A method for adjusting critical dimensions of photomask film growth
By growing a thin film on the surface of the photomask and combining plasma and dry etching technology to adjust the key dimensions of the photomask, the problem of inaccurate photomask size control in semiconductor manufacturing is solved, and the scrap rate and production cost are significantly reduced. Increased production capacity.
Patent Information
- Application Number
- CN202210709208.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-21
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-06-21
AI Technical Summary
In the semiconductor manufacturing process, it is difficult to accurately control the critical dimensions of high-end photomasks, resulting in high scrap rates and affecting production costs and throughput.
By growing a thin film material on the surface of the photomask, adjusting its lateral thickness and retaining the vertical thickness, a combination of plasma etching and dry etching is used to adjust the critical dimensions of the photomask.
A wider range of critical dimension adjustments are achieved, significantly reducing the scrap rate of photomask products, reducing production costs, and increasing production capacity.
Smart Images

Figure HDA0003706473480000011 
Figure HDA0003706473480000012 
Figure HDA0003706473480000013
Abstract
Description
Technical Field
[0001] The invention belongs to the field of semiconductor technology, and in particular relates to a method for adjusting a critical dimension. Background Art
[0002] With the development of semiconductor manufacturing technology, the area of semiconductor chips is getting smaller and smaller, so the precision of semiconductor technology has become more important. In the semiconductor manufacturing process, photolithography and etching are important processing links. The photolithography process mainly transfers the pattern on the mask to the wafer, while the etching process makes the pattern transferred on the wafer three-dimensional, and then other subsequent processes can be carried out to complete the production of the entire semiconductor device. In the photolithography and etching processes, a common concern includes the critical dimension (CD).
[0003] However, high-end photomasks have very strict requirements for photolithography and require precise control of pattern size. Once the critical size exceeds a certain specification, the photomask must be scrapped and remade unless there is a remedy. How to reduce the scrap rate of high-end photomasks to save production costs and increase production capacity is an urgent problem to be solved by technicians in this field.
[0004] Based on the above, this application provides a technical solution to solve the above technical problems. Summary of the invention
[0005] The present invention provides a method for adjusting the critical dimension of a photomask film growth, which can adjust the critical dimension of the photomask within a larger range, thereby effectively reducing the scrapping of photomask products, reducing costs and improving production capacity.
[0006] The present invention provides a method for preparing a semiconductor device, which can adjust the key size of a photomask within a wider range, thereby effectively reducing the scrapping of photomask products, reducing costs and improving production capacity.
[0007] A first aspect of the present invention provides a method for adjusting critical dimensions of a photomask film by growth, comprising the following steps:
[0008] providing a first photomask;
[0009] Growing a thin film material on the surface of the photomask to obtain a second photomask, wherein the surface of the second photomask has a thin film of a desired thickness;
[0010] removing all or part of the lateral thickness of the second photomask;
[0011] A portion or all of the vertical thickness of the second photomask is retained to adjust the critical dimension.
[0012] In a preferred embodiment of the present invention, the film with the required thickness on the surface of the second photomask comprises a nano low-temperature carbon crystal tube film.
[0013] In a preferred embodiment of the present invention, the thickness of the second photomask surface is no greater than 50 nanometers.
[0014] Preferably, the thickness of the second photomask surface is no greater than 20-30 nanometers, more preferably about 10 nanometers.
[0015] In a preferred embodiment of the present invention, plasma etching is used to remove the lateral thickness of the second photomask.
[0016] In a preferred embodiment of the present invention, the lateral thickness of the second photomask is removed so that the top surface of the first photomask is partially or completely exposed.
[0017] Specifically, the lateral thickness of the second photomask is removed so that the top surface of the first photomask is partially or completely exposed.
[0018] More specifically, the lateral thickness of the second photomask is removed so that the top surface of the first photomask is completely exposed.
[0019] In a preferred embodiment of the present invention, the critical dimension is further adjusted.
[0020] In a preferred embodiment of the present invention, the critical dimension can be adjusted within the range of ±30 nanometers.
[0021] Specifically, the CD can be adjusted in the range of -30 to +30 nanometers.
[0022] Specifically, the CD can be adjusted in the range of -20 to +20 nanometers.
[0023] Specifically, the CD can be adjusted in the range of -10 to +10 nanometers.
[0024] In a preferred embodiment of the present invention, dry etching is used to further adjust the critical dimension.
[0025] In a preferred embodiment of the present invention, when dry etching is used to further adjust the critical dimension, the critical dimension can be adjusted within a range of ±30 nanometers.
[0026] Specifically, the dry etching method is used to adjust the critical dimension in the range of -30 to +30 nanometers.
[0027] Specifically, the adjustment range of the critical dimension using dry etching is -20 to +20 nanometers.
[0028] Specifically, the dry etching method is used to adjust the critical dimension in the range of -10 to +10 nanometers.
[0029] A second aspect of the present invention provides a method for preparing a semiconductor device, wherein the method steps include the method for adjusting critical dimensions by growing a photomask film as described in the present invention.
[0030] The present invention can bring at least one of the following beneficial effects:
[0031] 1. Adjust the critical dimensions of the photomask within a wider range.
[0032] 2. It can effectively reduce the scrapping of photomask products, reduce costs and increase production capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The preferred implementation scheme will be described below in a clear and understandable manner with reference to the accompanying drawings to further illustrate the above-mentioned characteristics, technical features, advantages and their implementation methods.
[0034] Figure 1 A cross-sectional schematic diagram showing, by way of example, the growth of a thin film material on the surface of a photomask while retaining the vertical thickness;
[0035] Figure 2 The cross-sectional schematic diagram of the lateral and vertical growth of thin film materials and dry etching on the surface of the photomask is exemplarily shown;
[0036] Figure 3 The cross-sectional schematic diagram in which the lateral thickness is removed and the vertical thickness is retained is exemplarily shown. DETAILED DESCRIPTION
[0037] Various aspects of the present invention are described in further detail below.
[0038] Unless otherwise defined or indicated, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein can be applied to the method of the present invention.
[0039] Unless otherwise clearly specified and limited, the "or" mentioned in the present invention includes the relationship of "and". The "and" is equivalent to the Boolean logic operator "AND", the "or" is equivalent to the Boolean logic operator "OR", and "AND" is a subset of "OR".
[0040] It is to be understood that although the terms "first", "second", etc. may be used herein to describe different elements, these elements should not be limited by these terms. These terms are only used to distinguish one element from another element. Therefore, the first element may be referred to as the second element without departing from the teachings of the present invention.
[0041] In the present invention, the terms "comprising", "including" or "comprising" indicate that various components can be applied together in the mixture or composition of the present invention. Therefore, the terms "consisting mainly of" and "consisting of" are included in the terms "comprising", "including" or "comprising".
[0042] Unless otherwise clearly specified and limited, the terms "connected", "connected" and "connection" in the present invention should be understood in a broad sense, for example, it can be a fixed connection, or it can be connected through an intermediary medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0043] For example, if an element (or component) is referred to as being on, coupled to, or connected to another element, the element may be directly formed on, coupled to, or connected to the other element, or there may be one or more intervening elements between them. In contrast, if the expressions "directly on," "directly coupled to," and "directly connected to" are used herein, then no intervening elements are indicated. Other words used to describe the relationship between elements should be similarly interpreted, such as "between" and "directly between," "attached" and "directly attached," "adjacent" and "directly adjacent," and the like.
[0044] It should also be noted that the words "front", "rear", "left", "right", "upper" and "lower" used in the following description refer to directions in the drawings. The words "inner" and "outer" used refer to directions toward or away from the geometric center of a particular component, respectively. It can be understood that these terms are used here to describe the relationship of one element, layer or region relative to another element, layer or region as shown in the drawings. In addition to the orientations described in the drawings, these terms should also include other orientations of the device.
[0045] Other aspects of the present invention will be apparent to those skilled in the art in view of the disclosure herein.
[0046] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the specific implementation methods of the present invention will be described below with reference to the accompanying drawings. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings and other implementation methods can be obtained based on these drawings without creative work.
[0047] It should also be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present application. The drawings only show the components related to the present application and are not drawn according to the number, shape and size of the components in actual implementation. The type, quantity and proportion of each component in actual implementation may be changed arbitrarily, and the component layout may also be more complicated. For example, the thickness of the components in the drawings may be exaggerated for the sake of clarity.
[0048] Example
[0049] In the current adjustment of key dimensions, the following are common scenarios that lead to new problems, as well as the corresponding solutions adopted to solve the new problems:
[0050] Scenario 1: Limitations on the critical dimensions of photomasks in existing technologies
[0051] Due to the limitation of process window, after the photomask is produced, the critical dimensions may still deviate from the quality specifications due to reasons such as pattern density, drift of process conditions, slight changes in the environment, etc.
[0052] Scenario 2: Limitations on the critical dimensions of photomasks in existing technologies
[0053] Generally speaking, there is a certain amount of room for trimming the key dimensions of the photomask using dry etching, and the adjustable range is also very narrow.
[0054] In order to address the deficiencies in the above-mentioned scenarios, in the present invention, the inventors have conducted extensive and in-depth experiments and provided a new process method, which can effectively correct the quality of the critical dimensions of the photomask and reduce the scrap rate of high-end photomasks, so as to achieve the purpose of saving production costs and improving production capacity.
[0055] The technical concepts adopted in the present invention include:
[0056] First, the specific process is to grow thin film material on the surface of the photomask. After the film grows to the required thickness (which can be several to tens of nanometers), the lateral thickness of the film is removed (for example, by using precisely controlled plasma etching) to expose the original photomask surface. Because the vertical part of the film is still retained, the graphic size can be increased.
[0057] Secondly, optionally, dry etching can be used to further control and adjust the pattern size to fully meet the specifications of the lithography.
[0058] The following is further described in conjunction with the accompanying drawings. It should be understood that each aspect of the present invention is exemplary rather than restrictive, and the various aspects can be freely combined to obtain an optional technical solution.
[0059] A first aspect of the present invention provides a method for adjusting critical dimensions of a photomask film by growth, comprising the following steps:
[0060] providing a first photomask;
[0061] Growing a thin film material on the surface of the photomask to obtain a second photomask, wherein the surface of the second photomask has a thin film of a desired thickness;
[0062] removing all or part of the lateral thickness of the second photomask;
[0063] A portion or all of the vertical thickness of the second photomask is retained to adjust the critical dimension.
[0064] See Figure 1 , exemplarily showing a specific implementation, a cross-sectional schematic diagram of growing a thin film material on the surface of a photomask while retaining the vertical thickness.
[0065] In a preferred embodiment of the present invention, the film with the required thickness on the surface of the second photomask comprises a nano-low temperature carbon crystal tube film. The advantage of the nano-low temperature carbon crystal tube is that the uniformity of the growth of the obtained nano-scale low temperature carbon crystal tube film is very good; therefore, it is easier to make a larger range of corrections on the critical dimensions of the completed photomask.
[0066] It should be noted that thin film growth can have multiple options when conditions permit, and low-temperature carbon crystal growth is only one type.
[0067] Therefore, it should be understood that those skilled in the art can adjust the type of the film as long as it does not limit the purpose of the invention.
[0068] In a preferred embodiment of the present invention, the thickness of the second photomask surface is no greater than 50 nanometers.
[0069] It should be understood that, in theory, 50-nanometer thin film growth is achievable, but the thicker the film, the greater the requirement for thickness uniformity control, which increases the complexity of the process.
[0070] Preferably, the thickness of the second photomask surface is no greater than 20-30 nanometers, more preferably about 10 nanometers.
[0071] In a preferred embodiment of the present invention, plasma etching is used to remove the lateral thickness of the second photomask.
[0072] The inventors have found that plasma etching can more accurately control the removal of lateral thickness.
[0073] It should be understood that other etching methods can also be applied by those skilled in the art as long as they do not limit the purpose of the invention.
[0074] In a preferred embodiment of the present invention, the lateral thickness of the second photomask is removed so that the top surface of the first photomask is partially or completely exposed.
[0075] It should be understood that when the lateral thickness of the second photomask is removed, it is usually completely removed. However, the lateral thickness of the second photomask may also be partially removed as long as it does not affect the purpose of the invention. For example, it can be adjusted to the point where the final phase and transmittance measurement have no obvious impact.
[0076] Specifically, the lateral thickness of the second photomask is removed so that the top surface of the first photomask is partially or completely exposed.
[0077] More specifically, the lateral thickness of the second photomask is removed so that the top surface of the first photomask is completely exposed.
[0078] The inventors found that when removing the lateral thickness of the second photomask, it is necessary to balance the influence of the film uniformity and the light transmittance of the non-transparent film.
[0079] Generally, the uniformity of the film growth thickness is acceptable when it is not too thick, so the preferred technical solution is to remove the grown film to expose the original pattern surface, which can reduce the impact of the transparency.
[0080] However, it should be understood that those skilled in the art can also adjust the technical solution of the present invention according to specific circumstances. For example, although the non-transparent film will affect the light transmittance, the effect will not be very obvious because of its small thickness, and it can be ignored if it is within an acceptable range after measurement.
[0081] In a preferred embodiment of the present invention, the critical dimension is further adjusted.
[0082] In a preferred embodiment of the present invention, the critical dimension can be adjusted within the range of ±30 nanometers.
[0083] The advantage of the present invention is that the use of the auxiliary method of thin film growth of the present invention can increase the adjustable range of key dimension etching to about twice the thickness of the thin film.
[0084] For example: a thin film grows by 20 nanometers, which roughly represents an adjustable range of -20 nanometers to +20 nanometers, depending on actual needs.
[0085] Specifically, the CD can be adjusted in the range of -30 to +30 nanometers.
[0086] Specifically, the CD can be adjusted in the range of -20 to +20 nanometers.
[0087] Specifically, the CD can be adjusted in the range of -10 to +10 nanometers.
[0088] In a preferred embodiment of the present invention, dry etching is used to further adjust the critical dimension.
[0089] Figure 2 The cross-sectional schematic diagram of the lateral and vertical growth of thin film materials and dry etching on the surface of a photomask is exemplified, showing the thin film growth; plasma unidirectional controlled surface etching, and finally dry etching to adjust the critical dimensions.
[0090] See Figure 3 , which exemplarily shows a cross-sectional schematic diagram in which the lateral thickness is removed and the vertical thickness is retained.
[0091] In a preferred embodiment of the present invention, when dry etching is used to further adjust the critical dimension, the critical dimension can be adjusted within a range of ±30 nanometers.
[0092] Specifically, the dry etching method is used to adjust the critical dimension in the range of -30 to +30 nanometers.
[0093] Specifically, the adjustment range of the critical dimension using dry etching is -20 to +20 nanometers.
[0094] Specifically, the dry etching method is used to adjust the critical dimension in the range of -10 to +10 nanometers.
[0095] A second aspect of the present invention provides a method for preparing a semiconductor device, wherein the method steps include the method for adjusting critical dimensions by growing a photomask film as described in the present invention.
[0096] In summary, the present invention realizes a solution for adjusting the critical dimensions of a photomask within a larger range, which can effectively reduce the scrapping of photomask products, reduce costs, and improve production capacity.
[0097] Based on this application, it should be understood by those skilled in the art that one aspect described herein can be implemented independently of any other aspect, and two or more of these aspects can be combined in various ways. For example, any number and aspect described herein can be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein can be used to implement this device and / or practice this method.
[0098] It should be noted that the above embodiments can be freely combined as needed. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered as the protection scope of the present invention.
[0099] All documents mentioned in the present invention are cited as references in this application, just as each document is cited as reference separately. In addition, it should be understood that after reading the above content of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.
Claims
1. A method for adjusting critical dimensions of photomask film growth, characterized in that: The steps include: providing a first photomask; Growing a thin film material on the surface of the first photomask to obtain a second photomask, wherein the surface of the second photomask has a thin film of a desired thickness; removing all or part of the lateral thickness of the second photomask; A portion or all of the vertical thickness of the second photomask is retained to adjust the critical dimension.
2. The method for adjusting critical dimensions of photomask film growth according to claim 1, characterized in that: The film with the required thickness on the surface of the second photomask includes a nano low-temperature carbon crystal tube film.
3. The method for adjusting critical dimensions of photomask film growth according to claim 1, characterized in that: The thickness of the second photomask surface is no greater than 50 nanometers.
4. The method for adjusting critical dimensions of photomask film growth according to claim 1, characterized in that: When the lateral thickness of the second photomask is removed, a plasma etching method is used.
5. The method for adjusting critical dimensions of photomask film growth according to claim 1, characterized in that: The lateral thickness of the second photomask is removed so that the top surface of the first photomask is partially or fully exposed.
6. The method for adjusting critical dimensions of photomask film growth according to any one of claims 1 to 4, characterized in that: It also includes further adjustments to critical dimensions.
7. The method for adjusting critical dimensions of photomask film growth according to claim 6, characterized in that: Key dimensions can be tuned within a range of ±30 nm.
8. The method for adjusting critical dimensions of photomask film growth according to claim 6, characterized in that: The critical dimension is further adjusted by dry etching.
9. The method for adjusting critical dimensions of photomask film growth according to claim 8, characterized in that: When dry etching is used to further adjust the critical dimensions, the critical dimensions can be adjusted within the range of ±30 nanometers.
10. A method for preparing a semiconductor device, characterized in that: The method steps include the method for adjusting critical dimensions by growing a photomask film as described in any one of claims 1-9.