Optical glass and optical components
By optimizing the component content and ratio of optical glass, its acid resistance and weather resistance are improved, and the problem of insufficient durability of medium-refractive index glass in the prior art is solved, and significant improvement of acid resistance and weather resistance and thermal stability are achieved. .
Patent Information
- Application Number
- CN202210426006.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-07-18
- Filing Date
- 2018-08-01
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2038-08-01
AI Technical Summary
The existing glass with medium refractive index and dispersion have shortcomings in acid resistance and weather resistance, and it is difficult to meet the requirements of high durability, especially in applications such as on-board vehicles.
By adjusting the component content of the optical glass, it ensures that it contains the total content and ratio of cations such as Li+, Na+, K+, P5+, B3+, Ba2+, Al3+, Ln3+, Ti4+, Zr4+, Nb5+, Ta5+, Bi3+ and W6+, and optimizes the phosphate glass. network structure to improve its acid resistance and weather resistance.
It realizes optical glass with excellent acid resistance and weather resistance, reduces the glass transition temperature, improves thermal stability and light transmission, and is suitable for high durability applications.
Smart Images

Figure CN114890668B_ABST
Abstract
Description
[0001] This application is a divisional application of the invention patent application with application number 201810863708.8. The application date of the original application is August 1, 2018, and the name of the invention is “Optical Glass and Optical Elements”. Technical Field
[0002] The present invention relates to an optical glass having excellent acid resistance and weather resistance and an optical element formed of the optical glass. Background Art
[0003] In recent years, as the image quality and resolution of digital cameras and the like have been improved, aspherical lenses have been widely used, and therefore, glass having a moderate refractive index, a moderate dispersion, and a high transmittance has been required.
[0004] However, conventionally, the acid resistance and weather resistance of medium-refractive-index and medium-dispersion glasses are not sufficient, and therefore, further improvements are required in applications requiring high durability, such as automotive applications.
[0005] Patent Document 1 discloses an optical glass having a medium refractive index and medium dispersion, but the acid resistance is not sufficient.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2016-533312. Summary of the invention
[0009] Problem that the invention aims to solve
[0010] The present invention has been made in view of such actual circumstances, and an object of the present invention is to provide an optical glass and an optical element having excellent acid resistance and weather resistance.
[0011] Solutions for solving problems
[0012] The present inventors have conducted intensive studies to achieve the above-mentioned object and have found that the object can be achieved by adjusting the content ratio of various glass components (hereinafter referred to as glass components) constituting glass. Based on this finding, the present invention has been completed.
[0013] That is, the gist of the present invention is as follows.
[0014] (1) An optical glass comprising Li + 、Na + and K + One or more alkali metal ions and P 5+ , B 3+ And Ba 2+Phosphate glass as a cationic component,
[0015] Al 3+ , Ln 3+ 、Ti 4+ 、Zr 4+ , Nb 5+ 、 5+ 、Bi 3+ and W 6+ Total content [Al 3+ +Ln 3+ +Ti 4+ +Zr 4+ +Nb 5+ +Ta 5 + +Bi 3+ +W 6+ ] is 10 cation % or more, among which Ln 3+ Indicates La 3+ , Gd 3+ , Y 3+ , Yb 3+ Lu 3+ Total content [La 3+ +Gd 3 + +Y 3+ +Yb 3+ +Lu 3+ ],
[0016] P 5+ and B 3+ The total content [P 5+ +B 3+ ] is 30 to 50 cation%,
[0017] P 5+ The content of P 5+ and B 3+ The total cation content ratio [P 5+ / (P 5+ +B 3+ )] is 0.50 or more and 0.84 or less,
[0018] Li + 、Na + and K + Total content [Li + +Na + +K + ] is 5 cation % or more,
[0019] Ba 2+ The content of cationic is more than 5%,
[0020] Mg 2+ , Ca2+ , Sr 2+ And Ba 2+ Total content [Mg 2+ +Ca 2+ +Sr 2+ +Ba 2+ ] is 10 cation % or more,
[0021] The Abbe number νd is 40 or more.
[0022] (2) The optical glass according to (1), wherein
[0023] P 5+ The content of cations is 20-40%,
[0024] B 3+ The content of cations is 4-15%,
[0025] Li + The content is 5 to 30 cation %.
[0026] (3) The optical glass according to (1) or (2), wherein:
[0027] The acid resistance weight reduction rate Da based on JOGIS is less than 0.8%.
[0028] (4) The optical glass according to any one of (1) to (3), wherein
[0029] The acid resistance based on JOGIS is 1 to 3 levels.
[0030] (5) The optical glass according to any one of (1) to (4), wherein
[0031] Weather resistance D based on JOGIS H It is level 1.
[0032] (6) The optical glass according to any one of (1) to (5), wherein
[0033] The glass transition temperature Tg is 590°C or lower.
[0034] (7) An optical glass, wherein:
[0035] The acid resistance weight reduction rate Da based on JOGIS is less than 0.8%,
[0036] The glass transition temperature Tg is below 590°C.
[0037] The Abbe number νd is 40 or more.
[0038] (8) An optical element formed of the optical glass according to any one of (1) to (7) above.
[0039] Effects of the Invention
[0040] According to the present invention, an optical glass and an optical element having excellent acid resistance and weather resistance can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 The optical glass according to the first embodiment of the present invention is shown in FIG. 3+ , Ln 3+ 、Ti 4+ 、Zr 4+ , Nb 5+ 、 5+ 、Bi 3+ and W 6+ A graph showing the relationship between the total content of and the acid resistance weight reduction rate Da. DETAILED DESCRIPTION
[0042] Hereinafter, an embodiment of the present invention will be described. In this embodiment, the optical glass of the present invention will be described based on the content ratio of each component expressed as cation %. Therefore, unless otherwise specified, each content is expressed as cation %.
[0043] In this specification, unless otherwise specified, the refractive index refers to the refractive index nd of the d-line (wavelength 587.56 nm) of helium.
[0044] The Abbe number νd is used as a value indicating a property related to dispersion and is represented by the following equation (1): nF is the refractive index at the F line (wavelength 486.13 nm) of blue hydrogen, and nC is the refractive index at the C line (656.27 nm) of red hydrogen.
[0045] νd=(nd-1) / (nF-nC)···(1)
[0046] The cation % expression refers to the molar percentage when the content of all cationic components is set to 100%. In addition, the total content refers to the total amount of the contents of multiple cationic components (including the case where the content is 0%). In addition, the cation ratio refers to the ratio (ratio) of the contents of the cationic components to each other (including the total content of multiple cationic components) in the cation % expression.
[0047] The valence of the cationic component (e.g., B 3+ The valence is +3, Si 4+ The valence is +4, La 3+The valence of the anion component (e.g., O) is a value determined by convention, which is the same as when B, Si, and La as glass components are expressed as B2O3, SiO2, and La2O3 on an oxide basis. Therefore, when analyzing the glass composition, the valence of the cation component does not need to be analyzed. In addition, the valence of the anion component (e.g., O 2- The valence of the anion is -2) is also a value determined according to the convention, which is the same as expressing the glass components in the oxide standard as B2O3, SiO2, La2O3 as mentioned above. Therefore, when analyzing the glass composition, the valence of the anion component does not need to be analyzed.
[0048] The content of the glass component can be quantified by a known method such as inductively coupled plasma atomic emission spectrometry (ICP-AES), inductively coupled plasma mass spectrometry (ICP-MS), etc. In addition, in this specification and the present invention, the content of a constituent component of 0% means that the constituent component is not substantially contained, and the inclusion of the constituent component at an unavoidable impurity level is allowed.
[0049] Hereinafter, the optical glass of the present invention will be described based on the glass composition as a first embodiment, and the optical glass of the present invention will be described based on the physical property values as a second embodiment.
[0050] First Embodiment
[0051] The optical glass according to the first embodiment is characterized in that:
[0052] It is selected from Li + 、Na + and K + One or more alkali metal ions and P 5+ , B 3+ And Ba 2+ Phosphate glass as a cationic component,
[0053] Al 3+ , Ln 3+ 、Ti 4+ 、Zr 4+ , Nb 5+ 、 5+ 、Bi 3+ and W 6+ Total content [Al 3+ +Ln 3+ +Ti 4+ +Zr 4+ +Nb 5+ +Ta 5 + +Bi 3+ +W 6+ ] is 10 cation % or more (wherein, Ln3+ Indicates La 3+ , Gd 3+ , Y 3+ , Yb 3+ Lu 3+ Total content [La 3+ +Gd 3 + +Y 3+ +Yb 3+ +Lu 3+ ] ),
[0054] P 5+ and B 3+ The total content [P 5+ +B 3+ ] is 30 to 50 cation%,
[0055] P 5+ The content of P 5+ and B 3+ The total cation content ratio [P 5+ / (P 5+ +B 3+ )] is 0.50 or more and 0.84 or less,
[0056] Li + 、Na + and K + Total content [Li + +Na + +K + ] is 5 cation % or more,
[0057] Ba 2+ The content of cationic is more than 5%,
[0058] Mg 2+ , Ca 2+ , Sr 2+ And Ba 2+ Total content [Mg 2+ +Ca 2+ +Sr 2+ +Ba 2+ ] is 10 cation % or more,
[0059] The Abbe number νd is 40 or more.
[0060] Hereinafter, the optical glass according to the first embodiment will be described in detail.
[0061] The optical glass of the first embodiment includes a + 、Na + and K + One or more alkali metal ions and P 5+ , B3+ And Ba 2+ In addition, the optical glass contains P as a network forming component of the glass. 5+ Phosphate glass as the main component. 5+ and B 3+ As a glass component, the devitrification resistance is improved. In addition, by including alkali metal ions, the devitrification resistance and thermal stability of the glass are improved, and the glass transition temperature is reduced. Here, the alkali metal ion is Li + 、Na + , K + Furthermore, by including Ba 2+ , thereby suppressing the decrease in the refractive index nd and also suppressing the devitrification during vitrification.
[0062] In the optical glass of the first embodiment, Al 3+ , Ln 3+ 、Ti 4+ 、Zr 4+ , Nb 5+ 、 5+ 、Bi 3+ and W 6+ Total content [Al 3+ +Ln 3+ +Ti 4+ +Zr 4+ +Nb 5+ +Ta 5+ +Bi 3+ +W 6+ ] is 10% or more. Total content [Al 3+ +Ln 3+ +Ti 4+ +Zr 4+ +Nb 5+ +Ta 5+ +Bi 3+ +W 6+ The lower limit of ] is preferably 12%, and more preferably 15% and 18%, respectively.
[0063] Here, Ln 3+ Indicates La 3+ , Gd 3+ , Y 3+ , Yb 3+ Lu 3+ Total content [La 3+ +Gd 3+ +Y 3+ +Yb 3+ +Lu 3+ ].
[0064] Al 3+ , Ln3+ 、Ti 4+ 、Zr 4+ , Nb 5+ 、 5+ 、Bi 3+ and W 6+ It is a component that helps to improve acid resistance. Figure 1 As shown, with the total content [Al 3+ +Ln 3+ +Ti 4+ +Zr 4+ +Nb 5+ +Ta 5+ +Bi 3+ +W 6+ ] increases, the acid resistance weight reduction rate Da decreases. Therefore, it is preferred to increase the total content [Al 3+ +Ln 3+ +Ti 4+ +Zr 4+ +Nb 5+ +Ta 5+ +Bi 3+ +W 6+ ] is set to the above range.
[0065] In the optical glass of the first embodiment, P 5+ and B 3+ The total content [P 5+ +B 3+ ] is 30 to 50%. The total content [P 5+ +B 3+ ] is preferably 32 to 48%, more preferably 34 to 46%, and further preferably 36 to 45%.
[0066] Furthermore, in the optical glass of the first embodiment, P 5+ The content of P 5+ and B 3+ The total cation content ratio [P 5+ / (P 5+ +B 3+ )] is 0.50 or more and 0.84 or less, and the cation ratio [P 5+ / (P 5+ +B 3+ The lower limit of the cation ratio [P 5+ / (P 5+ +B 3+ The upper limit of )] is preferably 0.83, and more preferably 0.82.
[0067] When containing P 5+ and B 3When used as a network-forming component of glass, it can improve the resistance to devitrification, but when contained in excessive amounts, weather resistance deteriorates. 5+ The ratio of is set to a predetermined range, thereby further improving the resistance to devitrification. Therefore, it is preferred to set the total content [P 5+ +B 3+ ] and cation ratio [P 5+ / (P 5+ +B 3+ )] is set to the above range.
[0068] In the optical glass of the first embodiment, Li + 、Na + , K + Total content [Li + +Na + +K + ] is 5% or more. + 、Na + , K + All of them have the effect of improving the thermal stability of glass and lowering the glass transition temperature Tg. On the other hand, when their total content increases, the acid resistance decreases. + +Na + +K + The lower limit of ] is preferably 6%, and more preferably 8% and 10% in that order. + +Na + +K + The upper limit of ] is preferably 30%, and more preferably 28%, 26%, and 25%, respectively.
[0069] In the optical glass of the first embodiment, Ba 2+ The content of Ba is more than 5%. 2+ The lower limit of the content of Ba is preferably 7%, and more preferably 9%, 11%, and 13%. 2+ The upper limit of the content of is preferably 30%, and more preferably 28%, 26%, and 24%, respectively.
[0070] By placing Ba 2+ By setting the content of MgO to the above range, a decrease in the refractive index nd can be suppressed, and devitrification during vitrification can be suppressed.
[0071] In the optical glass of the first embodiment, Mg 2+ , Ca 2+ , Sr 2+ And Ba 2+ Total content [Mg 2+ +Ca 2+ +Sr 2+ +Ba 2+] is 10% or more. Mg 2+ , Ca 2+ , Sr 2+ And Ba 2+ All of them are glass components that have the effect of improving the acid resistance, thermal stability and resistance to devitrification of glass. 2+ +Ca 2+ +Sr 2+ +Ba 2+ ] is set to 10% or more, thereby improving the acid resistance, thermal stability and devitrification resistance of the glass. 2+ +Ca 2+ +Sr 2+ +Ba 2+ The lower limit of [Mg] is preferably 15%, and further preferably 16%, 17%, and 18%. On the other hand, when the content of these glass components increases, the thermal stability and resistance to devitrification of the glass decrease. Therefore, the total content [Mg 2+ +Ca 2+ +Sr 2+ +Ba 2+ The upper limit of Mg is preferably 40%, and more preferably 38%, 36%, and 35%. From the viewpoint of maintaining thermal stability and resistance to devitrification, the total content [Mg 2+ +Ca 2+ +Sr 2+ +Ba 2 + ] is preferably within the above range.
[0072] In the optical glass of the first embodiment, the Abbe number νd is not less than 40. The Abbe number νd may be in the range of 40 to 65. The Abbe number νd is determined by, for example, 3+ , Ln 3+ 、Ti 4+ 、Zr 4+ , Nb 5+ 、 5+ 、Bi 3+ and W 6+ Total content [Al 3+ +Ln 3+ +Ti 4 + +Zr 4+ +Nb 5+ +Ta 5+ +Bi 3+ +W 6+ ] Increase Al 3+ The ratio of can be increased, and in addition, by reducing Al 3+ The ratio can thus be reduced.
[0073] (Glass composition)
[0074] Hereinafter, the contents and ratios of the glass components other than those described above in the optical glass of the first embodiment will be described in detail.
[0075] In the optical glass of the first embodiment, P 5+ The lower limit of the content of is preferably 20%, and more preferably 22%, 24%, and 26%. 5+ The upper limit of the content of is preferably 40%, and more preferably 39%, 38%, and 37%, respectively.
[0076] P 5+ It is a network-forming component of glass and also a component that improves the resistance to devitrification. 5 + When the weather resistance is poor. 5+ The content of is preferably within the above range.
[0077] In the optical glass of the first embodiment, B 3+ The lower limit of the content of is preferably 4%, and more preferably 5% and 6%. 3+ The upper limit of the content of is preferably 15%, and more preferably 13% and 12%, respectively.
[0078] B 3+ It is a network-forming component of glass and has the effect of improving the resistance of glass to devitrification. 3+ When the content of B is high, the acid resistance tends to decrease. 3+ The content of is preferably within the above range.
[0079] In the optical glass of the first embodiment, Si 4+ The upper limit of the content of Si is preferably 5%, and more preferably 4%, 3%, and 2%. 4+ The lower limit of the content of Si is preferably 0%. 4+ The content can be 0%.
[0080] Si 4+ It is a network-forming component of glass and has the function of improving the chemical durability of glass. 4 + When the content of Si is high, the devitrification resistance of the glass tends to decrease. 4+ The upper limit of the content is preferably within the above range.
[0081] In the optical glass of the first embodiment, Al 3+ The lower limit of the content of Al is preferably 1.0%, and more preferably 1.2% and 1.5%, respectively. 3+ The lower limit of the content of Al is set to 0%.3+ The upper limit of the content of Al is preferably 24%, and more preferably 23%, 22%, and 21%, respectively. 3+ The content can be 0%.
[0082] Al 3+ It is a glass component that improves the acid resistance of glass. 3+ When the content of Al increases, the devitrification resistance of the glass decreases. 3+ The content of is preferably within the above range.
[0083] In the optical glass of the first embodiment, Li + The lower limit of the content of Li is preferably 5%, and more preferably 6%, 8%, and 10%. + The upper limit of the content of is preferably 30%, and more preferably 28%, 26%, and 25%, in that order.
[0084] Li + It has the effect of lowering the glass transition temperature Tg. On the other hand, when Li + As the content of Li increases, acid resistance decreases. + The content of is preferably within the above range.
[0085] In the optical glass of the first embodiment, Na + The upper limit of the content of Na is preferably 12%, and more preferably 10%, 8%, 6%, and 4%. + The lower limit of the content of is preferably 0%. + The content can be 0%.
[0086] In the optical glass of the first embodiment, K + The upper limit of the content of is preferably 12%, and more preferably 10%, 8%, 6%, and 4%. + The lower limit of the content of is preferably 0%. + The content can be 0%.
[0087] Na + and K + It has the effect of improving the thermal stability of glass, but when their content increases, the refractive index, thermal stability and acid resistance decrease. + and K + Each content of is preferably within the above range.
[0088] Li + The content of Li + 、Na + and K + The total cation content ratio [Li+ / (Li + +Na + +K + )] is preferably 0.5 or more. + / (Li + +Na + +K + The lower limit of )] is preferably 0.6, and more preferably 0.7, 0.8, and 0.9, respectively.
[0089] By containing Li as a monovalent component + 、Na + and K + , thereby suppressing the increase of the glass transition temperature Tg. In addition, by including a large amount of Li + , thereby improving acid resistance and suppressing the decrease of refractive index nd. Therefore, it is preferred to increase the cation ratio [Li + / (Li + +Na + +K + )] is set to the above range.
[0090] In the optical glass of the first embodiment, Rb + The upper limit of the content of Rb is preferably 5%, and more preferably 4%, 3%, 2%, 1%, 0.5%, and 0.1%. + The lower limit of the content of Rb is preferably 0%. + The content can be 0%.
[0091] In the optical glass of the first embodiment, Cs + The upper limit of the content of Cs is preferably 5%, and more preferably 4%, 3%, 2%, 1%, 0.5%, and 0.1%. + The lower limit of the content of Cs is preferably 0%. + The content can be 0%.
[0092] R + and Cs + Both have the effect of improving the melting property of glass, but when their content increases, the refractive index nd, the thermal stability, acid resistance and weather resistance of glass decrease. + and Cs + Each content of is preferably within the above range.
[0093] In the optical glass of the first embodiment, Mg 2+ The upper limit of the content of Mg is preferably 15%, and more preferably 14%, 12%, and 10%, respectively. 2+ The lower limit of the content of Mg is preferably 0%. 2+The content can be 0%.
[0094] In the optical glass of the first embodiment, Ca 2+ The upper limit of the content of Ca is preferably 15%, and more preferably 14%, 12%, and 10%, respectively. 2+ The lower limit of the content of Ca is preferably 0%. 2+ The content can be 0%.
[0095] In the optical glass of the first embodiment, Sr 2+ The upper limit of the content of Sr is preferably 10%, and more preferably 9%, 8%, and 7%, respectively. 2+ The lower limit of the content of Sr is preferably 0%. 2+ The content can be 0%.
[0096] In the optical glass of the first embodiment, Zn 2+ The upper limit of the content of Zn is preferably 10%, and more preferably 9%, 8%, and 7%, respectively. 2+ The lower limit of the content of Zn is preferably 0%. 2+ The content can be 0%.
[0097] Zn 2+ It is a glass component that has the effect of lowering the transition temperature of glass and improving thermal stability. 2+ When the content of Zn is too high, the meltability deteriorates and the Abbe number νd decreases. 2+ The content of is preferably within the above range.
[0098] In the optical glass of the first embodiment, Y 3+ The upper limit of the content of Y is preferably 5%, and more preferably 4% and 3%. 3+ The lower limit of the content of Y is preferably 0%. 3+ The content can be 0%.
[0099] Y 3+ It is a component that has the effect of improving acid resistance. On the other hand, when Y 3+ When the content of Y becomes too much, the thermal stability and resistance to devitrification of the glass decrease. 3+ The content of is preferably within the above range.
[0100] In the optical glass of the first embodiment, La 3+ The upper limit of the content of La is preferably 5%, and more preferably 4% and 3%, respectively. 3+ The lower limit of the content of La is preferably 0%. 3+ The content can be 0%.
[0101] La 3+ It is a component that has the effect of improving acid resistance. On the other hand, when La 3+ When the content of La increases, the thermal stability and devitrification resistance of the glass decrease, and the glass is prone to devitrification during manufacturing. Therefore, from the perspective of suppressing the decrease in thermal stability and devitrification resistance, La 3+ The content of is preferably within the above range.
[0102] In the optical glass of the first embodiment, Gd 3+ The upper limit of the content of Gd is preferably 5%, and more preferably 4% and 3%, respectively. 3+ The lower limit of the content of Gd is preferably 0%. 3+ The content can be 0%.
[0103] G 3+ It is a component that has the effect of improving acid resistance. On the other hand, when Gd 3+ When the content of Gd becomes too high, the thermal stability and resistance to devitrification of the glass decrease, the glass is easy to devitrify during manufacturing, and the specific gravity increases. The specific gravity of the glass increases. When the specific gravity of the glass increases, the mass of the optical element increases. For example, when a heavy lens is assembled in an autofocus camera lens, the power required to drive the lens during autofocusing increases, and the battery consumption increases. Therefore, Gd 3+ The content of is preferably within the above range.
[0104] In the optical glass of the first embodiment, Yb 3+ The upper limit of the content of Yb is preferably 3%, and more preferably 2% and 1%, respectively. 3+ The lower limit of the content of Yb is preferably 0%. 3+ The content can be 0%.
[0105] Yb 3+ It is a component that has the effect of improving acid resistance. On the other hand, when Yb 3+ When the content of Yb becomes too high, the thermal stability and resistance to devitrification of the glass decrease, the glass is prone to devitrification during manufacturing, and the specific gravity increases. 3+ The content of is preferably within the above range.
[0106] In the optical glass of the first embodiment, Lu 3+ The upper limit of the content of Lu is preferably 3%, and more preferably 2% and 1% in that order. 3+ The lower limit of the content of Lu is preferably 0%. 3+ The content can be 0%.
[0107] Lu 3+ It is a component that has the effect of improving acid resistance. On the other hand, when Lu3+ When the content of Lu becomes too much, the thermal stability and resistance to devitrification of the glass decrease. In addition, the specific gravity increases. 3+ The content of is preferably within the above range.
[0108] In the optical glass of the first embodiment, La 3+ , Gd 3+ , Y 3+ , Yb 3+ Lu 3+ Total content [La 3+ +Gd 3+ +Y 3+ +Yb 3+ +Lu 3+ The upper limit of [La] is preferably 7%, and more preferably 6%, 5%, and 4%, respectively. 3+ +Gd 3+ +Y 3+ +Yb 3+ +Lu 3+ The lower limit of ] is preferably 0%. 3+ +Gd 3+ +Y 3+ +Yb 3+ +Lu 3+ ] can be 0%. 3+ +Gd 3+ +Y 3+ +Yb 3+ +Lu 3+ By being within the above range, acid resistance, thermal stability, and devitrification resistance can be improved.
[0109] In the optical glass of the first embodiment, Ti 4+ The upper limit of the content of Ti is preferably 7%, and more preferably 6%, 5%, and 4%, respectively. 4+ The lower limit of the content of Ti is preferably 0%. 4+ The content can be 0%.
[0110] Ti 4+ It is a component that has the effect of improving acid resistance. 4+ When the content of Ti becomes too high, the Abbe number decreases significantly. 4+ It is easy to increase the color of glass and also make the melting property worse. 4+ The content of is preferably within the above range.
[0111] In the optical glass of the first embodiment, Zr 4+ The upper limit of the content of Zr is preferably 7%, and more preferably 6% and 5%, respectively. 4+The lower limit of the content of Zr is preferably 0%. 4+ The content can be 0%.
[0112] Zr 4+ It is a glass component that improves the acid resistance of glass. 4+ When the content of Zr is too high, thermal stability and resistance to devitrification decrease. 4+ The content of is preferably within the above range.
[0113] In the optical glass of the first embodiment, Nb 5+ The upper limit of the content of Nb is preferably 15%, and more preferably 14%, 12%, and 10%, respectively. 5+ The lower limit of the content of Nb is preferably 0%. 5+ The content can be 0%.
[0114] Nb 5+ It is a glass component that improves the acid resistance of glass. It is also a glass component that improves the thermal stability of glass. 5+ When the content of Nb becomes too high, the Abbe number decreases significantly. In addition, there is a tendency for the coloring of the glass to increase. 5+ The content of is preferably within the above range.
[0115] In the optical glass of the first embodiment, Ta 5+ The upper limit of the content of Ta is preferably 5%, and more preferably 4%, 3%, and 2%. 5+ The lower limit of the content of Ta is preferably 0%. 5+ The content can be 0%.
[0116] Ta 5+ It is a glass component that improves the acid resistance of glass. 5+ When the content of Ta increases, the thermal stability of the glass decreases. 5+ The content of is preferably within the above range.
[0117] In the optical glass of the first embodiment, Bi 3+ The upper limit of the content of Bi is preferably 5%, and more preferably 4%, 3%, and 2%. 3+ The lower limit of the content of Bi is preferably 0%. 3+ The content can be 0%.
[0118] Bi 3+ By containing an appropriate amount, it has the effect of lowering Tg and improving the thermal stability of the glass. 3+ When the content of Bi increases, the coloring of the glass increases.3+ The content of is preferably within the above range.
[0119] In the optical glass of the first embodiment, W 6+ The upper limit of the content of W is preferably 5%, and more preferably 4%, 3%, and 2% in that order. 6+ The lower limit of the content of is preferably 0%. 6+ The content can be 0%.
[0120] W 6+ By containing an appropriate amount, it has the effect of lowering Tg and improving the thermal stability of the glass. 6+ When the content of W increases, the coloring of the glass increases. 6+ The content of is preferably within the above range.
[0121] In the optical glass of the first embodiment, Ga 3+ The upper limit of the content of Ga is preferably 5%, and more preferably 4%, 3%, 2.5%, 2%, 1.5%, 1%, 0.5%, 0.1%, and 0.05%. 3+ The lower limit of the content of Ga is preferably 0%. 3+ The content can be 0%.
[0122] In the optical glass of the first embodiment, In 3+ The upper limit of the content of In is preferably 5%, and more preferably 4%, 3%, 2.5%, 2%, 1.5%, 1%, 0.5%, 0.1%, and 0.05%. 3+ The lower limit of the content of In is preferably 0%. 3+ The content can be 0%.
[0123] In the optical glass of the first embodiment, Sc 3+ The upper limit of the content of Sc is preferably 5%, and more preferably 4%, 3%, 2.5%, 2%, 1.5%, 1%, 0.5%, 0.1%, and 0.05%. 3+ The lower limit of the content of Sc is preferably 0%. 3+ The content can be 0%.
[0124] In the optical glass of the first embodiment, Hf 4+ The upper limit of the content of Hf is preferably 5%, and more preferably 4%, 3%, 2.5%, 2%, 1.5%, 1%, 0.5%, 0.1%, and 0.05%. 4+ The lower limit of the content of Hf is preferably 0%. 4+ The content can be 0%.
[0125] In the optical glass of the first embodiment, Ge 4+ The upper limit of the content of Ge is preferably 5%, and more preferably 4%, 3%, 2.5%, 2%, 1.5%, 1%, 0.5%, 0.1%, and 0.05%. 4+ The lower limit of the content of Ge is preferably 0%. 4+ The content can be 0%.
[0126] In the optical glass of the first embodiment, Ti 4+ , Nb 5+ 、Bi 3+ and W 6+ The total content of Al 3+ , Ln 3+ 、Ti 4+ 、Zr 4+ , Nb 5+ 、 5+ 、Bi 3+ and W 6+ The total cation content ratio [(Ti 4+ +Nb 5+ +Bi 3+ +W 6+ ) / (Al 3+ +Ln 3+ +Ti 4+ +Zr 4+ +Nb 5+ +Ta 5+ +Bi 3+ +W 6+ The upper limit of )] is preferably 0.7, and more preferably 0.6, 0.5, and 0.4 in that order. In addition, the lower limit thereof may be 0.
[0127] By increasing the cation ratio [(Ti 4+ +Nb 5+ +Bi 3+ +W 6+ ) / (Al 3+ +Ln 3+ +Ti 4+ +Zr 4+ +Nb 5+ +Ta 5+ +Bi 3+ +W 6+ )] is set to the above range, and the Abbe number νd can be set to the desired range. In addition, it is also preferred in terms of obtaining good light transmittance.
[0128] In the optical glass of the first embodiment, Al 3+ The content of Al 3+ , Ln 3+ 、Ti 4+、Zr 4+ , Nb 5+ 、 5+ 、Bi 3+ and W 6+ The total content of cations is [Al 3+ / (Al 3+ +Ln 3+ +Ti 4+ +Zr 4+ +Nb 5+ +Ta 5+ +Bi 3+ +W 6+ )] may be 1. In addition, the lower limit thereof is preferably 0.2, and further preferably 0.3, 0.4, 0.5, and 0.6 in that order.
[0129] By increasing the cation ratio [Al 3+ / (Al 3+ +Ln 3+ +Ti 4+ +Zr 4+ +Nb 5+ +Ta 5+ +Bi 3+ +W 6+ )] is set to the above range, so that good acid resistance can be obtained and the Abbe number νd can be within the desired range.
[0130] The cationic component of the optical glass of the first embodiment is preferably mainly composed of the above-mentioned components, that is, Li + 、Na + and K + One or more alkali metal ions, P 5+ , B 3+ And Ba 2+ , Si as an optional component 4+ 、Al 3+ 、Na + , K + , Rb + , Cs + Mg 2+ , Ca 2+ , Sr 2+ 、Zn 2+ , Y 3+ ,La 3+ , Gd 3+ , Yb 3+ 、Ti 4+ 、Zr 4+ , Nb 5+ 、 5+ 、Bi 3+ , W 6+ , Ga 3+、In 3+ Sc 3 + , Hf 4+ 、Lu 3+ And Ge 4+ The total content of the above-mentioned components is preferably greater than 95%, more preferably greater than 98%, further preferably greater than 99%, and further more preferably greater than 99.5%.
[0131] The glass of the present invention is an oxide glass, and the main component of the anion component is O 2- O as an anionic component 2- The content is preferably in the range of 95 anion % or more and 100 anion % or less, more preferably in the range of more than 95 anion % and 100 anion % or less, further preferably in the range of more than 97 anion % and 100 anion % or less, and more preferably in the range of more than 99 anion % and 100 anion % or less, more than 99.5 % and 100 anion % or less, more than 99.9 % and 100 anion % or less, and 100 anion % or less, respectively.
[0132] The glass of the present invention may contain O 2- As anion components other than O 2- The anion components other than F - , Cl - Br - ,I - However, F - , Cl - Br - ,I - All of them are easily volatilized during the melting of glass. The volatilization of these components causes changes in the characteristics of the glass, a decrease in the homogeneity of the glass, and significant consumption of the melting equipment. Therefore, F - , Cl - Br - and I - The total content of is preferably less than 5 anion%, more preferably less than 3 anion%, further preferably less than 1 anion%, particularly preferably less than 0.5 anion%, further preferably less than 0.1 anion%, and further preferably 0 anion%.
[0133] In addition, the anion % is a molar percentage when the content of all anion components is 100%.
[0134] The optical glass of the first embodiment is preferably basically composed of the above components, but may contain other components within a range that does not hinder the effects of the present invention. In the present invention, inclusion of inevitable impurities is not excluded.
[0135] <Other ingredients>
[0136] Pb, As, Cd, Tl, Be, and Se are all toxic. Therefore, it is preferable that the optical glass of the first embodiment does not contain these elements as glass components.
[0137] U, Th, and Ra are all radioactive elements. Therefore, it is preferable that the optical glass of the first embodiment does not contain these elements as glass components.
[0138] V, Cr, Mn, Fe, Co, Ni, Cu, Pr, Nd, Pm, Sm, Eu, Tb, Dy, Ho, Er, Tm, and Ce increase the coloring of the glass and may become a source of fluorescence. Therefore, it is preferred that the optical glass of the first embodiment does not contain these elements as glass components.
[0139] Sb (Sb2O3), Sn (SnO2), and Ce (CeO2) are elements that can be added arbitrarily and function as clarifiers. Among them, Sb (Sb2O3) is a clarifier with a large clarification effect. However, Sb (Sb2O3) is highly oxidizing. When the amount of Sb (Sb2O3) added increases, during precision press molding, the Sb (Sb2O3) contained in the glass will oxidize the molding surface of the press molding mold. Therefore, during repeated precision press molding, the molding surface deteriorates significantly and precision press molding cannot be performed. In addition, the surface quality of the molded optical element decreases. Sn (SnO2) and Ce (CeO2) have a smaller clarification effect than Sb (Sb2O3). When Ce (CeO2) is added in large quantities, the coloring of the glass is enhanced. Therefore, when adding a clarifier, it is preferred to pay attention to the amount added and add Sb (Sb2O3).
[0140] The content of the clarifier described below is expressed as a value converted into oxides.
[0141] The content of Sb2O3 is expressed as an external addition amount. That is, when the total content of all glass components other than Sb2O3, SnO2 and CeO2 is set to 100 mass%, the content of Sb2O3 is preferably less than 1 mass%, more preferably less than 0.5 mass%, and further preferably less than 0.1 mass%. The content of Sb2O3 may be 0 mass%.
[0142] The content of SnO2 is also expressed by the amount of external addition. That is, when the total content of all glass components other than SnO2, Sb2O3 and CeO2 is set to 100 mass%, the content of SnO2 is preferably less than 2 mass%, more preferably less than 1 mass%, further preferably less than 0.5 mass%, and further preferably less than 0.1 mass%. The content of SnO2 may be 0 mass%. By setting the content of SnO2 to the above range, the clarity of the glass can be improved.
[0143] The content of CeO2 is also expressed by the amount of addition. That is, when the total content of all glass components other than CeO2, Sb2O3, and SnO2 is set to 100 mass%, the content of CeO2 is preferably less than 2 mass%, more preferably less than 1 mass%, further preferably less than 0.5 mass%, and further preferably less than 0.1 mass%. The content of CeO2 may be 0 mass%. By setting the content of CeO2 to the above range, the clarity of the glass can be improved.
[0144] (Glass properties)
[0145] <Refractive index nd>
[0146] In the optical glass of the first embodiment, the refractive index nd is preferably 1.58 or more, more preferably 1.59 or more, and 1.60 or more, in that order.
[0147] <Acid resistance weight reduction rate Da>
[0148] The measurement was carried out according to the provisions of the Japan Optical Glass Industry Association Standard JOGIS06-2009. Specifically, a weight of powdered glass (particle size 425-600 μm) equivalent to the specific gravity was placed in a platinum basket, immersed in a quartz glass round-bottom flask added with a 0.01 mol / L nitric acid aqueous solution, and treated in a boiling water bath for 60 minutes, and the weight reduction rate (%) before and after the treatment was measured. The grades based on the acid resistance weight reduction rate Da are shown in Table 1.
[0149] [Table 1]
[0150] Table 1
[0151] class Weight reduction rate (%) 1 Less than 0.20 2 0.02 or more and less than 0.35 3 0.35 or more and less than 0.65 4 0.65 or more and less than 1.20 5 1.20 or more and less than 2.20 6 2.20 and above
[0152] In the optical glass of the first embodiment, the acid resistance weight reduction rate Da is preferably less than 0.8%, more preferably less than 0.60%, and further preferably less than 0.30%. In addition, the grade thereof is preferably 1 to 4, more preferably 1 to 3, and further preferably 1 to 2. The acid resistance weight reduction rate Da is increased by increasing the total amount [Al 3+ +Ln3+ +Ti 4+ +Zr 4+ +Nb 5+ +Ta 5+ +Bi 3+ +W 6+ ]Thereby being able to reduce.
[0153] <Weather resistance D H >
[0154] The measurement was carried out according to the provisions of the Japan Optical Glass Industry Association standard JOGIS07-2009. Specifically, a 30×30×3mm double-sided polished glass sample was treated for 48 hours under the temperature cycle environment of high temperature and high humidity specified in the above standard, and the haze (%) (scattered light / incident light) at this time was measured. The grades based on the haze are shown in Table 2.
[0155] [Table 2]
[0156] Table 2
[0157] class Haze(%) 1 Less than 2 2 2 or more and less than 10 3 10 or more and less than 20 4 20 or more and less than 30 5 Less than 30
[0158] In the optical glass of the first embodiment, the weather resistance D H Preferably, it is grade 1. Weather resistance D H The haze in the 5 + and B 3+ The total content [P 5+ +B 3+ ] can be reduced by setting it to 30 to 50%.
[0159] <Glass transition temperature Tg>
[0160] The glass transition temperature Tg of the optical glass of the first embodiment is preferably 590° C. or lower, more preferably 570° C. or lower, 560° C. or lower, and 550° C. or lower in this order.
[0161] By satisfying the above range of the upper limit of the glass transition temperature Tg, the rise of the forming temperature and annealing temperature of the glass can be suppressed, and the thermal damage of the press forming equipment and the annealing equipment can be reduced. In addition, by satisfying the above range of the lower limit of the glass transition temperature Tg, it is easy to maintain the thermal stability of the glass well while maintaining the desired Abbe number and refractive index.
[0162] <Light Transmittance of Glass>
[0163] The light transmittance of the optical glass according to the first embodiment can be evaluated by the coloring degrees λ80 and λ5.
[0164] The spectral transmittance of a glass sample having a thickness of 10.0 mm±0.1 mm was measured in the wavelength range of 200 to 700 nm, with the wavelength at which the external transmittance was 80% being λ80 and the wavelength at which the external transmittance was 5% being λ5.
[0165] The λ80 of the optical glass of the first embodiment is preferably 450 nm or less, more preferably 440 nm or less, and further preferably 430 nm or less. In addition, the λ5 is preferably 350 nm or less, more preferably 340 nm or less, and further preferably 330 nm or less.
[0166] <Specific gravity of glass>
[0167] In the optical glass of the first embodiment, the specific gravity is preferably 4.0 or less, and more preferably 3.9 or less, and 3.8 or less. If the specific gravity of the glass is reduced, the weight of the lens can be reduced. As a result, the power consumption of the autofocus drive of the camera lens equipped with the lens can be reduced.
[0168] (Manufacture of optical glass)
[0169] The optical glass of the first embodiment of the present invention can be prepared by mixing glass raw materials in a manner to form the above-mentioned prescribed composition, and using the prepared glass raw materials according to a known glass manufacturing method. For example, a plurality of compounds are mixed and fully mixed to form a batch material, and the batch material is placed in a quartz crucible or a platinum crucible to make a rough melt. The molten material obtained by the rough melting is rapidly cooled and crushed to make cullet. Furthermore, the cullet is placed in a platinum crucible, heated, and remelted to make molten glass, which is then clarified and homogenized, and then the molten glass is formed and slowly cooled to obtain an optical glass. The forming and slow cooling of the molten glass can be applied by known methods.
[0170] In addition, if the desired glass components can be introduced into the glass in a desired content, the compounds used when preparing the batch are not particularly limited, and examples of such compounds include oxides, carbonates, phosphates, nitrates, sulfates, hydroxides, fluorides, chlorides, and the like.
[0171] (Manufacture of optical components, etc.)
[0172] When the optical glass of the first embodiment of the present invention is used to make an optical element, a known method can be used. For example, glass raw materials are melted to make molten glass, and the molten glass is poured into a casting mold to be formed into a plate shape to make a glass material formed by the optical glass of the present invention. The obtained glass material is appropriately cut, ground, and polished to make a cut piece of a size and shape suitable for press molding.
[0173] The slice is heated and softened, and then press-formed (reheat-pressed) by a known method to produce an optical element blank having a shape similar to that of the optical element. The optical element blank can be annealed, ground and polished by a known method to produce an optical element.
[0174] The slices can also be roughly polished (roller polished) to make the weight uniform and make the surface easy to adhere to the release agent, and the reheated and softened glass can be pressed into a shape similar to the desired optical element, and finally ground and polished to produce the optical element.
[0175] Alternatively, a molten glass of a predetermined weight may be separated from a molding die and directly press-molded, and finally ground and polished to produce an optical element.
[0176] The optical functional surface of the manufactured optical element may be coated with an anti-reflection film, a total reflection film, etc. according to the purpose of use.
[0177] Examples of the optical element include various lenses such as a spherical lens, a prism, a diffraction grating, and the like.
[0178] Second Embodiment
[0179] The optical glass according to the second aspect of the present invention is characterized in that:
[0180] The acid resistance weight reduction rate Da based on JOGIS is less than 0.8%,
[0181] The glass transition temperature Tg is below 590°C.
[0182] The Abbe number νd is 40 or more.
[0183] Hereinafter, the optical glass according to the second embodiment will be described in detail.
[0184] In the optical glass of the second embodiment, the acid resistance weight reduction rate Da based on JOGIS is less than 0.8%. The acid resistance weight reduction rate Da is preferably less than 0.60%, and more preferably less than 0.30%. In addition, its grade is preferably 1 to 4 grades, more preferably 1 to 3 grades, and further preferably 1 to 2 grades. The acid resistance weight reduction rate Da is increased by increasing the total amount [Al 3+ +Ln 3+ +Ti 4+ +Zr 4+ +Nb 5+ +Ta 5+ +Bi 3+ +W 6+ ]Thereby being able to reduce.
[0185] The acid-resistant weight reduction rate Da of the optical glass of the second embodiment can be measured by the same method as that of the first embodiment.
[0186] In the optical glass of the second embodiment, the glass transition temperature Tg is 590° C. or lower. The glass transition temperature Tg is preferably 570° C. or lower, more preferably 560° C. or lower, and particularly preferably 550° C. or lower.
[0187] In the optical glass of the second embodiment, the Abbe number νd is not less than 40. The Abbe number νd may be in the range of 40 to 65. The Abbe number νd is determined by, for example, 3+ , Ln 3+ 、Ti 4+ 、Zr 4+ , Nb 5+ 、 5+ 、Bi 3+ and W 6+ Total content [Al 3+ +Ln 3+ +Ti 4 + +Zr 4+ +Nb 5+ +Ta 5+ +Bi 3+ +W 6+ ] Increase Al 3+ The ratio of can be increased, and in addition, by reducing Al 3+ The ratio can thus be reduced.
[0188] (Glass composition)
[0189] Hereinafter, the glass components of the optical glass according to the second embodiment will be described in detail.
[0190] The optical glass of the second embodiment may contain a selected from Li + 、Na + and K + One or more alkali metal ions, P 5+ , B 3+ And Ba 2+ The optical glass preferably contains P as a network forming component of the glass. 5+ Phosphate glass as the main component. 5+ and B 3+ As a glass component, the devitrification resistance is improved. In addition, by including alkali metal ions, the devitrification resistance and thermal stability of the glass are improved, and the glass transition temperature is reduced. Here, the alkali metal ion is Li + 、Na + , K + Furthermore, by including Ba 2+, thereby suppressing the decrease in the refractive index nd and also suppressing the devitrification during vitrification.
[0191] In the optical glass of the second embodiment, Al 3+ , Ln 3+ 、Ti 4+ 、Zr 4+ , Nb 5+ 、 5+ 、Bi 3+ and W 6+ Total content [Al 3+ +Ln 3+ +Ti 4+ +Zr 4+ +Nb 5+ +Ta 5+ +Bi 3+ +W 6+ The lower limit of ] is preferably 10%, and more preferably 12%, 15%, and 18%, respectively.
[0192] Here, Ln 3+ Indicates La 3+ , Gd 3+ , Y 3+ , Yb 3+ Lu 3+ Total content [La 3+ +Gd 3+ +Y 3+ +Yb 3+ +Lu 3+ ].
[0193] Al 3+ , Ln 3+ 、Ti 4+ 、Zr 4+ , Nb 5+ 、 5+ 、Bi 3+ and W 6+ It is a component that helps to improve acid resistance. Figure 1 As shown, with the total content [Al 3+ +Ln 3+ +Ti 4+ +Zr 4+ +Nb 5+ +Ta 5+ +Bi 3+ +W 6+ ] increases, the acid resistance weight reduction rate Da decreases. Therefore, it is preferred to increase the total content [Al 3+ +Ln 3+ +Ti 4+ +Zr 4+ +Nb 5+ +Ta 5++Bi 3+ +W 6+ ] is set to the above range.
[0194] In the optical glass of the second embodiment, P 5+ and B 3+ The total content [P 5+ +B 3+ ] is preferably 30 to 50%, more preferably 32 to 48%, further preferably 34 to 46%, and particularly preferably 36 to 45%.
[0195] Furthermore, in the optical glass of the second embodiment, P 5+ The content of P 5+ and B 3+ The total cation content ratio [P 5+ / (P 5+ +B 3+ )] is preferably 0.50 or more and 0.84 or less, and the cation ratio [P 5+ / (P 5+ +B 3+ The lower limit of the cation ratio [P 5+ / (P 5+ +B 3+ The upper limit of )] is more preferably 0.83, and further preferably 0.82.
[0196] When containing P 5+ and B 3+ When used as a network-forming component of glass, it can improve the resistance to devitrification, but when contained in excessive amounts, weather resistance deteriorates. 5+ The ratio of is set to a predetermined range, thereby further improving the resistance to devitrification. Therefore, it is preferred to set the total content [P 5+ +B 3+ ] and cation ratio [P 5+ / (P 5+ +B 3+ )] is set to the above range.
[0197] In the optical glass of the second embodiment, Li + 、Na + and K + Total content [Li + +Na + +K + ] is preferably 5% or more, and more preferably 6%, 8%, and 10% in that order. + +Na + +K +The upper limit of ] is preferably 30%, and more preferably 28%, 26%, and 25%. + 、Na + and K + All of them have the effect of improving the thermal stability of glass and lowering the glass transition temperature Tg. On the other hand, when their total content increases, the acid resistance decreases. Therefore, it is preferred to increase the total content [Li + +Na + +K + ] is set to the above range.
[0198] In the optical glass of the second embodiment, Ba 2+ The lower limit of the content of Ba is preferably 5%, and more preferably 7%, 9%, 11%, and 13%. 2+ The upper limit of the content of is preferably 30%, and more preferably 28%, 26%, and 24%, respectively.
[0199] By placing Ba 2+ By setting the content of MgO to the above range, a decrease in the refractive index nd can be suppressed, and devitrification during vitrification can be suppressed.
[0200] In the optical glass of the second embodiment, Mg 2+ , Ca 2+ , Sr 2+ And Ba 2+ Total content [Mg 2+ +Ca 2+ +Sr 2+ +Ba 2+ The lower limit of ] is preferably 10%, and more preferably 15%, 16%, 17%, and 18%. 2+ +Ca 2+ +Sr 2+ +Ba 2+ The upper limit of Mg is preferably 40%, and more preferably 38%, 36%, and 35%. 2+ , Ca 2+ , Sr 2+ And Ba 2+ All of them are glass components that have the effect of improving the acid resistance, thermal stability and resistance to devitrification of glass. 2+ +Ca 2+ +Sr 2+ +Ba 2+ ] is set to 10% or more, thereby improving the acid resistance, thermal stability and devitrification resistance of the glass. On the other hand, when the content of these glass components increases, the thermal stability and devitrification resistance of the glass decrease. Therefore, from the perspective of maintaining thermal stability and devitrification resistance, the total content [Mg 2+ +Ca2+ +Sr 2+ +Ba 2+ ] is preferably within the above range.
[0201] In the optical glass of the second embodiment, the contents and ratios of the glass components other than those described above and other components can be set in the same manner as in the first embodiment.
[0202] (Glass properties)
[0203] <Refractive index nd>
[0204] In the optical glass of the second embodiment, the refractive index nd is preferably 1.58 or more, more preferably 1.59 or more, and 1.60 or more, in that order.
[0205] <Weather resistance D H >
[0206] In the optical glass of the second embodiment, the weather resistance D H Preferably, it is grade 1. Weather resistance D H The haze in the 5 + and B 3+ The total content [P 5+ +B 3+ ] can be reduced by setting it to 30 to 50%.
[0207] Weather resistance D of the optical glass of the second embodiment H The measurement can be performed by the same method as in the first embodiment.
[0208] <Light Transmittance of Glass>
[0209] The λ80 of the optical glass of the second embodiment is preferably 450 nm or less, more preferably 440 nm or less, and further preferably 430 nm or less. In addition, the λ5 is preferably 350 nm or less, more preferably 340 nm or less, and further preferably 330 nm or less.
[0210] The λ80 and λ5 of the optical glass of the second embodiment can be measured by the same method as that of the first embodiment.
[0211] <Specific gravity of glass>
[0212] In the optical glass of the second embodiment, the specific gravity is preferably 4.0 or less, and more preferably 3.9 or less, and 3.8 or less. If the specific gravity of the glass is reduced, the weight of the lens can be reduced. As a result, the power consumption of the autofocus drive of the camera lens equipped with the lens can be reduced.
[0213] The production of the optical glass and the production of the optical element and the like according to the second embodiment can be performed in the same manner as in the first embodiment.
[0214] [Example]
[0215] Hereinafter, the present invention will be described in further detail based on examples; however, the present invention is not limited to these examples.
[0216] (Example 1)
[0217] Glass samples having the glass compositions shown in Tables 3 to 6 were prepared according to the following procedures and subjected to various evaluations.
[0218] In addition, in Tables 3 to 6, the glass compositions are expressed in terms of cation %, and the total amount of anionic components in any composition is 0 2- That is, in the compositions described in Tables 3 to 6, O 2- The content of each is 100 anion%.
[0219] [Manufacture of optical glass]
[0220] Prepare oxides, hydroxides, carbonates and nitrates corresponding to the constituent components of the glass as raw materials, weigh and mix the raw materials so that the glass composition of the obtained optical glass becomes the compositions shown in Tables 3 to 6, and mix the raw materials thoroughly. Put the obtained prepared raw materials (batch materials) into a platinum crucible, heat at 1000°C to 1400°C for 2 hours to make molten glass, stir to achieve homogenization, clarify, and cast the molten glass into a mold preheated at an appropriate temperature. Heat treat the cast glass near the glass transition temperature Tg, and cool it to room temperature in a furnace to obtain a glass sample.
[0221] [Confirmation of glass composition]
[0222] The content of each glass component of the obtained glass sample was measured by inductively coupled plasma atomic emission spectrometry (ICP-AES), and it was confirmed that the composition was as shown in Tables 3 to 6.
[0223] [Determination of acid resistance weight reduction rate Da]
[0224] According to the Japanese Optical Glass Industry Association Standard JOGIS06-2009, the obtained glass sample was made into powder glass (particle size 425-600 μm) with a weight equivalent to the specific gravity, placed in a platinum basket, immersed in a quartz glass round-bottom flask added with a 0.01 mol / L nitric acid aqueous solution, and treated in a boiling water bath for 60 minutes. The weight reduction rate (%) before and after the treatment was measured. The results are shown in Tables 7 and 8.
[0225] [Weather resistance D HDetermination of
[0226] According to the Japanese Optical Glass Industry Association specification JOGIS07-2009, the obtained glass sample was double-sided polished with a size of 30×30×3 mm, and treated for 48 hours in a high temperature and high humidity high temperature cycle environment specified in the above specification, and the haze (%) (scattered light / incident light) at this time was measured. The results are shown in Tables 7 and 8.
[0227] [Measurement of optical properties]
[0228] The obtained glass sample was further annealed at about 30 minutes to about 2 hours near the glass transition temperature Tg, and then cooled to room temperature in a furnace at a temperature drop rate of -30°C / hour to obtain an annealed sample. The refractive index nd, Abbe number νd, specific gravity, glass transition temperature Tg, λ80 and λ5 of the obtained annealed sample were measured. The results are shown in Tables 7 and 8.
[0229] (i) Refractive index nd and Abbe number νd
[0230] The refractive indices nd, ng, nF, and nC of the annealed sample were measured by the refractive index measurement method of JIS standard JIS B 7071-1, and the Abbe number νd was calculated based on the following formula (1).
[0231] νd=(nd-1) / (nF-nC)···(1)
[0232] (ii) Specific gravity
[0233] The specific gravity was measured by the Archimedean method.
[0234] (iii) Glass transition temperature Tg
[0235] The glass transition temperature Tg was measured at a heating rate of 10° C. / min using a differential scanning calorimeter (DSC3300SA) manufactured by NETZSCH JAPAN.
[0236] (iv)λ80、λ5
[0237] The annealed sample was processed to have a thickness of 10 mm and parallel optically polished planes, and the spectral transmittance in the wavelength range of 280 nm to 700 nm was measured. The intensity of the light incident vertically on one optically polished plane was set as intensity A, and the intensity of the light emitted from the other plane was set as intensity B, and the spectral transmittance B / A was calculated. The wavelength at which the spectral transmittance was 80% was set as λ80, and the wavelength at which the spectral transmittance was 5% was set as λ5. In addition, the spectral transmittance also includes the reflection loss of the light on the sample surface.
[0238] [Table 3]
[0239]
[0240] [Table 4]
[0241]
[0242] [Table 5]
[0243]
[0244] [Table 6]
[0245]
[0246] [Table 7]
[0247]
[0248] [Table 8]
[0249]
[0250] In samples No. 5 to 45, optical glasses with excellent acid resistance and weather resistance were obtained. On the other hand, in sample No. 1, crystals were generated and λ80 and λ5 could not be measured. In addition, it was found that the weather resistance D H The value of is high, and the weather resistance is poor. In sample No. 2, many crystals are produced and devitrification occurs, so the refractive index nd, Abbe number νd, λ80 and λ5 cannot be measured. In samples No. 3 and 4, it can be seen that the value of the acid resistance weight reduction rate Da is high, and the acid resistance is poor.
[0251] (Example 2)
[0252] Glass samples having the glass compositions shown in Tables 9 and 10 were prepared in the same manner as in Example 1, and various evaluations were performed in the same manner as in Example 1. The results are shown in Table 11.
[0253] [Table 9]
[0254]
[0255] [Table 10]
[0256]
[0257] [Table 11]
[0258]
[0259] In addition, a glass sample having a composition in which 250 mass ppm of Sb2O3 was further added to the glass composition shown in Tables 3 and 4 was prepared in the same manner as in Example 1, and various evaluations were performed in the same manner as in Example 1. As a result, the same properties and evaluation results as those of the glass sample in Example 1 were obtained.
[0260] (Example 3)
[0261] Using the glass samples obtained in Examples 1 and 2, a preform for precision press molding was prepared by a known method. The obtained preform was heated and softened in a nitrogen atmosphere, and precision press molded using a press mold to mold the optical glass into the shape of an aspheric lens. Then, the molded optical glass was taken out from the press mold, annealed, and centered and edged to obtain an aspheric lens.
[0262] (Example 4)
[0263] The glass samples obtained in Examples 1 and 2 were cut and ground to produce slices. The slices were pressed and molded by reheat pressing to produce optical element blanks. The optical element blanks were precision annealed, and the refractive index was precisely adjusted to a desired refractive index, and then ground and polished by a known method to obtain various lenses such as biconvex lenses, biconcave lenses, plano-convex lenses, plano-concave lenses, concave meniscus lenses, and convex meniscus lenses.
[0264] The embodiments disclosed this time should be understood to be illustrative in all respects and not restrictive. The scope of the present invention is indicated by the claims rather than the above description, and includes all modifications within the scope equivalent to the claims and the scope.
[0265] For example, the optical glass of one embodiment of the present invention can be produced by adjusting the composition described in the specification to the glass composition exemplified above.
[0266] Furthermore, it is of course possible to arbitrarily combine two or more items described as examples or preferred ranges in the specification.
Claims
1. An optical glass comprising Li + 、Na + and K + One or more alkali metal ions and P 5+ , B 3+ And Ba 2+ Phosphate glass as a cationic component, Al 3+ , Ln 3+ 、Ti 4+ 、Zr 4+ , Nb 5+ 、 5+ 、Bi 3+ and W 6+ Total content [Al 3+ +Ln 3+ +Ti 4+ +Zr 4+ +Nb 5+ +Ta 5+ +Bi 3 + +W 6+ ] is 12 cation % or more, wherein, Ln 3+ Indicates La 3+ , Gd 3+ , Y 3+ , Yb 3+ Lu 3+ Total content [La 3+ +Gd 3+ +Y 3+ +Yb 3+ +Lu 3+ ], P 5+ and B 3+ The total content [P 5+ +B 3+ ] is 30 to 50 cation%, P 5+ The content of P 5+ and B 3+ The total cation content ratio [P 5+ / (P 5+ +B 3+ )] is 0.50 or more and 0.84 or less, Li + 、Na + and K + Total content [Li + +Na + +K + ] is 10 cation % or more, Ba 2+ The content of cationic is 5% or more, Mg 2+ , Ca 2+ , Sr 2+ And Ba 2+ Total content [Mg 2+ +Ca 2+ +Sr 2+ +Ba 2+ ] is 10 cation % or more, La 3+ , Gd 3+ , Y 3+ , Yb 3+ Lu 3+ Total content [La 3+ +Gd 3+ +Y 3+ +Yb 3+ +Lu 3+ ] is less than 5 cation %, Al 3+ The content of Al 3+ , Ln 3+ 、Ti 4+ 、Zr 4+ , Nb 5+ 、 5+ 、Bi 3+ and W 6+ The total content of cations is [Al 3+ / (Al 3+ +Ln 3+ +Ti 4+ +Zr 4+ +Nb 5+ +Ta 5+ +Bi 3+ +W 6+ )] is 0.4 or more, The Abbe number νd is 40 or more, O as anion component 2- The content is 95 anion % or more and 100 anion % or less.
2. The optical glass according to claim 1, wherein: P 5+ The content of cations is 20-40%, B 3+ The content of cations is 4-15%, Li + The content is 5 to 30 cation %.
3. The optical glass according to claim 1 or 2, wherein: The acid resistance weight reduction rate Da based on JOGIS is less than 0.8%.
4. The optical glass according to claim 1 or 2, wherein: The acid resistance based on JOGIS is 1 to 3 levels.
5. The optical glass according to claim 1 or 2, wherein: Weather resistance D based on JOGIS H It is level 1.
6. The optical glass according to claim 1 or 2, wherein: The glass transition temperature Tg is 590°C or lower.
7. An optical glass, wherein: Li + 、Na + and K + Total content [Li + +Na + +K + ] is 10 cation % or more, P 5+ The content of P 5+ and B 3+ The total cation content ratio [P 5+ / (P 5+ +B 3+ )] is 0.50~0.84, La 3+ , Gd 3+ , Y 3+ , Yb 3+ Lu 3+ Total content [La 3+ +Gd 3+ +Y 3+ +Yb 3+ +Lu 3+ ] is less than 5 cation %, The acid resistance weight reduction rate Da based on JOGIS is less than 0.8%, The glass transition temperature Tg is below 590°C. The Abbe number νd is 40 or more, P 5+ and B 3+ The total content [P 5+ +B 3+ ] is 30 to 50 cation%, Al 3+ , Ln 3+ 、Ti 4+ 、Zr 4+ , Nb 5+ 、 5+ 、Bi 3+ and W 6+ Total content [Al 3+ +Ln 3+ +Ti 4+ +Zr 4+ +Nb 5+ +Ta 5+ +Bi 3 + +W 6+ ] is 12 cation % or more, among which Ln 3+ Indicates La 3+ , Gd 3+ , Y 3+ , Yb 3+ Lu 3+ Total content [La 3+ +Gd 3+ +Y 3+ +Yb 3+ +Lu 3+ ], Al 3+ The content of Al 3+ , Ln 3+ 、Ti 4+ 、Zr 4+ , Nb 5+ 、 5+ 、Bi 3+ and W 6+ The total content of cations is [Al 3+ / (Al 3+ +Ln 3+ +Ti 4+ +Zr 4+ +Nb 5+ +Ta 5+ +Bi 3+ +W 6+ )] is 0.4 or more, O as anion component 2- The content is 95 anion % or more and 100 anion % or less.
8. The optical glass according to claim 7, wherein: P 5+ The content of cations is 20-40%, B 3+ The content of cations is 4-15%, Li + The content is 5 to 30 cation %.
9. The optical glass according to claim 7 or 8, wherein: The acid resistance weight reduction rate Da based on JOGIS is less than 0.8%.
10. The optical glass according to claim 7 or 8, wherein: The acid resistance based on JOGIS is 1 to 3 levels.
11. The optical glass according to claim 7 or 8, wherein: Weather resistance D based on JOGIS H It is level 1. 12 . An optical element formed of the optical glass according to claim 1 .
Citation Information
Patent Citations
Optical glass and optical elements
JP2016533312A
Optical glass, optical element and performing object
CN103058515A
Optical glass, optical element and perform
CN103420611A
Phosphoric acid optical glass
JP1988011544A
Optical glass for mold press
JP1997278479A