A fast-response thin-film thermocouple on alloy surface and preparation method thereof
By using vacuum ion plating technology to deposit AlCrN-based thin films in thin film thermocouples and performing thermal oxidation treatment, combined with magnetron sputtering technology to prepare hot electrode films, and forming a dense aluminum oxide protective film on the surface, it solves the problem of high load in thin film thermocouples. Reliability issues in the environment are achieved, and temperature measurement effects with high stability and rapid response are achieved.
Patent Information
- Application Number
- CN202210588653.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-26
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-05-26
AI Technical Summary
The oxide insulating film of existing thin-film thermocouples is not dense enough to be suitable for high-load working environments, and the ceramic oxide film is easy to peel off under alternating thermal stress, resulting in a decrease in sensor reliability.
Vacuum ion plating technology is used to deposit AlCrN-based films, and thermal oxidation treatment is used to form a dense high-resistance thermal oxidation insulating film. NiCr and NiSi hot electrode films are prepared using magnetron sputtering technology, and finally dense amorphous aluminum oxide is formed on the surface. Protective film to improve the stability and reliability of thin film thermocouples.
A thin film thermocouple with high bonding force has been achieved, with good process repeatability and fast response characteristics. It can meet the needs of accurate and fast temperature measurement on the surface of metal workpieces in harsh environments, and improves the stability and reliability of the sensor.
Smart Images

Figure CN114993496B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of temperature sensors, and in particular to an alloy surface fast-response thin-film thermocouple and a preparation method thereof. Background Art
[0002] Smart sensor is a component that can convert the measured signal into an electrical signal and output it according to a certain rule. It has a great role and demand in promoting the development of science and technology, increasing the strength of weapons and equipment, and promoting the progress of the national economy. In the advanced manufacturing and aerospace industries, there are a large number of high-temperature and transient temperature measurement occasions, which put forward stringent requirements on temperature sensors. Not only the temperature measurement components are required to be highly accurate, but also the response speed is fast, the volume is small, and the heat capacity is small. However, the traditional thermocouple temperature sensor cannot meet the requirements of fast response dynamic temperature measurement due to the thick hot junction. Thin film thermocouples have the advantages of small heat capacity, fast response speed, thin structure size, small interference to the measurement environment, small impact on the physical properties of the test parts, and no need for special mechanical processing methods for fixation. Therefore, thin film thermocouples have broad application prospects in the measurement of the temperature of the workpiece surface and other parts.
[0003] At present, the preparation process of thin-film thermocouples on the surface of metal workpieces is relatively complicated. It is necessary to deposit a layer of Al2O3 or SiO2 film on the surface of the metal workpiece, which not only plays an insulating role, but also prevents the metal elements in the metal workpiece from diffusing into the thermocouple film, thereby ensuring the stability of the thin-film thermocouple. However, the bonding strength between the oxide film and the metal substrate is poor, and it cannot be used in high-load working environments; and under the action of alternating thermal stress, the ceramic oxide film and the metal workpiece are prone to peeling, resulting in reduced sensor reliability. Therefore, it is urgent to develop a thin-film thermocouple with stable performance and fast response.
[0004] In view of the above-mentioned defects, the inventors of the present invention finally obtained the present invention after a long period of research and practice. Summary of the invention
[0005] The purpose of the present invention is to solve the problems that the density of the oxide insulating film of the existing thin film thermocouple is insufficient, and under the action of alternating thermal stress, the ceramic oxide film and the metal workpiece are prone to peeling, resulting in reduced reliability of the sensor and inability to be suitable for high-load working environments. A thin film thermocouple with a fast response on an alloy surface and a preparation method thereof are provided.
[0006] In order to achieve the above object, the present invention discloses a method for preparing a fast-response thin-film thermocouple on an alloy surface, comprising the following steps:
[0007] S1: Alloy substrate pretreatment: The surface of the alloy substrate to be tested is ground and polished to a roughness Ra of less than 0.1 μm, and then ultrasonically cleaned with ethanol and deionized water in turn, and then dried for standby use;
[0008] S2: Preparation of AlCrN-based thin film: AlCrN-based thin film is deposited on the surface of alloy substrate by vacuum ion plating technology, Cr and CrN layers are used as bonding layer and transition layer, and the film thickness is 1-5 μm;
[0009] S3: Preparation of thermal oxidation film: Place the alloy substrate treated in step S2 in a vacuum heat treatment furnace, evacuate and heat to maintain 700-1000°C, then introduce oxygen, maintain the gas pressure at 0.01-0.05MPa, and perform thermal oxidation treatment for 1-6 hours to obtain a thermal oxidation insulating film with a resistance value greater than 1MΩ;
[0010] S4: Preparation of thermocouple functional film: Use magnetron sputtering technology to prepare K-type thermocouple thin film material on the surface of thermal oxide film, select NiCr and NiSi alloy targets, and use mask plates to prepare NiCr thermocouple film and NiSi thermocouple film respectively. The sputtering target voltage is 800-1000V, the sputtering current is 1-3A, and the thermocouple film thickness is 0.5-3μm. Then, lead wires are set on NiCr thermocouple and NiSi thermocouple respectively.
[0011] S5: Preparation of protective film: A high-power magnetron sputtering technique is used to form an aluminum oxide film as a protective layer on the surface of the alloy substrate treated in step S4, with a thickness greater than 1 μm and a resistance value greater than 10 MΩ, thereby obtaining the fast-response thin-film thermocouple described in the present invention.
[0012] The alloy in step S1 is any one of cemented carbide, titanium alloy and nickel-based alloy.
[0013] In the step S2, the AlCrN-based film is a multi-element film, including AlCrN, AlCrSiN, AlCrTiN, AlCrYN, and AlCrSiON films, and the atomic percentage of Al element in the AlCrN-based film is greater than 30%.
[0014] In the step S3, the thermal oxidation film includes aluminum oxide and chromium oxide.
[0015] In the step S4, the line widths of the NiCr hot electrode and the NiSi hot electrode are both 0.1-5 mm.
[0016] In the step S4, the atomic percentage of the NiCr thermode functional film is: Ni 85-93%, Cr 7-15%, and the atomic percentage of the NiSi thermode functional film is: Ni 92-99%, Si 1-8%.
[0017] In the step S5, the protective film is dense amorphous aluminum oxide.
[0018] The invention also discloses an alloy surface fast-response thin-film thermocouple prepared by the preparation method.
[0019] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention adopts vapor deposition technology to pre-deposit a high-bonding nitride film on the surface of a metal workpiece, and forms a dense high-resistance thermal oxidation insulating film on the nitride film through thermal oxidation. The surface of the sensing functional film is smooth and dense, with good process repeatability and rapid response characteristics, which effectively improves the stability and reliability of the thin film thermocouple and can meet the requirements of accurate and rapid temperature measurement on the surface of metal workpieces under harsh service environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Schematic diagram of the film structure of the thin film thermocouple of the present invention;
[0021] Figure 2 It is a schematic diagram of the thermoelectrode structure of the thin film thermocouple of the present invention;
[0022] Figure 3 This is a SEM image of the cross-sectional structure of the thermal oxidation insulating film of Example 1;
[0023] Figure 4 This is the XPS spectrum of the thermal oxidation insulating film surface of Example 1;
[0024] Figure 5 This is a diagram of electrical properties of the thermal oxidation insulating film of Example 1;
[0025] Figure 6 This is the XRD pattern of the hot electrode film of Example 2;
[0026] Figure 7 is a graph showing the relationship between the thermoelectric potential and temperature of the thin film thermocouple of Example 1;
[0027] Figure 8 This is a graph showing the relationship between the thermoelectric potential and temperature of the thin film thermocouple of Example 2.
[0028] The numbers in the figure represent:
[0029] 1-alloy substrate; 2-Cr bonding layer; 3-CrN transition layer; 4-AlCrN-based film; 5-thermal oxidation film; 6-NiCr thermode; 7-NiSi thermode; 8-protective film; 9-thermal junction, 10-NiCr thermode lead, 11-NiSi thermode lead. DETAILED DESCRIPTION
[0030] The above and other technical features and advantages of the present invention are described in more detail below in conjunction with the accompanying drawings.
[0031] Example 1
[0032] A fast-response thin-film thermocouple is prepared on the surface of a cemented carbide substrate as a workpiece to be tested, comprising the following steps:
[0033] S1, alloy substrate pretreatment: mechanically grind and polish the surface of the cemented carbide substrate to be tested until the roughness Ra is less than 50nm, and ultrasonically clean the cemented carbide substrate in ethanol and deionized water for 15 minutes in turn, and then dry it for use.
[0034] S2, preparation of AlCrN-based thin films: Cr / CrN / AlCrSiN thin films were deposited on the surface of cemented carbide in sequence using arc ion plating technology. The deposition pressure was 3.5 Pa, the deposition temperature was 450°C, the substrate bias was -50 V, the thickness of the AlCrSiN film was close to 1.6 μm, and the contents of each element in the film were Al: 31 at.%, Cr: 18 at.%, Si: 4 at.%, and N: 47 at.%.
[0035] S3, preparation of thermal oxidation film: place the cemented carbide sheet with AlCrSiN film in a vacuum heat treatment furnace, evacuate and heat, maintain the vacuum furnace temperature at 800°C, introduce oxygen, maintain the gas pressure at 0.04MPa, perform thermal oxidation treatment for 2 hours, and obtain a thermal oxidation insulating film.
[0036] S4, preparation of thermocouple functional film: NiCr-NiSi K-type thermocouple material was prepared by magnetron sputtering technology. First, a NiCr thermocouple mask with a line width of 1 mm was placed on the thermal oxide insulating film to deposit the thermocouple NiCr functional film. Then, the NiSi thermocouple mask was replaced to deposit the thermocouple NiSi functional film. The hot junction area was 1 mm×1 mm. The atomic percentages of the selected NiCr and NiSi alloy targets were 90:10 and 97:3, respectively. The sputtering target voltage of the two alloy targets was 930 V, the sputtering current was 1.5 A, and the deposition time was 15 min. A thermocouple metal sensitive film was obtained on the thermal oxide insulating film. Finally, high-temperature conductive silver glue was used to bond the leads to the thermocouple lead ends.
[0037] S5, preparation of protective film: high-power pulsed magnetron sputtering technology is used to prepare an aluminum oxide protective film on the surface of the alloy substrate deposited with the sensing functional film. A high-purity Al target (purity 99.99%) is used, oxygen is introduced, and a 1.5 μm thick dense and high-temperature resistant aluminum oxide film is obtained by changing the deposition time, thereby obtaining the fast-response thin film thermocouple described in the present invention.
[0038] Figure 3 This is a SEM image of the cross-sectional structure of the thermally oxidized insulating film of this embodiment.
[0039] Figure 4This is the XPS spectrum of the thermally oxidized insulating film surface of this embodiment. The film layer is mainly composed of aluminum oxide and chromium oxide components.
[0040] Figure 5 This is the electrical property of the thermally oxidized insulating film of this embodiment. The dense oxide film generated after oxidation treatment has a resistance value of up to 1.2 megohms, which plays a good insulating role between the metal sensing functional film and the metal workpiece.
[0041] Example 2
[0042] A titanium alloy substrate is used as a workpiece to be tested, and a fast-response thin-film thermocouple is prepared on its surface, comprising the following steps:
[0043] S1, alloy substrate pretreatment: mechanically grind and polish the surface of the titanium alloy substrate to be tested until the roughness Ra is less than 70nm, and ultrasonically clean the titanium alloy sheet in ethanol and deionized water for 15 minutes in turn, and then dry it for use.
[0044] S2, preparation of AlCrN-based thin films: Cr / CrN / AlCrN thin films were deposited on the surface of cemented carbide in sequence using arc ion plating technology. The deposition pressure was 3.5 Pa, the deposition temperature was 480°C, the substrate bias was -50 V, the thickness of the AlCrN film was close to 3 μm, and the contents of each element in the film were Al: 38 at.%, Cr: 14 at.%, and N: 48 at.%.
[0045] S3, preparation of thermal oxidation film: place the cemented carbide sheet with AlCrN film in a vacuum heat treatment furnace, evacuate and heat, maintain the vacuum furnace temperature at 800°C, introduce oxygen, maintain the gas pressure at 0.04MPa, perform thermal oxidation treatment for 2 hours, and obtain a thermal oxidation insulating film.
[0046] S4, preparation of thermocouple functional film: NiCr-NiSi K-type thermocouple material was prepared by magnetron sputtering technology. First, thermocouple A mask with a line width of 0.5 mm was placed on the thermal oxide insulating film to deposit the thermocouple NiCr functional film; then, thermocouple B mask was replaced to deposit the thermocouple NiSi functional film. The hot junction area was 0.5 mm×2 mm. The atomic percentages of NiCr and NiSi alloy targets were 90:10 and 97:3, respectively. The sputtering target voltage of the two alloy targets was 930 V, the sputtering current was 1.5 A, and the deposition time was 15 min. A thermocouple metal sensitive film was obtained on the thermal oxide insulating film. Finally, high-temperature conductive silver glue was used to bond the leads to the thermocouple lead ends.
[0047] S5, preparation of protective film: high-power pulsed magnetron sputtering technology is used to prepare an aluminum oxide protective film on the surface of the alloy substrate deposited with the sensing functional film. A high-purity Al target (purity 99.99%) is used, oxygen is introduced, and a 2μm thick dense and high-temperature resistant aluminum oxide film is obtained by changing the deposition time, thereby obtaining the fast-response thin film thermocouple described in the present invention.
[0048] Figure 6 is the XRD diagram of the thermoelectrode functional film of this embodiment. It can be seen that both thermoelectrode materials present a single-phase structure.
[0049] The thin film thermocouple prepared as above was statically calibrated. By measuring the thermoelectric potential values at different temperatures and performing linear fitting, the Seebeck coefficient of the thin film thermocouple of Example 1 was obtained to be 40.2 μV / °C ( Figure 7 As shown), the Seebeck coefficient of the thin film thermocouple of Example 2 is 41.2μV / ℃ (as shown Figure 8 As shown in the figure, it is basically close to the Seebeck coefficient of the standard K-type thermocouple (40.0μV / ℃), the discrete degree of the thermoelectric potential value is small, and it is almost linearly distributed, thus ensuring the stability and reliability of the sensor.
[0050] The above description is only a preferred embodiment of the present invention, which is only illustrative and not restrictive of the present invention. Those skilled in the art understand that many changes, modifications, and even equivalences may be made to the present invention within the spirit and scope defined by the claims of the present invention, but all of them will fall within the scope of protection of the present invention.
Claims
1. A method for preparing a fast-response thin-film thermocouple on an alloy surface, characterized in that: The following steps are involved: S1: Alloy substrate pretreatment: The surface of the alloy substrate to be tested is ground and polished to a roughness Ra of less than 0.1 μm, and then ultrasonically cleaned with ethanol and deionized water in turn, and then dried for standby use; S2: Preparation of AlCrN-based thin film: AlCrN-based thin film is deposited on the surface of alloy substrate by vacuum ion plating technology, Cr and CrN layers are used as bonding layer and transition layer, and the film thickness is 1-5 μm; S3: Preparation of thermal oxidation film: Place the alloy substrate treated in step S2 in a vacuum heat treatment furnace, evacuate and heat to maintain 700-1000°C, then introduce oxygen, maintain the gas pressure at 0.01-0.05MPa, and perform thermal oxidation treatment for 1-6h to obtain a thermal oxidation insulating film with a resistance value greater than 1MΩ; S4: Preparation of thermocouple functional film: Use magnetron sputtering technology to prepare K-type thermocouple thin film material on the surface of thermal oxide film, select NiCr and NiSi alloy targets, and use mask plates to prepare NiCr thermocouple film and NiSi thermocouple film respectively. The sputtering target voltage is 800-1000V, the sputtering current is 1-3A, and the thermocouple film thickness is 0.5-3μm. Then, lead wires are set on NiCr thermocouple and NiCr thermocouple respectively. S5: Preparation of protective film: Aluminum oxide film is formed on the surface of the alloy substrate treated in step S4 by high-power magnetron sputtering technology as a protective layer, with a thickness greater than 1 μm and a resistance value greater than 10 MΩ, thereby obtaining the fast-response thin film thermocouple.
2. The method for preparing a fast-response thin-film thermocouple on an alloy surface as claimed in claim 1, characterized in that: The alloy in step S1 is any one of cemented carbide, titanium alloy and nickel-based alloy.
3. The method for preparing a fast-response thin-film thermocouple on an alloy surface as claimed in claim 1, characterized in that: In the step S2, the AlCrN-based film is a multi-element film, including AlCrN, AlCrSiN, AlCrTiN, and AlCrYN films, and the atomic percentage of Al element in the AlCrN-based film is greater than 30%.
4. The method for preparing a fast-response thin-film thermocouple on an alloy surface as claimed in claim 1, characterized in that: In the step S3, the thermal oxidation film includes aluminum oxide and chromium oxide.
5. The method for preparing a fast-response thin-film thermocouple on an alloy surface as claimed in claim 1, characterized in that: In the step S4, the line widths of the NiCr hot electrode and the NiSi hot electrode are both 0.1-5 mm.
6. The method for preparing a fast-response thin-film thermocouple on an alloy surface as claimed in claim 1, characterized in that: In step S4, the atomic percentage of the NiCr hot electrode film is: Ni 85-93%, Cr 7-15%, and the atomic percentage of the NiSi hot electrode film is: Ni 92-99%, Si 1-8%.
7. The method for preparing a fast-response thin-film thermocouple on an alloy surface as claimed in claim 1, characterized in that: In the step S5, the protective film is dense amorphous aluminum oxide.
8. An alloy surface fast response thin film thermocouple prepared by the preparation method according to any one of claims 1 to 7.