherein the core comprises ZnSe 1- x Te x , where 0 < x < 1, wherein the at least one shell is selected from ZnS, ZnSe, ZnTe, and their alloys, and wherein the full width at half maximum (FWHM) of the nanostructure is from about 20 nm to about 30 nm.

[0009] In some embodiments, the FWHM is from about 25 nm to about 30 nm.

[0010] In some embodiments, the emission wavelength of the nanostructure is from about 440 nm to about 460 nm. In some embodiments, the emission wavelength of the nanostructure is 450 - 460 nm.

[0011] In some embodiments, the core of the nanostructure is surrounded by two shells.

[0012] In some embodiments, at least one shell of the nanostructure comprises ZnS or ZnSe.

[0013] In some embodiments, at least one shell of the nanostructure comprises ZnSe.

[0014] In some embodiments, at least one shell of the nanostructure comprises ZnS.

[0015] In some embodiments, at least one shell of the nanostructure comprises from about 4 to about 6 monolayers of ZnSe.

[0016] In some embodiments, at least one shell of the nanostructure comprises about 6 monolayers of ZnSe.

[0017] In some embodiments, at least one shell of the nanostructure comprises from about 4 to about 6 monolayers of ZnS.

[0018] In some embodiments, at least one shell of the nanostructure comprises about 4 monolayers of ZnS.

[0019] In some embodiments, the nanostructures have a photoluminescence quantum yield of about 75% to about 90%.

[0020] In some embodiments, the photoluminescence quantum yield of the nanostructure is between 80% and 90%.

[0021] In some embodiments, the FWHM of the nanostructures is from about 15 nm to about 19 nm.

[0022] In some embodiments, the nanostructure comprises two shells, wherein the first shell comprises ZnSe and the second shell comprises ZnS.

[0023] In some embodiments, the nanostructures are quantum dots.

[0024] In some embodiments, the nanostructures are free of cadmium.

[0025] In some embodiments, devices comprising the nanostructures of the present disclosure are provided.

[0026] The present disclosure also provides a method for preparing ZnSe 1-x Te x A method for nanocrystals comprising:

[0027] (a) mixing a tellurium source, at least one ligand and a reducing agent to prepare a reaction mixture;

[0028] (b) contacting the reaction mixture obtained in (a) with a solution comprising at least one ligand, zinc fluoride and a selenium source; and

[0029] (c) contacting the reaction mixture obtained in (b) with a zinc source;

[0030] To provide ZnSe 1-x Te x Nanocrystals.

[0031] In some embodiments, the selenium source is selected from trioctylphosphine selenide, tri(n-butyl)phosphine selenide, tri(sec-butyl)phosphine selenide, tri(tert-butyl)phosphine selenide, trimethylphosphine selenide, triphenylphosphine selenide, diphenylphosphine selenide, phenylphosphine selenide, cyclohexylphosphine selenide, octaselenol, dodecaselenol, selenophenol, elemental selenium, hydrogen selenide, bis(trimethylsilyl)selenide, and mixtures thereof. In some embodiments, the selenium source is trioctylphosphine selenide.

[0032] In some embodiments, the at least one ligand in (b) is selected from trioctylphosphine oxide, trioctylphosphine, diphenylphosphine, triphenylphosphine oxide, and tributylphosphine oxide. In some embodiments, the at least one ligand in (b) is diphenylphosphine.

[0033] In some embodiments, the tellurium source is selected from trioctylphosphine telluride, tri(n-butyl)phosphine telluride, trimethylphosphine telluride, triphenylphosphine telluride, tricyclohexylphosphine telluride, elemental tellurium, hydrogen telluride, bis(trimethylsilyl) telluride, and mixtures thereof. In some embodiments, the tellurium source is trioctylphosphine telluride.

[0034] In some embodiments, the reducing agent is selected from diborane, sodium hydride, sodium borohydride, lithium borohydride, sodium cyanoborohydride, calcium hydride, lithium hydride, lithium aluminum hydride, diisobutylaluminum hydride, sodium triethylborohydride, and lithium triethylborohydride. In some embodiments, the reducing agent is lithium triethylborohydride.

[0035] In some embodiments, the zinc source in (c) is selected from diethyl zinc, dimethyl zinc, diphenyl zinc, zinc acetate, zinc acetylacetonate, zinc iodide, zinc bromide, zinc chloride, zinc fluoride, zinc carbonate, zinc cyanide, zinc nitrate, zinc oxide, zinc peroxide, zinc perchlorate and zinc sulfate. In some embodiments, the zinc source in (c) is diethyl zinc.

[0036] In some embodiments, the method further comprises:

[0037] (d) contacting the reaction mixture of (c) with a zinc carboxylate and a selenium source.

[0038] In some embodiments, the zinc carboxylate in (d) is selected from zinc oleate, zinc hexanoate, zinc octoate, zinc laurate, zinc myristate, zinc palmitate, zinc stearate, zinc dithiocarbamate, and mixtures thereof. In some embodiments, the zinc carboxylate in (d) is zinc oleate.

[0039] In some embodiments, the selenium source in (d) is selected from trioctylphosphine selenide, tri(n-butyl)phosphine selenide, tri(sec-butyl)phosphine selenide, tri(tert-butyl)phosphine selenide, trimethylphosphine selenide, triphenylphosphine selenide, diphenylphosphine selenide, phenylphosphine selenide, cyclohexylphosphine selenide, octylselenol, dodecanol, phenylselenol, elemental selenium, hydrogen selenide, bis(trimethylsilyl)selenide, and mixtures thereof. In some embodiments, the selenium source in (d) is trioctylphosphine selenide.

[0040] In some embodiments, the mixing in (a) is performed at about room temperature.

[0041] In some embodiments, the contacting in (b) is performed at a temperature of about 250°C to about 350°C. In some embodiments, the contacting in (b) is performed at a temperature of about 280°C.

[0042] In some embodiments, the contacting in (c) is performed at a temperature of about 250°C to about 350°C. In some embodiments, the contacting in (c) is performed at a temperature of about 280°C.

[0043] In some embodiments, the contacting in (c) further comprises at least one ligand. In some embodiments, the at least one ligand is trioctylphosphine or diphenylphosphine.

[0044] In some embodiments, the contacting in (d) is performed at a temperature of about 250° C. to about 350° C. In some embodiments, the contacting in (d) is performed at a temperature of about 310° C.

[0045] In some embodiments, the contacting in (d) further comprises at least one ligand. In some embodiments, the at least one ligand is trioctylphosphine or diphenylphosphine.

[0046] The present disclosure also provides a method for preparing a core / shell nanostructure, comprising:

[0047] (e) ZnSe prepared by any of the above methods 1-x Te x mixing the nanocrystals with a solution comprising a zinc source; and

[0048] (f) contacting the reaction mixture of (e) with a selenium source or a sulfur source.

[0049] In some embodiments, the method further comprises:

[0050] (g) contacting the reaction mixture of (f) with a selenium source or a sulfur source; wherein the source used in (g) is different from the source used in (f).

[0051] In some embodiments, the mixing in (e) is performed at a temperature of about 20°C to about 310°C. In some embodiments, the mixing in (e) is performed at a temperature of about 20°C to about 100°C.

[0052] In some embodiments, the zinc source of (e) is selected from the group consisting of diethyl zinc, dimethyl zinc, diphenyl zinc, zinc acetate, zinc acetylacetonate, zinc iodide, zinc bromide, zinc chloride, zinc fluoride, zinc carbonate, zinc cyanide, zinc nitrate, zinc oleate, zinc oxide, zinc peroxide, zinc perchlorate, zinc sulfate, zinc hexanoate, zinc octanoate, zinc laurate, zinc myristate, zinc palmitate, zinc stearate, zinc dithiocarbamate, zinc oleate, zinc hexanoate, zinc octanoate, zinc laurate, zinc myristate, zinc palmitate, zinc stearate, zinc dithiocarbamate, and mixtures thereof.

[0053] In some embodiments, the contacting in (f) is performed at a temperature of about 200° C. to about 350° C. In some embodiments, the contacting in (f) is performed at a temperature of about 310° C.

[0054] In some embodiments, the reaction mixture is contacted with a selenium source in (f). In some embodiments, the selenium source is selected from trioctylphosphine selenide, tri(n-butyl)phosphine selenide, tri(sec-butyl)phosphine selenide, tri(tert-butyl)phosphine selenide, trimethylphosphine selenide, triphenylphosphine selenide, diphenylphosphine selenide, phenylphosphine selenide, cyclohexylphosphine selenide, octylselenol, dodecanol, phenylselenol, elemental selenium, hydrogen selenide, bis(trimethylsilyl)selenide, and mixtures thereof.

[0055] In some embodiments, the reaction mixture is contacted with a sulfur source in (f). In some embodiments, the sulfur source is selected from elemental sulfur, octyl mercaptan, dodecanethiol, octadecyl mercaptan, tributylphosphine sulfide, cyclohexyl isothiocyanate, α-toluene mercaptan, ethylene trithiocarbonate, allyl mercaptan, bis(trimethylsilyl) sulfide, trioctylphosphine sulfide, and mixtures thereof.

[0056] In some embodiments, the contacting in (f) is performed at a temperature of about 200° C. to about 350° C. In some embodiments, the contacting in (f) is performed at a temperature of about 310° C.

[0057] In some embodiments, the reaction mixture is contacted with a selenium source in (g). In some embodiments, the selenium source is selected from trioctylphosphine selenide, tri(n-butyl)phosphine selenide, tri(sec-butyl)phosphine selenide, tri(tert-butyl)phosphine selenide, trimethylphosphine selenide, triphenylphosphine selenide, diphenylphosphine selenide, phenylphosphine selenide, cyclohexylphosphine selenide, octylselenol, dodecanol, phenylselenol, elemental selenium, hydrogen selenide, bis(trimethylsilyl)selenide, and mixtures thereof.

[0058] In some embodiments, the reaction mixture is contacted with a sulfur source in (g). In some embodiments, the sulfur source is selected from elemental sulfur, octyl mercaptan, dodecanethiol, octadecyl mercaptan, tributylphosphine sulfide, cyclohexyl isothiocyanate, α-toluene mercaptan, ethylene trithiocarbonate, allyl mercaptan, bis(trimethylsilyl) sulfide, trioctylphosphine sulfide, and mixtures thereof.

[0059] In some embodiments, the mixture in (e) further comprises at least one ligand. In some embodiments, the at least one ligand is selected from trioctylphosphine oxide, trioctylphosphine, diphenylphosphine, triphenylphosphine oxide and tributylphosphine oxide. In some embodiments, the at least one ligand is trioctylphosphine or trioctylphosphine oxide.

[0060] In some embodiments, the nanostructures exhibit a photoluminescence quantum yield of about 75% to about 90%. In some embodiments, the nanostructures exhibit a photoluminescence quantum yield of about 80% to about 90%.

[0061] In some embodiments, the full width at half maximum of the nanostructure is about 20 nm to about 30 nm. In some embodiments, the full width at half maximum of the nanostructure is about 25 nm to about 30 nm.

[0062] The present disclosure also provides a method for preparing ZnSe 1-x Te x A method for nanocrystals comprising:

[0063] (a) mixing a selenium source and at least one ligand to prepare a reaction mixture;

[0064] (b) contacting the reaction mixture obtained in (a) with a solution comprising a tellurium source, a reducing agent and a zinc carboxylate; and

[0065] (c) contacting the reaction mixture obtained in (b) with a zinc source;

[0066] To provide ZnSe 1-x Te x Nanocrystals.

[0067] In some embodiments, the selenium source mixed in (a) is selected from trioctylphosphine selenide, tri(n-butyl)phosphine selenide, tri(sec-butyl)phosphine selenide, tri(tert-butyl)phosphine selenide, trimethylphosphine selenide, triphenylphosphine selenide, diphenylphosphine selenide, phenylphosphine selenide, cyclohexylphosphine selenide, octylselenol, dodecanol, phenylselenol, elemental selenium, hydrogen selenide, bis(trimethylsilyl)selenide and mixtures thereof.

[0068] In some embodiments, the selenium source mixed in (a) is trioctylphosphine selenide.

[0069] In some embodiments, the at least one ligand mixed in (a) is selected from trioctylphosphine oxide, trioctylphosphine, diphenylphosphine, triphenylphosphine oxide, and tributylphosphine oxide.

[0070] In some embodiments, at least one ligand mixed in (a) is trioctylphosphine.

[0071] In some embodiments, the tellurium source in (b) is selected from trioctylphosphine telluride, tri(n-butyl)phosphine telluride, trimethylphosphine telluride, triphenylphosphine telluride, tricyclohexylphosphine telluride, elemental tellurium, hydrogen telluride, bis(trimethylsilyl) telluride, and mixtures thereof.

[0072] In some embodiments, the tellurium source in (b) is trioctylphosphine telluride.

[0073] In some embodiments, the reducing agent in (b) is selected from diborane, sodium hydride, sodium borohydride, lithium borohydride, sodium cyanoborohydride, calcium hydride, lithium hydride, lithium aluminum hydride, diisobutylaluminum hydride, sodium triethylborohydride, and lithium triethylborohydride.

[0074] In some embodiments, the reducing agent in (b) is lithium triethylborohydride.

[0075] In some embodiments, the zinc carboxylate in (b) is selected from zinc oleate, zinc hexanoate, zinc octoate, zinc laurate, zinc myristate, zinc palmitate, zinc stearate, zinc dithiocarbamate, and mixtures thereof.

[0076] In some embodiments, the zinc carboxylate in (b) is zinc oleate.

[0077] In some embodiments, the zinc source in (c) is selected from diethylzinc, dimethylzinc, diphenylzinc, zinc acetate, zinc acetylacetonate, zinc iodide, zinc bromide, zinc chloride, zinc fluoride, zinc carbonate, zinc cyanide, zinc nitrate, zinc oxide, zinc peroxide, zinc perchlorate, and zinc sulfate.

[0078] In some embodiments, the zinc source in (c) is diethylzinc.

[0079] In some embodiments, the preparation of ZnSe 1-x Te x The method of nanocrystals further comprises:

[0080] (d) contacting the reaction mixture of (c) with a zinc source and a selenium source.

[0081] In some embodiments, the zinc source in (d) is selected from diethylzinc, dimethylzinc, diphenylzinc, zinc acetate, zinc acetylacetonate, zinc iodide, zinc bromide, zinc chloride, zinc fluoride, zinc carbonate, zinc cyanide, zinc nitrate, zinc oxide, zinc peroxide, zinc perchlorate, and zinc sulfate.

[0082] In some embodiments, the zinc source in (d) is diethylzinc.

[0083] In some embodiments, the selenium source in (d) is selected from trioctylphosphine selenide, tri(n-butyl)phosphine selenide, tri(sec-butyl)phosphine selenide, tri(tert-butyl)phosphine selenide, trimethylphosphine selenide, triphenylphosphine selenide, diphenylphosphine selenide, phenylphosphine selenide, cyclohexylphosphine selenide, octylselenol, dodecanol, phenylselenol, elemental selenium, hydrogen selenide, bis(trimethylsilyl)selenide, and mixtures thereof.

[0084] In some embodiments, the selenium source in (d) is trioctylphosphine selenide.

[0085] In some embodiments, the mixing in (a) is performed at a temperature of about 250°C to about 350°C.

[0086] In some embodiments, the mixing in (a) is performed at a temperature of about 300°C.

[0087] In some embodiments, the contacting in (b) is performed at a temperature of about 250°C to about 350°C.

[0088] In some embodiments, the contacting in (b) is performed at a temperature of about 300 °C.

[0089] In some embodiments, the contacting in (b) further comprises at least one ligand.

[0090] In some embodiments, the contacting in (c) is performed at a temperature of about 250°C to about 350°C.

[0091] In some embodiments, the contacting in (c) is performed at a temperature of about 300 °C.

[0092] In some embodiments, the contacting in (c) further comprises at least one ligand. In some embodiments, the at least one ligand is trioctylphosphine or diphenylphosphine.

[0093] In some embodiments, the contacting in (d) is performed at a temperature of about 250°C to about 350°C.

[0094] In some embodiments, the contacting in (d) is performed at a temperature of about 300 °C.

[0095] In some embodiments, the contacting in (d) further comprises at least one ligand. In some embodiments, the at least one ligand is trioctylphosphine or diphenylphosphine.

[0096] In some embodiments, the selenium source in (a) is trioctylphosphine selenide, the tellurium source in (b) is trioctylphosphine telluride, the reducing agent in (b) is lithium triethylborohydride, the zinc carboxylate in (b) is zinc oleate, and the zinc source in (c) is diethylzinc.

[0097] In some embodiments, the selenium source in (a) and (c) is trioctylphosphine selenide, the tellurium source in (b) is trioctylphosphine telluride, the reducing agent in (b) is lithium triethylborohydride, the zinc carboxylate in (b) is zinc oleate, and the zinc source in (c) and (d) is diethylzinc,

[0098] The present disclosure provides a method for preparing a core / shell nanostructure, comprising:

[0099] (e) ZnSe prepared by the method disclosed herein 1-x Te x The nanocrystals are mixed with a solution comprising a zinc source;

[0100] (f) contacting the reaction mixture of (e) with a selenium source or a sulfur source.

[0101] In some embodiments, the method of preparing a core / shell nanostructure further comprises:

[0102] (g) contacting the reaction mixture of (f) with a selenium source or a sulfur source; wherein the source used in (g) is different from the source used in (f).

[0103] In some embodiments, the mixing in (e) is performed at a temperature of about 20°C to about 310°C.

[0104] In some embodiments, the mixing in (e) is performed at a temperature of about 20°C to about 100°C.

[0105] In some embodiments, the zinc source of (e) is selected from the group consisting of diethyl zinc, dimethyl zinc, diphenyl zinc, zinc acetate, zinc acetylacetonate, zinc iodide, zinc bromide, zinc chloride, zinc fluoride, zinc carbonate, zinc cyanide, zinc nitrate, zinc oleate, zinc oxide, zinc peroxide, zinc perchlorate, zinc sulfate, zinc hexanoate, zinc octanoate, zinc laurate, zinc myristate, zinc palmitate, zinc stearate, zinc dithiocarbamate, zinc oleate, zinc hexanoate, zinc octanoate, zinc laurate, zinc myristate, zinc palmitate, zinc stearate, zinc dithiocarbamate, and mixtures thereof.

[0106] In some embodiments, the contacting in (f) is performed at a temperature of about 200°C to about 350°C.

[0107] In some embodiments, the contacting in (f) is performed at a temperature of about 310 °C.

[0108] In some embodiments, the reaction mixture in (f) is contacted with a selenium source.

[0109] In some embodiments, the selenium source is selected from trioctylphosphine selenide, tri(n-butyl)phosphine selenide, tri(sec-butyl)phosphine selenide, tri(tert-butyl)phosphine selenide, trimethylphosphine selenide, triphenylphosphine selenide, diphenylphosphine selenide, phenylphosphine selenide, cyclohexylphosphine selenide, octylselenol, dodecanol, phenylselenol, elemental selenium, hydrogen selenide, bis(trimethylsilyl)selenide, and mixtures thereof.

[0110] In some embodiments, the reaction mixture in (f) is contacted with a sulfur source.

[0111] In some embodiments, the sulfur source is selected from elemental sulfur, octyl mercaptan, dodecanethiol, octadecyl mercaptan, tributylphosphine sulfide, cyclohexyl isothiocyanate, α-toluene mercaptan, ethylene trithiocarbonate, allyl mercaptan, bis(trimethylsilyl) sulfide, trioctylphosphine sulfide, and mixtures thereof.

[0112] In some embodiments, the contacting in (f) is performed at a temperature of about 200°C to about 350°C.

[0113] In some embodiments, the contacting in (f) is performed at a temperature of about 310°C.

[0114] In some embodiments, the reaction mixture in (g) is contacted with a selenium source.

[0115] In some embodiments, the selenium source is selected from trioctylphosphine selenide, tri(n-butyl)phosphine selenide, tri(sec-butyl)phosphine selenide, tri(tert-butyl)phosphine selenide, trimethylphosphine selenide, triphenylphosphine selenide, diphenylphosphine selenide, phenylphosphine selenide, cyclohexylphosphine selenide, octylselenol, dodecanol, phenylselenol, elemental selenium, hydrogen selenide, bis(trimethylsilyl)selenide, and mixtures thereof.

[0116] In some embodiments, the reaction mixture in (g) is contacted with a sulfur source.

[0117] In some embodiments, the sulfur source is selected from elemental sulfur, octyl mercaptan, dodecanethiol, octadecyl mercaptan, tributylphosphine sulfide, cyclohexyl isothiocyanate, α-toluene mercaptan, ethylene trithiocarbonate, allyl mercaptan, bis(trimethylsilyl) sulfide, trioctylphosphine sulfide, and mixtures thereof.

[0118] In some embodiments, the admixture in (e) further comprises at least one ligand.

[0119] In some embodiments, the at least one ligand is selected from trioctylphosphine oxide, trioctylphosphine, diphenylphosphine, triphenylphosphine oxide, and tributylphosphine oxide.

[0120] In some embodiments, the at least one ligand is trioctylphosphine or trioctylphosphine oxide.

[0121] In some embodiments, the photoluminescence quantum yield of the nanostructures provided by the method is from about 75% to about 90%.

[0122] In some embodiments, the photoluminescence quantum yield of the nanostructures provided by the method is from about 80% to about 90%.

[0123] In some embodiments, the full width at half maximum of the nanostructures provided by the method is from about 20 nm to about 30 nm.

[0124] In some embodiments, the full width at half maximum of the nanostructures provided by the method is from about 15 nm to about 19 nm.

[0125] The present disclosure also provides a nanostructure molded article, comprising:

[0126] (a) a first conductive layer;

[0127] (b) a second conductive layer; and

[0128] (c) a nanostructure layer located between the first conductive layer and the second conductive layer, wherein the nanostructure layer comprises a population of nanostructures, the nanostructures comprising a core surrounded by at least one shell, wherein the core comprises ZnSe 1-x Te x , where 0 < x < 1, wherein the at least one shell is selected from ZnS, ZnSe, ZnTe, and alloys thereof, and wherein the full width at half maximum (FWHM) of the nanostructures is from about 20 nm to about 30 nm.

[0129] In some embodiments, the nanostructures in the nanostructure molded article comprise two shells.

[0130] In some embodiments, at least one shell of the nanostructures in the nanostructure molded article is selected from those in which at least one shell comprises ZnS or ZnSe.

[0131] In some embodiments, at least one shell of the nanostructures in the nanostructure molded article comprises ZnSe.

[0132] In some embodiments, at least one shell of the nanostructures in the nanostructure molded article comprises ZnS.

[0133] In some embodiments, at least two shells of the nanostructures in the nanostructure molded article comprise zinc.

[0134] In some embodiments, at least one shell of the nanostructures in the nanostructure molding comprises ZnSe and at least one shell comprises ZnS.

[0135] In some embodiments, the photoluminescence quantum yield of the nanostructures in the nanostructure molding is from about 75% to about 90%.

[0136] In some embodiments, the photoluminescence quantum yield of the nanostructures in the nanostructure molding is from about 80% to about 90%.

[0137] In some embodiments, the full width at half maximum of the nanostructures in the nanostructured molded article is from about 20 nm to about 30 nm.

[0138] In some embodiments, the nanostructured molding has a full width at half maximum of about 15 nm to about 19 nm.

[0139] In some embodiments, the nanostructures in the nanostructured molded article comprise at least one shell comprising ZnSe and at least one shell comprising ZnS.

[0140] In some embodiments, the nanostructures in the nanostructured molded article are quantum dots. BRIEF DESCRIPTION OF THE DRAWINGS

[0141] Figure 1 Comparison of the co-injection method for synthesizing ZnSe 1-x Te x Nuclei and ZnSe synthesis using offset injection 1-x Te x Flowchart of the kernel.

[0142] Figure 2 The ZnSe core prepared by the co-injection method is shown. 1-x Te x Core and ZnSe prepared using bias injection method 1-x Te x Photoluminescence spectra of nuclei in solution. DETAILED DESCRIPTION

[0143] definition

[0144] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those generally understood by those of ordinary skill in the art to which the invention belongs. The following definitions supplement the definitions in the prior art and are for current applications and should not be attributed to any related or unrelated circumstances, such as any jointly owned patents or applications. Although any methods and materials similar or equivalent to those described herein can be used in the practice or testing of the present invention, the present invention describes preferred materials and methods. Therefore, the terms used herein are only used for the purpose of describing specific embodiments and are not intended to be limiting.

[0145] As used in this specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. Thus, for example, reference to "a nanostructure" includes a plurality of such nanostructures, and the like.

[0146] As used herein, the term "about" means that the value of a given quantity varies by ± / - 10% of the stated value, for example, "about 100 nm" includes a size range from 90 nm to 110 nm (including the endpoint values).

[0147] "Nanostructure" is a structure with at least one size less than the region or characteristic size of about 500nm. In some embodiments, the nanostructure has a size less than about 200nm, less than about 100nm, less than about 50nm, less than about 20nm or less than about 10nm. Typically, the region or characteristic size will be along the minimum axis of the structure. The example of this structure includes nanowires, nanorods, nanotubes, branched nanostructures, nano four needles, three needles, bipins, nanocrystals, nanodots, quantum dots, nanoparticles, etc. Nanostructure can be, for example, substantially crystalline, substantially monocrystalline, polycrystalline, amorphous or its combination. In some embodiments, each of the three dimensions of the nanostructure has a size less than about 500nm, less than about 200nm, less than about 100nm, less than about 50nm, less than about 20nm or less than about 10nm.

[0148] When used for nanostructures, the term "heterostructure" refers to a nanostructure characterized by at least two different and / or distinguishable material types. Typically, one region of the nanostructure contains a first material type, while a second region of the nanostructure contains a second material type. In certain embodiments, the nanostructure comprises a core of a first material and a shell of at least one second (or third, etc.) material, wherein the different material types are radially distributed, for example, around the long axis of a nanowire, the long axis of an arm of a branched nanowire, or the center of a nanocrystal. The shell may, but need not, completely cover an adjacent material that is considered a shell or a nanostructure that is considered a heterostructure; for example, a nanocrystal characterized by a core of one material being covered by an island of a second material is a heterostructure. In other embodiments, different material types are distributed at different locations within the nanostructure; for example, along the major axis (long axis) of a nanowire or along the long axis of an arm of a branched nanowire. Different regions within a heterostructure may contain completely different materials, or different regions may contain a matrix material (e.g., silicon) with different dopants or different concentrations of the same dopant.

[0149] As used herein, the "diameter" of a nanostructure refers to the diameter of a cross-section perpendicular to a first axis of the nanostructure, where the difference in length of the first axis relative to a second and third axis (the second and third axes being the two axes whose lengths are closest to being equal to each other) is the largest. The first axis is not necessarily the longest axis of the nanostructure; for example, for a disc-shaped nanostructure, the cross-section will be a substantially circular cross-section perpendicular to the short longitudinal axis of the disc. If the cross-section is not circular, the diameter is the average of the major and minor axes of the cross-section. For elongated or high aspect ratio nanostructures, such as nanowires, the diameter is measured in a cross-section perpendicular to the longest axis of the nanowire. For spherical nanostructures, the diameter is measured from one side to the other through the center of the sphere.

[0150] When used for nanostructures, the term "crystalline" or "substantially crystalline" refers to the fact that the nanostructure generally exhibits long-range order in one or more dimensions of the structure. Those skilled in the art will understand that the term "long-range order" will depend on the absolute size of the particular nanostructure, since the ordering of a single crystal cannot extend beyond the boundaries of the crystal. In this case, "long-range order" will mean that it is substantially ordered at least in most dimensions of the nanostructure. In some cases, the nanostructure may be provided with an oxide or other coating, or may consist of a core and at least one shell. In these cases, it is understood that the oxide, shell or other coating may but need not exhibit such order (e.g., it may be amorphous, polycrystalline or other). In these cases, the phrase "crystalline", "substantially crystalline", "substantially single crystal" or "single crystal" refers to the central core of the nanostructure (excluding the coating or shell). The term "crystalline" or "substantially crystalline" used herein is intended to also include structures containing various defects, stacking dislocations, atomic substitutions, etc., as long as the structure exhibits long-range order (e.g., order exceeds at least about 80% of the length of at least one axis of the nanostructure or its core). In addition, it should be understood that the interface between the core and the exterior of the nanostructure or between the core and the adjacent shell or between the shell and the second adjacent shell may contain non-crystalline regions and may even be amorphous. This does not prevent the nanostructure from being crystalline or substantially crystalline as defined in the present invention.

[0151] The term "single crystalline" when applied to a nanostructure means that the nanostructure is substantially crystalline and consists essentially of a single crystal. When applied to a nanostructure comprising a core and one or more shells, "single crystalline" means that the core is substantially crystalline and consists essentially of a single crystal.

[0152] "Nanocrystal" is a substantially monocrystalline nanostructure.Therefore, nanocrystal has at least one size less than the region or characteristic size of about 500nm.In some embodiments, the nanocrystal has a size less than about 200nm, less than about 100nm, less than about 50nm, less than about 20nm or less than about 10nm.The term "nanocrystal" is intended to include a substantially monocrystalline nanostructure containing various defects, stacking dislocations, atomic substitutions, etc., and a substantially monocrystalline nanostructure without these defects, dislocations or substitutions.In the case of a nanocrystal heterostructure comprising a core and one or more shells, the core of the nanocrystal is typically substantially monocrystalline, but the shell does not need to be like this.In some embodiments, each of the three-dimensional dimensions of the nanocrystal has a size less than about 500nm, less than about 200nm, less than about 100nm, less than about 50nm, less than about 20nm or less than about 10nm.

[0153] The term "quantum dot" (or "dot") refers to a nanocrystal that exhibits quantum confinement or exciton confinement. Quantum dots can be substantially homogeneous in material properties, or in certain embodiments can be heterogeneous, for example comprising a core and at least one shell. The optical properties of quantum dots can be affected by their particle size, chemical composition, and / or surface composition, and can be determined by appropriate optical tests available in the art. The ability to customize nanocrystal size (e.g., in the range of about 1 nm to about 15 nm) enables light emission coverage across the spectrum to provide great diversity in color rendering.

[0154] A "ligand" is a molecule capable of interacting (whether weakly or strongly) with one or more faces of a nanostructure, for example through covalent, ionic, van der Waals or other molecular interactions with the nanostructure surface.

[0155] "Photoluminescence quantum yield" is the ratio of photons emitted to photons absorbed, for example, by a nanostructure or population of nanostructures. As is known in the art, quantum yield is typically determined by comparison methods using well-characterized standard samples with known quantum yield values.

[0156] "Peak emission wavelength" (PWL) is the wavelength where the radiation emission spectrum of the light source reaches its maximum.

[0157] As used herein, the term "shell" refers to the material deposited on the core or previously deposited shells with the same or different composition, and is produced by a single deposition of the shell material. The exact shell thickness depends on the input and conversion of the material and precursor, and can be reported in nanometers or monolayers. As used herein, "target shell thickness" refers to the expected shell thickness for calculating the required precursor amount. As used herein, "actual shell thickness" refers to the actual deposition amount of the shell material after synthesis, and can be measured by methods known in the art. For example, the actual shell thickness can be measured by comparing the particle diameter determined by the transmission electron microscope (TEM) image of the nanocrystal before and after the shell synthesis.

[0158] As used herein, the term "monolayer" is a unit of measure of shell thickness derived from the bulk crystal structure of the shell material as the closest distance between the relevant lattice planes. For example, for a cubic lattice structure, the thickness of one monolayer is determined as the distance between adjacent lattice planes in the

[111] direction. For example, one cubic ZnSe monolayer corresponds to 0.328 nm, and one cubic ZnS monolayer corresponds to 0.31 nm thickness. The monolayer thickness of an alloyed material can be determined from the alloy composition by Vegard's law.

[0159] As used herein, the term "full width at half maximum" (FWHM) is a measure of quantum dot size distribution. The emission spectrum of a quantum dot typically has the shape of a Gaussian curve. The width of the Gaussian curve is defined as the FWHM and gives an idea of ​​the particle size distribution. A smaller FWHM corresponds to a narrower quantum dot nanocrystal size distribution. The FWHM also depends on the emission wavelength maximum.

[0160] As used herein, the term "external quantum efficiency" (EQE) is the ratio of the number of photons emitted from a light emitting diode (LED) to the number of electrons passing through the device. EQE measures how efficiently an LED converts electrons into photons and allows them to escape. EQE can be measured using the following formula: EQE = [Injection efficiency] x [Solid-state quantum yield] x [Extraction efficiency]

[0161] in:

[0162] Injection efficiency = the fraction of electrons injected into the active region through the device;

[0163] Solid-state quantum yield = the fraction of all electron-hole recombination in the active region that are radioactive and thus generate photons; and

[0164] Extraction efficiency = the fraction of photons generated in the active region that escape from the device.

[0165] Unless expressly stated otherwise, the ranges listed herein include the endpoint values.

[0166] Various other terms are defined or otherwise described herein.

[0167] Preparation of nanostructures

[0168] Various colloidal synthesis methods for nanostructures are known in the art. These methods include techniques for controlling the growth of nanostructures, such as controlling the size and / or shape distribution of the resulting nanostructures.

[0169] In a typical colloidal synthesis, semiconductor nanostructures are produced by rapidly injecting a precursor that undergoes pyrolysis into a hot solution (e.g., a hot solvent and / or surfactant). The precursors can be injected simultaneously or sequentially. The precursors react rapidly to form a core. Nanostructure growth occurs by adding monomers to the core.

[0170] Surfactant molecules interact with the surface of the nanostructure. Under the growth temperature, the surfactant molecules adsorb and desorb quickly from the nanostructure surface to allow the nanostructure to add and / or remove atoms from the nanostructure while the nanostructure that suppresses growth gathers. Usually, the surfactant with the weak coordination of the nanostructure surface allows the fast growth of the nanostructure, while the surfactant with the stronger combination of the nanostructure surface causes the slower nanostructure growth. The surfactant can also interact with a kind of (or multiple) precursors to slow down the nanostructure growth.

[0171] Nanostructure growth in the presence of a single surfactant generally results in spherical nanostructures. However, using a mixture of two or more surfactants allows the growth to be controlled so that non-spherical nanostructures can be produced, for example, if the two (or more) surfactants are differentially adsorbed on different crystal faces of the growing nanostructure.

[0172] Therefore, many parameters are known to affect nanostructure growth and can be manipulated independently or in combination to control the size and / or shape distribution of the resulting nanostructures. These include, for example, temperature (nucleation and / or growth), precursor composition, time-dependent precursor concentration, the ratio of precursors to each other, surfactant composition, surfactant quantity, and the ratio of surfactants to each other and / or to precursors.

[0173] The synthesis of Group II-VI nanostructures has been described, for example, in U.S. Patent Nos. 6,225,198, 6,322,901, 6,207,229, 6,607,829, 7,060,243, 7,374,824, 6,861,155, 7,125,605, 7,566,476, 8,158,193, and 8,101,234, and U.S. Patent Application Publication Nos. 2011 / 0262752 and 2011 / 0263062.

[0174] Although, as described above, Group II-VI nanostructures (e.g., CdSe / CdS / ZnS core / shell quantum dots) can exhibit desirable luminescent behavior, issues such as toxicity of cadmium limit the applications in which such nanostructures can be used. Therefore, less toxic alternatives with favorable luminescent properties are highly desirable.

[0175] In some embodiments, the nanostructure does not contain cadmium. As used herein, the term "does not contain cadmium" refers to a nanostructure that contains less than 100 ppm (weight) of cadmium. The compliance definition of the Restriction of Hazardous Substances (RoHS) requires that the cadmium in a homogeneous precursor raw material must not exceed 0.01 weight % (100 ppm). The cadmium content in the cadmium-free nanostructure of the present invention is limited by the trace metal concentration in the precursor material. The trace metal (including cadmium) concentration in the precursor material for the cadmium-free nanostructure is measured by inductively coupled plasma mass spectrometry (ICP-MS) analysis and is at the parts per billion (ppb) level. In some embodiments, the "cadmium-free" nanostructure comprises less than about 50 ppm, less than about 20 ppm, less than about 10 ppm, or less than about 1 ppm of cadmium.

[0176] ZnSe 1-x Te x Preparation of nuclei

[0177] Using density functional theory (DFT) calculations, it is expected that the positioning of Te atoms at the center of the ZnSe core will result in a red shift in the observed emission spectrum while maintaining type I overlap between the electron and hole wave functions in the conduction band and the valence band. Type I overlap occurs in nanocrystals where the exciton-exciton interaction is attractive and therefore the interaction energy is negative. Piryatinski, A. et al., Nano Letters 7(1):108-115(2007). On the other hand, by spatially separating electrons and holes, the repulsive component of the interaction energy can be increased, which can reverse the sign of the interaction energy. In the case of strongly confined type II nanocrystals, this strategy results not only in overall exciton-exciton repulsion, but also in large interaction energy amplitudes, which can be generated due to very small separations between the interacting charges.

[0178] It is believed that the variation in the position and number of Te atoms throughout the quantum dot core will lead to peak broadening. Trioctylphosphine telluride is known to decompose into elemental Te, which is only slowly reduced to Te 2- See U.S. Patent No. 8,637,082. This reaction does not match the reaction between diethylzinc and trioctylphosphine selenide and results in low and poorly controlled incorporation of Te atoms into ZnSe. Improved ZnTe nanomaterials are obtained by using a strong reducing agent in combination with trioctylphosphine telluride to promote the incorporation of Te. 2- See Zhang, J. et al., J. Phys. Chem. C. 112(14):5454-5458 (2008), which describes the use of zinc carboxylates to prevent the formation of elemental zinc.

[0179] Conventional methods for preparing ZnSe cores include reducing trioctylphosphine telluride with superhydride in an oleylamine solution, which forms a purple solution. The purple solution is mixed with 1 equivalent of zinc carboxylate dissolved in trioctylphosphine, which results in the formation of a colorless milky mixture that still has a low enough viscosity for rapid injection. The milky mixture is co-injected with diethylzinc into trioctylphosphine selenide (at a level of 8 mole percent telluride). After core growth and washing, the cores are coated with a shell as described in U.S. Patent Application Publication No. 2017 / 066965, the entire text of which is incorporated herein by reference.

[0180] In some embodiments, the nanostructure comprises ZnSe 1-x Te x cores, where 0 < x < 1, 0 < x < 0.5, 0 < x < 0.25, 0 < x < 0.1, 0 < x < 0.05, 0 < x < 0.02, 0 < x < 0.01, 0.01 < x < 0.5, 0.01 < x < 0.25, 0.01 < x < 0.1, 0.01 < x < 0.05, 0.01 < x < 0.02, 0.02 < x < 0.5, 0.02 < x < 0.25, 0.02 < x < 0.1, 0.02 < x < 0.05, 0.05 < x < 0.5, 0.05 < x < 0.25, 0.05 < x < 0.1, 0.1 < x < 0.5, 0.1 < x < 0.25 or 0.5 < x < 0.25.

[0181] The ZnSe 1-x Te x core diameter can be controlled by varying the amount of precursor provided. The diameter of the ZnSe 1-x Te x cores can be determined using techniques known to those skilled in the art. In some embodiments, the diameter of the ZnSe 1-x Te x cores is determined using transmission electron microscopy (TEM).

[0182] In some embodiments, each ZnSe 1-x Te xThe diameter of the core is about 1.0 nm to about 7.0 nm, about 1.0 nm to about 6.0 nm, about 1.0 nm to about 5.0 nm, about 1.0 nm to about 4.0 nm, about 1.0 nm to about 3.0 nm, about 1.0 nm to about 2.0 nm, about 2.0 nm to about 7.0 nm, about 2.0 nm to about 6.0 nm, about 2.0 nm to about 5.0 nm, about 2.0 nm to about 4.0 nm, about 2.0 nm to about 3.0 nm, about 3.0 nm to about 7.0 nm, about 3.0 nm to about 6.0 nm, about 3.0 nm to about 5.0 nm, about 3.0 nm to about 4.0 nm, about 4.0 nm to about 7.0 nm, about 4.0 nm to about 6.0 nm, about 4.0 nm to about 5.0 nm, about 5.0 nm to about 7.0 nm, about 5.0 nm to about 6.0 nm, or about 6.0 nm to about 7.0 nm. In some embodiments, the ZnSe 1-x Te x The diameter of the core is about 3.0 nm to about 5.0 nm.

[0183] The present disclosure also provides a method for preparing ZnSe 1-x Te x A method for nanocrystals comprising:

[0184] (a) mixing a tellurium source, at least one ligand and a reducing agent to prepare a reaction mixture;

[0185] (b) contacting the reaction mixture obtained in (a) with a solution comprising at least one ligand, zinc fluoride and a selenium source; and

[0186] (c) contacting the reaction mixture obtained in (b) with a zinc source;

[0187] To provide ZnSe 1-x Te x Nanocrystals.

[0188] In some embodiments, the present invention provides a method for preparing ZnSe 1-x Te x A method for nanocrystals comprising:

[0189] (a) mixing a selenium source and at least one ligand to prepare a reaction mixture;

[0190] (b) contacting the reaction mixture obtained in (a) with a solution comprising a tellurium source, a reducing agent and a zinc carboxylate; and

[0191] (c) contacting the reaction mixture obtained in (b) with a zinc source;

[0192] To provide ZnSe 1-x Te x Nanocrystals.

[0193] In some embodiments, the present invention provides a method for preparing ZnSe 1-x Te x A method for nanocrystals comprising:

[0194] (a) mixing a selenium source and at least one ligand to prepare a reaction mixture;

[0195] (b) contacting the reaction mixture obtained in (a) with a solution comprising a tellurium source, a reducing agent and a zinc carboxylate; and

[0196] (c) contacting the reaction mixture obtained in (b) with a zinc source;

[0197] (d) contacting the reaction mixture of (c) with a zinc source and a selenium source;

[0198] To provide ZnSe 1-x Te x Nanocrystals.

[0199] In some embodiments, the selenium source is selected from trioctylphosphine selenide, tri(n-butyl)phosphine selenide, tri(sec-butyl)phosphine selenide, tri(tert-butyl)phosphine selenide, trimethylphosphine selenide, triphenylphosphine selenide, diphenylphosphine selenide, phenylphosphine selenide, cyclohexylphosphine selenide, octylselenol, dodecanol, phenylselenol, elemental selenium, hydrogen selenide, bis(trimethylsilyl)selenide and mixtures thereof. In some embodiments, the selenium source is trioctylphosphine selenide (TOPSe).

[0200] In some embodiments, the ZnSe 1-x Te x The core is synthesized in the presence of at least one nanostructure ligand. The ligand can, for example, enhance the miscibility of the nanostructure in a solvent or polymer (thereby allowing the nanostructure to be distributed in the entire composition so that the nanostructure does not gather together), increase the quantum yield of the nanostructure, and / or keep the nanostructure luminous (for example, when the nanostructure is incorporated into a matrix). In some embodiments, the ligand used for the core synthesis and for the shell synthesis is identical. In some embodiments, the ligand used for the core synthesis and for the shell synthesis is different. After the synthesis, any ligand on the nanostructure surface can be exchanged for different ligands with other desired properties. Examples of ligands are disclosed in U.S. Patent Application Publication Nos. 2005 / 0205849, 2008 / 0105855, 2008 / 0118755, 2009 / 0065764, 2010 / 0140551, 2013 / 0345458, 2014 / 0151600, 2014 / 0264189, and 2014 / 0001405.

[0201] In some embodiments, it is suitable for synthesizing nanostructure cores (comprising ZnSe1-x Te x In some embodiments, the ligand is a fatty acid selected from lauric acid, caproic acid, myristic acid, palmitic acid, stearic acid and oleic acid. In some embodiments, the ligand is an organic phosphine or organic phosphine oxide selected from trioctylphosphine oxide (TOPO), trioctylphosphine (TOP), diphenylphosphine (DPP), triphenylphosphine oxide and tributylphosphine oxide. In some embodiments, the ligand is an amine selected from dodecylamine, oleylamine, hexadecylamine and octadecylamine. In some embodiments, the ligand is trioctylphosphine (TOP). In some embodiments, the ligand is oleylamine.

[0202] In some embodiments, the core is prepared in the presence of a mixture of ligands. In some embodiments, the core is prepared in the presence of a mixture comprising 2, 3, 4, 5 or 6 different ligands. In some embodiments, the core is prepared in the presence of a mixture comprising 3 different ligands. In some embodiments, the mixture of ligands comprises oleylamine, diphenylphosphine and trioctylphosphine.

[0203] In some embodiments, the mixture of the selenium source and the ligand in (a) is heated to about 250°C to about 350°C, about 250°C to about 320°C, about 250°C to about 300°C, about 250°C to about 290°C, about 250°C to about 280°C, about 250°C to about 270°C, about 270°C to about 350°C, about 270°C to about 320°C, about 270°C to about 300°C, about 270°C to about 290°C. , about 270° C. to about 280° C., about 280° C. to about 350° C., about 280° C. to about 320° C., about 280° C. to about 300° C., about 280° C. to about 290° C., about 290° C. to about 350° C., about 290° C. to about 320° C., about 290° C. to about 300° C., about 300° C. to about 350° C., about 300° C. to about 320° C., or about 320° C. to about 350° C. In some embodiments, the mixing of the selenium source and the ligand in (a) is carried out at a reaction temperature of about 300° C.

[0204] In some embodiments, the reaction mixture after combining the selenium source and the ligand in (a) is maintained at an elevated temperature for about 2 to about 20 minutes, about 2 to about 15 minutes, about 2 to about 10 minutes, about 2 to about 8 minutes, about 2 to about 5 minutes, about 5 to about 20 minutes, about 5 to about 15 minutes, about 5 to about 10 minutes, about 5 to about 8 minutes, about 8 to about 20 minutes, about 8 to about 15 minutes, about 8 to about 10 minutes, about 10 to about 20 minutes, about 10 to about 15 minutes, or about 15 to about 20 minutes.

[0205] In some embodiments, the solution comprising the tellurium source, the reducing agent, and the zinc carboxylate in (b) is prepared separately. In some embodiments, the solution comprising the tellurium source, the reducing agent, and the zinc carboxylate in (b) is prepared in situ.

[0206] In some embodiments, the solution comprising a tellurium source, a reducing agent, and a zinc carboxylate in (b) is prepared separately. In some embodiments, the method for preparing a tellurium solution comprises:

[0207] (a) mixing a tellurium source and a ligand to prepare a reaction mixture;

[0208] (b) contacting the reaction mixture in (a) with a reducing agent; and

[0209] (c) contacting the reaction mixture of (b) with a zinc carboxylate;

[0210] To prepare a tellurium solution.

[0211] In some embodiments, the tellurium source is selected from trioctylphosphine telluride, tri(n-butyl)phosphine telluride, trimethylphosphine telluride, triphenylphosphine telluride, tricyclohexylphosphine telluride, elemental tellurium, hydrogen telluride, bis(trimethylsilyl) telluride, and mixtures thereof. In some embodiments, the tellurium source is trioctylphosphine telluride (TOPTe).

[0212] In some embodiments, the reducing agent is selected from diborane, sodium hydride, sodium borohydride, lithium borohydride, sodium cyanoborohydride, calcium hydride, lithium hydride, lithium aluminum hydride, diisobutylaluminum hydride, sodium triethylborohydride, and lithium triethylborohydride. In some embodiments, the reducing agent is lithium triethylborohydride.

[0213] In some embodiments, the zinc carboxylate is prepared by reacting a zinc salt with a carboxylic acid.

[0214] In some embodiments, the zinc salt is selected from zinc acetate, zinc fluoride, zinc chloride, zinc bromide, zinc iodide, zinc nitrate, zinc trifluoromethanesulfonate, zinc toluenesulfonate, zinc methanesulfonate, zinc oxide, zinc sulfate, zinc acetylacetonate, zinc toluene-3,4-dithiol, zinc p-toluenesulfonate, zinc diethyldithiocarbamate, zinc dibenzyldithiocarbamate, and mixtures thereof.

[0215] In some embodiments, the carboxylic acid is selected from acetic acid, propionic acid, butyric acid, valeric acid, hexanoic acid, heptanoic acid, octanoic acid, decanoic acid, undecanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, acrylic acid, methacrylic acid, but-2-enoic acid, but-3-enoic acid, pent-2-enoic acid, pent-4-enoic acid, hex-2-enoic acid, hex-3-enoic acid, hex-4-enoic acid, hex-5-enoic acid, hept-6-enoic acid, oct-2-enoic acid, dec-2-enoic acid, undec-10-enoic acid, dodec-5-enoic acid, oleic acid, gadoleic acid, erucic acid, linoleic acid, α-linolenic acid, octadecatrienoic acid, eicosadienoic acid, eicosatrienoic acid, arachidonic acid, octadecatrienoic acid, benzoic acid, p-toluic acid, o-toluic acid, m-toluic acid, hydrocinnamic acid, cyclohexaneic acid, cinnamic acid, p-toluenesulfonic acid, and mixtures thereof.

[0216] In some embodiments, the zinc carboxylate is zinc stearate or zinc oleate. In some embodiments, the zinc carboxylate is zinc oleate.

[0217] In some embodiments, the temperature is about 250°C to about 350°C, about 250°C to about 320°C, about 250°C to about 300°C, about 250°C to about 290°C, about 250°C to about 280°C, about 250°C to about 270°C, about 270°C to about 350°C, about 270°C to about 320°C, about 270°C to about 300°C, about 270°C to about 290°C, about 270°C to about 280°C, about 280°C to about The solution comprising the tellurium source, the reducing agent, and the zinc carboxylate in (b) is added to the reaction mixture at a reaction temperature of about 350° C., about 280° C. to about 320° C., about 280° C. to about 300° C., about 280° C. to about 290° C., about 290° C. to about 350° C., about 290° C. to about 320° C., about 290° C. to about 300° C., about 300° C. to about 350° C., about 300° C. to about 320° C., or about 320° C. to about 350° C. In some embodiments, the solution comprising the tellurium source, the reducing agent, and the zinc carboxylate in (b) is added to the reaction mixture at a reaction temperature of about 300° C.

[0218] In some embodiments, after adding the solution comprising a tellurium source, a reducing agent, and a zinc carboxylate in (b), the reaction mixture is contacted with a zinc source in (c).

[0219] In some embodiments, the zinc source in (c) is added to the reaction mixture about 1 second to about 5 minutes, about 1 second to about 3 minutes, about 1 second to about 1 minute, about 1 second to about 30 seconds, about 1 second to about 10 seconds, about 1 second to about 5 seconds, about 5 seconds to about 5 minutes, about 5 seconds to about 3 minutes, about 5 seconds to about 1 minute, about 5 seconds to about 30 seconds, about 5 seconds to about 10 seconds, about 10 seconds to about 5 minutes, about 10 seconds to about 3 minutes, about 10 seconds to about 1 minute, about 10 seconds to about 30 seconds, about 30 seconds to about 5 minutes, about 30 seconds to about 3 minutes, about 30 seconds to about 1 minute, about 1 minute to about 5 minutes, about 1 minute to about 3 minutes, or about 3 minutes to about 5 minutes after the solution comprising the tellurium source, the reducing agent, and the zinc carboxylate is added in (b). In some embodiments, the zinc source in (c) is added to the reaction mixture about 1 second to 5 seconds after the solution comprising the tellurium source, the reducing agent, and the zinc carboxylate is added in (b).

[0220] In some embodiments, the temperature is about 250°C to about 350°C, about 250°C to about 320°C, about 250°C to about 300°C, about 250°C to about 290°C, about 250°C to about 280°C, about 250°C to about 270°C, about 270°C to about 350°C, about 270°C to about 320°C, about 270°C to about 300°C, about 270°C to about 290°C, about 270°C to about 280°C, The zinc source is added to the reaction mixture in (c) at a reaction temperature of about 280° C. to about 350° C., about 280° C. to about 320° C., about 280° C. to about 300° C., about 280° C. to about 290° C., about 290° C. to about 350° C., about 290° C. to about 320° C., about 290° C. to about 300° C., about 300° C. to about 350° C., about 300° C. to about 320° C., or about 320° C. to about 350° C. In some embodiments, the zinc source in (c) is added to the reaction mixture at a reaction temperature of about 300° C.

[0221] In some embodiments, the zinc source in (c) is a dialkyl zinc compound. In some embodiments, the zinc source is diethyl zinc, dimethyl zinc, diphenyl zinc, zinc acetate, zinc acetylacetonate, zinc iodide, zinc bromide, zinc chloride, zinc fluoride, zinc carbonate, zinc cyanide, zinc nitrate, zinc oxide, zinc peroxide, zinc perchlorate or zinc sulfate. In some embodiments, the zinc source is diethyl zinc or dimethyl zinc. In some embodiments, the zinc source is diethyl zinc.

[0222] In some embodiments, the molar percentage of the tellurium source to the zinc source is from about 1% to about 20%, from about 1% to about 15%, from about 1% to about 10%, from about 1% to about 8%, from about 1% to about 6%, from about 1% to about 4%, from about 1% to about 2%, from about 2% to about 20%, from about 2% to about 15%, from about 2% to about 10%, from about 2% to about 8%, from about 2% to about 6%, from about 2% to about 4%, from about 4% to about 20%, from about 4% to about 15%, from about 4% to about 10%, from about 4% to about 8%, from about 4% to about 6%, from about 6% to about 20%, from about 6% to about 15%, from about 6% to about 10%, from about 6% to about 8%, from about 8% to about 20%, from about 8% to about 15%, from about 8% to about 10%, from about 10% to about 20%, from about 10% to about 15%, or from about 15% to about 20%. In some embodiments, the molar ratio of the tellurium source to the zinc source is about 6% to about 10%. In some embodiments, the molar ratio of the tellurium source to the zinc source is about 8%.

[0223] In some embodiments, after adding the zinc source in (c), the reaction mixture is contacted with a zinc source and a selenium source. In some embodiments, in (d), the temperature is from about 250°C to about 350°C, from about 250°C to about 320°C, from about 250°C to about 300°C, from about 250°C to about 290°C, from about 250°C to about 280°C, from about 250°C to about 270°C, from about 270°C to about 350°C, from about 270°C to about 320°C, from about 270°C to about 300°C, from about 270°C to about 290°C, from about 270°C to about 280°C In some embodiments, the zinc source and the selenium source are added to the reaction mixture at a reaction temperature of about 0° C., about 280° C. to about 350° C., about 280° C. to about 320° C., about 280° C. to about 300° C., about 280° C. to about 290° C., about 290° C. to about 350° C., about 290° C. to about 320° C., about 290° C. to about 300° C., about 300° C. to about 350° C., about 300° C. to about 320° C., or about 320° C. to about 350° C. In some embodiments, the zinc source and the selenium source are added to the reaction mixture at a reaction temperature of about 280° C. in (d).

[0224] In some embodiments, the time for adding the zinc source and the selenium source in (d) is from about 2 to about 120 minutes, from about 2 to about 60 minutes, from about 2 to about 30 minutes, from about 2 to about 20 minutes, from about 2 to about 15 minutes, from about 2 to about 10 minutes, from about 2 to about 8 minutes, from about 2 to about 5 minutes, from about 5 to about 120 minutes, from about 5 to about 60 minutes, from about 5 to about 30 minutes, from about 5 to about 20 minutes, from about 5 to about 15 minutes, from about 5 to about 10 minutes, from about 5 to about 8 minutes, from about 8 to about 120 minutes, from about 8 to about 60 minutes, from about 8 to about 30 minutes. In some embodiments, the zinc source and the selenium source are added for a period of about 20 minutes to about 30 minutes. In some embodiments, the zinc source and the selenium source are added for a period of about 20 minutes to about 30 minutes.

[0225] In some embodiments, after adding the zinc source and the selenium source in (d), the reaction mixture is maintained at an elevated temperature for about 2 to about 20 minutes, about 2 to about 15 minutes, about 2 to about 10 minutes, about 2 to about 8 minutes, about 2 to about 5 minutes, about 5 to about 20 minutes, about 5 to about 15 minutes, about 5 to about 10 minutes, about 5 to about 8 minutes, about 8 to about 20 minutes, about 8 to about 15 minutes, about 8 to about 10 minutes, about 10 to about 20 minutes, about 10 to about 15 minutes, or about 15 to about 20 minutes. In some embodiments, after adding the zinc source and the selenium source in (d), the reaction mixture is maintained at an elevated temperature for about 2 to about 10 minutes.

[0226] In order to prevent ZnSe 1-x Te x The core is precipitated as additional precursors are added, and additional ligands may be added during the growth phase. If too much ligand is added during the initial nucleation phase, the concentrations of the zinc, selenium, and tellurium sources will be too low and will prevent efficient nucleation. Therefore, ligands are added slowly throughout the growth phase. In some embodiments, the additional ligand is oleylamine.

[0227] In ZnSe 1-x Te x After the core reaches the desired thickness and diameter, it can be cooled. 1-x Te x The core is cooled to room temperature. In some embodiments, an organic solvent is added to dilute the ZnSe 1-x Te xNuclear reaction mixture.

[0228] In some embodiments, the organic solvent is hexane, pentane, toluene, benzene, ether, acetone, ethyl acetate, dichloromethane (methylene chloride), chloroform, dimethylformamide or N-methylpyrrolidone. In some embodiments, the organic solvent is toluene.

[0229] In some embodiments, separation of ZnSe 1-x Te x In some embodiments, ZnSe is precipitated from a solvent. 1-x Te x To separate ZnSe 1-x Te x In some embodiments, ZnSe is isolated by precipitation with ethanol. 1-x Te x nuclear.

[0230] ZnSe prepared using the method described herein 1-x Te x The size distribution of the core can be relatively narrow. In some embodiments, the full width at half maximum of the photoluminescence spectrum of the population or core / shell nanostructure prepared using the methods described herein is about 10nm to about 30nm, about 10nm to about 25nm, about 10nm to about 20nm, about 10nm to about 22nm, about 10nm to about 15nm, about 15nm to about 30nm, about 15nm to about 25nm, about 15nm to about 22nm, about 15nm to about 20nm, about 20nm to about 30nm, about 20nm to about 25nm, about 20nm to about 22nm, about 22nm to about 30nm, about 22nm to about 25nm, or about 25nm to about 30nm. In some embodiments, the population or ZnSe prepared using the methods described herein is 1-x Te x The full width at half maximum of the photoluminescence spectrum of the core is from about 15 nm to about 22 nm.

[0231] Shell preparation

[0232] In some embodiments, the nanostructures of the present invention comprise a core and at least one shell. In some embodiments, the nanostructures of the present invention comprise a core and at least two shells. The shells can, for example, increase the quantum yield and / or stability of the nanostructure. In some embodiments, the core and the shell comprise different materials. In some embodiments, the nanostructure comprises shells of different shell materials.

[0233] In some embodiments, a shell comprising a mixture of Group II and Group VI elements is deposited on a core or core / shell structure. In some embodiments, the deposited shell is a mixture of at least two of a zinc source, a selenium source, a sulfur source, and a tellurium source. In some embodiments, the deposited shell is a mixture of two of a zinc source, a selenium source, a sulfur source, and a tellurium source. In some embodiments, the deposited shell is a mixture of three of a zinc source, a selenium source, a sulfur source, and a tellurium source. In some embodiments, the shell comprises zinc and sulfur; zinc and selenium; zinc, sulfur, and selenium; zinc and tellurium; zinc, tellurium, and sulfur; or zinc, tellurium, and selenium.

[0234] In some embodiments, the shell comprises more than one monolayer of shell material. The number of monolayers is an average of all nanostructures; thus, the number of monolayers in a shell may be a fraction. In some embodiments, the number of monolayers in the shell is from about 0.25 to about 10, from about 0.25 to about 8, from about 0.25 to about 7, from about 0.25 to about 6, from about 0.25 to about 5, from about 0.25 to about 4, from about 0.25 to about 3, from about 0.25 to about 2, from about 2 to about 10, from about 2 to about 8, from about 2 to about 7, from about 2 to about 6, from about 2 to about 5, from about 2 to about 4, from about 2 to about 3, from about 3 to about 10, from about 3 to about 8, from about 3 to about 7, from about 3 to about 6, from about 3 to about 5, from about 3 to about 4, from about 4 to about 10, from about 4 to about 8, from about 4 to about 7, from about 4 to about 6, from about 4 to about 5, from about 5 to about 10, from about 5 to about 8, from about 5 to about 7, from about 5 to about 6, from about 6 to about 10, from about 6 to about 8, from about 6 to about 7, from about 7 to about 10, from about 7 to about 8, or from about 8 to about 10. In some embodiments, the shell comprises from about 3 to about 6 monolayers.

[0235] The thickness of the shell can be controlled by varying the amount of precursor provided. For a given shell thickness, at least one of the precursors is optionally provided in an amount such that when the growth reaction is substantially complete, a shell of predetermined thickness is obtained. If more than one different precursor is provided, the amount of each precursor can be limited, or one of the precursors can be provided in a limited amount while the other precursors are provided in excess.

[0236] The thickness of each shell can be determined using techniques known to those skilled in the art. In some embodiments, the thickness of each shell is determined by comparing the average diameter of the nanostructures before and after adding each shell. In some embodiments, the average diameter of the nanostructures before and after adding each shell is determined by transmission electron microscopy (TEM). In some embodiments, the thickness of each shell is from about 0.05nm to about 3.5nm, from about 0.05nm to about 2nm, from about 0.05nm to about 0.9nm, from about 0.05nm to about 0.7nm, from about 0.05nm to about 0.5nm, from about 0.05nm to about 0.3nm, from about 0.05nm to about 0.1nm, from about 0.1nm to about 3.5nm, from about 0.1nm to about 2nm, from about 0.1nm to about 0.9nm, from about 0.1nm to about 0.7nm, from about 0.1nm to about 0.5nm, from about 0.1nm to about 0.3nm , about 0.3nm to about 3.5nm, about 0.3nm to about 2nm, about 0.3nm to about 0.9nm, about 0.3nm to about 0.7nm, about 0.3nm to about 0.5nm, about 0.5nm to about 3.5nm, about 0.5nm to about 2nm, about 0.5nm to about 0.9nm, about 0.5nm to about 0.7nm, about 0.7nm to about 3.5nm, about 0.7nm to about 2nm, about 0.7nm to about 0.9nm, about 0.9nm to about 3.5nm, about 0.9nm to about 2nm, or about 2nm to about 3.5nm.

[0237] In some embodiments, each shell is synthesized in the presence of at least one nanostructure ligand. The ligand can, for example, enhance the miscibility of the nanostructure in a solvent or polymer (allowing the nanostructure to be distributed throughout the composition so that the nanostructure will not gather together), increase the quantum yield of the nanostructure and / or keep the nanostructure luminous (for example, when the nanostructure is incorporated into a matrix). In some embodiments, the ligand used for nucleosynthesis and for shell synthesis is the same. In some embodiments, the ligand used for nucleosynthesis and for shell synthesis is different. After synthesis, any ligand on the nanostructure surface can be exchanged for different ligands with other desired properties. The example of ligand is disclosed in U.S. Patent Nos. 7,572,395, 8,143,703, 8,425,803, 8,563,133, 8,916,064, 9,005,480, 9,139,770 and 9,169,435 and U.S. Patent Application Publication No. 2008 / 0118755.

[0238] Suitable ligands for shell synthesis are known to those skilled in the art. In some embodiments, the ligand is a fatty acid selected from lauric acid, caproic acid, caprylic acid, myristic acid, palmitic acid, stearic acid and oleic acid. In some embodiments, the ligand is an organic phosphine or organic phosphine oxide selected from trioctylphosphine oxide (TOPO), trioctylphosphine (TOP), diphenylphosphine (DPP), triphenylphosphine oxide and tributylphosphine oxide. In some embodiments, the ligand is an amine selected from dodecylamine, oleylamine, hexadecylamine, dioctylamine and octadecylamine. In some embodiments, the ligand is trioctylphosphine oxide, trioctylphosphine or lauric acid.

[0239] In some embodiments, each shell is prepared in the presence of a mixture of ligands. In some embodiments, each shell is prepared in the presence of a mixture comprising 2, 3, 4, 5, or 6 different ligands. In some embodiments, each shell is prepared in the presence of a mixture comprising 3 different ligands. In some embodiments, the mixture of ligands comprises tributylphosphine oxide, trioctylphosphine, and lauric acid.

[0240] In some embodiments, each shell is prepared in the presence of a solvent. In some embodiments, the solvent is selected from 1-octadecene, 1-hexadecene, 1-eicosene, eicosane, octadecane, hexadecane, tetradecane, squalene, squalane, trioctylphosphine oxide, and dioctyl ether.

[0241] In some embodiments, the core or core / shell and shell precursors are heated at about 20°C to about 310°C, about 20°C to about 280°C, about 20°C to about 250°C, about 20°C to about 200°C, about 20°C to about 150°C, about 20°C to about 100°C, about 20°C to about 50°C, about 50°C to about 310°C, about 50°C to about 280°C, about 50°C to about 250°C, about 50°C to about 200°C, about 50°C to about 150°C, about 50°C to about 100°C, about 10 ... The mixture is mixed at a temperature of about 100°C to about 280°C, about 100°C to about 250°C, about 100°C to about 200°C, about 100°C to about 150°C, about 150°C to about 310°C, about 150°C to about 280°C, about 150°C to about 250°C, about 150°C to about 200°C, about 200°C to about 310°C, about 200°C to about 280°C, about 200°C to about 250°C, about 250°C to about 310°C, about 250°C to about 280°C, or about 280°C to about 310°C.

[0242] In some embodiments, after mixing the core or core / shell and shell precursors, the temperature of the reaction mixture is increased to an elevated temperature of about 200°C to about 310°C, about 200°C to about 280°C, about 200°C to about 250°C, about 200°C to about 220°C, about 220°C to about 310°C, about 220°C to about 280°C, about 220°C to about 250°C, about 250°C to about 310°C, about 250°C to about 280°C, or about 280°C to about 310°C.

[0243] In some embodiments, the time after mixing the core or core / shell and the shell precursor, the temperature reaches the elevated temperature is from about 2 to about 240 minutes, about 2 to about 200 minutes, about 2 to about 100 minutes, about 2 to about 60 minutes, about 2 to about 40 minutes, about 5 to about 240 minutes, about 5 to about 200 minutes, about 5 to about 100 minutes, about 5 to about 60 minutes, about 5 to about 40 minutes, about 10 to about 240 minutes, about 10 to about 200 minutes, about 10 to about 100 minutes, about 10 to about 60 minutes, about 10 to about 40 minutes, about 40 to about 240 minutes, about 40 to about 200 minutes, about 40 to about 100 minutes, about 40 to about 60 minutes, about 60 to about 240 minutes, about 60 to about 200 minutes, about 60 to about 100 minutes, about 100 to about 240 minutes, about 100 to about 200 minutes, or about 200 to about 240 minutes.

[0244] In some embodiments, after mixing the core or core / shell and the shell precursor, the temperature of the reaction mixture is maintained at an elevated temperature for 2 to about 240 minutes, about 2 to about 200 minutes, about 2 to about 100 minutes, about 2 to about 60 minutes, about 2 to about 40 minutes, about 5 to about 240 minutes, about 5 to about 200 minutes, about 5 to about 100 minutes, about 5 to about 60 minutes, about 5 to about 40 minutes, about 10 to about 240 minutes, about 10 to about 200 minutes, about 10 to about 100 minutes, about 10 to about 60 minutes, about 10 to about 40 minutes, about 40 to about 240 minutes, about 40 to about 200 minutes, about 40 to about 100 minutes, about 40 to about 60 minutes, about 60 to about 240 minutes, about 60 to about 200 minutes, about 60 to about 100 minutes, about 100 to about 240 minutes, about 100 to about 200 minutes, or about 200 to about 240 minutes.

[0245] In some embodiments, additional shells are prepared by further adding shell material precursors that are added to the reaction mixture and then maintained at an elevated temperature. Typically, additional shell precursors are provided after the reaction of the previous shell is substantially complete (e.g., when at least one of the previous precursors is exhausted or removed from the reaction, or when no additional growth is detected). Further addition of precursors produces additional shells.

[0246] In some embodiments, the nanostructure is cooled prior to adding additional shell material precursor to provide a further shell. In some embodiments, the nanostructure is maintained at an elevated temperature prior to adding shell material precursor to provide a further shell.

[0247] After sufficient shell layers have been added to bring the nanostructure to the desired thickness and diameter, the nanostructure can be cooled. In some embodiments, the core / shell nanostructure is cooled to room temperature. In some embodiments, an organic solvent is added to dilute the reaction mixture containing the core / shell nanostructure.

[0248] In some embodiments, the organic solvent used to dilute the reaction mixture is ethanol, hexane, pentane, toluene, benzene, ether, acetone, ethyl acetate, dichloromethane (methylene chloride), chloroform, dimethylformamide or N-methylpyrrolidone. In some embodiments, the organic solvent is toluene.

[0249] In some embodiments, the core / shell nanostructures are isolated. In some embodiments, the core / shell nanostructures are isolated by precipitation using an organic solvent. In some embodiments, the core / shell nanostructures are isolated by flocculation with ethanol.

[0250] The number of monolayers will determine the size of the core / shell nanostructure. The size of the core / shell nanostructure can be determined using techniques known to those skilled in the art. In some embodiments, the size of the core / shell nanostructure is determined using TEM. In some embodiments, the core / shell nanostructures have an average diameter of about 1 nm to about 15 nm, about 1 nm to about 10 nm, about 1 nm to about 9 nm, about 1 nm to about 8 nm, about 1 nm to about 7 nm, about 1 nm to about 6 nm, about 1 nm to about 5 nm, about 5 nm to about 15 nm, about 5 nm to about 10 nm, about 5 nm to about 9 nm, about 5 nm to about 8 nm, about 5 nm to about 7 nm, about 5 nm to about 6 nm, about 6 nm to about 15 nm, about 6 nm to about 10 nm, about 6 nm to about 9 nm, about 6 nm to about 8 nm, about 6 nm to about 7 nm, about 7 nm to about 15 nm, about 7 nm to about 10 nm, about 7 nm to about 9 nm, about 7 nm to about 8 nm, about 8 nm to about 15 nm, about 8 nm to about 10 nm, about 8 nm to about 9 nm, about 9 nm to about 15 nm, about 9 nm to about 10 nm, or about 10 nm to about 15 nm.

[0251] In some embodiments, the core / shell nanostructure is subjected to an acid etching step prior to depositing the additional shell.

[0252] Preparation of ZnSe shell

[0253] In some embodiments, the shell deposited on the core or core / shell nanostructure is a ZnSe shell.

[0254] In some embodiments, the shell precursor contacted with the core or core / shell nanostructure to prepare the ZnSe shell comprises a zinc source and a selenium source.

[0255] In some embodiments, the zinc source is a dialkyl zinc compound. In some embodiments, the zinc source is a zinc carboxylate. In some embodiments, the zinc source is diethyl zinc, dimethyl zinc, zinc acetate, zinc acetylacetonate, zinc iodide, zinc bromide, zinc chloride, zinc fluoride, zinc carbonate, zinc cyanide, zinc nitrate, zinc dioleate, zinc oxide, zinc peroxide, zinc perchlorate, zinc sulfate, zinc hexanoate, zinc octoate, zinc laurate, zinc myristate, zinc palmitate, zinc stearate, zinc dithiocarbamate or its mixture. In some embodiments, the zinc source is zinc oleate, zinc hexanoate, zinc octoate, zinc laurate, zinc myristate, zinc palmitate, zinc stearate, zinc dithiocarbamate or its mixture. In some embodiments, the zinc source is zinc dioleate.

[0256] In some embodiments, the selenium source is an alkyl-substituted selenourea. In some embodiments, the selenium source is phosphine selenide. In some embodiments, the selenium source is selected from trioctylphosphine selenide, tri (n-butyl) phosphine selenide, tri (sec-butyl) phosphine selenide, tri (tert-butyl) phosphine selenide, trimethylphosphine selenide, triphenylphosphine selenide, diphenylphosphine selenide, phenylphosphine selenide, tricyclohexylphosphine selenide, cyclohexylphosphine selenide, 1-octylselenol, 1-dodecanol, phenylselenol, elemental selenium, hydrogen selenide, bis (trimethylsilyl) selenide, selenourea and mixtures thereof. In some embodiments, the selenium source is tri (n-butyl) phosphine selenide, tri (sec-butyl) phosphine selenide or tri (tert-butyl) phosphine selenide. In some embodiments, the selenium source is trioctylphosphine selenide.

[0257] In some embodiments, the molar ratio of the core to the zinc source used to prepare the ZnSe shell is from about 1:2 to about 1:1000, from about 1:2 to about 1:100, from about 1:2 to about 1:50, from about 1:2 to about 1:25, from about 1:2 to about 1:15, from about 1:2 to about 1:10, from about 1:2 to about 1:5, from about 1:5 to about 1:1000, from about 1:5 to about 1:100, from about 1:5 to about 1:50, from about 1:5 to about 1:25, from about 1:5 to about 1:15, from about 1:5 to about 1:10, from about 1:5 to about 1:1000, from about 1:5 to about 1:100, from about 1:5 to about 1:50, from about 1:5 to about 1:25, from about 1:5 to about 1:15, from about 1:5 to about 1:10, from about 1:10 to about 1:100. In some embodiments, the present invention relates to a polymerizable compound having a molecular weight of at least about 1:10 to about 1:100, about 1:10 to about 1:50, about 1:10 to about 1:25, about 1:10 to about 1:15, about 1:15 to about 1:1000, about 1:15 to about 1:100, about 1:15 to about 1:50, about 1:15 to about 1:25, about 1:25 to about 1:1000, about 1:25 to about 1:100, about 1:25 to about 1:50, about 1:50 to about 1:1000, about 1:50 to about 1:100, or about 1:100 to about 1:1000.

[0258] In some embodiments, the molar ratio of the core to the selenium source for making the ZnSe shell is from about 1:2 to about 1:1000, from about 1:2 to about 1:100, from about 1:2 to about 1:50, from about 1:2 to about 1:25, from about 1:2 to about 1:15, from about 1:2 to about 1:10, from about 1:2 to about 1:5, from about 1:5 to about 1:1000, from about 1:5 to about 1:100, from about 1:5 to about 1:50, from about 1:5 to about 1:25, from about 1:5 to about 1:15, from about 1:5 to about 1:10, from about 1:5 to about 1:100. In some embodiments, the present invention relates to a method for preparing an aqueous solution of at least one embodiment of the present invention. The aqueous solution may be selected from the group consisting of: about 1:10 to about 1:100, about 1:10 to about 1:50, about 1:10 to about 1:25, about 1:10 to about 1:15, about 1:15 to about 1:1000, about 1:15 to about 1:100, about 1:15 to about 1:50, about 1:15 to about 1:25, about 1:25 to about 1:1000, about 1:25 to about 1:100, about 1:25 to about 1:50, about 1:50 to about 1:1000, about 1:50 to about 1:100, or about 1:100 to about 1:1000.

[0259] In some embodiments, the number of monolayers in the ZnSe shell is about 0.25 to about 10, about 0.25 to about 8, about 0.25 to about 7, about 0.25 to about 6, about 0.25 to about 5, about 0.25 to about 4, about 0.25 to about 3, about 0.25 to about 2, about 2 to about 10, about 2 to about 8, about 2 to about 7, about 2 to about 6, about 2 to about 5, about 2 to about 4, about 2 to about 3, about 3 to about 10, about 3 to about 8, about 3 to about 7, about 3 to about 6, about 3 to about 5, about 3 to about 4, about 4 to about 10, about 4 to about 8, about 4 to about 7, about 4 to about 6, about 4 to about 5, about 5 to about 10, about 5 to about 8, about 5 to about 7, about 5 to about 6, about 6 to about 10, about 6 to about 8, about 6 to about 7, about 7 to about 10, about 7 to about 8, or about 8 to 10. In some embodiments, the ZnSe shell comprises 2 to 8 monolayers. In some embodiments, the ZnSe shell comprises 4 to 6 monolayers.

[0260] In some embodiments, the thickness of the ZnSe monolayer is about 0.328 nm.

[0261] In some embodiments, the thickness of the ZnSe shell is from about 0.08 nm to about 3.5 nm, from about 0.08 nm to about 2 nm, from about 0.08 nm to about 0.9 nm, from about 0.08 nm to about 0.7 nm, from about 0.08 nm to about 0.5 nm, from about 0.08 nm to about 0.2 nm, from about 0.2 nm to about 3.5 nm, from about 0.2 nm to about 2 nm, from about 0.2 nm to about 0.9 nm, from about 0.2 nm to about 0.7 nm, from about 0.2 nm to about 0.5 nm, from about 0.5 nm to about 3.5 nm, from about 0.5 nm to about 2 nm, from about 0.5 nm to about 0.9 nm, from about 0.5 nm to about 0.7 nm, from about 0.7 nm to about 3.5 nm, from about 0.7 nm to about 2 nm, from about 0.7 nm to about 0.9 nm, from about 0.9 nm to about 3.5 nm, from about 0.9 nm to about 2 nm, or from about 2 nm to about 3.5 nm.

[0262] Preparation of ZnS shell

[0263] In some embodiments, the shell deposited onto the core or core / shell nanostructure is a ZnS shell.

[0264] In some embodiments, the shell precursor contacted with the core or core / shell nanostructure to prepare the ZnS shell comprises a zinc source and a sulfur source.

[0265] In some embodiments, the ZnS shell passivates defects at the particle surface, which leads to an increase in quantum yield and higher efficiency when used in devices such as LEDs and lasers. In addition, spectral impurities caused by defect states can be eliminated by passivation, which improves color saturation.

[0266] In some embodiments, the zinc source is a dialkyl zinc compound. In some embodiments, the zinc source is a zinc carboxylate. In some embodiments, the zinc source is diethyl zinc, dimethyl zinc, zinc acetate, zinc acetylacetonate, zinc iodide, zinc bromide, zinc chloride, zinc fluoride, zinc carbonate, zinc cyanide, zinc nitrate, zinc oleate, zinc oxide, zinc peroxide, zinc perchlorate, zinc sulfate, zinc hexanoate, zinc octoate, zinc laurate, zinc myristate, zinc palmitate, zinc stearate, zinc dithiocarbamate or its mixture. In some embodiments, the zinc source is zinc oleate, zinc hexanoate, zinc octoate, zinc laurate, zinc myristate, zinc palmitate, zinc stearate, zinc dithiocarbamate or its mixture. In some embodiments, the zinc source is zinc oleate.

[0267] In some embodiments, the sulfur source is selected from elemental sulfur, octyl mercaptan, dodecanethiol, octadecyl mercaptan, tributylphosphine sulfide, cyclohexyl isothiocyanate, α-toluene mercaptan, ethylene trithiocarbonate, allyl mercaptan, bis(trimethylsilyl) sulfide, trioctylphosphine sulfide and mixtures thereof. In some embodiments, the sulfur source is alkyl-substituted zinc dithiocarbamate. In some embodiments, the sulfur source is octyl mercaptan. In some embodiments, the sulfur source is tributylphosphine sulfide.

[0268] In some embodiments, the molar ratio of the core to the zinc source used to prepare the ZnS shell is from about 1:2 to about 1:1000, from about 1:2 to about 1:100, from about 1:2 to about 1:50, from about 1:2 to about 1:25, from about 1:2 to about 1:15, from about 1:2 to about 1:10, from about 1:2 to about 1:5, from about 1:5 to about 1:1000, from about 1:5 to about 1:100, from about 1:5 to about 1:50, from about 1:5 to about 1:25, from about 1:5 to about 1:15, from about 1:5 to about 1:10, from about 1:5 to about 1:1000. In some embodiments, the present invention relates to a method for preparing an aqueous solution of at least one embodiment of the present invention. The aqueous solution may be selected from the group consisting of: about 1:10 to about 1:100, about 1:10 to about 1:50, about 1:10 to about 1:25, about 1:10 to about 1:15, about 1:15 to about 1:1000, about 1:15 to about 1:100, about 1:15 to about 1:50, about 1:15 to about 1:25, about 1:25 to about 1:1000, about 1:25 to about 1:100, about 1:25 to about 1:50, about 1:50 to about 1:1000, about 1:50 to about 1:100, or about 1:100 to about 1:1000.

[0269] In some embodiments, the molar ratio of the core to the sulfur source used to prepare the ZnS shell is from about 1:2 to about 1:1000, from about 1:2 to about 1:100, from about 1:2 to about 1:50, from about 1:2 to about 1:25, from about 1:2 to about 1:15, from about 1:2 to about 1:10, from about 1:2 to about 1:5, from about 1:5 to about 1:1000, from about 1:5 to about 1:100, from about 1:5 to about 1:50, from about 1:5 to about 1:25, from about 1:5 to about 1:15, from about 1:5 to about 1:10, from about 1:5 to about 1:100. In some embodiments, the present invention relates to a method for preparing an aqueous solution of at least one embodiment of the present invention. The aqueous solution may be selected from the group consisting of: about 1:10 to about 1:100, about 1:10 to about 1:50, about 1:10 to about 1:25, about 1:10 to about 1:15, about 1:15 to about 1:1000, about 1:15 to about 1:100, about 1:15 to about 1:50, about 1:15 to about 1:25, about 1:25 to about 1:1000, about 1:25 to about 1:100, about 1:25 to about 1:50, about 1:50 to about 1:1000, about 1:50 to about 1:100, or about 1:100 to about 1:1000.

[0270] In some embodiments, the number of monolayers in the ZnS shell is about 0.25 to about 10, about 0.25 to about 8, about 0.25 to about 7, about 0.25 to about 6, about 0.25 to about 5, about 0.25 to about 4, about 0.25 to about 3, about 0.25 to about 2, about 2 to about 10, about 2 to about 8, about 2 to about 7, about 2 to about 6, about 2 to about 5, about 2 to about 4, about 2 to about 3, about 3 to about 10, about 3 to about 8, about 3 to about 7, about 3 to about 6, about 3 to about 5, about 3 to about 4, about 4 to about 10, about 4 to about 8, about 4 to about 7, about 4 to about 6, about 4 to about 5, about 5 to about 10, about 5 to about 8, about 5 to about 7, about 5 to about 6, about 6 to about 10, about 6 to about 8, about 6 to about 7, about 7 to about 10, about 7 to about 8, or about 8 to 10. In some embodiments, the ZnS shell comprises 2 to 8 monolayers. In some embodiments, the ZnS shell comprises 4 to about 6 monolayers.

[0271] In some embodiments, the ZnS monolayer has a thickness of about 0.31 nm.

[0272] In some embodiments, the thickness of the ZnS shell is from about 0.08 nm to about 3.5 nm, from about 0.08 nm to about 2 nm, from about 0.08 nm to about 0.9 nm, from about 0.08 nm to about 0.7 nm, from about 0.08 nm to about 0.5 nm, from about 0.08 nm to about 0.2 nm, from about 0.2 nm to about 3.5 nm, from about 0.2 nm to about 2 nm, from about 0.2 nm to about 0.9 nm, from about 0.2 nm to about 0.7 nm, from about 0.2 nm to about 0.5 nm, from about 0.5 nm to about 3.5 nm, from about 0.5 nm to about 2 nm, from about 0.5 nm to about 0.9 nm, from about 0.5 nm to about 0.7 nm, from about 0.7 nm to about 3.5 nm, from about 0.7 nm to about 2 nm, from about 0.7 nm to about 0.9 nm, from about 0.9 nm to about 3.5 nm, from about 0.9 nm to about 2 nm, or from about 2 nm to about 3.5 nm.

[0273] Core / shell nanostructures

[0274] In some embodiments, the core / shell nanostructure is ZnSe 1-x Te x / ZnSe / ZnS core / shell nanostructure. In some embodiments, the core / shell nanostructure is ZnSe 1-x Te x / ZnSe / ZnS core / shell quantum dots.

[0275] In some embodiments, the core / shell nanostructures exhibit high photoluminescence quantum yields. In some embodiments, the photoluminescence quantum yields of the core / shell nanostructures are about 30% to about 99%, about 30% to about 95%, about 30% to about 90%, about 30% to about 85%, about 30% to about 80%, about 30% to about 60%, about 30% to about 50%, about 30% to about 40%, about 40% to about 99%, about 40% to about 95%, about 40% to about 90%, about 40% to about 85%, about In some embodiments, the photoluminescence quantum yield of the core / shell nanostructure is about 50% to about 60%. In some embodiments, the photoluminescence quantum yield of the core / shell nanostructure is about 75% to about 90%.

[0276] In some embodiments, the emission maximum of the photoluminescence spectrum of the core / shell nanostructure is between about 300 nm and about 590 nm, between about 300 nm and about 550 nm, between about 300 nm and about 450 nm, between about 450 nm and about 590 nm, between about 450 nm and about 550 nm, or between about 550 nm and about 590 nm. In some embodiments, the emission maximum of the photoluminescence spectrum of the core / shell nanostructure is between about 420 nm and about 480 nm. In some embodiments, the emission maximum of the photoluminescence spectrum of the core / shell nanostructure is between about 440 nm and about 460 nm. In some embodiments, the emission maximum of the photoluminescence spectrum of the core / shell nanostructure is between about 450 nm and about 460 nm.

[0277] The size distribution of the core / shell nanostructures can be relatively narrow. In some embodiments, the full width at half maximum (FWHM) of the photoluminescence spectrum of a population of the core / shell nanostructures can be from about 10 nm to about 30 nm, from about 10 nm to about 25 nm, from about 10 nm to about 20 nm, from about 10 nm to about 22 nm, from about 10 nm to about 15 nm, from about 15 nm to about 30 nm, from about 15 nm to about 25 nm, from about 15 nm to about 22 nm, from about 15 nm to about 20 nm, from about 20 nm to about 30 nm, from about 20 nm to about 25 nm, from about 20 nm to about 22 nm, from about 22 nm to about 30 nm, from about 22 nm to about 25 nm, or from about 25 nm to about 30 nm. In some embodiments, the full width at half maximum (FWHM) of the photoluminescence spectrum of a population of core / shell nanostructures can be from about 15 nm to about 22 nm. In some embodiments, the full width at half maximum (FWHM) of the photoluminescence spectrum of a population of core / shell nanostructures can be from about 20 nm to about 30 nm.

[0278] Nanostructure film

[0279] In some embodiments, the core / shell nanostructures prepared by the methods described herein are incorporated into a nanostructure film. In some embodiments, the nanostructure film is incorporated into a quantum dot enhanced film (QDEF).

[0280] In some embodiments, the present disclosure provides a nanostructure film comprising at least one population of nanostructures, wherein the nanostructures comprise a core surrounded by at least one shell, wherein the core comprises ZnSe 1-x Te x , where 0 < x < 1, wherein the at least one shell comprises ZnS or ZnSe, and wherein the full width at half maximum (FWHM) of the nanostructures is from about 20 nm to about 30 nm.

[0281] In some embodiments, the nanostructures are quantum dots.

[0282] In some embodiments, the present disclosure provides a nanostructured film comprising:

[0283] (a) at least one nanostructure population, wherein the nanostructures comprise a core surrounded by at least one shell, wherein the core comprises ZnSe 1-x Te x , where 0 < x < 1, wherein the at least one shell comprises ZnS or ZnSe, and wherein the full width at half maximum (FWHM) of the nanostructures is from about 20 nm to about 30 nm; and

[0284] (b) at least one organic resin.

[0285] In some embodiments, the nanostructures are quantum dots.

[0286] In some embodiments, the core / shell nanostructures are embedded in a matrix. As used herein, the term "embedded" is used to mean that the nanostructures are encapsulated or surrounded by a matrix material that constitutes the major component of the matrix. In some embodiments, the nanostructures are uniformly distributed throughout the matrix material. In some embodiments, the nanostructures are distributed according to an application-specific uniform distribution function.

[0287] In some embodiments, the nanostructures can comprise a homogeneous population having sizes that emit in the blue visible wavelength spectrum, the green visible wavelength spectrum, or the red visible wavelength spectrum. In some embodiments, the nanostructures can comprise a first nanostructure population having sizes that emit in the blue visible wavelength spectrum, a second nanostructure population having sizes that emit in the green visible wavelength spectrum, and a third nanostructure population having sizes that emit in the red visible wavelength spectrum.

[0288] The host material can be any suitable host matrix material capable of accommodating the nanostructure. Suitable host materials can be chemically and optically compatible with the nanostructure and any surrounding packaging materials or layers for applying the nanostructure film to the device. Suitable host materials can comprise non-yellowing optical materials that are transparent to both primary and secondary light, thereby allowing primary and secondary light to be transmitted through the host material. Host materials can comprise polymers and organic and inorganic oxides. Suitable polymers for the host material can be any polymer known to those of ordinary skill that can be used for the purpose. The polymer can be substantially translucent or substantially transparent. The matrix material may include, but is not limited to, epoxies, acrylates, norbornene, polyethylene, poly(vinyl butyral):poly(vinyl acetate), polyurea, polyurethanes; siloxanes and siloxane derivatives, including but not limited to aminosiloxanes (AMS), polyphenylmethylsiloxanes, polyphenylalkylsiloxanes, polydiphenylsiloxanes, polydialkylsiloxanes, silsesquioxanes, fluorinated siloxanes, and vinyl and hydride substituted siloxanes; acrylic polymers and copolymers formed from monomers including but not limited to methyl methacrylate, butyl methacrylate, and lauryl methacrylate; styrene-based polymers such as polystyrene, aminopolystyrene (APS), and poly(acrylonitrile vinyl styrene) (AES); polymers crosslinked with difunctional monomers such as divinylbenzene; crosslinking agents suitable for crosslinking ligand materials, epoxides combined with ligand amines (e.g., APS or polyethyleneimine ligand amines) to form epoxy resins, and the like.

[0289] In some embodiments, the matrix material includes scattering beads, such as TiO2 beads, ZnS beads, or glass beads, which can improve the light conversion efficiency of the nanostructure film. In some embodiments, the matrix material can include light blocking elements.

[0290] In some embodiments, the matrix material can have low oxygen and moisture permeability, exhibit high light stability and chemical stability, exhibit a favorable refractive index, and adhere to the outer surface of the nanostructures, thereby providing an airtight seal to protect the nanostructures. In another embodiment, the matrix material can be cured by UV or thermal curing methods to facilitate roll-to-roll processing.

[0291] In some embodiments, the nanostructure film can be formed by mixing the nanostructures in a polymer (e.g., a photoresist) and casting the nanostructure-polymer mixture on a substrate, mixing the nanostructures with monomers and polymerizing them together, mixing the nanostructures in a sol-gel to form an oxide, or any other method known to those skilled in the art.

[0292] In some embodiments, the formation of the nanostructured film may include a film extrusion process. The film extrusion process may include forming a uniform mixture of a core-shell nanostructure (e.g., a nanostructure functionalized with a metal halide and / or a metal carboxylate) coated with a matrix material and a barrier layer, and introducing the uniform mixture into a top-mounted hopper that feeds an extruder. In some embodiments, the uniform mixture may be in the form of particles. The film extrusion process may further include extruding the nanostructured film from a slot die, and passing the extruded nanostructured film through a cooling roller. In some embodiments, the extruded nanostructured film may have a thickness of less than about 75 μm, for example, having a thickness in the range of about 70 μm to about 40 μm, about 65 μm to about 40 μm, about 60 μm to about 40 μm, or about 50 μm to about 40 μm. In some embodiments, the nanostructured film has a thickness of less than about 10 μm. In some embodiments, the formation of the nanostructured film may optionally include a secondary process after the film extrusion process. The secondary process may include processes such as coextrusion, thermoforming, vacuum forming, plasma treatment, molding and / or embossing to provide a texture to the top surface of the nanostructure film layer. A nanostructure film having a textured top surface may help improve, for example, the optical diffusion characteristics and / or the angular optical emission characteristics of the nanostructure film. Quantum dots on glass LED display devices

[0293] In some embodiments, the nanostructure film is incorporated into quantum dots on a glass LCD display device. The LCD display device may include a nanostructure film formed directly on a light guide plate (LGP) without an intermediate substrate or barrier layer. In some embodiments, the nanostructure film may be a thin film. In some embodiments, the nanostructure film may have a thickness of 500 μm or less, 100 μm or less, or 50 μm or less. In some embodiments, the nanostructure film is a thin film with a thickness of about 15 μm or less.

[0294] The LGP may include an optical cavity having one or more sides (including at least one top side) comprising glass. Glass provides excellent resistance to impurities including moisture and air. In addition, glass can be formed into a thin substrate while maintaining structural rigidity. Therefore, the LGP may be formed at least in part from a glass surface to provide a substrate with sufficient barrier and structural properties.

[0295] In some embodiments, the nanostructure film can be formed on the LGP. In some embodiments, the nanostructure film comprises a nanostructure population embedded in a matrix material (e.g., a resin). The nanostructure film can be formed on the LGP by any method known in the art, such as wet coating, coating, spin coating, or screen printing. After deposition, the resin of the nanostructure film can be cured. In some embodiments, the resin of one or more nanostructure films can be partially cured, further processed, and then finally cured. The nanostructure film can be deposited as a layer or as a separate plurality of layers, and the separate layers can include different characteristics. The width and height of the nanostructure film can be any desired size, depending on the size of the viewing panel of the display device. For example, in small display device embodiments such as watches and phones, the nanostructure film can have a relatively small surface area, or in large display device embodiments such as TVs and computer monitors, the nanostructure film can have a large surface area.

[0296] In some embodiments, by any method known in the art, such as vacuum deposition, vapor deposition, etc., an optically transparent substrate is formed on the nanostructure film. The optically transparent substrate can be configured to provide environmental sealing to the bottom layer and / or structure of the nanostructure film. In some embodiments, a light blocking element can be included in the optically transparent substrate. In some embodiments, the light blocking element can be included in the second polarizing filter, which can be positioned between the substrate and the nanostructure film. In some embodiments, the light blocking element can be a two-way color filter, such as it can reflect primary secondary light (such as, a combination of blue light, UV light or UV light and blue light) while transmitting secondary light. The light blocking element can include a specific UV light filter assembly to remove any unconverted UV light of red and green sub-pixels, and / or the UV light of blue sub-pixels.

[0297] On-chip and near-chip placement of quantum dots

[0298] In some embodiments, the nanostructures are incorporated into the display device by "on-chip" placement. As used herein, "on-chip" refers to placing the nanostructures in an LED cup. In some embodiments, the nanostructures are dissolved in a resin or fluid to fill the LED cup.

[0299] In some embodiments, the nanostructures are incorporated into a display device via "near sheet" placement. As used herein, "near sheet" refers to coating the top surface of an LED component with nanostructures such that the exiting light passes through the nanostructure film.

[0300] Display device with nanostructured color conversion layer

[0301] In some embodiments, the present invention provides a display device comprising:

[0302] (a) a display panel emitting a first light;

[0303] (b) a backlight unit configured to provide a first light to the display panel; and

[0304] (c) A color filter comprising at least one pixel region, the pixel region comprising a color conversion layer.

[0305] In some embodiments, the color filter includes at least 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 pixel areas. In some embodiments, when blue light is incident on the color filter, red light, white light, green light and / or blue light can be emitted through the pixel area, respectively. In some embodiments, the color filter is described in U.S. Patent Application Publication No. 2017 / 153366, the entire contents of which are incorporated herein by reference.

[0306] In some embodiments, each pixel region comprises a color conversion layer. In some embodiments, the color conversion layer comprises nanostructures described herein configured to convert incident light into light of a first color. In some embodiments, the color conversion layer comprises nanostructures described herein configured to convert incident light into blue light.

[0307] In some embodiments, the display device comprises 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 color conversion layers. In some embodiments, the display device comprises 1 color conversion layer comprising the nanostructures described herein. In some embodiments, the display device comprises 2 color conversion layers comprising the nanostructures described herein. In some embodiments, the display device comprises 3 color conversion layers comprising the nanostructures described herein. In some embodiments, the display device comprises 4 color conversion layers comprising the nanostructures described herein. In some embodiments, the display device comprises at least one red conversion layer, at least one green conversion layer and at least one blue conversion layer.

[0308] In some embodiments, the color conversion layer has a thickness of about 3 μm to about 10 μm, about 3 μm to about 8 μm, about 3 μm to about 6 μm, about 6 μm to about 10 μm, about 6 μm to about 8 μm, or about 8 μm to about 10 μm. In some embodiments, the color conversion layer has a thickness of about 3 μm to about 10 μm.

[0309] The nanostructure color conversion layer can be deposited by any suitable method known in the art, including but not limited to coating, spraying, solvent spraying, wet coating, adhesive coating, spin coating, tape coating, roller coating, flow coating, inkjet printing, photoresist patterning, drop casting, scraper coating, mist deposition or a combination thereof. In some embodiments, the nanostructure color conversion layer is deposited by photoresist patterning. In some embodiments, the nanostructure color conversion layer is deposited by inkjet printing.

[0310] Inkjet printing

[0311] The dispersion of nanostructure in organic solvent is used to form thin film, which is usually realized by coating technology (such as spin coating). However, these coating technologies are usually not suitable for forming thin film on a large area, and the mode of the deposited layer described in patterning is not provided, so the use is limited. Inkjet printing allows the accurate patterning of low-cost large-scale thin film to be placed. Inkjet printing also allows the accurate patterning of nanostructure layer, thereby allowing the pixels of printed display, and eliminating light patterning. Therefore, inkjet printing is very attractive for industrial applications, especially in display applications.

[0312] Solvents commonly used in inkjet printing are dipropylene glycol monomethyl ether acetate (DPMA), polyglycidyl methacrylate (PGMA), diethylene glycol monoethyl ether acetate (EDGAC) and propylene glycol methyl ether acetate (PGMEA). Volatile solvents are also often used in inkjet printing because they allow fast drying. Volatile solvents include ethanol, methanol, 1-propanol, 2-propanol, acetone, methyl ethyl ketone, methyl isobutyl ketone, ethyl acetate and tetrahydrofuran. Traditional nanostructures are usually not dissolved in these solvents. However, the hydrophilicity increased by the nanostructure as described herein increases the solubility in these solvents.

[0313] In some embodiments, the nanostructures for inkjet printing described herein are dispersed in a solvent selected from DPMA, PGMA, EDGAC, PGMEA, ethanol, methanol, 1-propanol, 2-propanol, acetone, methyl ethyl ketone, methyl isobutyl ketone, ethyl acetate, tetrahydrofuran, chloroform, chlorobenzene, cyclohexane, hexane, heptane, octane, hexadecane, undecane, decane, dodecane, xylene, toluene, benzene, octadecane, tetradecane, butyl ether, or a combination thereof. In some embodiments, the nanostructures comprising the poly(oxyalkylene) ligands for inkjet printing described herein are dispersed in a solvent selected from DPMA, PGMA, EDGAC, PGMEA, ethanol, methanol, 1-propanol, 2-propanol, acetone, methyl ethyl ketone, methyl isobutyl ketone, ethyl acetate, tetrahydrofuran, or a combination thereof.

[0314] For application by inkjet printing or microdispensing, the inkjet composition comprising the nanostructures should be dissolved in a suitable solvent. The solvent must be capable of dispersing the nanostructure composition and must not have any deleterious effects on the selected print head.

[0315] In some embodiments, the inkjet composition further comprises one or more additional components, such as surface active compounds, lubricants, wetting agents, dispersants, hydrophobic agents, binders, flow improvers, defoamers, deaerators, diluents, adjuvants, colorants, dyes, pigments, sensitizers, stabilizers and inhibitors.

[0316] In some embodiments, the nanostructure composition described herein comprises from about 0.01% to about 20% by weight of the inkjet composition. In some embodiments, the nanostructures as described herein comprise from about 0.01% to about 20%, from about 0.01% to about 15%, from about 0.01% to about 10%, from about 0.01% to about 5%, from about 0.01% to about 2%, from about 0.01% to about 1%, from about 0.01% to about 0.1%, from about 0.01% to about 0.05%, from about 0.05% to about 20%, from about 0.05% to about 15%, from about 0.05% to about 10%, from about 0.05% to about 5%, from about 0.05% to about 2%, from about 0.05% to about 1%, from about 0.05% to about 0.1%, from about 0.1% to about 20%, from about 0.1% to about 15%, from about 0.1 ... From about 1% to about 20%, from about 1% to about 15%, from about 1% to about 10%, from about 0.1% to about 5%, from about 0.1% to about 2%, from about 0.1% to about 1%, from about 0.5% to about 20%, from about 0.5% to about 15%, from about 0.5% to about 10%, from about 0.5% to about 5%, from about 0.5% to about 2%, from about 0.5% to about 1%, from about 1% to about 20%, from about 1% to about 15%, from about 1% to about 10%, from about 1% to about 5%, from about 1% to about 2%, from about 2% to about 20%, from about 2% to about 15%, from about 2% to about 10%, from about 2% to about 5%, from about 5% to about 20%, from about 5% to about 15%, from about 5% to about 10%, from about 10% to about 20%, from about 10% to about 15%, or from about 15% to about 20%.

[0317] In some embodiments, an inkjet composition comprising a nanostructure or nanostructure composition as described herein is used in the formulation of an electronic device. In some embodiments, an inkjet composition comprising a nanostructure or nanostructure composition as described herein is used in the formulation of an electronic device selected from the group consisting of a nanostructure film, a display device, a lighting device, a backlight unit, a color filter, a surface luminescent device, an electrode, a magnetic storage device, and a battery pack. In some embodiments, an inkjet composition comprising a nanostructure composition as described herein is used in the formulation of a light emitting device.

[0318] Nanostructured Moldings

[0319] In some embodiments, the nanostructured composition is used to form nanostructured moldings. In some embodiments, the nanostructured moldings are liquid crystal displays (LCDs) or light emitting diodes (LEDs). In some embodiments, the nanostructured composition is used to form an emissive layer of a lighting device. The lighting device can be used in a wide range of applications such as flexible electronic devices, touchscreens, displays, televisions, mobile phones, and any other high-resolution displays. In some embodiments, the lighting device is a light emitting diode or a liquid crystal display. In some embodiments, the lighting device is a quantum dot light emitting diode (QLED). An example of a QLED is disclosed in U.S. Patent Application No. 15 / 824,701, the entire content of which is incorporated herein by reference.

[0320] In some embodiments, the present disclosure provides a light emitting diode comprising:

[0321] (a) a first conductive layer;

[0322] (b) a second conductive layer; and

[0323] (c) an emissive layer located between the first conductive layer and the second conductive layer, wherein the emissive layer comprises at least one nanostructure population, wherein the nanostructure comprises a core surrounded by at least one shell, wherein the core comprises ZnSe 1-x Te x , where 0 < x < 1, wherein the at least one shell comprises ZnS or ZnSe, and wherein the full width at half maximum (FWHM) of the nanostructure is from about 20 nm to about 30 nm.

[0324] In some embodiments, the emissive layer is a nanostructured film.

[0325] In some embodiments, the light emitting diode comprises a first conductive layer, a second conductive layer, and an emissive layer, wherein the emissive layer is disposed between the first conductive layer and the second conductive layer. In some embodiments, the emissive layer is a thin film.

[0326] In some embodiments, the light emitting diode comprises additional layers between the first conductive layer and the second conductive layer, such as a hole injection layer, a hole transport layer, and an electron transport layer. In some embodiments, the hole injection layer, the hole transport layer, and the electron transport layer are thin films. In some embodiments, the layers are stacked on a substrate.

[0327] When a voltage is applied to the first conductive layer and the second conductive layer, holes injected into the first conductive layer move to the emission layer through the hole injection layer and / or the hole transport layer, and electrons injected from the second conductive layer move to the emission layer through the electron transport layer. The holes and electrons recombine in the emission layer to generate excitons.

[0328] Preparation of nanostructured layers

[0329] In some embodiments, the nanostructure layer can be embedded in a polymer matrix. As used herein, the term "embedded" is used to represent that the nanostructure colony is encapsulated or wrapped by a polymer that constitutes a major component of a matrix. In some embodiments, at least one nanostructure colony is suitably evenly distributed in the entire matrix. In some embodiments, at least one nanostructure colony is distributed according to an application-specific distribution. In some embodiments, the nanostructure is mixed in a polymer and applied to a substrate surface.

[0330] In some embodiments, the nanostructure composition is deposited to form a nanostructure layer. In some embodiments, the nanostructure composition can be deposited by any suitable method known in the art, including but not limited to coating, spraying, solvent spraying, wet coating, adhesive coating, spin coating, tape coating, roller coating, flow coating, inkjet steam injection, drop casting, scraping, mist deposition or its combination. The nanostructure composition can be directly coated on the required substrate layer. Alternatively, the nanostructure composition can be formed as a solid layer as an independent element, and is applied to the substrate subsequently. In some embodiments, the nanostructure composition can be deposited on one or more barrier layers.

[0331] In some embodiments, the nanostructure layer is cured after deposition. Suitable curing methods include light curing, such as UV curing and thermal curing. Conventional lamination film processing methods, tape coating methods and / or roll-to-roll manufacturing methods can be used to form the nanostructure layer.

[0332] Spin coating

[0333] In some embodiments, the nanostructure composition is deposited on a substrate using spin coating. In spin coating, a small amount of material is usually deposited on the center of the substrate loaded on the machine (called a spin coater), which is fixed by vacuum. High-speed rotation is applied on the substrate by the spin coater, which causes centripetal force to diffuse the material from the center of the substrate to the edge. Although most of the material can be spun off, a certain amount of material remains on the substrate, thereby forming a material film on the surface as the rotation continues. Except for the parameters selected for the spin process, such as rotation speed, acceleration and rotation time, the final thickness of the film is determined by the performance and substrate of the deposited material. In some embodiments, a rotation speed of 1500rpm to 6000rpm is used, and the rotation time is 10-60 seconds.

[0334] Fog deposition

[0335] In some embodiments, the nanostructured composition is deposited on the substrate using mist deposition. Mist deposition occurs at room temperature and atmospheric pressure and allows precise control of film thickness by varying process conditions. During mist deposition, the liquid source material is turned into a very fine mist and carried into the deposition chamber by nitrogen. The mist is then drawn to the wafer surface by a high voltage between the field screen and the wafer holder. Once the droplets coalesce on the wafer surface, the wafer is removed from the chamber and thermally cured to evaporate the solvent. The liquid precursor is a mixture of a solvent and the material to be deposited. It is delivered to the atomizer by pressurized nitrogen. Price, SC et al., "Formation of Ultra-Thin Quantum Dot Films by MistDeposition," ESC Transactions 11: 89-94 (2007).

[0336] Spraying

[0337] In some embodiments, the nanostructured composition is deposited on a substrate using spraying. Typical devices for spraying include nozzles, atomizers, precursor solutions and carrier gases. In the spray deposition process, the precursor solution is crushed into micron-sized droplets by means of a carrier gas or by atomization (e.g., ultrasound, gas spray or static electricity). The droplets from the atomizer are accelerated by the substrate surface through the nozzle with the help of a carrier gas, and the carrier gas is controlled and regulated as required. The relative motion between the nozzle and the substrate is determined by design for the purpose of fully covering the substrate.

[0338] In some embodiments, the application of the nanostructure composition further comprises a solvent. In some embodiments, the solvent used to apply the nanostructure composition is water, an organic solvent, an inorganic solvent, a halogenated organic solvent, or a mixture thereof. Illustrative solvents include, but are not limited to, water, D2O, acetone, ethanol, dioxane, ethyl acetate, methyl ethyl ketone, isopropanol, anisole, gamma, butyrolactone, dimethylformamide, N-methylpyrrolidone, dimethylacetamide, hexamethylphosphoramide, toluene, dimethyl sulfoxide, cyclopentanone, tetramethylene sulfoxide, xylene, ε-caprolactone, tetrahydrofuran, tetrachloroethylene, chloroform, chlorobenzene, dichloromethane, 1,2-dichloroethane, 1,1,2,2-tetrachloroethane, or a mixture thereof.

[0339] In some embodiments, the nanostructure composition is thermally cured to form the nanostructure layer. In some embodiments, the composition is cured using UV light. In some embodiments, the nanostructure composition is directly coated on the barrier layer of the nanostructure film, and then an additional barrier layer is deposited on the nanostructure layer to produce the nanostructure film. A support substrate can be used below the barrier film to increase strength, stability, and coating uniformity, and to prevent material inconsistency, bubble formation, and wrinkling or folding of barrier layer materials or other materials. In addition, one or more barrier layers are preferably deposited on the nanostructure layer to seal the material between the top and bottom barrier layers. Suitably, the barrier layer can be deposited as a laminated film, and optionally sealed or further processed, and then the nanostructure film is incorporated into a specific lighting device. As will be understood by those of ordinary skill in the art, the nanostructure composition deposition process can include additional or variable components. This type of embodiment will allow online process adjustment of nanostructure emission characteristics (e.g., brightness and color) (e.g., adjusting the quantum dot film white point) and nanostructure film thickness and other characteristics. In addition, these embodiments will allow for periodic testing of the nanostructured film properties during the manufacturing process, as well as any switching required to achieve precise nanostructured film properties. Such testing and adjustments can also be accomplished without changing the mechanical configuration of the production line, as the respective amounts of the mixture used to form the nanostructured film can be electronically changed using a computer program.

[0340] Barrier layer

[0341] In some embodiments, the molded article comprises one or more barrier layers disposed on either or both sides of the nanostructure layer. Suitable barrier layers protect the nanostructure layer and the molded article from environmental conditions such as high temperature, oxygen and moisture. Suitable barrier materials include non-yellowing transparent optical materials that are hydrophobic, chemically and mechanically compatible with the molded article, have optical and chemical stability, and can withstand high temperatures. In some embodiments, the one or more barrier layers are index matched with the molded article. In some embodiments, the matrix material of the molded article and the one or more adjacent barrier layers are index matched to have similar refractive indices so that most of the light transmitted to the molded article through the barrier layers is transmitted from the barrier layers to the nanostructure layer. This index matching reduces the light loss at the interface between the barrier and the matrix material.

[0342] The barrier layer is suitably a solid material and may be a solidified liquid, gel or polymer. Depending on the specific application, the barrier layer may comprise a flexible or non-flexible material. The barrier layer is preferably a planar layer and may comprise any suitable shape and surface area configuration, depending on the specific lighting application. In some embodiments, the one or more barrier layers will be compatible with laminate film processing technology, whereby the nanostructure layer is disposed on at least the first barrier layer, and at least the second barrier layer is disposed on the nanostructure layer on the side opposite to the nanostructure layer to form a molded article according to an embodiment. Suitable barrier materials include any suitable barrier materials known in the art. In some embodiments, suitable barrier materials include glass, polymers and oxides. Suitable barrier layer materials include, but are not limited to, polymers such as polyethylene terephthalate (PET); oxides such as silicon oxide, titanium oxide or aluminum oxide (e.g., SiO2, Si2O3, TiO2 or Al2O3); and appropriate combinations thereof. Preferably, each barrier layer of the molded article comprises at least two layers comprising different materials or compositions, so that the multilayer barrier layer eliminates or reduces the pinhole defect arrangement in the barrier layer, thereby providing an effective barrier to oxygen and moisture penetration into the nanostructure layer. The nanostructure layer can comprise any suitable material or combination of materials, and any suitable number of barrier layers on either or both sides of the nanostructure layer. The material, thickness and number of barrier layers will depend on the specific application, and will be appropriately selected to maximize the barrier protection and brightness of the nanostructure layer while minimizing the thickness of the molded article. In a preferred embodiment, each barrier layer comprises a laminated film, preferably a double laminated film, wherein the thickness of each barrier layer is thick enough to eliminate wrinkling in a roll-to-roll or lamination manufacturing process. In an embodiment where the nanostructure comprises heavy metals or other toxic materials, the number or thickness of the barrier layers may further depend on statutory toxicity guidelines, which may require more or thicker barrier layers. Other considerations for the barrier layers include cost, availability and mechanical strength.

[0343] In some embodiments, the nanostructured film comprises two or more barrier layers adjacent to each side of the nanostructured layer, for example, two or more layers on each side of the nanostructured layer or two barrier layers on each side. In some embodiments, each barrier layer comprises a thin glass sheet, for example, a glass sheet having a thickness of about 100 μm, 100 μm or less, or 50 μm or less.

[0344] As will be appreciated by one of ordinary skill in the art, each barrier layer of the molded article may have any suitable thickness, depending on the specific requirements and characteristics of the lighting device and application, as well as the individual film components, such as the barrier layer and the nanostructure layer. In some embodiments, each barrier layer may have a thickness of 50 μm or less, 40 μm or less, 30 μm or less, 25 μm or less, 20 μm or less, or 15 μm or less. In certain embodiments, the barrier layer comprises an oxide coating, which may include materials such as silicon oxide, titanium oxide, and aluminum oxide (e.g., SiO2, Si2O3, TiO2, or Al2O3). The oxide coating may have a thickness of about 10 μm or less, 5 μm or less, 1 μm or less, or 100 nm or less. In certain embodiments, the barrier comprises a thin oxide coating having a thickness of about 100 nm or less, 10 nm or less, 5 nm or less, or 3 nm or less. The top and / or bottom barrier may consist of a thin oxide coating, or may comprise the thin oxide coating and one or more additional layers of material.

[0345] Molded articles with improved properties

[0346] In some embodiments, the EQE of the molded article prepared using the nanostructure is about 1.5% to about 20%, about 1.5% to about 15%, about 1.5% to about 12%, about 1.5% to about 10%, about 1.5% to about 8%, about 1.5% to about 4%, about 1.5% to about 3%, about 3% to about 20%, about 3% to about 15%, about 3% to about 12%, about 3% to about 10%, about 3% to about 8%, about 8% to 20%, about 8% to about 15%, about 8% to about 12%, about 8% to about 10%, about 10% to about 20%, about 10% to about 15%, about 10% to about 12%, about 12% to about 20%, about 12% to about 15%, or about 15% to about 20%. In some embodiments, the nanostructure is a quantum dot. In some embodiments, the molded article is a light emitting diode.

[0347] In some embodiments, the maximum emission value of the photoluminescence spectrum of the molded article prepared using the nanostructure is between 450nm and 550nm. In some embodiments, the maximum emission value of the photoluminescence spectrum of the molded article prepared using the nanostructure is between 450nm and 460nm. In some embodiments, the emission maximum of the photoluminescence spectrum of the core / shell nanostructure is between about 450nm and about 460nm.

[0348] The following examples are illustrative and non-limiting of the products and methods described herein. Appropriate modifications and adjustments to the various conditions, formulations and other parameters commonly encountered in the art, as well as modifications and adjustments that are obvious to those skilled in the art based on this disclosure, are within the spirit and scope of the present invention.

[0349] Example

[0350] Example 1

[0351] Synthesis of ZnSe using coinjection method 1-x Te x Alloy Nanostructure

[0352] The TOPTe precursor mixture was first prepared by diluting TOPTe (1.0 M in Te, 460 μL) with 5.0 mL of dried and distilled oleylamine. Lithium triethylborohydride (1.0 M in THF, 460 μL) was added to the solution to give a dark purple solution. Finally, zinc oleate (0.5 M in TOP, 920 μL) was added to give a colorless, opaque, viscous gel that could be drawn into a syringe.

[0353] Oleylamine (30.0mL) is added to a 250mL three-necked flask and vacuum degassed at 110°C for 30 minutes. The mixture is heated to 300°C under a nitrogen stream. Once the temperature is reached, a TOP solution (5.8mL in total) of trioctylphosphine selenide (TOPSe, 5.4mmol) and diphenylphosphine (535μL) is added to the flask. Once the temperature rises to 300°C, a TOP solution (2.0mL) of the above-mentioned TOPTe precursor preparation and diethylzinc (590μL) is quickly and simultaneously injected from a separate syringe. The temperature is set to 280°C, and after 5 minutes, a TOP solution (7.6mL in total) of diethylzinc (588μL) and TOPSe (8.45mmol) is started to be injected at a rate of 1.0mL / minute, interrupted for 10 minutes after adding 7.6mL. After the precursor injection is completed, the reaction mixture is kept at 280°C for 5 minutes, and then cooled to room temperature. The growth solution was diluted with an equal volume of toluene and the nanocrystals were precipitated by adding ethanol. The supernatant was discarded after centrifugation and the nanocrystals were redispersed in toluene. The concentration as dry weight was measured by evaporating the solvent from the aliquot. The dried material was further subjected to thermogravimetric analysis to determine the inorganic content.

[0354] Example 2

[0355] Synthesis of ZnSe using bias injection method 1-x Te x Alloy Nanostructure

[0356] The TOPTe precursor mixture was first prepared by diluting TOPTe (1.0 M in Te, 460 μL) with 5.0 mL of dried and distilled oleylamine. Lithium triethylborohydride (1.0 M in THF, 460 μL) was added to the solution to give a dark purple solution. Finally, zinc oleate (0.5 M in TOP, 920 μL) was added to give a colorless, opaque, viscous gel that could be drawn into a syringe.

[0357] Oleylamine (30 mL) was added to a 100 mL three-necked flask and vacuum degassed at 110° C. for 30 minutes. The mixture was heated to 300° C. under a nitrogen stream. Once the temperature was reached, a TOP solution (5.8 mL in total) of trioctylphosphine selenide (TOPSe, 5.4 mmol) and diphenylphosphine (535 μL) was added to the flask. Once the temperature returned to 300° C., the above TOPTe precursor preparation was quickly injected. After 3 seconds, a TOP solution (2.0 mL) of diethylzinc (590 μL) was injected. The temperature was set to 280° C., and after 5 minutes, a TOP solution (7.6 mL in total) of diethylzinc (588 μL) and TOPSe (8.45 mmol) was injected at a rate of 1.0 mL / min, interrupted for 10 minutes after adding 7.6 mL. After the precursor injection was completed, the reaction mixture was kept at 280° C. for 5 minutes, and then cooled to room temperature. The growth solution was diluted with an equal volume of toluene, and nanocrystals were precipitated by adding ethanol. After centrifugation the supernatant was discarded and the nanocrystals were redispersed in toluene. The concentration was measured as dry weight by evaporating the solvent from an aliquot. The dried material was further subjected to thermogravimetric analysis to determine the inorganic content.

[0358] Example 3

[0359] ZnSe 1-x Te x Synthesis of ZnSe / ZnS core / shell nanostructures

[0360] The ZnSe 1-x Te x Coating of ZnSe shells or ZnSe / ZnS multi-shells on alloy nanocrystals.

[0361] Example 4

[0362] ZnSe 1-x Te x Properties of core / shell nanostructures

[0363] ZnSe prepared by co-injection and bias injection 1-x Te x The solution photoluminescence spectra of ZnSe / ZnS core / shell / shell nanostructures are shown in Figure 2 In. Figure 2 As shown, the red shift is achieved by co-injection and bias injection. The bias injection method results in a narrower peak because it promotes the formation of ZnTe. ZnSe 1-x Te x / ZnSe core / shell or ZnSe 1-x Te x The optical properties of ZnSe / ZnS core / shell / shell nanostructures can be tuned by varying the number of shell monolayers, as shown in Table 1.

[0364] Table 1

[0365]

[0366]

[0367] Example 5

[0368] ZnSe with low FWHM and high QY 1-x Te x Alloy Nanocrystals and ZnSe 1-x Te x / ZnSe / ZnS quantum dots

[0369] A: Synthesis of ZnSe using reduced TOP-Te 1-x Te x Alloy Nanocrystals

[0370] A Te precursor mixture was first prepared by diluting TOPTe (1M in Te, 690 μL) with 4.0 mL of dried and distilled oleylamine. Lithium triethylborohydride (1M in THF, 690 μL) was added to the solution to give a dark purple solution. Finally, zinc oleate (0.5M in TOP, 1180 μL) was added to give a colorless, opaque, viscous gel that could be drawn into a syringe. (In entry 7 of Table 2 below, 1036 μL of TOPTe, 1036 μL of LiEt3BH, and 2.08 mL of ZnOA2 / TOP were used instead)

[0371] Oleylamine (30 mL) and anhydrous zinc fluoride (118 mg, 1.04 mmol) were added to a 250 mL three-necked flask and degassed at 110 ° C for 30 min under vacuum. (Entry 7 does not contain ZnF2; all other entries do). The mixture was then heated to 300 ° C under a nitrogen stream. Once this temperature was reached, a TOP solution (5.8 mL in total) of trioctylphosphine selenide (TOPSe, 5.4 mmol) and diphenylphosphine (535 uL) was added to the flask. Once the temperature returned to 280 ° C, the above Te precursor preparation was quickly injected. After 3 seconds, a TOP solution (2.0 mL) of diethylzinc (590 μL) was quickly injected. The temperature was set to 280 ° C, and after 5 minutes, a TOP solution (7.6 mL in total) of diethylzinc (588 μL) and TOPSe (8.4 mmol) was injected at a rate of 1.0 mL / min until all 7.6 mL was completely added. After the precursor injection was completed, the reaction mixture was kept at 280°C for 5 minutes and then cooled to room temperature. The growth solution was diluted with an equal volume of toluene (60 mL) and the nanocrystals were precipitated by adding ethanol (120 mL). The supernatant was discarded after centrifugation and the nanocrystals were redispersed in hexane (5 mL). The concentration as dry weight was measured by evaporating the solvent from an aliquot. The dried material was further subjected to thermogravimetric analysis to determine the inorganic content.

[0372] B: ZnSe 1-x Te x Synthesis of ZnSe / Buffer Nanocrystals

[0373] This example describes the ZnSe with an average diameter of 2.3 nm. 1-x Te x Coating of a single monolayer ZnSe buffer layer on the alloy nanocrystals with a target shell thickness of 1 ML of ZnSe. (Entries 1 and 3-7 of Table 2 contain this reaction sequence.)

[0374] Zinc oleate (6.23 g), lauric acid (3.96 g), trioctylphosphine oxide (4.66 g), zirconium fluoride (644 mg) and TOP (9.4 mL) were charged into a 100 mL three-necked flask. (The reactions of entries 1 and 6 of Table 2 did not contain lauric acid.) The flask was then subjected to three cycles of vacuum and nitrogen backfill, followed by heating to 100° C. and then degassing for 30 min. The reaction mixture was placed under a nitrogen blanket, and ZnSe 1-x Te xThe solution of core (4.0mL, 28.0mg / mL in hexane) was mixed with TOP-Se (1.8mL of 0.3M selenium in TOP) and added to the flask. The flask was then evacuated for 2min and then heated to 310°C under a nitrogen stream. Once the temperature was reached, the solution was immediately cooled to room temperature. The reaction mixture was diluted with toluene (45mL). The largest core / shell nanocrystals were precipitated by adding ethanol (64mL), and then separated by centrifugation, decanting the supernatant, and disposing of the granulated nanocrystals. The supernatant from the previous step was then completely precipitated by adding ethanol (75mL), and then separated by centrifugation, decanting the supernatant and redispersing in hexane (5mL). The solution was filtered through a PTFE 0.45μm syringe filter. The concentration as dry weight was measured by evaporating the solvent from the aliquot. The dried material was further subjected to thermogravimetric analysis to determine the inorganic content.

[0375] C: ZnSe 1-x Te x Synthesis of ZnSe / Buffer Nanocrystals

[0376] This example describes the ZnSe with an average diameter of 4.0 nm. 1-x Te x Coating of ZnSe buffer layer on alloy nanocrystals with a target shell thickness of 4 ml ZnSe.

[0377] Zinc oleate (6.23 g), trioctylphosphine oxide (4.66 g), zirconium fluoride (644 mg), and TOP (9.4 mL) were charged to a 100 mL three-necked flask. (In some cases, zinc fluoride (333.8 mg) was also added; the reaction that gave Table 2 entry #2 also contained lauric acid (3.39 g), while the remaining reactions did not; the reaction that gave Table 2 entry 4 contained tri-n-octylamine (TOA) instead of trioctylphosphine oxide; and the reactions that gave Table 2 entries 3-5 contained both zirconium fluoride and zinc fluoride). The flask was then subjected to three cycles of vacuum and nitrogen backfill, followed by heating to 100°C and degassing for 30 min. The reaction mixture was placed under a nitrogen blanket, and ZnSe mixed with TOP-Se (1.8 mL of 0.3 M selenium in TOP) was added. 1-x Te xA solution of the core (4.0 mL, 28.0 mg / mL in hexane) was added to a flask. The flask was evacuated for 2 min and then heated to 310° C. under a stream of nitrogen. Once the temperature was reached, TOP-Se (10.4 mL, 0.3 M in TOP) was slowly injected at a rate of 0.325 mL / min. The reaction was maintained at 310° C. for 5 minutes after the selenium injection was complete and then cooled to room temperature. (The reaction mixture obtained for entries 3-5 of Table 2 was maintained at 340° C.) The reaction mixture was diluted with toluene (45 mL). The core / shell nanocrystals were precipitated by adding ethanol (135 mL) and then separated by centrifugation, the supernatant was decanted, and the nanocrystals were redispersed in hexane (5 mL). The solution was filtered through a PTFE 0.22 μm syringe filter and the concentration was measured as dry weight by evaporating the solvent from an aliquot. The dried material was further subjected to thermogravimetric analysis to determine the inorganic content.

[0378] D: ZnSe 1-x Te x Synthesis of ZnSe / ZnS Core / Shell Nanocrystals

[0379] This example describes the ZnSe with an average diameter of 6.1 nm. 1-x Te x Coating of ZnS shells with a target shell thickness of 2-4 ML of ZnS on ZnSe alloy nanocrystals. (Entries 1-3 and 5 of Table 2)

[0380] Zinc oleate (375 mg), trioctylphosphine oxide (281 mg), lauric acid (259 mg), zinc fluoride (648 mg) and TOP (0.566 mL) were charged into a 25 mL three-necked flask. (Only the reaction mixture that gave Table 2 entry #2 contained lauric acid in this step; the reaction mixtures that gave Table 2 entries 3 and 5 contained 389 mg of zinc fluoride.) To the reaction mixtures that gave Table 2 entries 3 and 5, zirconium fluoride (75 mg) was also added. The flask was then subjected to three cycles of vacuum and nitrogen backfill, followed by heating to 100°C and degassing for 30 min. The reaction mixture was placed under a nitrogen blanket, and ZnSe mixed with zinc oleate / TOP-S (0.064 mL of 2.0 M sulfur in TOP + 0.254 mL of 0.5 M zinc oleate in TOP) was added. 1-x Te xThe solution of core (from above C, 0.30mL, 216.0mg / mL in hexane) is added to the flask. The flask is evacuated for 2min, and then heated to 310°C under a nitrogen stream. Once the temperature is reached, zinc oleate / TOP-S (2mL, 0.3M in TOP) is slowly injected at a rate of 0.103mL / min. After the sulfur injection is completed, the reaction is kept at 310°C for 5 minutes, and then cooled to room temperature. (The reaction mixture of Table 2 entries 3&5 is kept at 340°C.) The reaction mixture is diluted with toluene (5mL). The core / shell nanocrystals are precipitated by adding ethanol (10mL), then by centrifugation, the supernatant is decanted, and the nanocrystals are redispersed in hexane (5mL). The precipitation is repeated once with ethanol (10mL), and finally the nanocrystals are redispersed in octane (3mL). The solution was filtered through a PTFE 0.22 μm syringe filter and the concentration was adjusted to 18 mg / mL after measuring the dry weight of an aliquot.

[0381] The optical properties of the nanostructures prepared according to this example are shown in Table 2. Unexpectedly, these nanostructures show much higher QY compared to the nanostructures prepared according to Example 4.

[0382] # PWL / nm FWHM / nm QY / % 1 445 25 81 2 448 28 88 3 451 28 87 4 452 30 89 5 454 25 83 6 456 30 78 7 461 30 74

[0383] Table 2

[0384] Although various embodiments have been described above, it should be understood that they are presented as examples only and not as limitations. It will be apparent to those skilled in the relevant art that various changes may be made in form and detail without departing from the spirit and scope of the present invention. Therefore, the breadth and scope should not be limited by any of the above exemplary embodiments, but should only be limited according to the appended claims and their equivalents.

[0385] All publications, patents, and patent applications mentioned in this specification are indicative of the levels of skill of those skilled in the art to which this invention pertains, and are incorporated herein by reference to the same extent as if each individual publication, patent, or patent application was specifically and individually indicated to be incorporated by reference.

Claims

1. A method for preparing ZnSe 1-x Te x Nanocrystal method, wherein include: (a) mixing a tellurium source, at least one ligand, and a reducing agent to prepare a reaction mixture; (b) contacting the reaction mixture obtained in (a) with a solution comprising at least one ligand, zinc fluoride and a selenium source; and (c) contacting the reaction mixture obtained in (b) with a zinc source; To provide ZnSe 1-x Te x Nanocrystals, where 0 <x<1, The reducing agent is selected from diborane, sodium hydride, sodium borohydride, lithium borohydride, sodium cyanoborohydride, calcium hydride, lithium hydride, lithium aluminum hydride, diisobutylaluminum hydride, sodium triethylborohydride and lithium triethylborohydride.

2. The method according to claim 1, wherein the selenium source is selected from the group consisting of trioctylphosphine selenide, tri(n-butyl)phosphine selenide, tri(sec-butyl)phosphine selenide, tri(tert-butyl)phosphine selenide, trimethylphosphine selenide, triphenylphosphine selenide, diphenylphosphine selenide, phenylphosphine selenide, cyclohexylphosphine selenide, octylselenol, dodecanol, phenylselenol, elemental selenium, hydrogen selenide, bis(trimethylsilyl)selenide, and mixtures thereof.

3. The method according to claim 1 or 2, wherein the selenium source is trioctylphosphine selenide.

4. The method according to claim 1 or 2, wherein the at least one ligand in (b) is selected from trioctylphosphine oxide, trioctylphosphine, diphenylphosphine, triphenylphosphine oxide and tributylphosphine oxide.

5. The method of claim 1 or 2, wherein the at least one ligand in (b) is diphenylphosphine.

6. The method of claim 1 or 2, wherein the tellurium source is selected from trioctylphosphine telluride, tri(n-butyl)phosphine telluride, trimethylphosphine telluride, triphenylphosphine telluride, tricyclohexylphosphine telluride, elemental tellurium, hydrogen telluride, bis(trimethylsilyl) telluride, and mixtures thereof.

7. The method of claim 1 or 2, wherein the tellurium source is trioctylphosphine telluride.

8. The method according to claim 1 or 2, wherein the reducing agent is lithium triethylborohydride.

9. The method according to claim 1 or 2, wherein the zinc source in (c) is selected from diethyl zinc, dimethyl zinc, diphenyl zinc, zinc acetate, zinc acetylacetonate, zinc iodide, zinc bromide, zinc chloride, zinc fluoride, zinc carbonate, zinc cyanide, zinc nitrate, zinc oxide, zinc peroxide, zinc perchlorate and zinc sulfate.

10. The process according to claim 1 or 2, wherein the zinc source in (c) is diethylzinc.

11. The method according to claim 1 or 2, further comprising: include: (d) contacting the reaction mixture of (c) with a zinc carboxylate and a selenium source.

12. The method of claim 11, wherein the zinc carboxylate in (d) is selected from zinc oleate, zinc hexanoate, zinc octoate, zinc laurate, zinc myristate, zinc palmitate, zinc stearate, zinc dithiocarbamate, and mixtures thereof.

13. The method of claim 11, wherein the zinc carboxylate in (d) is zinc oleate.

14. The method of claim 11, wherein the selenium source in (d) is selected from trioctylphosphine selenide, tri(n-butyl)phosphine selenide, tri(sec-butyl)phosphine selenide, tri(tert-butyl)phosphine selenide, trimethylphosphine selenide, triphenylphosphine selenide, diphenylphosphine selenide, phenylphosphine selenide, cyclohexylphosphine selenide, octylselenol, dodecanol, phenylselenol, elemental selenium, hydrogen selenide, bis(trimethylsilyl)selenide, and mixtures thereof.

15. The method of claim 11, wherein the selenium source in (d) is trioctylphosphine selenide.

16. The method according to claim 1 or 2, wherein the mixing in (a) is performed at room temperature.

17. The method of claim 1 or 2, wherein the contacting in (b) is performed at a temperature of 250°C to 350°C.

18. The method of claim 1 or 2, wherein the contacting in (b) is performed at a temperature of 280°C.

19. The method of claim 1 or 2, wherein the contacting in (c) is performed at a temperature of 250°C to 350°C.

20. The method of claim 1 or 2, wherein the contacting in (c) is performed at a temperature of 280°C.

21. The method of claim 1 or 2, wherein the contacting in (c) further comprises at least one ligand.

22. The method of claim 21, wherein the at least one ligand is trioctylphosphine or diphenylphosphine.

23. The method of claim 11, wherein the contacting in (d) is performed at a temperature of 250°C to 350°C.

24. The method of claim 11, wherein the contacting in (d) is performed at a temperature of 310°C.

25. The method of claim 11, wherein the contacting in (d) further comprises at least one ligand.

26. The method of claim 25, wherein the at least one ligand is trioctylphosphine or diphenylphosphine.

27. A method for preparing a core / shell nanostructure, wherein include: (e) Preparation of ZnSe according to any one of claims 1 to 26 1-x Te x Nanocrystals, the ZnSe prepared by the method according to any one of claims 1-26 1-x Te x The nanocrystals are mixed with a solution containing a zinc source, wherein 0 <x<1; (f) contacting the reaction mixture of (e) with a selenium source or a sulfur source.

28. The method according to claim 27, further comprising include: (g) contacting the reaction mixture of (f) with a selenium source or a sulfur source; wherein the source used in (g) is different from the source used in (f).

29. The method of claim 27 or 28, wherein the mixing in (e) is carried out at a temperature of 20°C to 310°C.

30. The method of claim 27 or 28, wherein the mixing in (e) is performed at a temperature of 20°C to 100°C.

31. The method of claim 27 or 28, wherein the zinc source of (e) is selected from the group consisting of diethyl zinc, dimethyl zinc, diphenyl zinc, zinc acetate, zinc acetylacetonate, zinc iodide, zinc bromide, zinc chloride, zinc fluoride, zinc carbonate, zinc cyanide, zinc nitrate, zinc oleate, zinc oxide, zinc peroxide, zinc perchlorate, zinc sulfate, zinc hexanoate, zinc octoate, zinc laurate, zinc myristate, zinc palmitate, zinc stearate, zinc dithiocarbamate, and mixtures thereof.

32. The method of claim 27 or 28, wherein the contacting in (f) is performed at a temperature of 200°C to 350°C.

33. The method of claim 27 or 28, wherein the contacting in (f) is performed at a temperature of 310°C.

34. The process of claim 27 or 28, wherein in (f) the reaction mixture is contacted with a selenium source.

35. The method of claim 34, wherein the selenium source is selected from the group consisting of trioctylphosphine selenide, tri(n-butyl)phosphine selenide, tri(sec-butyl)phosphine selenide, tri(tert-butyl)phosphine selenide, trimethylphosphine selenide, triphenylphosphine selenide, diphenylphosphine selenide, phenylphosphine selenide, cyclohexylphosphine selenide, octylselenol, dodecanol, phenylselenol, elemental selenium, hydrogen selenide, bis(trimethylsilyl)selenide, and mixtures thereof.

36. The process of claim 27 or 28, wherein in (f) the reaction mixture is contacted with a sulfur source.

37. The method of claim 36, wherein the sulfur source is selected from elemental sulfur, octyl mercaptan, dodecanethiol, octadecyl mercaptan, tributylphosphine sulfide, cyclohexyl isothiocyanate, α-toluene mercaptan, ethylene trithiocarbonate, allyl mercaptan, bis(trimethylsilyl) sulfide, trioctylphosphine sulfide, and mixtures thereof.

38. The method of claim 28, wherein in (g) the reaction mixture is contacted with a selenium source.

39. The method of claim 38, wherein the selenium source is selected from the group consisting of trioctylphosphine selenide, tri(n-butyl)phosphine selenide, tri(sec-butyl)phosphine selenide, tri(tert-butyl)phosphine selenide, trimethylphosphine selenide, triphenylphosphine selenide, diphenylphosphine selenide, phenylphosphine selenide, cyclohexylphosphine selenide, octylselenol, dodecanol, phenylselenol, elemental selenium, hydrogen selenide, bis(trimethylsilyl)selenide, and mixtures thereof.

40. The process of claim 28, wherein in (g) the reaction mixture is contacted with a sulfur source.

41. The method of claim 40, wherein the sulfur source is selected from elemental sulfur, octyl mercaptan, dodecanethiol, octadecyl mercaptan, tributylphosphine sulfide, cyclohexyl isothiocyanate, α-toluene mercaptan, ethylene trithiocarbonate, allyl mercaptan, bis(trimethylsilyl) sulfide, trioctylphosphine sulfide, and mixtures thereof.

42. The method of claim 28, wherein the admixture in (e) further comprises at least one ligand.

43. The method of claim 42, wherein the at least one ligand is selected from the group consisting of trioctylphosphine oxide, trioctylphosphine, diphenylphosphine, triphenylphosphine oxide, and tributylphosphine oxide.

44. The method of claim 42 or 43, wherein the at least one ligand is trioctylphosphine or trioctylphosphine oxide.

45. The method of claim 27 or 28, wherein the nanostructures exhibit a photoluminescence quantum yield of 75% to 90%.

46. ​​The method of claim 27 or 28, wherein the nanostructures exhibit a photoluminescence quantum yield of 80% to 90%.

47. The method of claim 27 or 28, wherein the nanostructures have a full width at half maximum of 20 nm to 30 nm.

48. The method of claim 27 or 28, wherein the nanostructures have a full width at half maximum of 25 nm to 30 nm.