Lightweight, oil-resistant, and anti-skid foamed sole and preparation method thereof
By using a combination of specific nanofillers and accelerators in the soles, combined with nitrile rubber and foaming agent, the existing anti-slip oil-resistant shoes have solved the problems of complex process, high price and limited application environment, and the production is excellent and light in performance. The anti-slip sole is suitable for places with severe oil pollution and meets the needs of high oil resistance and anti-slip.
Patent Information
- Application Number
- CN202210384042.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-04-13
AI Technical Summary
The manufacturing process of anti-slip and oil-resistant shoes on the existing market is complex, expensive and has limited applicable environments. In order to be light, the sole density is often required, which leads to light weight but has a large safety hazard, especially in environments such as kitchens with severe water and oil pollution. slip.
Nanofillers (concave and convex rod soil, asbestos fiber, mica powder) and accelerators (fat alcohol polyoxyethylene ether sodium sulfate, stearic acid, dimethylsiloxane) are used to foam with nitrile rubber and azodiformamide The agent and crosslinking agent BIBP are prepared by intensive refining and double-rolling mixing machine to prepare lightweight oil-resistant and anti-slip foamed sole to improve its oil resistance and anti-slip properties.
The lightweight oil-resistant and anti-slip foamed sole prepared has an anti-slip coefficient of more than 0.32 on the oil-contaminated interface, which has better performance than the existing technology, and has a weight smaller than that of the oil-resistant and anti-slip sole sold on the market. It is suitable for environments with severe oil-contaminated conditions, such as kitchens and ships. Ship, petrochemical plants, etc., and the process is simple and easy to industrially produce.
Smart Images

Figure BDA0003593988830000011 
Figure BDA0003593988830000021 
Figure BDA0003593988830000041
Abstract
Description
Technical Field
[0001] The invention belongs to the field of foamed sole preparation, and in particular relates to a lightweight, oil-resistant and anti-skid foamed sole and a preparation method thereof. Background Art
[0002] Nowadays, when people buy shoes, they no longer just consider the appearance of the shoes, but also focus on the safety of the shoes, especially the anti-slip performance is particularly important. Catering industry workers walk in and out of the kitchen for a long time, and there are often a lot of liquid media such as water and oil left on the floor of the kitchen, which reduces the friction between the soles of the shoes and the ground. It can be said that the friction is almost zero. At this time, people can easily slip and have accidents, posing a great safety hazard.
[0003] At present, the anti-slip and oil-resistant shoes on the market are not only complicated in manufacturing process, but also several times more expensive than ordinary shoes, and the applicable environment is very limited. In addition, in order to be light when working, the density of the sole is often required to be small, so that the weight of the shoes will be reduced and convenient for movement. Summary of the invention
[0004] The object of the present invention is to overcome the disadvantages of the prior art and provide a lightweight, oil-resistant and non-slip foamed sole. Another object of the present invention is to provide a method for preparing the foamed sole.
[0005] The present invention adopts the following technical solution:
[0006] A lightweight, oil-resistant, and anti-skid foamed sole comprises the following raw materials in parts by weight:
[0007]
[0008]
[0009] The nano filler is composed of attapulgite, asbestos fiber and mica powder in a mass ratio of 1:2-3:1.5-2.2.
[0010] Furthermore, the accelerator is composed of sodium fatty alcohol polyoxyethylene ether sulfate, stearic acid, and dimethylsiloxane in a mass ratio of 0.27-0.36:1:1.27-1.49.
[0011] Furthermore, the foaming agent is azodicarbonamide.
[0012] Furthermore, the cross-linking agent is cross-linking agent BIBP.
[0013] Furthermore, the acrylonitrile content in the nitrile rubber is 18-24%.
[0014] A method for preparing a lightweight, oil-resistant, and non-slip rubber foam sole comprises the following steps:
[0015] Step 1: First, put the raw materials except the foaming agent, accelerator and cross-linking agent into an internal mixer for internal mixing. When the internal mixing temperature reaches 112-115°C, remove the glue and place at room temperature for more than 24 hours.
[0016] Step 2, mixing the mixture after banburying on a double-roll mill, adding accurately weighed foaming agent, accelerator, and crosslinking agent, and mixing the materials evenly into sheets to obtain a foamed sheet;
[0017] Step 3, cutting the foamed sheet into the shape of a sole and putting it into a sole mold for foaming and molding, the foaming temperature is 145-155° C., and the lightweight, oil-resistant and non-slip foamed sole is obtained.
[0018] Furthermore, in step one, the banburying process specifically includes: firstly, ethylene-vinyl acetate copolymer, maleic anhydride grafted EVA, SBS thermoplastic elastomer and nitrile rubber are mixed and put into a banburying mixer for banburying, and the mixture is mixed and banburying for 15 minutes; then, the raw materials other than the foaming agent, the accelerator and the cross-linking agent are added and mixed and banburying for 10 minutes; then, the banburying temperature is adjusted to 90°C, and the mixture is turned over once after being kept for 5 minutes; when the banburying temperature rises to 98°C, the mixture is turned over twice; when the banburying temperature rises to 103°C, the mixture is turned over three times; when the banburying temperature rises to 108°C, the mixture is turned over four times; when the banburying temperature rises to 112-115°C, the mixture is turned over five times, and then the mixture is banburying for 2 minutes, the glue is discharged, and the mixture is placed at room temperature for more than 24 hours.
[0019] Furthermore, in step 2, the EVA foam sheet is thinned at least twice in a double-roll mill to produce a sheet with a thickness of 2-3 mm.
[0020] It can be seen from the above description of the present invention that, compared with the prior art, the present invention has the following beneficial effects:
[0021] First, the present application specifies that ethylene-vinyl acetate copolymer, nitrile rubber, and SBS thermoplastic elastomer are mixed with each other, and maleic anhydride grafted EVA is added to increase the compatibility and adhesion between the raw materials, so as to improve the oil resistance and anti-skid properties of the foamed sole, and ensure the overall mechanical properties of the foamed sole; wherein, mica powder is added as a partial filler, and the mica powder has strong adhesion and plays a gripping role. When combined with nitrile rubber, it can improve the oil resistance and anti-skid properties at the same time, so that the prepared sole has an anti-skid coefficient of 0.32 or more on the oil-contaminated interface;
[0022] Second, the addition of nitrile rubber will lead to a large shrinkage rate during the molding of the foamed sole. By adding SBS thermoplastic elastomer, combined with attapulgite powder and asbestos fiber as fillers, the shrinkage rate during the molding of the foamed sole can be effectively reduced, thereby ensuring the overall mechanical properties of the foamed sole; and asbestos fiber is a very good lightweight material, which can effectively reduce the overall density of the foamed sole and reduce the quality of the foamed sole when combined with SBS thermoplastic elastomer to meet the use requirements;
[0023] Third, a compound of sodium fatty alcohol polyoxyethylene ether sulfate, stearic acid, and dimethylsiloxane is limited as an accelerator and combined with a foaming agent to make the vulcanization rate of the rubber roughly synchronized with the foaming rate to obtain a uniform closed-cell structure, and the formed closed-cell structure is independent of each other, and the bubbles are not connected to each other, so that the foamed sole has better mechanical properties. DETAILED DESCRIPTION
[0024] The present invention is further described below through specific implementation modes.
[0025] A lightweight, oil-resistant, and anti-skid foamed sole comprises the following raw materials in parts by weight:
[0026]
[0027] The nanofiller is composed of attapulgite, asbestos fiber and mica powder in a mass ratio of 1:2-3:1.5-2.2; the accelerator is composed of sodium fatty alcohol polyoxyethylene ether sulfate, stearic acid and dimethylsiloxane in a mass ratio of 0.27-0.36:1:1.27-1.49; the foaming agent is azodicarbonamide; the crosslinking agent is crosslinking agent BIBP; and the acrylonitrile content in the nitrile rubber is 18-24%.
[0028] The preparation method thereof comprises the following steps:
[0029] Step 1: first, mix ethylene-vinyl acetate copolymer, maleic anhydride grafted EVA, SBS thermoplastic elastomer and nitrile rubber into a mixer and mix and mix for 15 minutes; then continue to add raw materials except foaming agent, accelerator and cross-linking agent and mix and mix for 10 minutes; then adjust the mixing temperature to 90°C, keep it for 5 minutes and then turn the material once; when the mixing temperature rises to 98°C, turn the material twice; when the mixing temperature rises to 103°C, turn the material three times; when the mixing temperature rises to 108°C, turn the material four times; when the mixing temperature rises to 112-115°C, turn the material five times, mix for 2 minutes, discharge the glue, and leave it at room temperature for more than 24 hours;
[0030] Step 2, mixing the mixture after banburying on a double-roll mill, adding accurately weighed foaming agent, accelerator, and crosslinking agent, and mixing the materials evenly into sheets to obtain a foamed sheet;
[0031] Step 3, cutting the foamed sheet into the shape of a sole and putting it into a sole mold for foaming and molding, the foaming temperature is 145-155° C., and the lightweight, oil-resistant and non-slip foamed sole is obtained.
[0032] The EVA foam sheet is thinned at least twice in a double-roll mill and is produced with a thickness of 2-3 mm.
[0033] Example 1
[0034] A lightweight, oil-resistant, and anti-skid foamed sole comprises the following raw materials in parts by weight:
[0035]
[0036] The nano filler is composed of attapulgite, asbestos fiber and mica powder in a mass ratio of 1:2:1.5; the accelerator is composed of sodium sulfate of fatty alcohol polyoxyethylene ether, stearic acid and dimethylsiloxane in a mass ratio of 0.27:1:1.49; and the acrylonitrile content in the nitrile rubber is 18-24%.
[0037] The preparation method thereof comprises the following steps:
[0038] Step 1: first, mix ethylene-vinyl acetate copolymer, maleic anhydride grafted EVA, SBS thermoplastic elastomer and nitrile rubber into a mixer and mix and mix for 15 minutes; then continue to add raw materials except foaming agent, accelerator and cross-linking agent and mix and mix for 10 minutes; then adjust the mixing temperature to 90°C, keep it for 5 minutes and then turn the material once; when the mixing temperature rises to 98°C, turn the material twice; when the mixing temperature rises to 103°C, turn the material three times; when the mixing temperature rises to 108°C, turn the material four times; when the mixing temperature rises to 112°C, turn the material five times, mix for 2 minutes, discharge the glue, and leave it at room temperature for more than 24 hours;
[0039] Step 2, mixing the mixture after banburying on a double-roll mill, adding accurately weighed foaming agent, accelerator, and crosslinking agent, and mixing the materials evenly into sheets to obtain a foamed sheet;
[0040] Step three, cutting the foamed sheet into the shape of a sole and putting it into a sole mold for foaming and molding, the foaming temperature is 145° C., and the lightweight, oil-resistant and non-slip foamed sole is obtained.
[0041] The EVA foam sheet is thinned at least twice in a double-roll mill and is produced into a sheet with a thickness of 2 mm.
[0042] Example 2
[0043] A lightweight, oil-resistant, and anti-skid foamed sole comprises the following raw materials in parts by weight:
[0044]
[0045] The nano filler is composed of attapulgite, asbestos fiber and mica powder in a mass ratio of 1:3:2.2; the accelerator is composed of sodium sulfate of fatty alcohol polyoxyethylene ether, stearic acid and dimethylsiloxane in a mass ratio of 0.36:1:1.27; and the acrylonitrile content in the nitrile rubber is 18-24%.
[0046] The preparation method thereof comprises the following steps:
[0047] Step 1: first, mix ethylene-vinyl acetate copolymer, maleic anhydride grafted EVA, SBS thermoplastic elastomer and nitrile rubber into a mixer and mix and mix for 15 minutes; then continue to add raw materials except foaming agent, accelerator and cross-linking agent and mix and mix for 10 minutes; then adjust the mixing temperature to 90°C, keep it for 5 minutes and then turn the material once; when the mixing temperature rises to 98°C, turn the material twice; when the mixing temperature rises to 103°C, turn the material three times; when the mixing temperature rises to 108°C, turn the material four times; when the mixing temperature rises to 115°C, turn the material five times, mix for 2 minutes, discharge the glue, and leave it at room temperature for more than 24 hours;
[0048] Step 2, mixing the mixture after banburying on a double-roll mill, adding accurately weighed foaming agent, accelerator, and crosslinking agent, and mixing the materials evenly into sheets to obtain a foamed sheet;
[0049] Step three, cutting the foamed sheet into the shape of a sole and putting it into a sole mold for foaming and molding, the foaming temperature is 155° C., and the lightweight, oil-resistant and non-slip foamed sole is obtained.
[0050] The EVA foam sheet is thinned at least twice in a double-roll mill and is produced into a sheet with a thickness of 3 mm.
[0051] Example 3
[0052] A lightweight, oil-resistant, and anti-skid foamed sole comprises the following raw materials in parts by weight:
[0053]
[0054]
[0055] The nano filler is composed of attapulgite, asbestos fiber and mica powder in a mass ratio of 1:2.6:1.8; the accelerator is composed of sodium sulfate of fatty alcohol polyoxyethylene ether, stearic acid and dimethylsiloxane in a mass ratio of 0.32:1:1.35; and the acrylonitrile content in the nitrile rubber is 18-24%.
[0056] The preparation method thereof comprises the following steps:
[0057] Step 1: first, mix ethylene-vinyl acetate copolymer, maleic anhydride grafted EVA, SBS thermoplastic elastomer and nitrile rubber into a mixer and mix and mix for 15 minutes; then continue to add raw materials except foaming agent, accelerator and cross-linking agent and mix and mix for 10 minutes; then adjust the mixing temperature to 90°C, keep it for 5 minutes and then turn the material once; when the mixing temperature rises to 98°C, turn the material twice; when the mixing temperature rises to 103°C, turn the material three times; when the mixing temperature rises to 108°C, turn the material four times; when the mixing temperature rises to 113°C, turn the material five times, mix for 2 minutes, discharge the glue, and leave it at room temperature for more than 24 hours;
[0058] Step 2, mixing the mixture after banburying on a double-roll mill, adding accurately weighed foaming agent, accelerator, and crosslinking agent, and mixing the materials evenly into sheets to obtain a foamed sheet;
[0059] Step three, cutting the foamed sheet into the shape of a sole and putting it into a sole mold for foaming and molding, the foaming temperature is 150° C., and the lightweight, oil-resistant and non-slip foamed sole is obtained.
[0060] The EVA foam sheet is thinned at least twice in a double-roll mill and is produced into a sheet with a thickness of 2 mm.
[0061] The commercially available oil-resistant and non-slip foamed sole was used as comparative example 1, the commercially available oil-resistant and non-slip rubber sole was used as comparative example 2, and the oil-resistant and non-slip foamed soles prepared in Examples 1 to 3 were tested accordingly to obtain the following data:
[0062] Among them, the oil resistance test is tested according to ISO20344:2011; the static anti-slip coefficient is tested according to F1677:2005, and the dynamic anti-slip coefficient is tested according to ISO13287:2012 SRB mode (glycerol solution is dripped on the steel plate)
[0063] Table 1 Test data of each embodiment
[0064] project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 <![CDATA[Density (g / cm 3 )]]> 0.76 0.75 0.74 0.91 1.19 Oil resistance test (%) 4.7 9.5 3.3 11.0 9.8 Static anti-slip coefficient (high oil) 0.58 0.57 0.59 0.42 0.47 Static anti-slip coefficient (high oil and water) 0.58 0.56 0.58 0.40 0.44 Dynamic anti-slip coefficient (heel) 0.33 0.34 0.35 0.15 0.18 Dynamic anti-slip coefficient (smooth) 0.34 0.35 0.37 0.21 0.23
[0065] It can be seen from the above table that the oil resistance and anti-skid performance of the lightweight oil-resistant and anti-skid foamed sole prepared in the present application are slightly higher than those of the oil-resistant and anti-skid soles sold in the prior art, and the weight is much smaller than that of the oil-resistant and anti-skid soles sold in the prior art, and can be worn and used in places with high requirements for oil resistance and anti-skid performance, such as on ships, petrochemical plants, automobile repair shops, grease factories and other places with oil accumulation or oil splashing; and the production process is simple, easy to industrialize production, and has a good market prospect.
[0066] The present application stipulates that ethylene-vinyl acetate copolymer, nitrile rubber, and SBS thermoplastic elastomer are mixed with each other, and maleic anhydride grafted EVA is added to increase the compatibility and adhesion between the raw materials, so as to improve the oil resistance and anti-skid properties of the prepared foamed sole and ensure the overall mechanical properties of the foamed sole; wherein, mica powder is added as a partial filler, and the mica powder has strong adhesion and plays a gripping role. When combined with nitrile rubber, it can improve the oil resistance and anti-skid properties at the same time, so that the prepared sole has an anti-skid coefficient of more than 0.32 on the oil-contaminated interface.
[0067] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of implementation of the present invention. That is, equivalent changes and modifications made according to the scope of the patent application of the present invention and the contents of the specification should still fall within the scope covered by the patent of the present invention.
Claims
1. A lightweight, oil-resistant, non-slip foam sole, characterized in that: The invention comprises the following raw materials in parts by weight: 30-40 parts of ethylene-vinyl acetate copolymer Maleic anhydride grafted EVA 20-30 parts 15-22 parts of nitrile rubber SBS thermoplastic elastomer 10-15 parts Foaming agent 1.3-1.8 parts Accelerator 1.1-1.3 parts Crosslinking agent 1.0-1.2 parts Nano filler 5-10 parts Zinc stearate 1.0-1.2 parts 5-10 parts of naphthenic oil; The nano filler is composed of attapulgite, asbestos fiber and mica powder in a mass ratio of 1:2-3:1.5-2.2; The accelerator is composed of sodium fatty alcohol polyoxyethylene ether sulfate, stearic acid, and dimethyl siloxane in a mass ratio of 0.27-0.36:1:1.27-1.49; The preparation method thereof comprises the following steps: Step 1: First, put the raw materials except the foaming agent, accelerator and cross-linking agent into an internal mixer for internal mixing. When the internal mixing temperature reaches 112-115°C, remove the glue and place at room temperature for more than 24 hours. Step 2, mixing the mixture after banburying on a double-roll mill, adding accurately weighed foaming agent, accelerator, and crosslinking agent, and mixing the materials evenly into sheets to obtain a foamed sheet; Step three, cutting the foamed sheet into the shape of a sole and putting it into a sole mold for foaming and molding, the foaming temperature is 145-155° C., and the lightweight, oil-resistant and non-slip foamed sole is obtained.
2. A lightweight, oil-resistant, non-slip foamed sole according to claim 1, characterized in that: The foaming agent is azodicarbonamide.
3. A lightweight, oil-resistant, non-slip foamed sole according to claim 1, characterized in that: The cross-linking agent is cross-linking agent BIBP.
4. The lightweight, oil-resistant, non-slip foamed sole according to claim 1, characterized in that: The acrylonitrile content in the nitrile rubber is 18-24%.
5. The lightweight, oil-resistant, non-slip foamed sole according to claim 1, characterized in that: In step one, the mixing process specifically includes: firstly, ethylene-vinyl acetate copolymer, maleic anhydride grafted EVA, SBS thermoplastic elastomer and nitrile rubber are mixed and put into a mixer for mixing, and the mixing and mixing are carried out for 15 minutes; then, the raw materials other than the foaming agent, the accelerator and the cross-linking agent are continuously added and mixed and mixed for 10 minutes; then, the mixing temperature is adjusted to 90°C, and the material is turned over once after being kept for 5 minutes; when the mixing temperature rises to 98°C, the material is turned over twice; when the mixing temperature rises to 103°C, the material is turned over three times; when the mixing temperature rises to 108°C, the material is turned over four times; when the mixing temperature rises to 112-115°C, the material is turned over five times, and then the material is mixed for 2 minutes, the glue is discharged, and the material is placed at room temperature for more than 24 hours.
6. The lightweight, oil-resistant, non-slip foamed sole according to claim 1, characterized in that: In step 2, the EVA foam sheet is thinned at least twice in a double-roll mill to produce a sheet with a thickness of 2-3 mm.