A method for preparing a sulfide electrolyte membrane

By modifying the surface of polytetrafluoroethylene and grafting lithium sulfonate groups to improve its bonding and conductive capabilities, it can be used in the preparation of sulfide electrolyte membranes, which solves the problems of low inactive components and high energy consumption, and improves electrical conductivity. rate and energy density.

CN114927766BActive Publication Date: 2024-10-11SHANGHAI FIRM LITHIUM NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210653773.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-10
Publication Date
2024-10-11
Estimated Expiration
2042-06-10

AI Technical Summary

Technical Problem

The existing sulfide electrolyte membrane preparation methods have low inactive ingredients and high energy consumption in the film formation process, which affects the conductivity and energy density.

Method used

By surface modification of polytetrafluoroethylene and grafting of lithium sulfonate groups, it improves its bonding ability and imparts conductive ability, and is used for mixing and pressing with sulfide electrolytes.

Benefits of technology

It improves the bonding performance and conductivity of polytetrafluoroethylene, reduces the pressing temperature and energy consumption, and enhances the overall ionic conductivity of the sulfide electrolyte membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114927766B_ABST
    Figure CN114927766B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of energy, and provides a method for preparing a sulfide electrolyte membrane. The method comprises the following steps: step 1, pretreatment of polytetrafluoroethylene; step 2, grafting styrene on the pretreated polytetrafluoroethylene; step 3, sulfonating the styrene-grafted polytetrafluoroethylene; step 4, lithium ion exchange treatment of the sulfonated styrene-grafted polytetrafluoroethylene; step 5, mixing the sulfonated styrene-grafted polytetrafluoroethylene after lithium ion exchange with a sulfide electrolyte in a certain proportion, and pressing and molding under an argon environment. The present invention uses modified polytetrafluoroethylene as a binder to prepare a sulfide electrolyte membrane. By sulfonating and ionizing the polytetrafluoroethylene, the viscosity of the binder can be improved, which facilitates the rapid pressing of the electrolyte into a membrane, and at the same time reduces the influence of the introduction of the binder on the conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of energy, and specifically relates to a method for preparing a sulfide electrolyte membrane, and in particular to a modified binder for sulfide electrolyte membrane formation, which is mainly used in all-solid-state batteries with sulfide as electrolyte. Background Art

[0002] Lithium-ion batteries on the market mainly use liquid electrolytes as electrolytes, and graphite or silicon-doped graphite is used for the negative electrode. Limited by the low specific capacity of graphite or silicon-doped graphite, as well as the specific gravity of the electrolyte and the use of diaphragms, the energy density of liquid lithium-ion batteries has never been able to break through 400Wh / kg. Solid-state lithium-ion batteries use lithium with higher specific capacity as the negative electrode and use solid-state electrolytes, which can greatly improve the energy density of the battery.

[0003] Solid-state batteries use solid electrolytes, including oxide solid electrolytes, sulfide solid electrolytes and polymer solid electrolytes. Among them, the ionic conductivity of sulfide electrolytes shows an absolute advantage, which can reach 10-2S / cm at room temperature. However, the disadvantages of sulfide electrolytes are also obvious, and the film-forming and processing properties are not as good as polymer electrolytes. In existing articles, wet film formation and dry film formation are mainly used. The wet film formation mainly involves premixing the electrolyte and the binder, and then coating or spraying the film; in the dry film formation, the more common operation is to mix the binder and the electrolyte in a certain proportion, and then press and form.

[0004] At present, there are many reported patents for sulfide electrolyte film making, but the preparation methods are either complicated, or too many inactive ingredients are introduced, or the preparation requirements are relatively strict. For example, in the method mentioned in patent CN202110962425, a mixed solution of an ion-conductive polymer, a lithium salt, and a solvent is coated on the surface of the sulfide electrolyte particles by spraying, dried, and then the sulfide electrolyte membrane precursor is dispersed, and then the dispersed solution is coated on the surface of the release film, melted, and the sulfide electrolyte membrane is obtained. The characteristic of this method is that a polymer solid electrolyte prepared by a polymer and a lithium salt is used as a coating layer, but the lithium ion migration number of this type of polymer solid electrolyte is mostly ≤0.5, and the room temperature conductivity of this type of electrolyte is much lower than that of sulfide, which will reduce the overall ionic conductivity of the electrolyte membrane. The literature reports a dry method for preparing electrolyte membranes, in which polytetrafluoroethylene powder is ball-milled with sulfide electrolyte and then roll-formed at 80°C. Although 0.2 wt% polytetrafluoroethylene is used in this work, polytetrafluoroethylene is still an inactive ingredient and does not have conductive properties. This method uses hot rolling at 80°C, which increases energy consumption (Nano Lett 2021, 21, 5233-5239.)

[0005] Therefore, how to increase the inactive components in the sulfide electrolyte membrane and reduce the energy consumption in the membrane formation process are problems that need to be solved. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing a sulfide electrolyte membrane in order to solve the problem of low inactive components in the electrolyte membrane. The present invention is a modified binder for use in a sulfide electrolyte membrane preparation scheme. By surface-modifying polytetrafluoroethylene and grafting lithium sulfonate groups, the bonding ability of polytetrafluoroethylene can be improved on the one hand, and the binder itself can be made to have ion conduction ability on the other hand. The binder is used in sulfide electrolyte membrane making, which is easier to form a membrane and can reduce the loss of conductivity caused by the addition of the binder.

[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0008] The present invention provides a method for preparing a sulfide electrolyte membrane, the preparation method comprising the following steps:

[0009] Step 1, pretreatment of polytetrafluoroethylene;

[0010] Step 2, grafting styrene onto the pretreated polytetrafluoroethylene to obtain styrene-grafted polytetrafluoroethylene;

[0011] Step 3, sulfonating the styrene-grafted polytetrafluoroethylene to obtain sulfonated styrene-grafted polytetrafluoroethylene;

[0012] Step 4, subjecting the sulfonated styrene grafted polytetrafluoroethylene to lithium ion exchange treatment;

[0013] Step 5: Mix the sulfonated styrene grafted polytetrafluoroethylene after lithium ion exchange with the sulfide electrolyte, and press them into shape to obtain a sulfide electrolyte membrane.

[0014] Preferably, in step 1, the pretreatment of polytetrafluoroethylene is specifically as follows: polytetrafluoroethylene powder is stirred in a mixed solution of water and an organic solvent, then ultrasonically treated, and finally filtered and vacuum dried. The stirring is carried out at room temperature. After the pretreatment, oil stains, dust, etc. on the surface of PTFE can be cleaned so as to facilitate the grafting treatment in step 2. Water alone is not easy to disperse, and solvent alone is easy to volatilize, so a mixed solvent is used.

[0015] Preferably, the organic solvent includes one or more of ethanol and acetone. Such organic solvents have low viscosity and low boiling point.

[0016] Preferably, the volume ratio of water to the organic solvent is X:100-X, 10≤X≤90. The mass fraction of polytetrafluoroethylene in the mixed system is 10%-50%.

[0017] Preferably, the stirring time is 2-24 hours, the ultrasonic treatment time is 1-5 hours, and the drying temperature is 60-100°C.

[0018] Preferably, the styrene grafting in step 2 is specifically as follows: adding the polytetrafluoroethylene pretreated in step 1 to a mixture of styrene and dichloromethane, sealing in an inert atmosphere, irradiating to graft styrene to the polytetrafluoroethylene, taking out and cleaning, vacuum drying for standby use.

[0019] Preferably, the mass ratio of styrene to dichloromethane is X:100-X, 10≤X≤50. The amount of the mixed solution of polytetrafluoroethylene, styrene and dichloromethane added in step 2 is: 90-110 ml of the mixed solution corresponding to 50 g of polytetrafluoroethylene, more preferably 100 ml.

[0020] Preferably, the irradiation is carried out under 0.5-1.0 kGy / h of Co60 gamma rays. The irradiation is carried out under room temperature and the irradiation time is 60-80 hours.

[0021] Preferably, the cleaning is repeated cleaning with toluene and soaking for 12-24 hours. The cleaning can remove the monomers and homopolymers remaining on the surface.

[0022] Preferably, vacuum drying is performed at 50-70° C. for 24-48 hours.

[0023] Preferably, the sulfonation treatment in step 3 is specifically as follows: immersing the styrene-grafted polytetrafluoroethylene in a sulfonation solution, then heating the reaction, taking out the product after the reaction, washing it, then performing an alkali treatment to convert the sulfonic acid group into sodium sulfonate, then performing an acid treatment to neutralize the alkali solution, and drying to obtain the sulfonated polystyrene-grafted polytetrafluoroethylene. Sulfonation is for grafting sulfonic acid groups, alkali solution treatment is for converting sulfonic acid groups into sodium sulfonate, and acid treatment is for washing the involved alkali solution.

[0024] Preferably, the component of the sulfonation solution is a dichloromethane solution of chlorosulfonic acid or trifluoromethanesulfonic acid, and the concentration of chlorosulfonic acid or trifluoromethanesulfonic acid is 30-60%. The styrene-grafted polytetrafluoroethylene accounts for 10-50% of the mass of the sulfonation solution.

[0025] Preferably, the heating reaction temperature is 35-60°C, the time is 4-6 hours, and the heating reaction is carried out under nitrogen or argon protection conditions.

[0026] Preferably, the cleaning is performed by repeatedly cleaning with dichloromethane 3-5 times.

[0027] Preferably, the alkali treatment is to treat the obtained sulfonation reaction product with sodium hydroxide solution for 1-12 hours; the acid treatment is to treat the obtained sulfonation reaction product with dilute hydrochloric acid for 1-12 hours. The concentration of the sodium hydroxide solution is 0.5-2M, and the concentration of the dilute hydrochloric acid is 0.1-0.5M.

[0028] Preferably, step 4 specifically comprises: dispersing the sulfonated styrene grafted polytetrafluoroethylene in step 3 in a lithium salt aqueous solution, performing lithium ionization of the sulfonate group, and then filtering and vacuum drying.

[0029] Preferably, the lithium salt is one or more of lithium chloride and lithium bis(trifluoromethylsulfonyl)imide, and the concentration of the lithium salt aqueous solution is 0.5M-1M.

[0030] Preferably, the dispersion is carried out at a temperature of 30-80°C with stirring for 12-24 hours.

[0031] Preferably, in step 5, the mass ratio of the sulfonated styrene grafted polytetrafluoroethylene and the sulfide electrolyte after lithium ion exchange is X:100-X, 0.1≤X≤50.

[0032] Preferably, in step 5, the sulfide electrolyte includes Li2S-P2S5, Li 10 GeP2S 12 , Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 , Li 10 SnP2S 12 , Li6PS5Cl, Li6PS5I, Li6PS5Br, Li 5.5 PS 4.5 Cl 1.5 One or more of the .

[0033] Preferably, in step 5, the pressing temperature is 20-80° C., the pressing time is 1-10 minutes, the pressing method is isobaric static pressing or roller pressing, and the pressing is performed in an argon environment.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] (1) The modified polytetrafluoroethylene has sulfonic acid groups introduced on its surface, which has better bonding properties than unmodified polytetrafluoroethylene;

[0036] (2) The surface of the modified polytetrafluoroethylene has -SO2Li, which acts as a single ion conductor and can provide lithium ion conduction capability;

[0037] (3) The modified polytetrafluoroethylene is used for sulfide electrolyte film formation. Due to the increased viscosity, the pressing temperature can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0039] Figure 1 The modified tetrafluoroethylene of Example 1 and Comparative Example 1 are used for sulfide electrolyte film formation and then assembled into a battery, and the AC impedance spectrum is tested at room temperature. DETAILED DESCRIPTION

[0040] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. The following examples are implemented on the premise of the technical solution of the present invention, provide detailed implementation methods and specific operation processes, and will help those skilled in the art to further understand the present invention. It should be pointed out that the protection scope of the present invention is not limited to the following embodiments, and several adjustments and improvements made under the premise of the concept of the present invention all belong to the protection scope of the present invention.

[0041] Example 1

[0042] A method for preparing a sulfide electrolyte membrane, the method comprising the following steps:

[0043] 1. Pretreatment of polytetrafluoroethylene fiber: 50 g polytetrafluoroethylene was added to 100 ml water / acetone (volume ratio is 1 / 1) solution under stirring at room temperature, stirred for 12 hours, ultrasonically treated for 2 hours, then filtered and dried in vacuum at 80°C.

[0044] 2. Add the pretreated polytetrafluoroethylene in step 1 to a mixture of 100 ml of styrene and dichloromethane, the mass ratio of styrene to dichloromethane is 20:80, an inert atmosphere is passed into the above solution, the air is driven out, and the system is sealed with polytetrafluoroethylene tape. Finally, the sealed system is placed in 1.0 kGy / h Co60γ rays and irradiated for 60 hours at room temperature. The irradiated styrene-grafted polytetrafluoroethylene fiber is taken out and repeatedly washed and soaked in toluene for 12 hours to remove the monomers and homopolymers remaining on the surface, and then vacuum dried at 50 for 24 hours for standby use.

[0045] 3. Immerse the sample in step 2 in a dichloromethane solution with a concentration of 60% chlorosulfonic acid, then heat the mixed solution to 60°C and react for 6 hours under nitrogen or argon protection. After the reaction, take out the product and wash it three times with dichloromethane. Then treat the sulfonated material with 0.5M sodium hydroxide solution for 6 hours, then treat it with 0.1M dilute hydrochloric acid for 6 hours, and dry it to obtain sulfonated polystyrene grafted polytetrafluoroethylene.

[0046] 4. Disperse the sample obtained above in 0.5M lithium chloride saline solution and stir at 60°C for 20 hours, filter and dry in vacuum.

[0047] 5. The obtained polytetrafluoroethylene powder and Li6PS5Cl sulfide electrolyte were mixed in a mass ratio of 0.2:99.8, and rolled at 30° C. for 10 minutes to obtain a sulfide electrolyte membrane.

[0048] 6. Use stainless steel as the blocking electrode, cut the electrolyte membrane obtained in step 5 into 10 mm diameter discs, the electrolyte thickness is 50 μm, assemble the battery, and test the AC impedance spectrum at room temperature. Figure 1 shown.

[0049] Example 2

[0050] A method for preparing a sulfide electrolyte membrane, the method comprising the following steps:

[0051] 1. Pretreatment of polytetrafluoroethylene fiber: 50 g polytetrafluoroethylene was added to 100 ml water / acetone (volume ratio is 1 / 1) solution under stirring at room temperature, stirred for 12 hours, ultrasonically treated for 2 hours, then filtered and dried in vacuum at 80°C.

[0052] 2. Add the pretreated polytetrafluoroethylene in step 1 to a mixture of 100 ml of styrene and dichloromethane, the mass ratio of styrene to dichloromethane is 20:80, an inert atmosphere is passed into the above solution, the air is driven out, and the system is sealed with polytetrafluoroethylene tape. Finally, the sealed system is placed in 1.0 kGy / h Co60γ rays and irradiated for 60 hours at room temperature. The irradiated styrene-grafted polytetrafluoroethylene fiber is taken out and repeatedly washed and soaked in toluene for 12 hours to remove the monomers and homopolymers remaining on the surface, and then vacuum dried at 50 for 24 hours for standby use.

[0053] 3. Immerse the sample in step 2 in a dichloromethane solution with a concentration of 60% trifluoromethanesulfonic acid, then heat the mixed solution to 60°C and react for 6 hours under nitrogen or argon protection. After the reaction is completed, take out the product and wash it three times with dichloromethane. Then treat the sulfonated material with 0.5M sodium hydroxide solution for 6 hours, then treat it with 0.1M dilute hydrochloric acid for 6 hours, and then dry it to obtain sulfonated polystyrene grafted polytetrafluoroethylene.

[0054] 4. The sample obtained above was dispersed in a 0.5 M bistrifluoromethanesulfonyl imide lithium salt aqueous solution and stirred at 60°C for 20 hours, filtered and dried in vacuum.

[0055] 5. The obtained polytetrafluoroethylene powder and Li6PS5Cl sulfide electrolyte were mixed in a mass ratio of 0.2:99.8, and rolled at 30° C. for 10 minutes to obtain a sulfide electrolyte membrane.

[0056] Example 3

[0057] A method for preparing a sulfide electrolyte membrane, the method comprising the following steps:

[0058] 1. Pretreatment of polytetrafluoroethylene fiber: 50 g polytetrafluoroethylene was added to 100 ml water / acetone (volume ratio is 1 / 1) solution under stirring at room temperature, stirred for 12 hours, ultrasonically treated for 2 hours, then filtered and dried in vacuum at 80°C.

[0059] 2. Add the pretreated polytetrafluoroethylene in step 1 to a mixture of 100 ml of styrene and dichloromethane, the mass ratio of styrene to dichloromethane is 20:80, an inert atmosphere is passed into the above solution, the air is driven out, and the system is sealed with polytetrafluoroethylene tape. Finally, the sealed system is placed in 1.0 kGy / h Co60γ rays and irradiated for 60 hours at room temperature. The irradiated styrene-grafted polytetrafluoroethylene fiber is taken out and repeatedly washed and soaked in toluene for 12 hours to remove the monomers and homopolymers remaining on the surface, and then vacuum dried at 50 for 24 hours for standby use.

[0060] 3. Immerse the sample in step 2 in a dichloromethane solution with a concentration of 60% trifluoromethanesulfonic acid, then heat the mixed solution to 60°C and react for 6 hours under nitrogen or argon protection. After the reaction is completed, take out the product and wash it three times with dichloromethane. Then treat the sulfonated material with 0.5M sodium hydroxide solution for 6 hours, then treat it with 0.1M dilute hydrochloric acid for 6 hours, and then dry it to obtain sulfonated polystyrene grafted polytetrafluoroethylene.

[0061] 4. The sample obtained above was dispersed in a 0.5 M bistrifluoromethanesulfonyl imide lithium salt aqueous solution and stirred at 60°C for 20 hours, filtered and dried in vacuum.

[0062] 5. The obtained polytetrafluoroethylene powder and Li 10 GeP2S 12 The sulfide electrolyte was mixed in a mass ratio of 0.2:99.8 and then rolled at 30° C. for 10 minutes to obtain a sulfide electrolyte membrane.

[0063] Comparative Example 1

[0064] The preparation method of this comparative example only includes step 1 and step 5 in Example 1, specifically:

[0065] 1. Pretreatment of polytetrafluoroethylene fiber: 50 g polytetrafluoroethylene was added to 100 ml water / acetone (volume ratio is 1 / 1) solution under stirring at room temperature, stirred for 12 hours, ultrasonically treated for 2 hours, then filtered and dried in vacuum at 80°C.

[0066] 2. The obtained polytetrafluoroethylene powder and Li6PS5Cl sulfide electrolyte were mixed in a mass ratio of 0.2:99.8, and then rolled at 30° C. for 10 minutes to obtain a sulfide electrolyte membrane.

[0067] 3. Using stainless steel as the blocking electrode, the electrolyte membrane obtained in step 5 was cut into 10 mm diameter discs with a thickness of 50 μm. The battery was assembled and the AC impedance spectrum was tested at room temperature. Figure 1 shown.

[0068] Comparative Example 2

[0069] The preparation method of this comparative example only includes steps 1, 2 and 5 in Example 1, specifically:

[0070] 1. Pretreatment of polytetrafluoroethylene fiber: 50 g polytetrafluoroethylene was added to 100 ml water / acetone (volume ratio is 1 / 1) solution under stirring at room temperature, stirred for 12 hours, ultrasonically treated for 2 hours, then filtered and dried in vacuum at 80°C.

[0071] 2. Add the pretreated polytetrafluoroethylene in step 1 to a mixture of 100 ml of styrene and dichloromethane, the mass ratio of styrene to dichloromethane is 20:80, an inert atmosphere is passed into the above solution, the air is driven out, and the system is sealed with polytetrafluoroethylene tape. Finally, the sealed system is placed in 1.0 kGy / h Co60γ rays and irradiated for 60 hours at room temperature. The irradiated styrene-grafted polytetrafluoroethylene fiber is taken out and repeatedly washed and soaked in toluene for 12 hours to remove the monomers and homopolymers remaining on the surface, and then vacuum dried at 50 for 24 hours for standby use.

[0072] 3. The obtained polytetrafluoroethylene powder and Li6PS5Cl sulfide electrolyte were mixed in a mass ratio of 0.2:99.8, and rolled at 30° C. for 10 minutes to obtain a sulfide electrolyte membrane.

[0073] 4. Using stainless steel as the blocking electrode, the electrolyte membrane obtained in step 5 was cut into 10 mm diameter discs and assembled into a battery. The surface of polytetrafluoroethylene has no sulfonic acid groups introduced, and the bonding performance is poor.

[0074] Comparative Example 3

[0075] The preparation method of this comparative example only includes steps 1-3 and step 5 in Example 1, specifically:

[0076] 1. Pretreatment of polytetrafluoroethylene fiber: 50 g polytetrafluoroethylene was added to 100 ml water / acetone (volume ratio is 1 / 1) solution under stirring at room temperature, stirred for 12 hours, ultrasonically treated for 2 hours, then filtered and dried in vacuum at 80°C.

[0077] 2. Add the pretreated polytetrafluoroethylene in step 1 to a mixture of 100 ml of styrene and dichloromethane, the mass ratio of styrene to dichloromethane is 20:80, an inert atmosphere is passed into the above solution, the air is driven out, and the system is sealed with polytetrafluoroethylene tape. Finally, the sealed system is placed in 1.0 kGy / h Co60γ rays and irradiated for 60 hours at room temperature. The irradiated styrene-grafted polytetrafluoroethylene fiber is taken out and repeatedly washed and soaked in toluene for 12 hours to remove the monomers and homopolymers remaining on the surface, and then vacuum dried at 50 for 24 hours for standby use.

[0078] 3. Immerse the sample in step 2 in a dichloromethane solution with a concentration of 60% chlorosulfonic acid, then heat the mixed solution to 60°C and react for 6 hours under nitrogen or argon protection. After the reaction is completed, take out the product and wash it three times with dichloromethane. Then treat the sulfonated material with 0.5M sodium hydroxide solution for 6 hours, then treat it with 0.1M dilute hydrochloric acid for 6 hours, and then dry it to obtain sulfonated polystyrene grafted polytetrafluoroethylene.

[0079] 4. The obtained polytetrafluoroethylene powder and Li6PS5Cl sulfide electrolyte were mixed in a mass ratio of 0.2:99.8, and rolled at 30° C. for 10 minutes to obtain a sulfide electrolyte membrane.

[0080] 5. Using stainless steel as the blocking electrode, the electrolyte membrane obtained in step 5 was cut into 10 mm diameter discs and assembled into a battery. There is no -SO2Li on the surface of polytetrafluoroethylene, and the conductivity is poor.

[0081] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A method for preparing a sulfide electrolyte membrane, characterized in that: The preparation method comprises the following steps: Step 1, pretreatment of polytetrafluoroethylene; Step 2, grafting styrene onto the pretreated polytetrafluoroethylene to obtain styrene-grafted polytetrafluoroethylene; Step 3, sulfonating the styrene-grafted polytetrafluoroethylene to obtain sulfonated styrene-grafted polytetrafluoroethylene; Step 4, subjecting the sulfonated styrene grafted polytetrafluoroethylene to lithium ion exchange treatment; Step 5, mixing the sulfonated styrene grafted polytetrafluoroethylene after lithium ion exchange with the sulfide electrolyte, and pressing and molding to obtain a sulfide electrolyte membrane; The styrene grafting in step 2 is specifically as follows: adding the polytetrafluoroethylene pretreated in step 1 to a mixture of styrene and dichloromethane, sealing in an inert atmosphere, and then irradiating to graft styrene to the polytetrafluoroethylene, taking out and cleaning, and vacuum drying for standby use; the mass ratio of styrene to dichloromethane is X:100-X, 10≤X≤50; and the irradiation is carried out in a Co60γ ray of 0.5-1.0 kGy / h; In step 5, the mass ratio of the sulfonated styrene grafted polytetrafluoroethylene and the sulfide electrolyte after lithium ion exchange is X:100-X, 0.1≤X≤50; the sulfide electrolyte includes Li2S-P2S5, Li 10 GeP2S 12 , Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 , Li 10 SnP2S 12 , Li6PS5Cl, Li6PS5I, Li6PS5Br, Li 5.5 PS 4.5 Cl 1.5 One or more of the .

2. The preparation method according to claim 1, characterized in that: In step 1, the pretreatment of polytetrafluoroethylene is specifically as follows: polytetrafluoroethylene powder is stirred in a mixed solution of water and an organic solvent, then subjected to ultrasonic treatment, and finally filtered and vacuum dried.

3. The preparation method according to claim 1, characterized in that: The sulfonation treatment in step 3 is specifically as follows: immersing the styrene-grafted polytetrafluoroethylene in a sulfonation solution, and then performing a heating reaction. After the reaction is completed, the sulfonation reaction product is taken out and cleaned, and then subjected to an alkali treatment to convert the sulfonic acid group into sodium sulfonate, and then subjected to an acid treatment to neutralize the alkali solution, and then dried to obtain the sulfonated polystyrene-grafted polytetrafluoroethylene.

4. The preparation method according to claim 3, characterized in that: The component of the sulfonation solution is a dichloromethane solution of chlorosulfonic acid or trifluoromethanesulfonic acid, and the concentration of chlorosulfonic acid or trifluoromethanesulfonic acid is 30-60%.

5. The preparation method according to claim 3, characterized in that: The heating reaction temperature is 35-60°C and the time is 4-6 hours.

6. The preparation method according to claim 3, characterized in that: The alkali treatment is to treat the obtained sulfonation reaction product with sodium hydroxide solution for 1-12 hours; the acid treatment is to treat it with dilute hydrochloric acid for 1-12 hours.

7. The preparation method according to claim 1, characterized in that: Step 4 specifically comprises: dispersing the sulfonated styrene grafted polytetrafluoroethylene in step 3 in a lithium salt aqueous solution, and then filtering and vacuum drying.