Method for producing crystalline material from different materials

Through the remote plasma deposition process, crystal layers of lithium, different metals and counterions are formed on the substrate, which solves the problems of crystallization film production efficiency and uniformity in traditional technology, and achieves high-efficiency and high-speed crystallization film deposition, which is suitable for lithium ions Cathode material of the battery pack.

CN114929927BActive Publication Date: 2024-11-01DYSON TECH LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080092221.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-11-15
Filing Date
2020-11-10
Publication Date
2024-11-01
Estimated Expiration
2040-11-10

AI Technical Summary

Technical Problem

It is difficult for the prior art to produce highly ordered crystalline films, especially layered oxide materials, at a high rate, and traditional magnetron sputtering technology has problems of inefficiency and unevenness.

Method used

Using plasma deposition technology, lithium, different metals and counterions are sputtered from multiple target components from multiple target components to substrates using plasma generated remotely. By controlling the geometry and configuration of the target components, combining magnetic and electric fields, high-energy plasma is achieved. Independent control, the crystallization layer is formed directly on the substrate, reducing or avoiding the annealing step.

Benefits of technology

It realizes efficient deposition of crystalline materials with the required stoichiometric and crystal phases on the substrate, improves the charging speed and capacity of the lithium-ion battery pack, and the layered oxide structure of the material makes it easier to embed and deinstall lithium ions , improves the performance of solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114929927B_ABST
    Figure CN114929927B_ABST
Patent Text Reader

Abstract

A method of making a crystalline layer of material on a surface, the crystalline layer comprising lithium, at least one transition metal and at least one counter ion, wherein the method comprises the steps of: plasma sputtering material from a first target comprising lithium onto a surface of a substrate or a surface supported by a substrate, at least a first plume corresponding to the trajectory of particles from the first target to the surface, and plasma sputtering material from a second target comprising at least one transition metal onto the surface, at least a second plume corresponding to the trajectory of particles from the second target to the surface. The first target is positioned non-parallel to the second target, the first plume and the second plume converge at an area close to the surface of the substrate or the surface supported by the substrate, and the crystalline layer is formed on the surface of said area.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method of producing a layer of crystalline material on a surface. More particularly, but not exclusively, the present invention relates to producing a crystalline layer comprising lithium, at least one different metal and at least one counter ion using a plasma deposition process. Background Art

[0002] Plasma deposition systems are used in a wide variety of industries, from electronic device manufacturing to the production of wear-resistant coatings. In the field of electronic devices, there are many established plasma deposition technologies.

[0003] Forming a crystalline material layer comprising lithium, at least one different metal, and at least one counterion using a plasma deposition process generally requires an annealing step.

[0004] Conventional magnetron sputtering techniques often suffer from inefficient and uneven target utilization. JP2008045213 is an example of a proposal to use pulsed DC magnetron sputtering in an effort to achieve uniform plasma density over a relatively small target area. The method involves preheating a substrate to 200°C and then applying a pulsed DC power supply to a single sputtering target containing LiCoO2. A layer of material is formed on the substrate and a rapid thermal annealing process is performed in a short time to form a LiCoO2 crystalline layer with a desired crystal structure.

[0005] PCT publication WO 2011 / 131921 A1 discloses a method of using a remotely generated plasma and confining the plasma to a target in such a way that the target material is uniformly sputtered.

[0006] However, WO2011 / 131921A1 does not relate to the deposition or generation of crystalline thin films. It does not discuss or contemplate methods of in-situ deposition of crystalline films by manipulating certain parameters of a thin film deposition system utilizing remotely generated plasma. Furthermore, WO2011 / 131921A1 does not discuss apparatus or methods that allow for the desired stoichiometry to be achieved between a target material and a material formed by sputtering deposition of said material.

[0007] While techniques including those in the prior art are capable of producing thin films of high quality materials, there remains a long felt need for techniques that can produce crystalline films of highly ordered materials, such as layered oxide materials, at high rates, with desired stoichiometries, and using target materials efficiently.

[0008] The present invention seeks to alleviate one or more of the above problems.Alternatively or additionally, the present invention seeks to provide an improved method of forming a crystalline layer on or on a surface of a substrate. Summary of the invention

[0009] According to a first aspect of the present invention, there is provided a method for forming a crystalline layer on a surface of a substrate or a surface supported by a substrate, the crystalline layer comprising lithium, at least one different metal and counter ions. The method comprises sputtering material from each target onto a substrate using a plasma. A first target assembly is composed of one or more targets, each of which comprises lithium. A second target assembly is composed of one or more targets, each of which comprises a metal different from lithium, such as a transition metal. Plasma is generated using a remote plasma generator. The plasma is preferably generated away from the first target assembly and away from the second target assembly. The method comprises sputtering material from the first and second target assemblies onto a surface of a substrate or a surface supported by a substrate using a plasma. There is a first plume corresponding to a particle trajectory from the first target assembly to the surface, and there is a second plume corresponding to a particle trajectory from the second target assembly to the surface. The first target assembly is positioned non-parallel to the second target assembly. For example, the surface of the first target facing the plasma is planar, and the surface of the second target facing the plasma is planar, and the normal axes of the planes of such planar surfaces of the first and second targets are non-parallel. For example, such normal axes may converge with each other in a direction toward the surface of the substrate or the surface supported by the substrate. It may be the case that, at least for a cross section including a cross section of the first target assembly, the second target assembly and the substrate, the first target assembly is positioned non-parallel to the second target assembly. The cross section referred to may, for example, span a plane aligned with the length of the substrate and / or perpendicular to the plasma-facing surface of one or more targets. The first plume and the second plume converge at a region near the substrate surface or a surface supported by the substrate, at least as seen in the cross section above. A crystalline layer is formed on the surface at the region. Counterions to the crystalline material may be provided in gaseous form. The counterions may, for example, include oxygen.

[0010] Embodiments of the method according to this first aspect of the present invention can be used to in-situ manufacture multi-element crystalline materials on a surface. For example, the crystalline material can have a structure that provides excellent lithium ion mobility, and is therefore suitable for forming cathode materials for energy cells in lithium ion batteries. (Although batteries are mentioned herein, it should be understood that the present invention can be applied to other products or devices that may benefit from the use or inclusion of crystalline materials including lithium atoms / ions). The method of the present invention achieves such results by combining the use of remote plasma, the use of different targets for different elements required in the final crystalline material, and the geometry of the system. The plasma preferably contains argon ions. The remotely generated plasma allows the plasma energy to be controlled independently of the target. High-energy plasma can be generated, limited and controlled without interacting with any target, which is different from the prior art that may rely purely on target bias to generate plasma at the target. Sputtering can be achieved by applying a negative accelerating voltage (referred to herein alternatively as "bias power") to the target, which accelerates plasma ions toward the target and enters the target, thereby generating excited ions to sputter from the target. The sputtering threshold (plasma energy at the beginning of sputtering) depends on the target material. In general, the applied bias power determines the acceleration field of the ions in the plasma, which determines their bombardment energy and, therefore, the amount of sputtered material. Compared to transition metals such as cobalt, elemental lithium materials generally have lower sputtering yields, measured as the number of atoms produced per ion received at the surface at a given energy.

[0011] Thus, using a remotely generated plasma distinguishes the plasma generation process from the sputtering process, allowing for fine control of the kinetic energy of the sputtered material, for example on a per-target basis.

[0012] The size and geometry of the targets, the configuration of multiple targets relative to each other, and nearby magnetic and electric fields affect the geometry of the plumes and their charged ion concentrations.

[0013] The geometry of the plumes and how they mix and converge affects the stoichiometry of the material deposited on the surface. Tilting the targets relative to each other and to the substrate helps control the geometry of the plumes and, therefore, the stoichiometry of the deposited material.

[0014] The proportion of counter ions relative to the proportion of lithium ions can be independently controlled by means such as by controlling the flow of a gas into the plasma when the counter ions are produced by ionizing such a gas through the plasma.

[0015] Furthermore, providing a system / method that can control and / or configure these individual process parameters independently of one another facilitates depositing crystalline materials having a desired stoichiometry and having a desired crystalline phase.

[0016] In an embodiment of the present invention, the material is deposited directly on the surface of the substrate or on a surface supported by the substrate, so that the crystalline material is formed in situ when the material is deposited. Therefore, the crystalline material can be directly formed without substantially requiring an annealing step.

[0017] At least a portion and optionally all of the deposited material may have a hexagonal crystal structure. At least a portion and optionally all of the deposited material may have a crystalline "layered oxide" structure. This "layered oxide" structure is important when making solid-state batteries, such as lithium-ion batteries. The layered oxide structure makes it easier for lithium ions to escape from the crystal structure, thereby achieving faster charging, higher capacity solid-state batteries. It can also help maintain a stable crystal structure when lithium ions migrate out.

[0018] It is understood that intercalation refers to allowing ions to easily move in and out of a material without the material changing its phase (chemical and crystal structure). For example, a solid intercalation film remains solid during discharge and charge of an energy storage device.

[0019] According to the present invention, the crystalline material formed on the surface includes lithium, at least one different metal and at least one counter ion. The crystalline material can be in the form of a layered oxide structure (or skeleton), defined by the chemical formula LiBO2, wherein B is a different metal and the oxide is formed by the at least one counter ion. The different metals ("B") can be one or more redox active transition metals, one or more transition metals or mixtures thereof. Elemental metals in the so-called "post-transition metal" group, such as aluminum, can also be incorporated into the layered oxide skeleton. The different metals can include one or more of iron, cobalt, manganese, nickel, titanium, niobium, aluminum and vanadium. Cobalt is a preferred choice, for example, to produce crystalline LiCoO2.

[0020] Where the deposited material is LiCoO2, the material is optionally deposited in a hexagonal and / or rhombohedral lattice structure, optionally with The form in the space group Fd3m (also called "R3(bar)2 / m" space group or space group 166). This structure has many advantages, such as high available capacity and high charge and discharge speed compared to the low energy structure of LiCoO2 with the Fd3m space group structure (face-centered cubic structure). Space groups are believed to have better performance in typical battery applications due to higher reversibility and less structural changes during lithium insertion and extraction. Crystalline LiCoO2 in space group A is beneficial for solid-state battery applications.

[0021] During the execution of the method, the crystalline material can be grown essentially epitaxially from a surface on or supported by a substrate. Epitaxial growth is advantageous because it allows lithium ions to be more easily intercalated and deintercalated. In the case where the material is LiCoO2, the crystals are optionally aligned with (101) and (110) planes that are substantially parallel to the substrate. This is beneficial because it means that the ion channels of the film are oriented perpendicular to the substrate, making it easier for ions to be intercalated and deintercalated from the battery. This improves the working capacity and charging speed of the battery pack.

[0022] Embodiments of the present invention can be used to deposit Li a M1 b M2 c A crystalline material of O2, wherein the amount of lithium "a" is 0.5 to 1.5 (optionally 1), M1 is one or more transition metals (optionally one or more of cobalt, iron, nickel, niobium, manganese, titanium and vanadium), b is the total amount of the transition metal, M2 is, for example, aluminum, and c is the total amount of M2 (optionally zero). Optionally, a is 1, b is 1, and c is 0. Optionally, M1 is one of cobalt, nickel, vanadium, niobium and manganese.

[0023] Optionally, a is greater than 1 - such materials are sometimes referred to as "lithium-rich" materials. For example, such lithium-rich materials may be Where x = 0, 0.06, 0.12, 0.2, 0.3 and 0.4.

[0024] Another such material is The value of y is greater than 0.12 and equal to or less than 0.4.

[0025] Another such material is wherein x has a value equal to or greater than 0.175 and equal to or less than 0.325; and y has a value equal to or greater than 0.05 and equal to or less than 0.35.

[0026] is another such material wherein x is equal to or greater than 0 and equal to or less than 0.4; y is equal to or greater than 0.1 and equal to or less than 0.4; and z is equal to or greater than 0.02 and equal to or less than 0.3.

[0027] All lithium targets are considered to belong to the first target assembly. All targets containing the same different metal (or alternatively any non-lithium metal target) are considered to belong to the second target assembly. There may optionally be a third target assembly consisting of one or more targets, each comprising a different metal than the targets of the first and second target assemblies.

[0028] As described above, elemental lithium materials generally have a relatively low sputtering yield compared to other metals, measured as the number of atoms produced per ion received at the surface at a given energy. For example, for a given area, the targets of a first target assembly may receive more plasma energy than the targets of a second target assembly - for example, when the targets are of comparable size. For each target, more plasma energy may be received at the targets of the first target assembly than at the targets of the second target assembly. When viewed in the same cross section as described above, for a 1 mm strip of the target with 0.5 mm on either side of the cross section, the targets of the first target assembly receive greater total plasma energy than the targets of the second target assembly.

[0029] The targets may be arranged in pairs, with one target of the pair belonging to a first target assembly and the other target of the pair belonging to a second target assembly.

[0030] More plasma energy may be received at the target of the first target assembly (the target comprising lithium) than at the target of the second target assembly (the target comprising at least one transition metal), for example due to different bias voltages. Additionally or alternatively, this may be the result of, for example, the first target assembly being exposed to more plasma to a greater extent than the second target assembly. The first target assembly may be closer, on average, to the highest energy region in the plasma than the second target assembly. The target of the first target assembly closest to the highest energy region in the plasma may be closer to that region than the target of the second target assembly closest to the highest energy region.

[0031] For any given cross section through a majority of the width of the plasma, the targets of the second target assembly are at a different angle to the horizontal plane than the targets of the first target assembly.

[0032] One or more targets of the first target assembly may include different regions of the element lithium. One or more targets of the second target assembly may include different regions of elemental material, such as different regions of the element cobalt. "Different regions" may refer to the target itself or to a region of the target. There may be a composite target body including multiple different regions of different materials. Such a composite target body may therefore include targets of both the first target assembly and the second target assembly.

[0033] The targets of the first target assembly face the substrate in a first direction. In use, this direction may be considered to be the surface normal at the middle of the surface of the target facing the substrate. The adjacent target of the second target assembly may face the substrate in a second direction. Preferably, the first and second directions converge toward the substrate, as this may help control the convergence of the plume. In a cross section (the above cross section including the cross sections of the first target assembly, the second target assembly and the substrate), there may be a first imaginary line that is parallel to the first direction and extends from the center of the target surface of the first target assembly. In the same cross section, there may be a second imaginary line that is parallel to the second direction and extends from the center of the target surface of the second target assembly. Preferably, the first imaginary line intersects the second imaginary line at a position closer to the substrate / surface than to either target. In certain embodiments of the present invention, the directions facing the targets (when viewed in cross section) converge toward the substrate / surface and intersect each other at a position closer to the substrate than to either target. The location of intersection may be farther from the target than from the substrate. For example, the location of intersection may be at a position on the other side of the substrate opposite to the target (in the case where all such targets are on the same side of the substrate). In this case, the location of intersection may also be closer to the substrate than half the shortest distance from either target to the substrate.

[0034] The surface of the target of the first target assembly facing the substrate may be planar. In some embodiments, the surface of the target of the first target assembly facing the substrate may be curved, such as convex or concave. The surface of the target of the second target assembly facing the substrate may be planar. In some embodiments, the surface of the target of the second target assembly facing the substrate may be curved, such as convex or concave.

[0035] As used herein, the term substrate includes any structure having an exposed surface on which a film or layer is deposited, for example, to form an energy storage device. The term substrate is understood to include semiconductor wafers, plastic films, metal foils, thin glass, mica or polyimide materials, and other structures on which energy storage devices can be manufactured according to the description provided in the present disclosure. The term substrate is also used to refer to a structure in the process, which includes other layers that have been manufactured thereon. The substrate may include doped and undoped semiconductors, epitaxial semiconductor layers supported by substrate semiconductors or insulators, and other semiconductor structures familiar to those skilled in the art. Substrates are also used herein to describe any starting material that can be used for the manufacturing methods described in the present disclosure.

[0036] The materials may be deposited on opposite sides of the substrate simultaneously or sequentially.

[0037] The substrate may be flexible. The substrate may include a polymer material, such as a polymer substrate film having a thickness of 0.5 to 10 μm. The substrate may include a polymer carrier. The support is typically used to mechanically support other components of the substrate, if any such components are present, and to help it resist tensile and shear stresses. The substrate may include polyethylene terephthalate (PET) or polyethylene naphthalate (PEN). PEN and PET are quite flexible and have relatively high tensile strength due to their semi-crystalline structure.

[0038] The method may include depositing sputtered material on a first portion of the substrate, thereby forming crystalline material on the first portion of the substrate. The method may also include subsequently moving the substrate and depositing sputtered material on a second portion of the substrate, thereby forming crystalline material on the second portion of the substrate. The substrate may be stationary at some of the time that material is deposited thereon.

[0039] The substrate and at least one of the first and second target assemblies are moved as the crystalline layer is formed on the surface. For example, the substrate may be moved continuously while the material is deposited thereon. The substrate may be moved relative to the target assembly while the crystalline layer is formed on the substrate. The target may also be moved. The target may be moved slower than the substrate, so that the substrate also moves relative to the target. The particle plume may sweep across the substrate surface or a surface supported by the substrate.

[0040] The substrate may comprise a sheet or be in the form of a sheet, optionally an elongated sheet. Such a sheet may be provided in the form of a roll. This facilitates simple storage and handling of the substrate. The substrate may comprise a sheet or be in the form of a sheet, optionally an elongated sheet. Such a sheet may be provided in the form of a roll. This facilitates simple storage and handling of the substrate. Alternatively, the substrate may be provided in the form of discrete sheets, which are handled and stored in relatively flat sheets. When the material is deposited on the substrate, the shape of the substrate may be planar. This may be the case when the substrate is provided in the form of discrete sheets, which are not transferred to or from a roller. The sheets may each be mounted on a carrier having greater structural rigidity. This may allow the use of a thinner substrate than in the case of a substrate film held on a roller.

[0041] The substrate may be movably mounted to facilitate movement of the substrate (optionally in sheet form). The substrate may be mounted in a roll-to-roll manner. The substrate upstream of the plasma deposition process may be held on a roller or drum. The substrate downstream of the plasma deposition process may be held on a roller or drum. This facilitates simple and rapid handling of flexible substrates. A baffle may be provided to allow a portion of the substrate to be exposed to the remotely generated plasma.

[0042] At least a portion of the substrate may be carried by a rotating drum.The method may include the steps of unwinding the substrate from a roll of material, and conveying the substrate to a location where a sputter deposition technique is performed.

[0043] When the material is deposited on the substrate, the shape of the substrate may be curved. This may be the case when the substrate is in the form of a roll of material, carried by a roller or otherwise transferred to or from a reel. In the same cross-section as previously described, the substrate may have a radius of curvature at the region where the first plume and the second plume converge. The targets are arranged circumferentially around the substrate, preferably around the center of such radius of curvature of the substrate.

[0044] The substrate may have a width and a length, the length being longer than the width. The aforementioned cross section may be perpendicular to the width of the substrate and / or may be parallel to the length of the substrate. There may be a step of conveying the substrate along a predetermined path, which is not parallel to the width of the substrate. The path may be curved, at least partially curved. The substrate may be in the form of a sheet, for example conveyed at least partially along a predetermined path by one or more rollers. When the crystalline layer is formed on the substrate, the substrate may be supported by rollers.

[0045] The substrate may be conveyed along a predetermined path as material is sputtered from the target onto the substrate. The predetermined path can be defined by a line contained within the cross-sectional plane.

[0046] The substrate may be movably mounted to facilitate movement of the substrate. The substrate may be mounted in a roll-to-roll manner. The substrate upstream of the plasma deposition process may be held on a roller or drum. The substrate downstream of the plasma deposition process may be held on a roller or drum. This facilitates simple and rapid handling of elongated flexible substrates. A baffle may be provided to allow a portion of the substrate to be exposed to the remotely generated plasma.

[0047] Using a roll-to-roll arrangement has many possible advantages. It facilitates high material throughput and allows a large cathode area to be deposited on a large substrate, although a series of depositions are performed on the first portion of the substrate, followed by the second portion of the substrate, and so on. One of the main advantages of a roll-to-roll process is that it allows a large number of depositions to be performed without breaking the vacuum. This saves both time and energy compared to systems that require the chamber to be returned from vacuum to atmospheric pressure after deposition in order to load a new substrate.

[0048] The plasma deposition process may be performed in a chamber. The upstream roller or roll for carrying the substrate may be located in the chamber or outside the chamber. The downstream roller or roll for carrying the substrate may be located in the chamber or outside the chamber.

[0049] The substrate may optionally not exceed its temperature corrected yield strength at any point as it passes between the upstream and downstream rollers or drums. This is important because roll-to-roll processing machines require the substrate to be under tension as it is fed through the various rollers, rolls, and drums. As the polymer heats up, its yield strength may begin to decrease. If the polymer temperature rises too much, the polymer may begin to deform as it passes through the roll-to-roll machine. This may cause deformation, clogging, and / or uneven deposition on the substrate.

[0050] During the plasma deposition process, the temperature of the substrate may not exceed 500 degrees Celsius at any time, and optionally may not exceed 200 degrees Celsius.

[0051] The step of depositing the material onto the substrate using the sputtering deposition technique can be performed at a temperature such that an area of ​​1 cm 2 The maximum temperature reached by any given square of substrate material at any given time, measured on the surface opposite to the surface on which the material is deposited and averaged over a period of 1 second, may not exceed 500°C, optionally not exceed 300°C, optionally not exceed 200°C, optionally not exceed 150°C, optionally not exceed 120°C and optionally not exceed 100°C.

[0052] The method may also optionally include sputtering the material using oxygen as a reactive gas under a reactive sputtering regime.

[0053] In the reactive sputtering method, the reactive gas is introduced into the process together with an inert sputtering gas. The inert sputtering gas can be argon. This allows the use of elemental targets and the formation of oxides during the plasma sputtering process. In general, the structure and form of the produced oxide can be adjusted by providing the reactive oxygen gas at a higher or lower flow rate.

[0054] The ratio of the power used to generate the plasma to the power associated with the bias voltage on the target may be greater than or equal to 1:1, optionally less than or equal to 7:2, optionally less than or equal to 3:2. Applicants have found that such a power ratio may be advantageous for depositing crystalline material without the need to anneal the material so deposited.

[0055] The actual power in the plasma may be less than the power used to generate the plasma. In this regard, the efficiency of plasma generation ([actual power in the plasma / power used to generate the plasma]×100) may typically be 50% to 85%, typically about 50%.

[0056] Remotely generated plasma can be highly energetic.

[0057] The remotely generated plasma may be high density. In this regard, the plasma may have a density of at least 10 11 cm-3 ion density.

[0058] The power density associated with the target bias voltage is optionally greater than 1 W cm -2 , and optionally up to 100Wcm 2 .

[0059] The surface on which the material is deposited may have an X S or less surface roughness, where X S = 100 nm, and the deposited material may form a layer having a thickness of 0.01-10 μm and a surface roughness not exceeding X1, where X1 is equal to F and X S where F is a factor in the range 1-2.

[0060] X S It can be no more than 10% of the substrate thickness. S The product of the number of 5 nm 2 .

[0061] The substrate, optionally a polymeric substrate, may be provided with embedded particles and of all embedded particles in or on the polymeric material, the particles contributing to the surface roughness of the substrate have a majority having a median size of 10% to 125% of Xs.

[0062] Alternatively, the substrate, optionally a polymeric substrate, may be provided with embedded particles and of all embedded particles in or on the polymeric material, the majority of particles contributing to the substrate surface roughness have a median size of not less than 150% of Xs.

[0063] The method may include the step of depositing a material onto the surface using sputter deposition to form a further layer having a thickness of from 0.01 to 10 μm and not exceeding X S The surface roughness of 150%, the material composition of the crystalline layer is different from the material composition of the other layer.

[0064] The electron density distribution of the plasma is relatively uniform for different cross-sections taken over its volume. Magnets and / or electrostatics can be used to constrain or limit the plasma to have a certain overall shape, the width and / or length of the overall shape is much greater than its thickness. The width and length of the plasma cloud can each be at least five times the thickness. The plasma can have a width aligned with the width of the substrate. There can be a pair of antennas on opposite sides of the plasma, separated by a distance L (the length direction of the plasma), each antenna having a length W (the width direction of the plasma). The thickness of the plasma can be defined by the maximum range of the glow in the visible spectrum or the maximum distance measured in the direction perpendicular to L and W, which covers 90% of the free electrons in the plasma.

[0065] The generation of the plasma may be performed by at least one antenna extending in a direction parallel to the width of the substrate. Preferably there is a pair of such antennas. Preferably, the or each antenna extends across most of the width of the substrate, possibly at least substantially the entire width of the substrate.

[0066] Magnetic and / or electrostatic fields may be used to confine the plasma, for example, so as to extend and propagate proximate to the target and within a substantially common plane of the target and substrate.

[0067] The magnetic and / or electrostatic fields may confine the plasma by propagating the plasma in a direction transverse to the width of the substrate.

[0068] The method preferably includes using a magnetic field and / or an electrostatic field to confine the plasma so that the electron density distribution of the plasma forms a blanket and / or a sheet (e.g., a confined plasma cloud, although not necessarily planar in shape, has a thickness that does not vary significantly along at least one of the width and length of the plasma cloud). The plasma can be confined to form a sheet and / or a blanket extending in a direction along the width of the substrate and in a direction along the length of the substrate.

[0069] The working distance between the at least one target of the first target assembly and the substrate may be within + / - 50% of the theoretical mean free path of the system.

[0070] Without wishing to be bound by theory, it is believed that the working distance has an effect on the "ad atom" energy of the sputtered material when deposited onto the substrate. Where the working distance is greater than the mean free path of the system, it is believed that ions in the sputtering flux are more likely to collide before reaching the substrate, resulting in relatively low "ad atom" energies. Conversely, if the working distance is shorter than the mean free path of the system, the "ad atom" energy is relatively high. The difference in the separation of the individual targets of the first and second target assemblies from the substrate can be used as an additional control over the stoichiometry of the deposited material.

[0071] The definition of mean free path is the average distance between ion collisions in a plasma. The mean free path is calculated based on the volume of interaction (which varies with the operating distance) and the number of molecules per unit volume (which varies with the operating pressure).

[0072] The working distance is optionally at least 3.0 cm, optionally at least 4.0 cm and optionally 5.0 cm. The working distance is optionally no more than 20 cm, optionally no more than 15 cm, and optionally no more than 13 cm. The working distance may be from 4.0 cm to 13 cm, optionally from 6.0 cm to 10 cm, and optionally from 8.0 cm to 9.0 cm. The working distance between the at least one target of the first target assembly and the substrate may be from 5 cm to 20 cm.

[0073] The operating pressure may be from 0.00065 mBar to 0.010 mBar, optionally from 0.001 to 0.007 mBar. Higher operating pressures within this range may result in higher deposition rates. This is because higher operating pressures result in more process ions (usually Ar+) bombarding the target surface, so material is sputtered from the target at a higher rate.

[0074] When the working distance is 8.0 to 9.0 cm, the available crystallite size range can be narrower, for example, if a working pressure of 0.0010 mBar to 0.0065 mBar is used. The crystallite size can be 14 to 25 nm. This demonstrates that within these parameter ranges, thin films with a narrow and predictable film range can be formed.

[0075] The working distance between the at least one target of the second target assembly and the substrate may be within + / - 50% of a theoretical mean free path of the system.

[0076] The working distance between the at least one target of the first target assembly and the substrate may be within + / - 50% of the working distance between the at least one target of the second target assembly and the substrate.

[0077] The thickness of the crystalline layer formed on the surface may be 0.001 to 10 μm, optionally 0.5 to 10 μm. When the method is completed, the thickness of the deposited material may not exceed 1.0 micrometer.

[0078] The substrate may have a thickness of up to 10 μm. For example, the substrate may have a thickness of 0.1 to 10 μm. The thickness of the substrate may optionally be no more than 1.6 microns. The thickness of the substrate may optionally be less than 1.0 microns, such as 0.9 microns.

[0079] This is beneficial when designing a solid-state battery that is as thin as possible for the substrate (if the substrate is to form part of the final product). This allows the manufacture of batteries with higher energy density. Preferably, if thinner substrates become available that meet the preferred requirements of relatively high temperature corrected yield strength and / or high degradation point, such substrates will be used in this method.

[0080] The substrate may be retained as part of an end-use electronic product or component.

[0081] The substrate may be a sacrificial substrate. The substrate may be removed before the material layer. Some or all of the substrate may be removed before the crystalline layer or a portion thereof is integrated into an electronic product package, component, or other final product. For example, the crystalline material layer may be peeled off from the substrate. There may be other intermediate material layers between the base substrate and the crystalline material. This layer may be peeled off with the crystalline material or assist in the separation of the crystalline material from the base substrate. Laser-based peeling techniques may be used. The substrate may be removed by a process utilizing laser ablation.

[0082] Similar techniques are described in the prior art. For example, KR20130029488 describes a method for manufacturing a battery pack, including the use of a sacrificial substrate and laser radiation to harvest the battery layers.

[0083] According to another aspect of the invention, there is provided a method of manufacturing an electronic component, comprising forming a multilayer sheet of different materials, integrating the multilayer sheet or a portion thereof into an electronic product. At least one layer of the sheet is preferably a crystalline layer of a conductive or semiconducting material made by performing the method of the invention as described or claimed herein. The electronic component may be a battery, a functional layer of a battery, an energy storage device or a cell of a battery.

[0084] According to another aspect of the present invention, a battery pack is provided, comprising one or more crystalline material layers formed by performing the method of the present invention as described or claimed herein. Such a battery pack may include a plurality of stacked cathode layers, a plurality of stacked electrolyte layers, and a plurality of stacked anode layers. At least two of the plurality of stacked cathode layers may be made by performing the method of the present invention as described or claimed herein.

[0085] It will of course be appreciated that features described in relation to one aspect of the invention may be incorporated into other aspects of the invention. For example, the method of the invention may incorporate any features described with reference to the apparatus of the invention, and vice versa. BRIEF DESCRIPTION OF THE DRAWINGS

[0086] Embodiments of the invention will now be described, by way of example only, and with reference to the accompanying schematic drawings which can be briefly summarized as follows.

[0087] Figure 1ais a schematic side view of a plasma deposition chamber used according to a first example;

[0088] Figure 1b The steps of a method of manufacturing a battery cathode according to a first example are shown;

[0089] Figures 1c to 1h It is a schematic cross-sectional view of various polymer substrate materials;

[0090] Figure 2a is a schematic side view of a plasma deposition chamber used according to a second example method;

[0091] Figure 2b is an X-ray diffraction (XRD) spectrum of a first sample of a battery cathode manufactured according to the method of the second example;

[0092] Figure 2c is the Raman spectrum of the battery cathode, from which Figure 2b XRD data of

[0093] Figure 2d is an XRD spectrum of a second sample of a battery cathode manufactured according to the method of the second example;

[0094] Figure 2e is the Raman spectrum of the battery cathode, from which we obtain Figure 2d XRD data of

[0095] Figure 3a is a schematic side view of a plasma deposition chamber used in a method according to a third example;

[0096] Figure 3b yes Figure 3a A schematic plan view of a plasma deposition chamber shown in FIG.

[0097] Figure 3c yes Figure 3a and 3b Another schematic side view of the plasma deposition chamber shown in ;

[0098] Figure 3d is a graph comparing the sputtering yields of cobalt and lithium as a function of energy;

[0099] Figure 3e is a schematic side view of a plasma deposition chamber used in a method according to a fourth example;

[0100] Figure 4a is a cross-sectional scanning electron micrograph of a battery cathode associated with a first sample prepared according to the method of the second example;

[0101] Figure 4bis a bird's-eye view of a scanning electron micrograph of a battery cathode associated with a second sample prepared according to the method of the second example;

[0102] Figure 5a is a schematic cross-sectional view through a battery cathode associated with a first sample prepared using the method of the fifth example;

[0103] Figure 5b is a schematic cross-sectional view through a battery cathode associated with a second sample prepared using the method of the fifth example;

[0104] Figure 5c The steps of a method for manufacturing a half-cell of a battery cathode according to a fifth example are shown;

[0105] Figure 6 is a schematic diagram of an example of a method of manufacturing a battery cell according to a sixth example;

[0106] Figure 7a is a schematic diagram of an example of a method of manufacturing a solid-state thin-film battery according to a seventh example;

[0107] Figure 7b is a schematic cross-sectional view through a solid-state thin film battery of a first sample according to a seventh example;

[0108] Figure 7c is a schematic cross-sectional view of a sample solid-state thin film battery manufactured by the second sample according to the seventh example;

[0109] Figure 8a is a schematic diagram of a method for determining an optimal working distance for a remote plasma deposition system configured for depositing a layered oxide material according to an eighth example;

[0110] Figure 8b Shown as Figure 8a a plurality of X-ray diffraction spectra collected as part of the method, wherein the characterization technique is X-ray diffraction, characterized by characteristic X-ray diffraction peaks associated with a layered oxide structure;

[0111] Figure 9a is a micrograph of a sample film formed according to a first example of the present invention;

[0112] Figure 9b is from Figure 9a X-ray diffraction spectra obtained for the films shown in;

[0113] Fig.10a schematically illustrates an example of a method of determining an optimal operating pressure for a remote plasma deposition system configured for depositing a layered oxide material according to a ninth example;

[0114] Fig.10b Shown as a reference Fig.10a two X-ray diffraction spectra collected as part of the described method, wherein the characterization technique is X-ray diffraction, characterized by characteristic X-ray diffraction peaks associated with layered oxide structures;

[0115] Fig.11a is an example of steps of a method of determining a crystallite size of a layered oxide material according to a tenth embodiment;

[0116] Fig.11b is a graph showing how to determine the crystallite size at different working pressures for a working distance of 16 cm according to a tenth example, showing the crystallite size of a plurality of films deposited according to the first embodiment;

[0117] Fig.11c is a graph showing how to determine the crystallite size at different working pressures for a working distance of 8.5 cm according to a tenth example, showing the crystallite size of a plurality of films deposited according to the first embodiment;

[0118] Fig.12 is a schematic diagram of a method for depositing a material on a substrate according to an eleventh example of the present invention;

[0119] Fig.13 is a schematic diagram of an example of a method for manufacturing a component for an electronic device according to a twelfth example;

[0120] Fig.14 is a schematic diagram of an example of a method for manufacturing a component for an electronic device according to a thirteenth example of the present invention;

[0121] Fig.15 is a schematic diagram of an example of a method of manufacturing a light emitting diode (LED) according to a fourteenth example of the present invention;

[0122] Fig.16 is a schematic diagram of an example of a method of manufacturing a permanent magnet according to a fifteenth example of the present invention; and

[0123] Fig.17 is a schematic diagram of an example of a method of manufacturing an electronic device including an indium tin oxide (ITO) layer according to a sixteenth example of the present invention. DETAILED DESCRIPTION

[0124] Figure 1a 1 is a schematic side view of a plasma deposition process apparatus used in a method for depositing a (crystalline) material onto a substrate according to a first example. The method is generally indicated by reference numeral 1001 and is Figure 1bSchematically shown in , the method comprises: generating 1002 a plasma away from one or more targets, exposing 1003 the one or more plasma targets to the plasma so that target material is sputtered from the one or more targets; and exposing 1004 a first portion of a substrate to the sputtered material so that the sputtered material is deposited on the first portion of the substrate, thereby forming a crystalline material on the first portion of the substrate. The method of depositing (crystalline) material onto a substrate can be performed as part of a method of manufacturing a battery cathode.

[0125] The crystalline material in this example is in the form of ABO2. In this example, the ABO2 material is in a layered oxide structure. In this example, the ABO2 material is LiCoO2. However, the method of this example has been shown to be applicable to a wide range of ABO2 materials. In other examples, the ABO2 material structure includes at least one of the following compounds (described here using non-specific stoichiometry): LiCoO, LiCoAlO, LiNiCoAlO, LiMnO, LiNiMnO, LiNiMnCoO, LiNiO, and LiNiCoO. These materials are potential candidate materials for manufacturing battery cathodes. Those skilled in the art will recognize that the stoichiometry can vary.

[0126] In this example, the ABO2 material is LiCoO2 and is deposited as a layer approximately 1 micron thick. In other examples, the ABO2 material is deposited as a layer approximately 5 microns thick. In further examples, the ABO2 material is deposited as a layer approximately 10 microns thick.

[0127] refer to Figure 1a , a plasma deposition processing apparatus is generally indicated by reference numeral 100 and includes a plasma target assembly 102, which includes a target 104, a remote plasma generator 106, a series of electromagnets 108 for confining the plasma generated by the remote plasma generator 106, a target power supply 110, a remote plasma source power supply 112, and a housing 114. The remote plasma generator 106 includes two pairs of radio frequency (RF) antennas 116. The housing 114 includes a vacuum outlet 120, which is connected to a series of vacuum pumps located outside the chamber so that a chamber 122 defined by the housing 114 can be evacuated. The housing 114 is also provided with a gas inlet 124, which can be connected to a gas source (not shown) to introduce one or more gases into the chamber 122. In other examples, the gas inlet 124 can be positioned on the surface of the target assembly 102. From Figure 1a It can be seen that the plasma is generated away from the target 104 .

[0128] In this example, the target 104 comprises the material LiCoO2. In short, the chamber 122 is evacuated until a sufficiently low pressure is reached. The power provided by the power supply 112 is used to power the remote plasma generator 106 to generate a plasma. Power is applied to the target 104 so that the plasma interacts with the target 104, resulting in the sputtering of LiCoO2 from the target 104 onto a substrate 128. In this example, the substrate 128 comprises a polymer sheet that is introduced into the housing 114 via an inlet 130 and is led out of the housing 114 via an outlet 132. Powered rollers 134 are used to help move the substrate 128. LiCoO2 is deposited on the substrate 128 as a crystalline (non-amorphous) material.

[0129] The apparatus 100 also includes a shield 136 for limiting deposition of sputtered material onto the substrate 128, and an input 138 for cooling the platen. The shield 136 allows a portion of the substrate 128 to be exposed to the sputtered material.

[0130] As described above, the powered roller 134 is used to help move the substrate 128 into and out of the plasma deposition apparatus 100. The powered roller 134 is part of a roll-to-roll substrate processing apparatus (not shown) that includes at least a first storage roller upstream of the plasma deposition apparatus 100 and a second storage roller downstream of the plasma deposition apparatus 100. The roll-to-roll substrate processing apparatus is a convenient way to process, store and move thin flexible substrates, such as the polymer substrates used in this example. This roll-to-roll system has many other advantages. It allows high material throughput and allows a large cathode area to be deposited on one substrate, although a series of depositions are performed on the first part of the substrate, followed by the second part of the substrate, and so on. In addition, this roll-to-roll processing allows a large amount of deposition to occur without breaking the vacuum. This saves both time and energy compared to systems that require the chamber to be restored from vacuum to atmospheric pressure after deposition in order to load a new substrate. In other examples, sheet-to-sheet processing is used instead of roll-to-roll processing, in which the substrate is provided with a support. Alternatively, the substrate can be provided in the form of discrete sheets that are processed and stored in relatively flat sheets. When the material is deposited on the substrate, the shape of the substrate can be planar. This may be the case when the substrate is provided in the form of discrete sheets, not transferred to or from a roller. The sheets can each be mounted on a carrier having greater structural rigidity. This can allow the use of a thinner substrate than in the case of a substrate film held on a roller. The substrate can be a sacrificial substrate. The substrate can be removed before the material layer. Before the crystalline layer or a portion thereof is integrated into an electronic product package, component or other final product, part or all of the substrate can be removed. For example, the crystalline material layer can be peeled off from the substrate. There may be other intermediate material layers between the base substrate and the crystalline material. This layer can be peeled off together with the crystalline material or help separate the crystalline material from the base substrate. Laser-based peeling techniques can be used. The substrate can be removed by a process utilizing laser ablation.

[0131] Similar techniques are described in the prior art. For example, KR20130029488 describes a method for manufacturing a battery pack, including the use of a sacrificial substrate and laser radiation to harvest the battery pack layer. In other examples, another suitable processing scheme is used, as long as it can have a sufficiently high production volume.

[0132] The polymer substrate 128 is under tension as it moves through the system, for example, being subjected to a tension of at least 0.001 N during at least a portion of the processing. The polymer is strong enough that it does not deform under tensile stress when the polymer is fed through a roll-to-roll machine. In this example, the polymer is polyethylene terephthalate (PET) and the substrate 128 has a thickness of 1 micron or less, 0.9 microns in the example. The substrate 128 is pre-coated with a current collector layer made of an inert metal. In this example, the inert metal used as the current collector layer is platinum. The yield strength of the PET film is strong enough that the substrate does not yield or plastically deform under the stress of the roll-to-roll processing equipment. The inert metal used in other examples may alternatively be gold, iridium, copper, aluminum or nickel.

[0133] Using such a thin polymer substrate is beneficial because it facilitates the fabrication of batteries with higher energy density. In other examples, a non-polymeric material is used, provided that it can be fabricated in a sufficiently thin and flexible manner to allow for high battery density and ease of handling post-deposition.

[0134] However, the plasma deposition process and subsequent manufacturing processes face technical challenges associated with using such thin layers.

[0135] Before the substrate 128 is so pre-coated, it has a surface roughness that is carefully designed so as to be (a) large enough to mitigate undesirable effects caused by electrostatic forces (e.g., increasing the force required to unwind the polymer film from the roller to which it is attached) and (b) small enough that the roughness does not cause problems when the material is deposited onto the substrate. In this example, the surface roughness is designed to be about 50 nm. It should be noted that the product of the thickness of the substrate (0.9 microns) and the surface roughness is 4.5×10 4 nm 2 , so in this example it is less than 10 5 nm 2 and less than 5×10 4 nm 2 It has been found that the roughness required to facilitate processing of thin films increases as thickness decreases. In general, it has been found that the roughness required to improve processing of thinner substrates (i.e., less than 10 microns, particularly less than 1 micron) increases as the thickness of the substrate decreases.

[0136] Figure 1c A typical thin film polymer is shown (not to scale) with a thickness of about 1 micron and with embedded particles providing roughness. The roughness of the surface features provided by the particles is at least 90 nm and may be higher. This is too rough for the particular example envisioned (although it may be acceptable for other examples).

[0137] Figure 1dOne way in which the desired roughness can be achieved is shown (not to scale). Spherical particles of polystyrene are embedded in a substrate material such that at least 90% of those particles that contribute to the substrate roughness protrude from the local substrate surface by no more than half the volume of the particle. The particles have a diameter of about 90 nm. Thus, most of the embedded particles that contribute to the substrate surface roughness have a median size of about 180% of the substrate surface roughness. In other examples, the embedded spherical particles are made of a different material, such as silicon oxide.

[0138] Figure 1e Shown (not to scale) is an alternative way in which the desired roughness may be achieved. Spherical embedded particles of polystyrene are present on the surface of the substrate material such that at least 90% of those particles contributing to the substrate roughness protrude from the local substrate surface by more than half the particle volume. Figure 1e The particles used in the examples are smaller than Figure 1d Particles used in the examples.

[0139] For example Figure 1d and 1e Examples such as those in are able to deposit high-quality thin films as crystalline materials on thin substrates in a manufacturing environment. The advantages of the presence of embedded particles are retained, but potential disadvantages can be avoided or reduced by carefully controlling the location and size distribution of such particles. Figures 1f to 1h Schematic diagram showing the formation of a crystalline material layer on the substrate surface corresponding to Figures 1c to 1e A cross section of the substrate is shown in FIG. Figures 1f to 1h The intermediate layer of metal current collector is omitted. Figure 1c and 1f The roughness of the substrate shown in posed a problem. The main protrusions caused by some embedded particles 152 led to shadowing and competing crystal growth, which was Figure 1f This is schematically shown by contrasting shading 154 in FIG. Such competing crystal growth aligned in conflicting directions can lead to discontinuities in the layer, which can affect the properties of the final product. In addition, there are surprisingly profound effects on the likelihood that the deposited material layer will delaminate from the substrate. This can be a result of poor contact between the deposited layer and the underlying substrate, in areas close to any embedded particles protruding from the mid-plane of the surface (denoted by Figure 1f The gap 156 in the figure is schematically shown), where the local roughness radius is smaller. In contrast, Figure 1g and 1h It can be seen that no such problem occurs. The surface roughness of the material deposited on the substrate is about 50nm.

[0140] The roughness of a substrate can be measured using a profilometer. This instrument has a fixed stylus. The surface to be measured is translated under the stylus, and the deflection of the stylus measures the surface profile, from which various roughness parameters are calculated.

[0141] Roughness can also be measured using a "non-contact" method. A suitable machine for measuring roughness is the "Omniscan MicroXAM 5000B 3d", which uses optical phase-shift interferometry to measure surface profile.

[0142] The roughness Ra can be calculated using the following formula:

[0143]

[0144] where, for n data points, the deviation y from the smooth surface is measured.

[0145] The surface roughness Sa of area A extending in the x- and y-directions can be calculated using the following formula:

[0146]

[0147] where Z is the deviation from a mathematically perfectly smooth surface.

[0148] In this example, the average surface roughness is measured by a non-contact method.

[0149] The remotely generated plasma is generated by power provided to the antenna 116 by the power supply 112. Therefore, there is a measurable power related to the power used to generate the plasma. The plasma is accelerated to the target by the electrically biased target 104, thereby generating an associated current. Therefore, there is a power associated with the bias on the target 104. In this example, the ratio of the power used to generate the plasma to the power associated with the bias on the target is greater than 1:1, and optionally greater than 1.0:1.0. Note that in this example, this ratio is calculated assuming a 50% power efficiency of the plasma generation source. The power associated with the bias on the target is at least 1 Wcm -2 .

[0150] In a further example, the ratio of the power used to generate the plasma to the power associated with the bias voltage on the target is greater than 1:1 and does not exceed 7:2, optionally 7.0:2.0. In a further example, the power associated with the bias voltage on the target is greater than 1:1 and does not exceed 3:2, optionally 3.0:2.0. In some examples, the power efficiency of the plasma generation source is taken as 80%. In some examples, the power associated with the bias voltage on the target is 10 W cm -2 In a further example, the power associated with the bias voltage on the target is 100 W cm -2 In a further example, the power associated with the bias voltage on the target is 800 W cm -2 In other examples, the efficiency of the plasma generating source may be different and the power ratio may be different.

[0151] When the LiCoO2 film is deposited on a substrate, it forms a crystalline film of LiCoO2. The crystalline structure formed on the substrate This structure is a layered oxide structure. Compared with the low energy structure of LiCoO2 with the Fd3m space group structure, this structure has many advantages, such as higher available capacity and higher charge and discharge rates. Space group Crystalline LiCoO2 is generally preferred for solid-state battery applications.

[0152] Throughout the plasma deposition process, the temperature of the substrate 128 does not exceed the degradation point of the polymer substrate 128. In addition, the temperature of the substrate is low enough throughout the deposition process so that the temperature-adjusted yield stress of the polymer substrate remains high enough so that the polymer substrate does not deform under the stress applied by the roll-to-roll processing machine.

[0153] The general shape of the confined plasma produced by the remote plasma generator 106 is given by Figure 1a 1 is shown by dashed line B in FIG. A series of electromagnets 108 are used to confine the plasma to the desired shape / volume.

[0154] It should be noted that while in this first example, the substrate 128 is fed into the chamber at the inlet 130 and exits the chamber at the outlet 132, alternative arrangements are possible. For example, a roll or other storage upstream of the baffle 136 may be within the processing chamber 122. A roll or other storage downstream of the baffle 136 may be internal to the processing chamber 122 or may be stored internal to the processing chamber 122.

[0155] Furthermore, the means 112 for powering the plasma source may be of RF, (direct current) DC or pulsed DC type.

[0156] In this first example, the target assembly 102 includes only one target 104. The target is made of LiCoO2. It should be understood that alternative and / or multiple target assemblies may be used, for example, including different regions of elemental lithium, different regions of elemental cobalt, different regions of lithium oxide, different regions of cobalt oxide, different regions of LiCo alloy, different regions of LiCoO2, or any combination thereof. In other examples, the ABO2 material may not be LiCoO2. In these examples, one or more target assemblies contain different A regions, different B regions, different regions of compounds containing A and / or B, and / or different regions containing ABO2.

[0157] For the avoidance of doubt, the target 104 of the target assembly 103 is used alone as a material source and does not function as a cathode when power is applied thereto from an RF, DC or pulsed DC power source.

[0158] In this example, the system has an operating pressure of 0.0050 mBar. The theoretical mean free path of the system is about 10 cm. The theoretical mean free path is the average distance between ion collisions in a plasma. The working distance between the target 104 and the substrate 128 is about 8.5 cm. Therefore, this working distance is about 85% of the theoretical mean free path of the system.

[0159] In this example, the working pressure is above a lower limit, below which crystalline material in the layered oxide structure does not form, but below an upper limit, above which observable damage to the substrate occurs. The working distance is shorter than an upper limit, above which crystalline material in the layered oxide structure does not form, and longer than a lower limit, below which the energy of the deposition causes observable damage to the substrate, or forms an unfavorable oxide state.

[0160] In this example, the average crystallite size of the crystallites formed on the film is about 20 nm. In other examples, the average crystallite size of the crystallites formed on the film is about 50 nm.

[0161] In an alternative example, the operating pressure of the system is 0.0020 mBar. The theoretical mean free path of the system is about 12 cm. The working distance between the target 104 and the substrate 128 is about 9 cm. Therefore, the working distance is about 75% of the theoretical mean free path of the system.

[0162] In an alternative example, the operating pressure of the system is 0.0065 mBar. The theoretical mean free path of the system is about 15 cm. The working distance between the target 104 and the substrate 128 is about 7.5 cm. Therefore, the working distance is about 50% of the theoretical mean free path of the system.

[0163] The second example method uses Figure 2a The device shown in FIG. will now be described Figure 1a equipment and Figure 2a The main difference between the devices. Figure 2a 1. It is shown that, instead of the flexible substrate 128 presented in the first example, a non-flexible flat glass substrate 228 is used. In addition, there is no roller in this example. The thickness of the glass substrate is in the order of millimeters. A single target 204 is used in this example. A thermal indicator label is attached to the surface of the glass slide opposite to the cathode material deposition surface. The thermal indicator label is configured to indicate whether the substrate 228 has experienced a temperature of 270°C or higher during the plasma deposition process. After deposition, the label indicates that the substrate has not experienced a temperature of 270°C or higher during the deposition process. The overall shape of the plasma is determined by Figure 2a The area enclosed by the dotted line B' is represented.

[0164] Table 1 shows the properties of the resulting exemplary battery cathode produced according to the second example:

[0165]

[0166] Table 1 – LiCoO2 cathode film properties versus deposition parameters

[0167] In Table 1 above, the elemental film compositions were determined by X-ray photoelectron spectroscopy using a Themo Fisher K-alpha spectrometer with a MAGCIS ion gun. The quoted compositions were taken from depth profiles measured at approximately 10 levels with the film. Plasma source power is the electrical power provided to generate the plasma. Sputtering power is the electrical power applied to the target 204. Process pressure is the pressure in the chamber. Film thickness and roughness measurements were made after deposition using an Omniscan MicroXAM 5000b 3d optical profiler. Film thickness was measured after deposition because step height at the mask edge and roughness measurements were made from a sample area of ​​approximately 400 microns by 500 microns.

[0168] Figure 2b The X-ray diffraction (XRD) spectrum of the battery cathode of Sample 1 is shown. CuKα radiation with nickel filtration was used. The structure of the films was characterized by X-ray diffraction using a diffractometer (Rigaku-Smartlab). The diffraction patterns were obtained at room temperature in the range of 10°<2θ<80° using a fixed incident angle of <5°. Data were collected using a step scan with a resolution of 0.04° / step and a counting time of 0.5 sec / step. The peak at approximately 37° is associated with the (101) plane of the crystal being oriented substantially parallel to the substrate surface. The peak at approximately 66° is associated with the crystal being oriented substantially such that the (110) plane is parallel to the substrate. The peak at approximately 55° is associated with the glass substrate and should be ignored for purposes of determining the crystal structure of LiCoO2.

[0169] The absence of additional reflections associated with the Fd3m space group is due to the deposited LiCoO2 Initial indices in space groups.

[0170] The peak associated with the (003) plane is also notably absent. This means that very few crystals are oriented in such a way that the (003) plane is parallel to the substrate surface. Crystals oriented in this way are rarely beneficial. A detailed explanation is beyond the scope of this application, but in short, the available capacity of the cathode increases when a higher proportion of crystals are arranged so that the (101) and (110) planes are parallel to the substrate, as opposed to being arranged so that the (003) plane is parallel to the substrate, because the apparent resistance to ion migration is lower. The crystals have been formed so that the longitudinal axis of the crystal is perpendicular to the substrate. In other words, the crystals are formed epitaxially.

[0171] Applicants have found that crystalline material is generally deposited if the ratio of the power used to generate the plasma to the power associated with the bias voltage of the target is greater than 1:1. In Sample 1, the ratio is 1800:500 (3.6:1), and in Sample 2, the ratio is 1800:800 (9:4). Note that in this example, the ratio is calculated assuming a 50% power efficiency of the plasma generation source.

[0172] In the comparative example, the experiment was repeated with a plasma source power of 1 kW and a power associated with the bias voltage to the target of 1 kW. The deposited material was essentially amorphous. The performance of the comparative example film as a cathode was investigated by depositing an electrolyte (LiPON in this case) and an anode metal on top of the cathode layer to manufacture a solid-state battery pack. The charge and discharge characteristics of the battery pack were investigated and found to be poor, with a cathode specific capacity of approximately 10 mAh / g. When similar batteries (such as those formed in Samples 1 and 2) were manufactured using crystalline LiCoO2, the charge and discharge characteristics were much better, with a typical cathode specific capacity of approximately 120 mAh / g.

[0173] Figure 2c The Raman spectrum of the battery cathode of Sample 1 is shown. The bonding environment of the membrane was characterized by Raman spectroscopy. Raman spectra were collected using a JY Horiba LabRAM ARAMIS imaging confocal Raman microscope using 532 nm excitation. Note that due to the non-physical nature of the peak sharpness, the 600 cm -1 The strong peak at 487 cm -1 The strong characteristic peaks observed at Space group crystal structure.

[0174] Figure 2d The XRD spectrum of the cathode of sample 2 (collected in the same manner as sample 1) is shown. The spectrum shown is similar to Figure 2b However, in Figure 2d In the graph, the relative intensity of the peak at about 66° is much stronger than that at 37°. This indicates that for sample 2, the number of crystals whose (110) planes are parallel to the substrate is higher than the number of crystals whose (101) planes are parallel to the substrate. This is beneficial because it means that the ion channels of the film are oriented perpendicular to the substrate, making it easier for ions to embed and de-embed from interstitial sites within the cathode crystal structure. This improves the available capacity and charge rate of the cathode. Figure 2e is the Raman spectrum of the cathode of sample 2; applicable to Figure 2c The same comments apply to Figure 2e .

[0175] Figures 3a to 3cAn alternative example of an apparatus used in another example of a method for producing a layer of crystalline material on a surface using plasma sputtering according to a third example is shown. The apparatus and method of production employed are similar to those described with reference to the first example. Only the significant differences will now be described. Identical parts are labeled with reference numerals sharing the same last two digits. For example, Figure 3a The rotating drum 334 and Figure 1a The same as the rotating drum 134 in. Figure 3a The apparatus includes a rotating drum 334 on which a polymer substrate 328 is supported within an area defined by a processing chamber 322 (for clarity, the walls of the chamber are omitted). The target assembly 302 includes a plurality of targets. A first target 304 consisting of elemental lithium and a plurality of targets 303 (now referred to as second targets) consisting of elemental cobalt are provided. The targets are all located at a working distance of about 10 cm from the substrate 328 (the working distance is the shortest spacing between them). The surface of each target 303, 304 facing the drum 334 is flat (and planar). The radius of the drum 334 is significantly greater than the working distance (for ease of illustration, the size of the drum 334 shown in the figure is relatively smaller than the actual size). The targets 303, 304 are arranged circumferentially around the circumference of the drum 334. The apparatus also includes a baffle 336 for limiting the deposition of sputtered material on the substrate 328.

[0176] A plasma of argon ions and electrons is generated by two spaced apart powered antennas 316. The plasma is confined and focused by a magnetic field controlled by two pairs of electromagnets 308, each pair of electromagnets being positioned close to one of the antennas 316 and the electric field generated by the system. The overall shape of the plasma (90% of its highest concentration is at Figure 3c 316) is in the shape of a blanket because the length and width of the plasma cloud are much greater than its thickness. The width of the plasma is controlled in part by the length of the antennas 316. The two pairs of antennas 316 are separated by a distance comparable to the length of the plasma. The length and width of the plasma are in the same general direction as the length and width of the substrate, respectively.

[0177] The plasma source is spaced from the target and can therefore be considered a remotely generated plasma. The theoretical mean free path of the system (i.e., the average distance between ion collisions in the plasma) is about 12 cm, meaning that most particles travel from the target to the substrate without colliding with any argon ions in the plasma.

[0178] Figure 3ais a partially schematic cross-sectional view showing a portion of a substrate traveling on a drum 334, and also schematically showing the trajectories of particles traveling from targets 303, 304 to the substrate. Thus, there is a first plume corresponding to the trajectory of particles from the first target 304 to the surface of the substrate 328 and a second plume corresponding to the trajectory of particles from the second target 303 to the surface of the substrate 328. The first plume is shown as a spotted area and each second plume is shown as a solid grey area. Figure 3a It can be seen that the first plume and the second plume converge in the area close to the substrate. Figure 3a It can also be seen in FIG. 1 that the first target 304 faces the substrate in a first direction (defined in this example by an imaginary line extending from the center of the surface of the target 304), and as shown in FIG. Figure 3a 303 faces the substrate in a second direction (defined in this example by an imaginary line extending from the center of the surface of the target 303). The first and second directions converge toward the substrate and intersect at a position just beyond the substrate (the position is about 3 cm outside the substrate). Oxygen is supplied to the processing chamber 322 through the inlet 325 at a controlled rate. The target is stationary while the substrate moves with the rotation of the drum. In other examples, an inert sputtering gas is introduced through the gas inlet (not shown here, but similar to Figure 1a The structure shown in is basically the same).

[0179] If there are distinct lithium oxide and cobalt oxide regions in targets 304, 303, the amount of oxygen introduced into the chamber may be reduced in some other examples, and in some examples the oxygen content in such targets may be high enough that no additional oxygen needs to be introduced into chamber 322 at all.

[0180] Figure 3b It is a view from the drum towards the target. Figure 3c 304 , the second target 303 , and the cross-sectional view of the substrate 328 on the drum 334 .

[0181] It can be seen that in Figure 3c (cross-sectional view), the first target 304 is angled relative to each second target 303.

[0182] When performing the method, the generated plasma is used to sputter material from the first target and from the second target onto the substrate.

[0183] like Figure 3dAs shown, the sputtering yield of elemental lithium material is lower than that of cobalt, measured as the number of atoms produced per ion received at the surface at a given energy (less than half at 10 keV). Therefore, the magnitude of the (negative) potential applied to the first target is greater than the potential applied to the second target. The first target also has a surface area exposed to the plasma that is slightly larger than the total area of ​​the second target. Therefore, the number of ionized Li atoms per unit reaching the substrate is essentially the same as the number of ionized Co atoms per unit reaching the substrate. There are also ionized oxygen atoms and electrons from the plasma. The high-energy particles generated by the remote plasma allow the in-situ formation of crystalline LiCoO2 material with a hexagonal crystal structure on the substrate surface.

[0184] The number of energetic particles from the plasma received at the first target 304 (over the entire surface area of ​​the target) is greater than the number of particles received at the second target 303 (the sum over the entire surface areas of the two second targets).

[0185] Figure 3e A schematic cross-sectional view of another example of an apparatus according to the fourth example is shown, similar to Figures 3a to 3c The apparatus shown in , but in which the targets are moved and arranged circumferentially in pairs around a drum 334. Each pair of targets (i.e., each assembly 302) is arranged to be tilted to face a position very close to the substrate on the drum. Each pair 302 includes a first target 304 of the element lithium and a second target 303 of the element cobalt. The targets are both located at a working distance of about 15 cm from the substrate, the working distance being the shortest spacing between them. The theoretical mean free path of the system (i.e., the average distance between ion collisions in the plasma) is about 20 cm. For each pair of targets (302), in use, there is a first particle plume from the first target (304) and a second particle plume from the second target (303), which converge at an area close to the substrate. The center of rotation of the main drum 334 is also the center of rotation of the targets. The targets move at an angular velocity around the center of rotation that is slower than that of the drum. The targets can be replaced as they move out of the plasma on a rotating basis, allowing material to be continuously deposited on a moving substrate.

[0186] Now refer to Figure 4a , 4b 5a describe an example of a battery cathode manufactured according to a second example. The substrate 428, 528 includes a current collecting layer 429, 529, in this case a platinum layer, on which a LiCoO2 layer 442, 542 is deposited. In other examples, another inert metal is used as the current collecting layer, such as gold, iridium, copper, aluminum, or nickel. In further examples, the current collecting layer can be carbon-based. In some examples, the current collecting layer is surface modified, and in some examples, the current collecting layer includes a rod-like structure.

[0187] like Figure 4a (Cross-sectional view of the first sample deposited film) and Figure 4b As shown in the scanning electron microscope (SEM) image of (aerial view of the deposited film of the second sample), the LiCoO2 film layers 442, 542 of both samples are polycrystalline in nature. Figure 4a , 4b The battery cathodes of 5a can also be manufactured according to the method of the third or fourth example.

[0188] Now refer to Figure 5a (First sample), Figure 5b (Second Sample) and Figure 5c A method for manufacturing a cathode half-cell according to a fifth example is described. The method is generally described by reference numeral 3001, and includes depositing 3002 a battery cathode material 542 onto a substrate (including a current collector layer 529 in this example), and depositing 3003 a battery electrolyte material 544 onto the battery cathode material 542. In this example, the material deposited for the electrolyte 544 is lithium phosphorus oxynitride (LiPON). In other examples, the deposited material is another suitable electrolyte material. In some samples of the fifth example of the present invention (e.g., the second sample), the half-cell may include an electrode material 544, while in other samples of the fifth example, the half-cell may not include an electrode material 544 (e.g., the first sample).

[0189] In this example, LiPON is deposited using a remotely generated plasma in substantially the same manner as the ABO2 material in the first, second, third, or fourth examples. However, in this example, the target material used is Li3PO4 and the deposition occurs in an active nitrogen atmosphere. In other examples, the target assembly may include multiple targets with different regions of lithium and / or phosphorus containing compounds, elemental lithium, or lithium oxide. In other examples, deposition additionally occurs in an active oxygen atmosphere.

[0190] Now refer to Figure 6 An example of a method of manufacturing a solid-state battery cell according to a sixth example is described. The method is generally indicated by reference numeral 5001 and includes manufacturing 5002 a cathode half-cell according to the fifth example (e.g., as described above with reference to Figure 5b and 5c ), and contacting the cathode half-cell with an anode 5003. In this example, the anode is deposited by a convenient method, including remote plasma sputtering, magnetron sputtering, CVD, etc. In other examples, the anode is deposited by thermal evaporation, electron beam evaporation, pulsed laser deposition, or simple DC sputtering.

[0191] Now refer to Figure 7aAn example of a method of manufacturing a solid-state battery pack according to a seventh example is described. The method is generally indicated by reference numeral 6001 and includes manufacturing 6002 a plurality of cathode half-cells of a solid-state thin film battery pack, manufacturing 6003 a plurality of anode half-cells of a solid-state thin film battery pack, and contacting the cathode and anode half-cells with each other 6004 to form at least one battery pack. The battery pack thus manufactured according to the first sample of the seventh example of the present invention is schematically shown in Figure 7b Reference Figure 7b , 628 and 628' are substrate materials, 629 and 629' are current collecting layers, 642 is the cathode material, in this case LiCoO2, and 644 is LiPON, which acts as both electrolyte and anode.

[0192] Alternatively, in other examples, the current collector material acts as the anode material. Alternatively, in the second sample of the seventh example of the present invention, additional anode material may be deposited. Figure 7c Reference Figure 7c , 628 and 628' are substrate materials, 629 and 629' are current collecting layers, 642 is the cathode material, in this case LiCoO2, 644 is LiPON, which acts as an electrolyte, and 646 is a suitable anode material.

[0193] Now refer to Figure 8a An example of a method for determining an optimal working distance for a remote plasma deposition system configured for depositing a layered oxide material according to an eighth example is described. The method is generally described by numeral 7001 and includes:

[0194] Select a 7002 working distance range where the working distance within the range is + / - 50% of the theoretical mean free path of the system,

[0195] For a plurality of test samples, for each corresponding sample, performing 7003 a method of depositing material according to the first example at a different working distance within a selected range,

[0196] Perform 7004 characterization techniques that are able to determine the characteristics of the layered oxide structure on each test sample after deposition has occurred,

[0197] Identify 7005 samples that have characterizing properties;

[0198] From those samples, the sample in which the (normalized) intensity of the characteristic peak is the highest is selected 7006, and then the working distance reached by the system used during deposition of the test sample is selected 7007.

[0199] In this eighth example, the characterization technique used is X-ray diffraction and the characterizing feature is a diffraction peak or a series of diffraction peaks. Figure 8bA plurality of X-ray diffraction patterns recorded for films deposited at different working distances are shown. From the top diffraction pattern to the bottom diffraction pattern, the working distances are 5 cm (731), 8 cm (733), 12 cm (735), and 15 cm (737), respectively. As can be seen from the figure, the working distance of 8 cm shows the highest intensity peak 733 at 19 degrees 2theta (this is one of the peak positions 739 required for hexagonal LiCoO2, and this particular peak does not exist in the cubic or spinel structure of LiCoO2). Therefore, in this example, 8 cm is selected as the working distance. In other examples, different characterization techniques other than X-ray diffraction can be used. The intensity of the diffraction pattern 731 measured at a working distance of 5 cm is lower at 19 degrees 2theta than the intensity of the diffraction pattern 733 at a working distance of 8 cm. The diffraction patterns collected for working distances of 12 cm 735 and 15 cm 737 do not show the characteristic peak of hexagonal LiCoO2 at 19 degrees 2theta at all.

[0200] In some examples, the test sample of the method is replaced with an average of multiple test samples, including multiple test samples, where the method of the first example has been performed multiple times at the same working distance and the average is taken. In some examples, the method can be performed multiple times so that the range of the optimal working distance for operating the system can be found.

[0201] Figure 9a The sample formed according to the first example during the execution of the method of the eighth example is shown, and a damaged substrate surface (with an undesirable oxide) formed due to deposition when the working distance is too short is shown. In this example, the working distance is 5 cm and the deposited material is LiCoO2. As can be seen from the figure, no crystallites are formed on the entire substrate surface, and deformation of the substrate can be seen. In addition, at this working distance, it can be seen that an undesirable cobalt oxide phase Co(II)O region is formed on the substrate. This is caused by Figure 9b The spectrum shown in , which shows peaks associated with the Co(II)O phase (identified at two values ​​843 of 2theta) detected in the diffraction pattern 831 obtained for a sample with a working distance of 5 cm, in addition to the hexagonal LCO peak (identified at five values ​​839 of 2theta). A structural refinement model 831' containing hexagonal LiCoO2 and Co(II)O phases was obtained from the collected diffraction pattern 831. The difference between the diffraction pattern 831 and the refinement model 831' is shown by the difference line 841. Therefore, in the method of the eighth example, a working distance that is too short cannot be selected as the optimal working distance.

[0202] Now refer to Fig.10aAn example of a method for determining an optimal range of operating pressure for a remote plasma deposition system configured for depositing layered oxide materials according to a ninth example is described. The method is generally described by numeral 8001, wherein the method includes:

[0203] Select the initial working pressure range of 8002, from 0.00065mBar to 0.01mBar (also available from 0.001 to 0.007mBar),

[0204] For a plurality of test samples, for each corresponding sample, performing 8003 the method of depositing material according to the first example at a different working pressure within a selected range,

[0205] Perform 7004 characterization techniques that are able to determine the characterization properties of the layered oxide structure on each test sample after deposition has occurred,

[0206] selecting 8005 the test sample deposited at the lowest operating pressure from the group of test samples exhibiting characteristic features of layered oxide materials, and setting 8006 the operating pressure as the lower limit of the range,

[0207] The test sample deposited at the highest operating pressure is selected 8007 from the group of test samples that showed no observable signs of substrate damage, and the operating pressure is set 8008 as the upper limit of the range.

[0208] In this ninth example, the characterization technique used is X-ray diffraction, and the characterizing feature is a feature comprising characterizing X-ray diffraction peaks of the layered oxide material. Fig.10b An example X-ray spectrum is shown showing how this feature is absent below a particular operating pressure. In this example, the presence of a peak at 19 degrees 2 theta in pattern 947 of a sample deposited at 0.0046 mBar results in the formation of a hexagonal phase, while pattern 945 of a sample deposited at 0.0012 mBar does not result in the formation of a hexagonal phase, as shown by the absence of the peak. In other examples, characterization techniques other than X-ray diffraction may be used.

[0209] In a further example, the test sample of the method is replaced with an average value of multiple test samples, including multiple test samples, wherein the method of the first example has been performed multiple times under the same working pressure and the average value is taken.

[0210] In some examples, the method further includes selecting an optimal operating pressure for the system within a desired range. In this example, the optimal operating pressure is an operating pressure within the range that results in a highest deposition rate.

[0211] Now refer to Fig.11aAn example of a method for determining a crystallite size for depositing a layered oxide material according to a tenth example is described. The method is generally described by the numeral 9001, wherein the method includes:

[0212] Select the initial range of 9002 working pressure, from 0.00065mBar to 0.01mBar,

[0213] For a plurality of test samples, for each corresponding sample, performing 9003 the method of depositing material according to the first example at a different working pressure within a selected range,

[0214] Perform 9004 characterization techniques that determine the crystallite size of each film for each test sample after deposition has occurred,

[0215] For example, the selected operating pressure range may be from 0.001 to 0.007 mBar.

[0216] Fig.11b FIG. 1 is a graph showing that after the method of the tenth example is performed within a given working pressure range, for a working distance of 16 cm, the crystallite size range formed by multiple films deposited at different working pressures between 0.001 mBar and 0.0065 mBar according to the first example is different from FIG. 1 . Fig.11c Compared to the relatively wide curve graph.

[0217] Fig.11c FIG. 1 is a graph showing that after the method of the tenth example is performed within a given working pressure range, for a working distance of 8.5 cm, the crystallite size range formed by multiple films deposited at different working pressures between 0.001 mBar and 0.0065 mBar according to the first example is different from FIG. 1 . Fig.11b Compared to the relatively narrow curve graph.

[0218] A narrow distribution of crystallite size is beneficial because it makes the crystallite size of films deposited on an industrial scale both predictable and reproducible.

[0219] Now refer to Fig.12 An example of a method for depositing a material on a substrate according to an eleventh example of the examples is described. The method is generally described by numeral 1101 and includes:

[0220] A plasma 1102 is generated away from a plasma target suitable for plasma sputtering,

[0221] exposing 1103 one or more plasma targets to a plasma to produce sputtered material from the one or more targets,

[0222] A sputtered material is deposited 1104 on a first portion of the substrate.

[0223] The method of depositing a material on a substrate as described in the eleventh example includes all the features of the deposition of the first example, although in this example, the target material can be any material. In this example, the target material is crystalline, but in other examples, the deposited material can take a semi-crystalline form, or be amorphous.

[0224] A twelfth example is also presented, which is directed to a method of manufacturing a component for an electronic device including a substrate, and will now be referred to Fig.13 It is described. The method is generally described by the number 1201 and includes depositing 1202 a material onto a substrate using a method as described in the eleventh example. The method of the eleventh example in this example is performed multiple times 1203 to deposit multiple layers. In this example, at least some of the multiple layers can be semiconductor layers. In this example, the method is therefore a method for manufacturing a semiconductor device or a portion thereof. In this example, adjacent layers are deposited using different parameters and / or target materials for depositing each layer to produce an electronic device. In other examples, multiple layers of multiple material layers are deposited using substantially the same target material and parameters.

[0225] In this example, the substrate includes an intermediate layer, which can optionally serve as a current collecting layer. In other examples, there are more intermediate layers, which help adhesion during the deposition step. In some other examples, there is no intermediate layer. The deposition of the intermediate layer on the substrate is carried out according to the method described in the eleventh example. In other examples, the deposition of the intermediate layer on the substrate is carried out by another suitable deposition technique, such as sputtering, thermal evaporation, electron beam evaporation, pulsed laser deposition or other thin film deposition techniques.

[0226] In this example, the method includes depositing a first semiconductor material layer. In this example, the first semiconductor layer is deposited on the intermediate material layer. In other examples, the first semiconductor layer is deposited directly on the substrate. In this example, the first semiconductor layer includes silicon. In other examples, the first semiconductor layer includes aluminum, and in some other examples, includes gallium nitride. In examples where the semiconductor material layer is gallium nitride, the deposition occurs under a reactive nitrogen atmosphere. In this example, the first semiconductor material layer is n-type doped. In this example, this is achieved by sputtering a target containing a phosphorus-containing compound. In other examples, this is achieved by using different dopants such as arsenic, antimony, bismuth, or lithium. In some further examples, the semiconductor material layer is p-type doped with a dopant such as boron, aluminum, gallium, or indium. In further examples, the semiconductor material layer is not doped and is an intrinsic semiconductor. In some of these examples, the dopant material is not introduced as a sputterable target, but is introduced as a gas after deposition so that the dopant diffuses into the surface of the semiconductor layer.

[0227] In this example, the method includes depositing a second semiconductor material layer onto the first semiconductor material layer. In other examples, the second semiconductor material layer is deposited directly on the substrate or the intermediate layer (if present). In this example, the second semiconductor material layer is an intrinsic semiconductor. In this example, the second semiconductor material layer is gallium nitride. In a further example, the second semiconductor material layer is n-type doped with a dopant such as phosphorus, arsenic, antimony, bismuth or lithium. In some further examples, the second semiconductor material layer is p-type doped with a dopant such as boron, aluminum, gallium or indium. In some of these examples, the dopant material is not introduced as a sputterable target, but is introduced as a gas after deposition so that the dopant diffuses into the surface of the semiconductor layer.

[0228] In this example, the method includes depositing a third semiconductor material layer. In this example, the third semiconductor layer is deposited on the second semiconductor material layer. In other examples, the third semiconductor layer is directly deposited on the first semiconductor layer, the second semiconductor layer, the intermediate layer or the substrate. In this example, the third semiconductor layer includes silicon. In other examples, the third semiconductor layer includes aluminum, and in some other examples, includes gallium nitride. In some examples where the semiconductor material layer is gallium nitride, the deposition occurs under a reactive nitrogen atmosphere. In this example, the third semiconductor material layer is doped p-type. In this example, this is achieved by sputtering a target containing a boron-containing compound. In other examples, this is achieved by using different dopants such as aluminum, gallium or indium. In some further examples, the third semiconductor material layer is n-type doped with dopants such as phosphorus, arsenic, antimony, bismuth or lithium. In further examples, the third semiconductor material layer is not doped and is an intrinsic semiconductor. In some of these examples, the dopant material is not introduced as a sputterable target, but is introduced as a gas after deposition so that the dopant diffuses into the surface of the semiconductor layer.

[0229] Thus, the method of this example can be used to form a pn or pin junction.

[0230] In this example, no further dopants are introduced into some of the semiconductor layers described so far. In some examples, germanium is introduced as a dopant into the first layer, the second layer and / or the third layer. Germanium changes the band gap of the electronic device and improves the mechanical properties of each semiconductor material layer. In some examples, nitrogen is introduced as a dopant in the first, second and / or third material layer. Nitrogen is used to improve the mechanical properties of the formed semiconductor layer.

[0231] A thirteenth example is also presented, which relates to a method of manufacturing a yttrium aluminum garnet (YAG) crystalline layer, which will now be referred to. Fig.14The method is generally described by numeral 1301 and includes using the method as described in the eleventh example 1302, wherein the YAG is doped 1303 with at least one f-block transition metal.

[0232] In this example, the dopant material is a lanthanide.

[0233] In this example, the dopant material includes neodymium. In other examples, the dopant material includes chromium or cerium in addition to neodymium. In this example, the crystalline layer of the material includes 1.0 mole percent neodymium. In some examples, the material also includes 0.5 mole percent cerium.

[0234] In yet another example, the dopant material includes erbium. In this example, the dopant material is provided as a target and sputtered as described in the eleventh example. In this further example, the crystalline layer of the material includes 40 mole percent erbium. In one example, the crystalline layer of the material includes 55% erbium.

[0235] In yet another example, the dopant material comprises ytterbium. In one of these examples, the crystalline layer of material comprises 15 mole percent ytterbium.

[0236] In an even further example, the dopant material comprises thulium. In an even further example, the dopant material comprises dysprosium. In an even further example, the dopant material comprises samarium. In an even further example, the dopant material comprises terbium.

[0237] In still further examples, the dopant material comprises cerium. In some examples where the dopant material comprises cerium, the dopant material further comprises gadolinium.

[0238] In some examples, rather than providing the dopant material as distinct regions of one or more targets, the dopant material is introduced at least partially after deposition of the layer of crystalline material by providing the dopant material as a gas so that it diffuses into the layer of crystalline material.

[0239] According to a fourteenth example, a method for manufacturing a light emitting diode is proposed, and now reference will be made to Fig.15 The method is generally described by numeral 1401 and includes performing a method according to a twelfth example 1402 and thereafter or therein performing a method according to a thirteenth example 1403, where the dopant used during the method of the thirteenth example includes cerium 1404, in this example, the cerium-doped YAG layer is used as a scintillator in an LED.

[0240] The methods according to the twelfth and thirteenth examples may be performed within the same process chamber.

[0241] According to the fifteenth example, a method for manufacturing a permanent magnet is proposed, which will now be referred to Fig.16 The method is generally depicted by numeral 1501 and includes performing a method 1502 according to an eleventh example, wherein different regions of one or more targets provided contain neodymium, iron, boron and dysprosium 1503, and the method includes treating a film 1504 such that the material layer becomes a permanent magnet.

[0242] In this example, the last layer of material includes 6.0 mole percent dysprosium. In further examples, the mole percent of dysprosium is less than 6.0.

[0243] The high target utilization provided by the current method is beneficial when building electronic devices with rare elements such as dysprosium. Dysprosium has limited earth abundance, so a deposition system with high target utilization can reduce material waste.

[0244] According to a sixteenth example, a method for manufacturing an indium tin oxide (ITO) layer is proposed, and now reference will be made to Fig.17 The method is generally described by numeral 1601 and includes performing a method according to an eleventh example 1602, wherein different regions of a target provided include indium and tin 1603. The ITO layer is deposited in such a way that it forms a transparent layer of crystalline material directly on the deposition 1604 on the substrate. In other examples, a composite target is used, which includes indium and tin. In further examples, the composite target includes oxides of indium and tin. Therefore, the number of targets used can be different in other examples, and a single target can be used.

[0245] In a further example, the target may include indium oxide or tin oxide.In a further example, the deposition process includes providing oxygen gas such that sputtered material from the target reacts with the oxygen gas to form indium tin oxide on the substrate.

[0246] According to a seventeenth example, not shown separately, a method for manufacturing a photovoltaic cell is provided. In this example, the method further includes depositing ITO as described in the fifteenth example. In a further example, no ITO layer is deposited. In this example, the method further includes depositing a layer of perovskite material between the n-type doped layer of semiconductor material and the p-type doped layer of semiconductor material. In this case, the perovskite material layer is deposited as described in the method of the eleventh example. In a further example, it is deposited by another suitable means, such as physical vapor deposition or wet chemical techniques. In a further example, no perovskite material layer is deposited.

[0247] In an alternative example, the method includes depositing a layer of copper indium gallium selenide according to the eleventh example. Copper, indium, gallium, and selenide are provided as different regions of one or more targets. In this example, copper is provided as an elemental target and indium, gallium, and selenide are provided as oxide targets. Other combinations of oxide, elemental, compound, or composite targets are used in other examples. Therefore, the number of targets used may be different in other examples, and a single target may be used.

[0248] In some examples, the method includes depositing a cadmium sulfide layer according to the eleventh example. In this example, the cadmium and sulfide are provided in oxide form as different regions of the target. Other combinations of oxides, elements, compounds, or composite targets are used in other examples. Therefore, the number of targets used can be different in other examples, and a single target can be used.

[0249] In some examples, the method includes depositing a cadmium telluride layer according to the eleventh example. In this example, the cadmium and telluride are provided as different regions of an elemental target. In other examples, the cadmium and tellurium are provided as different regions of one or more targets in the form of elements, oxides, composites, or any combination thereof. Thus, the number of targets used may be different in other examples, and a single target may be used.

[0250] While the foregoing description has been described and illustrated with reference to specific examples, those skilled in the art will appreciate that the present invention is susceptible to many different variations not specifically described herein.

[0251] In the foregoing description, where reference is made to integers or elements with known, obvious or foreseeable equivalents, these equivalents are incorporated herein as if set forth separately. Reference should be made to the claims to determine the true scope of this example, which should be interpreted as including any such equivalents. The reader will also understand that the entirety or features of the present invention described as preferred, advantageous, convenient, etc. are optional and do not limit the scope of the independent claims. In addition, it should be understood that such optional integers or features, while potentially beneficial in some embodiments of the present invention, may be undesirable in other embodiments and therefore may not exist.

Claims

1. A method of producing a crystalline layer of material on a surface, the crystalline layer comprising lithium, at least one transition metal and at least one counter ion, in, The method comprises the following steps: Use a remote plasma generator to generate plasma, sputtering a plasma of material from a first target comprising lithium onto a surface of a substrate or a surface supported by a substrate, with at least a first plume corresponding to the trajectory of particles from the first target onto the surface, and A material from a second target comprising at least one transition metal is plasma sputtered onto the surface, there being at least a second plume corresponding to the trajectory of particles from the second target onto the surface, and wherein: The first target is positioned non-parallel to the second target, The first plume and the second plume converge at a region proximate to a surface of the substrate or a surface supported by the substrate, and The crystal layer is formed on the surface at the region, The bias voltage is applied to the target so that the ratio of the power used to generate the plasma to the power associated with the bias voltage on the target is greater than 1:1 and less than 7:

2.

2. The method according to claim 1, in, The plasma energy received at the first target is greater than that received at the second target.

3. The method according to claim 1, in, The first target faces the substrate in a first direction, and the second target faces the substrate in a second direction, the first direction and the second direction converging toward the substrate.

4. The method according to claim 3, in, An imaginary line extending from the center of the surface of the first target and parallel to the first direction intersects an imaginary line extending from the center of the surface of the second target and parallel to the second direction at a position closer to the substrate than to either target.

5. The method according to claim 4, in, The location of intersection is closer to the substrate than half the shortest distance from either target to the substrate.

6. The method according to any one of the preceding claims 1 to 5, in, The substrate and at least one of the first and second targets are moving as a crystalline layer is formed on the surface.

7. The method according to any one of the preceding claims 1 to 5, in, The substrate has a radius of curvature at a region where the first plume and the second plume converge, and the targets are circumferentially arranged around a center of the radius of curvature.

8. The method according to any one of the preceding claims 1 to 5, in, At least a portion of the substrate is carried by the rotating drum.

9. The method according to any one of the preceding claims 1 to 5, in, The working distance between the first target and the substrate is within + / - 50% of a theoretical mean free path, which is the average distance between ion collisions in a plasma.

10. The method according to any one of the preceding claims 1 to 5, in, The working distance between the first target and the substrate is 1 cm to 50 cm.

11. The method according to any one of the preceding claims 1 to 5, in, The surfaces of the first target and the second target facing the substrate are planar.

12. The method according to any one of the preceding claims 1 to 5, in, The plasma is shaped to form a plasma sheet extending in a direction along a width of the substrate and in a direction along a length of the substrate.

13. The method according to any one of the preceding claims 1 to 5, in, The second target includes at least one transition metal selected from the group consisting of iron, cobalt, manganese, nickel, titanium, niobium, aluminum, and vanadium.

14. The method according to any one of the preceding claims 1 to 5, in, The substrate has a thickness of from 0.1 to 10 μm.

15. The method according to any one of the preceding claims 1 to 5, in, The crystal layer formed on the surface has a thickness of 0.001 to 10 μm.

16. The method according to any one of the preceding claims 1 to 5, in, The step of sputtering the material onto the surface is performed so that the area is 1 cm 2 The maximum temperature reached by any given square of substrate material at a given time does not exceed 500 degrees Celsius, measured on the surface opposite to the surface onto which the material is deposited and averaged over a period of 1 second.

17. A method of manufacturing an electronic component comprising forming a multilayer sheet of different materials, integrating the multilayer sheet or a portion thereof into an electronic product, in, At least one layer of the sheet is a crystalline layer of conductive or semiconductive material made by performing a method according to any of the preceding claims 1-16.

18. The method according to claim 17, in, The substrate is retained as part of the electronic component.

19. The method according to claim 18, in, The electronic component is a battery pack.

20. A battery comprising one or more layers of crystalline material formed by performing the method of any preceding claim 1-16.

21. A battery comprising a plurality of stacked cathode layers, a plurality of stacked electrolyte layers and a plurality of stacked anode layers, in, At least two of the plurality of stacked cathode layers are made by performing the method according to any one of claims 1 to 16.