A method for controlling the surface quality of longitudinally cut blank strip steel for galvanized pipe
Through multi-process control and optimization of process parameters, the quality problem of the steel edge of the longitudinal cutting blank strip of galvanized pipe is solved, and the effect of uniform thickness, strong adhesion and smooth surface is achieved, meeting the quality requirements of galvanized pipe products.
Patent Information
- Application Number
- CN202210606721.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-31
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-05-31
AI Technical Summary
The quality of the edges of the longitudinally cut blank strip for galvanized pipes is difficult to ensure, and there are problems such as roughness, scratches, and decarbonization, which affects the quality of galvanized pipe products. The traditional descaling method is not thorough, which affects the appearance quality of the coating, and the wear surface of the pinch roller is worn. Roughness affects the surface finish of the strip.
Multi-process control methods are adopted, including longitudinal cutting of casting, heating, post-furnace descaling, rough rolling, finishing rolling, laminar cooling, winding, and technologies such as flame cutting, iron oxide sheet removal device, and pinch roller online grinding device. Means, optimize each process parameters to eliminate edge defects and improve surface quality.
Effectively eliminate the quality defects in the edges of the longitudinally cut blank strip steel, improve the surface quality of the strip steel, ensure uniform thickness of the zinc layer, strong adhesion, and smooth surface, meet the use requirements of galvanized pipe products, and reduce dezincification and peeling.
Smart Images

Figure CN114985463B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a strip steel production process, in particular to a surface quality control method for longitudinally cut blank strip steel for galvanized pipes. Background Art
[0002] The hot-dip galvanized steel strip is heated to make the molten zinc react with the strip steel matrix to produce an alloy layer. The quality issues of hot-dip galvanized pipes mainly include two aspects: internal and appearance. The internal is mainly the coating thickness and adhesion. There are alloy layers and pure zinc layers in the coating. A thick and dense pure zinc layer covers the steel surface, which can prevent the steel matrix from contacting with any corrosive solution, protect the steel matrix from corrosion, and increase the service life. Adhesion refers to the mutual dissolution of zinc and iron, the firm combination, strong wear resistance, and not easy to peel off. The appearance is mainly the bright and delicate coating, no sagging, wrinkles, uniform coating thickness, no cracks, and coating shedding. At present, there are the following problems with strip steel for galvanized pipes: 1. Some steel enterprises have been eliminated due to backward production capacity and low production efficiency of small continuous casting machines. Steel mills cannot provide 380-600mm small-section continuous casting billets for galvanized pipes for rolling. Therefore, large-section billets such as 920mm, 1020mm, and 1380mm are required for longitudinal cutting, and cut into 380mm, 400mm, 450mm, 470mm, 500mm, 520mm, 570mm and other widths for rolling. The edge quality of the strip steel of the longitudinally cut billet for galvanized pipes has not been reliably guaranteed, and roughness, scratches, and decarburization appear on the longitudinally cut edges. Such products will be used by downstream galvanizing manufacturers. Problems such as uneven thickness of the zinc layer on the edge, peeling, dezincification, and graying of the surface will occur, which seriously affects the quality of the galvanized pipe products and causes the strip steel produced by the longitudinally cut billets to be unable to be used normally. 2. The traditional descaling method has the problem of incomplete descaling, which affects the appearance quality of the coating. 3. The worn surface of the pinch roller is rough, which affects the surface finish of the strip. Frequent disassembly and grinding of the pinch roller will affect the production rhythm. Summary of the invention
[0003] The purpose of the present invention is to solve the problems of the prior art and to provide a method for controlling the surface quality of longitudinally cut billet strip for galvanized pipes. The method improves the existing longitudinal cutting process, post-furnace descaling process, and coiling process. Through multi-process control, it effectively eliminates edge quality defects of longitudinally cut billet strip, improves the surface quality of the strip, and meets the quality requirements of galvanized pipe strip.
[0004] The problem described in the present invention is solved by the following technical solution:
[0005] A method for controlling the surface quality of longitudinally cut billet strip steel for galvanized pipes, comprising the following steps: longitudinally cutting of ingots, heating, descaling after furnace, rough rolling, finishing rolling, laminar cooling, and coiling.
[0006] The ingot longitudinal cutting process uses a flame cutting device to longitudinally cut the large-section ingot into small-section longitudinal ingots of 380-600mm. During the preheating process, the cutting gun flame is adjusted to a neutral flame, the ratio of oxygen to acetylene is 1.1:1, and the inner flame is used for preheating for 60-80s. When cutting begins, the cutting gun flame is gradually adjusted to a reducing flame as the cutting nozzle height changes, the ratio of oxygen to acetylene is 1:1.2, the cutting nozzle is about 40-50mm away from the ingot, and the cutting speed is 180-220mm / min.
[0007] In the heating process, the heating temperature of the casting is controlled at 1160-1180°C, and the time in the furnace is controlled at 100-120 minutes;
[0008] In the post-furnace descaling process, the surface and edge of the ingot are first descaled by the iron oxide scale removal device, and then descaled by the post-furnace high-pressure water descaling device for the second time;
[0009] The rolling temperature of the rough rolling process is controlled within the range of 1000-1100°C, the rough rolling speed is controlled within the range of 3.3-3.9 m / s, the reduction rate is controlled within the range of 25%-30%, and the rough rolling descaling pass is the same as the rolling pass;
[0010] The final rolling temperature of the finishing rolling process is controlled at 800-850℃;
[0011] The cooling speed of the coiling process is controlled at 15-20 m / s, and the coiling temperature is controlled at 610±15°C.
[0012] The above-mentioned method for controlling the surface quality of longitudinally cut billet strip for galvanized pipes, the iron oxide scale removing device is arranged between the heating furnace and the high-pressure water descaling device behind the furnace, the iron oxide scale removing device includes a descaling cover, an upper descaling roller, a lower descaling roller, a cleaning disk and an edge descaling assembly, the upper and lower descaling rollers are respectively located above and below the ingot, the upper and lower descaling rollers are respectively driven to rotate by a power mechanism, steel brushes are arranged on the cylindrical surfaces of the cylindrical upper and lower descaling rollers, the cleaning disk is located at the rear of the upper descaling roller, and a cleaning brush is arranged on the lower end face of the cleaning disk, and the diameter of the cleaning brush matches the width of the longitudinally cut ingot.
[0013] The above-mentioned method for controlling the surface quality of longitudinally cut billet strip for galvanized pipe comprises two sets of edge descaling components symmetrically arranged, which are respectively located on both sides of the ingot. The edge descaling components are provided with an edge descaling brush and a mounting seat, and the edge descaling brush and the mounting seat are fixedly connected in an adjustable position.
[0014] In the surface quality control method for longitudinally cut blank strip steel for galvanized pipe, the steel brushes of the upper and lower descaling rollers are distributed in a spiral manner.
[0015] The above-mentioned method for controlling the surface quality of longitudinally cut billet strip for galvanized pipes, the flame cutting device includes a support frame, a car body, a frame, an oxygen gun rod and an oxygen gun adjustment structure, a guide wheel is installed at the lower part of the car body, the guide wheel runs on the support frame, the guide wheel is connected to the drive motor by transmission, the frame is fixed on the car body, the lateral position of the frame relative to the car body is adjustable, the oxygen gun adjustment mechanism is arranged on the frame, the oxygen gun adjustment mechanism drives the oxygen gun rod to move up and down, and the oxygen gun is installed at the lower part of the oxygen gun rod; the oxygen gun adjustment mechanism is provided with an adjustment motor, the adjustment motor drives the oxygen gun adjustment screw to rotate, the oxygen gun adjustment screw and the oxygen gun adjustment nut are spirally matched, and the oxygen gun adjustment nut is connected to the oxygen gun rod.
[0016] The surface quality control method of longitudinally cut billet strip for galvanized pipe is as follows: the coiling process is provided with an online grinding device for pinch rollers, the online grinding device for pinch rollers comprises an oil cylinder, upper and lower rails, a grinding car and a grinding mechanism, the oil cylinder piston rod is connected to the grinding car, the grinding car runs between the upper and lower rails, two sets of grinding mechanisms are respectively installed at the front and rear parts of the grinding car, and the grinding wheels of each grinding mechanism correspond to the upper and lower pinch rollers respectively.
[0017] The above-mentioned method for controlling the surface quality of longitudinally cut blank strip steel for galvanized pipes comprises the following steps: the grinding mechanism is provided with a grinding motor, the grinding motor is connected to the grinding wheel via a reducer, the grinding motor is connected to the slider, the grinding wheel adjusting screw is rotatably connected to the slider, the grinding wheel adjusting screw is spirally connected to the grinding wheel adjusting nut, and the grinding wheel adjusting nut is fixed on the grinding vehicle.
[0018] The surface quality control method of longitudinally cut blank strip steel for galvanized pipes is as follows: track frames are provided on the outer sides of both ends of the lower clamping rollers, a lower beam is fixed on the track frame, two lower tracks are provided on the lower beam, both ends of the lower beam are connected to upper beam brackets, the upper beam brackets fix the upper beam, and an upper track is provided on the upper beam.
[0019] The above-mentioned method for controlling the surface quality of longitudinally cut billet strip for galvanized pipes, the composition of the longitudinally cut billet for galvanized pipes is: C content 0.05%~0.08%, Mn content 0.65%~0.75%, S content 0.015%~0.025%, P content 0.018%~0.025%, Si content 0.02%~0.08%, Als content 0.015%~0.030%.
[0020] Compared with the prior art, the main advantages of the method of the present invention are as follows: 1. The longitudinal cutting process uses a flame cutting device to longitudinally cut the ingot, controls relevant parameters, and uses a reducing flame for cutting, thereby eliminating or reducing the problem of decarburization at the edge of the longitudinally cut ingot caused by oxidizing flame cutting. 2. The heating furnace adopts a lower heating temperature and a shorter furnace time, which reduces the generation of furnace-born iron oxide scale and the loss of C element at the edge of the longitudinally cut ingot while ensuring subsequent rolling. 3. A roller brush iron oxide scale removal device is added before high-pressure water descaling, and the roller brush iron oxide scale removal device is used to remove the iron oxide scale on the surface and edge of the ingot, and then high-pressure water descaling is performed, thereby effectively and thoroughly removing the furnace-born iron oxide scale on the surface and edge of the ingot. 4. The rough rolling adopts low temperature, low pressure reduction and high-speed rolling, which ensures the rolling quality of the edge of the intermediate ingot while improving the continuity of secondary iron oxide, and the descaling is improved to open high-pressure water descaling for each pass to enhance the descaling effect. 5. The finishing rolling adopts low starting rolling temperature and low final rolling temperature, and the purge water between the stands and the cooling water of the stand strip are turned on to ensure the quality of the oxide film formed on the rollers and reduce the surface roughness of the strip. 6. An online grinding device for the pinch roller is set in the coiling process, and the size and surface accuracy of the pinch roller are timely trimmed online to ensure the surface finish of the strip. 7. The coiling adopts a high cooling rate cooling method and a low coiling temperature. While improving the strength of the strip, it also increases the yield platform of the edge of the strip and reduces the roughness of the edge caused by the yield mark. By adopting the method of the present invention, the surface of the finished strip is clean and smooth, without cracks, peeling, roughness and other problems on the edge, and the organization is uniform and without decarburization. Tracking the customer's galvanizing production process, the zinc layer on the edge of the strip is bright, and there is no dezincification, zinc layer peeling, graying of the plate surface and other problems. After testing, the coating thickness is uniform, which fully meets the user's use requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The present invention will be further described below in conjunction with the accompanying drawings.
[0022] Figure 1 It is a schematic diagram of the structure of a roller brush scale removal device;
[0023] Figure 2 yes Figure 1 AA section view;
[0024] Figure 3 is a schematic diagram of a flame cutting device;
[0025] Figure 4 yes Figure 3 Left view of
[0026] Figure 5 It is a schematic diagram of an online grinding device for pinch rollers;
[0027] Figure 6 yes Figure 5 B-direction view;
[0028] Figure 7 yes Figure 6 A partial enlarged view of point D in the middle;
[0029] Figure 8 It is a schematic diagram of the positional relationship among the track frame, the lower beam, the upper beam and the upper beam support frame.
[0030] The numbers in the figure are: 1. Iron oxide scale removal device, 1-1. Descaling cover, 1-2. Upper descaling roller, 1-3. Lower descaling roller, 1-4. Steel brush, 1-5. Cleaning disc, 1-6. Edge descaling brush, 1-7. Mounting seat, 2. Flame cutting device, 2-1. Car body, 2-2. Frame, 2-3. Oxygen gun rod, 2-4. Oxygen gun adjustment screw, 2-5. Oxygen gun adjustment screw, 2-6. Adjustment motor, 2-7. Oxygen gun, 2-8. Support frame, 2-9. Guide column, 2-10. Drive motor, 3. Pinch roller online grinding device, 3-1, oil cylinder, 3-2, grinding car, 3-3, upper track, 3-4, lower track, 3-5, roller, 3-6, grinding wheel adjusting screw, 3-7, slider, 3-8, grinding motor, 3-9, reducer, 3-10, grinding wheel, 3-11, slide, 3-12, hand wheel, 3-13, grinding wheel adjusting nut, 3-14, upper beam, 3-15, upper beam support frame, 3-16, lower beam, 3-17, track frame, 4, ingot, 5, high-pressure water descaling device after furnace, 6, metal detector, 7, upper pinch roller, 8, lower pinch roller. DETAILED DESCRIPTION
[0031] The chemical composition of the longitudinally cut billet for galvanized pipes of the present invention is as follows: C: 0.05% to 0.08%, Mn: 0.65% to 0.75%, S: 0.015% to 0.025%, P: 0.018% to 0.025%, Si: 0.02% to 0.08%, Als: 0.015% to 0.030%, and the balance is Fe and unavoidable impurities (Cr, Cu, Sn, V, Mo, Nb). The method of the present invention comprises the following steps: longitudinally cutting the ingot, heating, descaling after the furnace, rough rolling, finishing rolling, laminar cooling, and coiling.
[0032] The slab longitudinal cutting process uses 920mm, 1020mm, 1380mm large-section billets for longitudinal cutting, cutting into 380mm, 400mm, 450mm, 470mm, 500mm, 520mm, 570mm small-section billets. In order to solve the problems of decarburization and roughness on the edges of the longitudinally cut billets, the flame cutting device is used in the slab longitudinal cutting process to cut with reducing flame. By controlling the relevant parameters, the decarburization problem on the edges of the longitudinally cut billets caused by oxidizing flame cutting can be eliminated or reduced. Figure 3 , Figure 4The flame cutting device 2 includes a vehicle body 2-1, a frame 2-2, an oxygen gun rod 2-3, an oxygen gun adjustment structure and a support frame 2-8. A guide wheel is installed at the lower part of the vehicle body, a guide rail is provided on the support frame, and the guide wheel is located on the guide rail. The guide wheel is connected to the drive motor 2-10 by transmission, and the vehicle body is driven by the drive motor to move along the guide rail on the support frame. The ingot 4 is placed between the two support frames. The frame is fixed to the vehicle body, and a transverse groove is provided on the vehicle body. The frame is fixed to the vehicle body by bolts passing through the frame and the transverse groove. The transverse position of the frame can be adjusted by loosening the bolts to adapt to cutting ingots of different widths. An oxygen gun 2-7 is installed at the lower part of the oxygen gun rod. The oxygen gun adjustment mechanism is used to adjust the height position of the oxygen gun. The oxygen gun adjustment mechanism is arranged on the frame, and the oxygen gun adjustment mechanism is provided with an adjustment motor 2-6. The adjustment motor drives the oxygen gun adjustment screw 2-5 to rotate, and the oxygen gun adjustment screw is spirally matched with the oxygen gun adjustment nut 2-4, and the oxygen gun adjustment nut is connected to the oxygen gun rod. The oxygen gun adjustment screw nut and the guide column 2-9 slide together to ensure the smooth movement of the oxygen gun rod. The guide column is fixed on the frame. At the initial stage of cutting the ingot, the oxygen gun nozzle is 10-20mm away from the ingot, the preheating flame is adjusted to a neutral flame, the ratio of oxygen to acetylene is 1.1:1, preheating is 60-80s, the oxygen gun rod rises, and is raised by 30-40mm. When starting to cut, as the height of the oxygen gun cutting nozzle changes, the cutting flame is gradually adjusted to a reducing flame, the ratio of oxygen to acetylene is 1:1.2, and the oxygen gun nozzle is 40-50mm away from the ingot. The driving motor drives the car body to move, and the cutting speed is controlled to 180-220mm / min. Ensure that the ingot is not cut with an inner flame to avoid the reaction of oxygen with the C element in the ingot to cause decarburization.
[0033] The slitting billet is heated by a heating process. The heating furnace heats the slitting billet. The heating temperature is controlled at 1160-1180°C and the time in the furnace is 100-120 minutes. The present invention adopts a lower heating temperature and a shorter time in the furnace. On the basis of ensuring subsequent rolling, the amount of furnace-generated iron oxide scale and the loss of C element at the edge of the slitting billet are reduced; the tapping temperature is controlled below 1178°C, which can not only reduce the thickness of the iron oxide scale and the degree of decarburization, but also facilitate the descaling after the furnace.
[0034] The scale removal device is added to the post-furnace descaling process. The ingot is first descaled by the scale removal device and then descaled by high-pressure water. The purpose of setting the scale removal device is to make the steel brush contact the scale on the surface of the ingot, forcefully crush the scale, and then use the cleaning disk to remove the crushed scale to the roller groove; then the ingot is descaled by high-pressure water, so as to effectively and thoroughly remove the scale on the surface and edge of the slab, and solve the problem that the galvanizing effect is affected by the incomplete removal of scale. Figure 1 , Figure 2The iron oxide scale removal device 1 is arranged between the heating furnace and the high-pressure water descaling device 5 behind the furnace. The iron oxide scale removal device includes a descaling cover 1-1, an upper descaling roller 1-2, a lower descaling roller 1-3, a cleaning disc 1-5 and an edge descaling assembly. The upper and lower descaling rollers are respectively located at the upper and lower parts of the ingot 4, and the upper and lower descaling rollers are respectively driven to rotate by a power mechanism. Steel brushes 1-4 are embedded on the cylindrical surfaces of the cylindrical upper and lower descaling rollers, and the steel brushes are wound around the cylindrical surfaces of the upper and lower descaling rollers in a spiral manner. The rotation direction of the upper and lower descaling rollers is as follows: Figure 2 As shown. The cleaning disc 1-5 is located at the rear of the upper descaling roller, and a cleaning brush is provided on the lower end surface of the cleaning disc. The diameter of the cleaning brush distribution matches the width of the ingot. The cleaning disc is driven to rotate by a motor and a reducer to remove the broken iron oxide scale to the roller groove. The edge descaling assembly is used to remove the iron oxide scale on the edge of the ingot. The edge descaling assembly is symmetrically arranged in two sets, respectively located on both sides of the ingot. The edge descaling assembly is provided with an edge descaling brush 1-6 and a mounting seat 1-7. The mounting seat is fixed, and the brush handle of the edge descaling brush is connected to the mounting seat bolt. Loosening the bolt can adjust the lateral position of the edge descaling brush relative to the mounting seat to ensure that the edge descaling brush is in close contact with the edge of the ingot, and the iron oxide scale on the edge of the ingot is removed as the ingot runs. The metal detector 6 is installed in front of the iron oxide scale removal device. When the ingot is detected to pass, a signal is sent, and the control mechanism controls the upper and lower descaling rollers and the cleaning disc to start working. After the ingot passes, the upper and lower descaling rollers and the cleaning disc stop working.
[0035] The present invention improves the process of rough rolling, finishing rolling and coiling, wherein the rough rolling temperature is controlled within the range of 1000-1100°C, the rough rolling speed is controlled within the range of 3.3-3.9 m / s, the reduction rate is controlled within the range of 25%-30%, and the rough rolling descaling pass is the same as the rolling pass. The finishing rolling temperature is controlled within the range of 800-850°C, the coiling cooling speed is controlled within the range of 15-20 m / s, and the coiling temperature is controlled within the range of 610±15°C. Through low-temperature high-speed rolling and low-temperature coiling, the edge cracking of the strip is reduced, the surface roughness is reduced, the rate of austenite recrystallization is reduced, and the strength of the strip is improved.
[0036] In the prior art, after the pinch rollers have been used for a period of time, the turning surface must be removed and the uneven and dimensional changes of the worn pinch rollers must be trimmed. The problem with this traditional method is that the pinch rollers cannot be trimmed in time, resulting in the pinch rollers reducing the surface finish of the steel strip during the coiling process, which is also one of the reasons that affect the galvanizing effect. To solve this problem, the present invention provides an online grinding device for the pinch rollers in the coiling process. Figure 5-Figure 8The online grinding device 3 for the pinch roller includes an oil cylinder 3-1, a grinding car 3-2, an upper track 3-3, a lower track 3-4 and a grinding mechanism. The oil cylinder is arranged on a platform beside the roller track, and the oil cylinder piston rod is connected to the grinding car. The upper and lower parts of the grinding car correspond to the upper and lower tracks, respectively, and rollers 3-5 are arranged. The grinding car runs between the upper and lower tracks, and the upper and lower tracks guide and limit the running of the grinding car. Two sets of grinding mechanisms are respectively installed at the front and rear of the grinding car, and the grinding wheels of each grinding mechanism correspond to the upper pinch roller 7 and the lower pinch roller 8. With the reciprocating motion of the oil cylinder piston rod, the two sets of grinding mechanisms grind the surfaces of the upper pinch roller and the lower pinch roller online respectively. The grinding mechanism is provided with a grinding motor 3-8, and the grinding motor is connected to the grinding wheel 3-10 through the reducer 3-9. The grinding motor is connected to the slider 3-7, and the slider is slidably matched with the slide 3-11, and the slide is fixed to the grinding car. The grinding wheel adjusting screw 3-6 is connected to the slider and can rotate freely relative to the slider. The grinding wheel adjusting screw is spirally connected to the grinding wheel adjusting nut 3-13. The hand wheel 3-12 is installed at the end of the grinding wheel adjusting screw, and the grinding wheel adjusting nut is fixed to the grinding car. Turn the hand wheel, the grinding wheel adjusting screw rotates relative to the slider and drives the slider to move up or down. The slider drives the grinding motor, the reducer and the grinding wheel to move up and down to realize the feeding of the grinding wheel. A track frame 3-17 is provided on the outer side of both ends of the lower clamping roller. A lower beam 3-16 is fixed on the track frame. Two lower rails 3-4 are fixed on the lower beam. Upper beam brackets 3-15 are provided at both ends of the lower beam. An upper beam 3-14 is fixed on the upper part of the upper beam bracket. One or two upper rails 3-3 are fixed on the upper beam. The upper rail of the illustrated embodiment is provided with one upper rail. The cross-sectional shapes of the upper guide rail and the lower guide rail are both M-shaped, so as to limit the two sides of the roller.
[0037] The working process of the pinch roller online grinding device is as follows: the upper pinch roller is lifted, and the lower beam and upper beam are installed on the track frame; then the oil cylinder pushes the grinding car along the upper and lower tracks to enter between the upper and lower pinch rollers, the oil cylinder reciprocates, and the grinding motor drives the grinding wheel to grind the upper and lower pinch rollers; after the grinding is completed, the oil cylinder drives the grinding car to withdraw to the platform, remove the upper and lower beams, and reset the upper pinch roller. Since the pinch roller online grinding device can perform grinding in time according to the wear of the pinch roller surface, it ensures that the pinch roller surface has a high finish and dimensional accuracy, avoids the surface quality of the strip being affected by the rough surface of the pinch roller, and improves the grinding efficiency of the pinch roller.
[0038] The following provides examples:
[0039] The following provides embodiments of the present invention:
[0040] The chemical composition of the longitudinally cut billet is: C: 0.05% ~ 0.08%, Mn: 0.65% ~ 0.75%, S: 0.015% ~ 0.025%, P: 0.018% ~ 0.025%, Si: 0.02% ~ 0.08%, Als: 0.015% ~ 0.030%, and the remainder is Fe and unavoidable impurities (Cr, Cu, Sn, V, Mo, Nb).
[0041] The billet was cast into continuous casting billets of 10200mm×1020mm×200mm and 10200mm×920mm×200mm. The billet was flame cut into the following longitudinal sections. The details of the longitudinal section are shown in Table 1.
[0042] Table 1 Longitudinal section details of blanks
[0043]
[0044] Heating and insulation are carried out in the heating furnace with an average heating temperature of 1160℃~1180℃ and a furnace time of 100~120min. After the post-furnace iron oxide scale removal device and ≥19.5MPa high-pressure water descaling, it is sent to the rough rolling mill for 5~7 passes, with 19.5MPa high-pressure water descaling in each pass; the thickness of the intermediate billet is 27~35mm. It is sent to the finishing rolling through the intermediate roller, and the scale is broken by 1.2Mpa scale-breaking water before the flying shear, and then rolled through seven finishing rolling mills, with the inlet temperature controlled at 960-1000℃, the finishing speed controlled at 9.0-11.3m / s, and the outlet temperature controlled at 800℃-850℃; a total of 14 groups of cooling water are set for laminar cooling, the first to the second groups are closed, the third to the thirteenth groups of cooling water are opened, and the fourteenth group is used as auxiliary water replenishment, and the cooling rate of 15-20℃ / s is cooled to 590-620℃ for coiling, and finally cooled to room temperature by air cooling for 24 hours. The surface of the finished strip is clean and smooth by inspection, and no defects such as pits, cracks, rotten edges, and rough edges are produced. The process control of the comparison group is shown in Table 2. After testing the composition and mechanical properties of the strip, the performance of the traditional ingot has been significantly improved and improved. The details of the comparison group are shown in Table 3.
[0045] Table 2 Process control
[0046]
[0047]
[0048] Table 3 Composition and performance control
[0049]
[0050] Tracking the downstream usage, the pickled plate has no pits or pits, and the edges are rough. During the galvanizing process, the zinc layer thickness on the surface and edges of the strip is uniform and the color is normal. There is no dezincification, zinc layer peeling, graying of the plate surface, etc. The quality of the strip meets the customer's usage requirements. The tracking situation is shown in Table 4.
[0051] Table 4 Galvanizing production
[0052]
[0053]
Claims
1. A method for controlling the surface quality of longitudinally cut billet strip steel for galvanized pipes, comprising the following steps: longitudinally cutting of ingots, heating, descaling after furnace, rough rolling, finishing rolling, laminar cooling, and coiling, characterized in that: The ingot longitudinal cutting process uses a flame cutting device to longitudinally cut the large-section ingot into small-section longitudinal ingots of 380-600 mm. During the preheating process, the cutting gun flame is adjusted to a neutral flame, the ratio of oxygen to acetylene is 1.1:1, and the inner flame is used for preheating for 60-80 seconds. When cutting begins, the cutting gun flame is gradually adjusted to a reducing flame as the cutting nozzle height changes, the ratio of oxygen to acetylene is 1:1.2, the cutting nozzle is 40-50 mm away from the ingot, and the cutting speed is 180-220 mm / min. In the heating process, the heating temperature of the casting is controlled at 1160-1180°C, and the time in the furnace is controlled at 100-120 minutes; In the post-furnace descaling process, the surface and edge of the ingot are first descaled by the iron oxide scale removal device, and then descaled by the post-furnace high-pressure water descaling device for the second time; The rolling temperature of the rough rolling process is controlled within the range of 1000-1100°C, the rough rolling speed is controlled within the range of 3.3-3.9 m / s, the reduction rate is controlled within the range of 25%-30%, and the rough rolling descaling pass is the same as the rolling pass; The final rolling temperature of the finishing rolling process is controlled at 800-850℃; The cooling speed of the coiling process is controlled at 15-20 m / s, and the coiling temperature is controlled at 610±15°C.
2. The surface quality control method of longitudinally cut billet strip for galvanized pipe according to claim 1 is characterized in that: The iron oxide scale removing device is arranged between the heating furnace and the high-pressure water descaling device behind the furnace. The iron oxide scale removing device includes a descaling cover, an upper descaling roller, a lower descaling roller, a cleaning disk and an edge descaling component. The upper and lower descaling rollers are respectively located above and below the ingot, and the upper and lower descaling rollers are respectively driven to rotate by a power mechanism. Steel brushes are arranged on the cylindrical surfaces of the cylindrical upper and lower descaling rollers. The cleaning disk is located at the rear of the upper descaling roller. A cleaning brush is arranged on the lower end surface of the cleaning disk. The diameter of the cleaning brush matches the width of the longitudinally cut ingot.
3. The surface quality control method of longitudinally cut blank strip steel for galvanized pipe according to claim 2 is characterized in that: Two sets of edge descaling components are symmetrically arranged, respectively located at both sides of the ingot. The edge descaling components are provided with edge descaling brushes and mounting seats, and the edge descaling brushes and the mounting seats are adjustable and fixedly connected.
4. The method for controlling the surface quality of longitudinally cut billet strip for galvanized pipe according to claim 3 is characterized in that: The steel brushes of the upper and lower descaling rollers are distributed in a spiral pattern.
5. The surface quality control method of longitudinally cut blank strip steel for galvanized pipe according to claim 1 is characterized in that: The flame cutting device includes a support frame, a vehicle body, a frame, an oxygen gun rod and an oxygen gun adjustment structure. A guide wheel is installed at the lower part of the vehicle body, the guide wheel moves on the support frame, the guide wheel is connected to the driving motor by transmission, the frame is fixed on the vehicle body, and the lateral position of the frame relative to the vehicle body is adjustable. The oxygen gun adjustment mechanism is arranged on the frame, the oxygen gun adjustment mechanism drives the oxygen gun rod to move up and down, and the oxygen gun is installed at the lower part of the oxygen gun rod; the oxygen gun adjustment mechanism is provided with an adjustment motor, the adjustment motor drives the oxygen gun adjustment screw to rotate, the oxygen gun adjustment screw is screwed with the oxygen gun adjustment nut, and the oxygen gun adjustment nut is connected to the oxygen gun rod.
6. The method for controlling the surface quality of longitudinally cut billet strip for galvanized pipe according to claim 1, characterized in that: The coiling process is provided with an online grinding device for the pinch rollers, which includes an oil cylinder, upper and lower rails, a grinding car and a grinding mechanism. The oil cylinder piston rod is connected to the grinding car, which runs between the upper and lower rails. Two sets of grinding mechanisms are respectively installed at the front and rear parts of the grinding car, and the grinding wheels of each grinding mechanism correspond to the upper and lower pinch rollers respectively.
7. The method for controlling the surface quality of longitudinally cut billet strip for galvanized pipe according to claim 6, characterized in that: The grinding mechanism is provided with a grinding motor, which is connected to the grinding wheel via a reducer, the grinding motor is connected to the slider, the grinding wheel adjusting screw is rotatably connected to the slider, the grinding wheel adjusting screw is spirally connected to the grinding wheel adjusting nut, and the grinding wheel adjusting nut is fixed on the grinding vehicle.
8. The method for controlling the surface quality of longitudinally cut billet strip for galvanized pipe according to claim 7, characterized in that: Track frames are arranged on the outer sides of both ends of the lower pinch rollers, a lower beam is fixed on the track frame, two lower tracks are arranged on the lower beam, both ends of the lower beam are connected to the upper beam bracket, the upper beam bracket fixes the upper beam, and an upper track is arranged on the upper beam.
9. The method for controlling the surface quality of longitudinally cut billet strip for galvanized pipe according to claim 1, characterized in that: The composition of the longitudinally cut blank for the zinc pipe is as follows: C content 0.05%-0.08%, Mn content 0.65%-0.75%, S content 0.015%-0.025%, P content 0.018%-0.025%, Si content 0.02%-0.08%, Als content 0.015%-0.030%.