Pressure measuring sheet set, pressure measuring sheet, method for producing pressure measuring sheet set, method for producing pressure measuring sheet, sheet, dispersion, dispersion set, microcapsule
By using microcapsules containing chromogen in the sheet for pressure measurement, combining benzotriazole structure compounds and aromatic solvents, the problem of reducing chromogen concentration during storage of the sheet is solved, and high Stability and full hair color effect.
Patent Information
- Application Number
- CN202180012837.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-25
- Filing Date
- 2021-01-28
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-01-28
AI Technical Summary
The existing sheets for pressure measurement are reduced during storage, resulting in poor storage stability. In particular, the sheets containing microcapsules containing chromogens deteriorate under external light exposure, resulting in insufficient chromogens. .
Using microcapsules containing a chromogen containing a compound with a benzotriazole structure and an aromatic solvent, the sheet set for pressure measurement is formed by designing a laminated structure and a specific composition, using a specific sheet set for The color-producing agent and color-developer, combined with benzotriazole-structured compounds and aromatic solvents, improve the solubility and stability of microcapsules.
The storage stability of the sheet set for pressure measurement is achieved, the deterioration of the chromogen is suppressed, the chromogen concentration and image quality are improved, and the stability and sufficient chromogenization are ensured under external light irradiation conditions.
Smart Images

Figure CN115053115B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a pressure measuring sheet set, a pressure measuring sheet, a method for manufacturing a pressure measuring sheet set, a method for manufacturing a pressure measuring sheet, a sheet, a dispersion, a dispersion set and a microcapsule. Background Art
[0002] In recent years, the need to measure pressure distribution has tended to increase due to the high functionality and high precision of products.
[0003] For example, Patent Document 1 proposes a pressure measurement sheet using microcapsules containing a coloring agent.
[0004] Previous technical literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 55-137992 Summary of the invention
[0007] Technical issues to be solved by the invention
[0008] On the other hand, after the pressure measuring sheet (especially the sheet having a layer containing microcapsules containing a coloring agent) is stored, the coloring concentration may decrease. Hereinafter, in this specification, a case where the rate of change of the coloring concentration when the pressure measuring sheet set or the pressure measuring sheet (especially the sheet having a layer containing microcapsules containing a coloring agent) is stored is small is referred to as excellent storage stability.
[0009] As a result of studying the pressure measurement sheet described in Patent Document 1, the present inventors found that the pressure measurement sheet described in Patent Document 1 has poor storage stability.
[0010] In view of the above circumstances, an object of the present invention is to provide a pressure measurement sheet set and a pressure measurement sheet having excellent storage stability.
[0011] Furthermore, the present invention aims to provide a method for producing a pressure measuring sheet set, a method for producing a pressure measuring sheet, a sheet, a dispersion, a dispersion set, and microcapsules.
[0012] Means for solving technical problems
[0013] As a result of intensive studies on the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by the following configuration.
[0014] (1) A pressure measurement sheet set comprising:
[0015] A first sheet having a first layer, wherein the first layer comprises microcapsules containing a coloring agent; and
[0016] a second sheet having a second layer containing a developer,
[0017] The coloring agent is selected from the group consisting of a compound represented by the general formula (1) described below and a compound having an indole structure,
[0018] The microcapsules also contain compounds with benzotriazole structures and aromatic solvents.
[0019] The aromatic solvent includes a compound having at least one aromatic ring and no aromatic condensed ring.
[0020] (2) The pressure measurement sheet set according to (1), wherein:
[0021] The pH value of the extract obtained by immersing the second sheet having a size of 10 cm in length and 10 cm in width in 50 mL of water at 25°C for 10 minutes was in the range of 6.0 to 9.0 at 25°C.
[0022] (3) The pressure measurement sheet set according to (1) or (2), wherein:
[0023] Layer 2 also contains a pH adjuster.
[0024] (4) The pressure measurement sheet set according to any one of (1) to (3), wherein:
[0025] The aromatic solvent includes a compound having one or two aromatic rings and no aromatic condensed ring.
[0026] (5) The pressure measurement sheet set according to any one of (1) to (4), wherein:
[0027] The content of the compound having a benzotriazole structure is 10% by mass or more based on the content of the coloring agent.
[0028] (6) The pressure measurement sheet set according to any one of (1) to (5), wherein:
[0029] The molecular weight of the compound having a benzotriazole structure is 500 or less.
[0030] (7) The pressure measurement sheet set according to any one of (1) to (6), wherein:
[0031] The content of coloring agent is 0.10~1.20g / m 2 .
[0032] (8) The pressure measurement sheet set according to any one of (1) to (7), wherein:
[0033] The first sheet and the second sheet are stacked so that the first layer of the first sheet and the second layer of the second sheet face each other to form a stacked body, and a pressure is applied to the stacked body to cause the color to develop. * a * b * Chroma a in the color system * More than 30 and less than 80, chromaticity b * Over -50 and below 50.
[0034] (9) The pressure measurement sheet set according to any one of (1) to (8), wherein:
[0035] The first sheet is contained in the package.
[0036] (10) The pressure measurement sheet set according to (9), wherein:
[0037] The total light transmittance of the package body is less than 5.0%.
[0038] (11) The pressure measurement sheet set according to (9) or (10), wherein:
[0039] The thickness of the package body is 20 μm or more.
[0040] (12) A pressure measuring sheet comprising:
[0041] The first layer comprises microcapsules containing a coloring agent; and
[0042] The second layer comprises a developer,
[0043] The coloring agent is selected from the group consisting of a compound represented by the general formula (1) described below and a compound having an indole structure,
[0044] The microcapsules also contain compounds with benzotriazole structures and aromatic solvents.
[0045] The aromatic solvent includes a compound having at least one aromatic ring and no aromatic condensed ring.
[0046] (13) A method for manufacturing a pressure-measuring sheet set, which is the method for manufacturing a pressure-measuring sheet set according to any one of (1) to (11), comprising:
[0047] A process of forming microcapsules using a coloring agent, a compound having a benzotriazole structure, an aromatic solvent and a capsule wall material; and
[0048] A step of applying a first layer-forming composition containing microcapsules to form the first layer.
[0049] (14) A method for manufacturing a pressure measuring sheet, which is the method for manufacturing a pressure measuring sheet according to (12), comprising:
[0050] A process of forming microcapsules using a coloring agent, a compound having a benzotriazole structure, an aromatic solvent and a capsule wall material; and
[0051] A step of applying a first layer-forming composition containing microcapsules to form the first layer.
[0052] (15) A sheet having a layer containing microcapsules containing a coloring agent,
[0053] The coloring agent is selected from the group consisting of a compound represented by the general formula (1) and a compound having an indole structure,
[0054] The microcapsules also contain compounds with benzotriazole structures and aromatic solvents.
[0055] The aromatic solvent includes a compound having at least one aromatic ring and no aromatic condensed ring.
[0056] (16) A dispersion liquid for forming a layer used in combination with a layer containing a color developer for pressure measurement and containing microcapsules containing a color developer,
[0057] The coloring agent is selected from the group consisting of a compound represented by the general formula (1) described below and a compound having an indole structure,
[0058] The microcapsules further contain a compound having a benzotriazole structure and an aromatic solvent, wherein the aromatic solvent includes a compound having at least one aromatic ring and no aromatic condensed ring.
[0059] (17) The dispersion according to (16), wherein
[0060] The molecular weight of the compound having a benzotriazole structure is 500 or less.
[0061] (18) A dispersion set comprising:
[0062] The dispersion described in (16) or (17); and
[0063] A dispersion liquid containing a developer used to form a layer containing a developer.
[0064] (19) A dispersion liquid for forming a layer for pressure measurement, comprising microcapsules containing a color former and a color developer,
[0065] The coloring agent is selected from the group consisting of a compound represented by the general formula (1) described below and a compound having an indole structure,
[0066] The microcapsules further contain a compound having a benzotriazole structure and an aromatic solvent, wherein the aromatic solvent includes a compound having at least one aromatic ring and no aromatic condensed ring.
[0067] (20) The dispersion according to (19), wherein
[0068] The molecular weight of the compound having a benzotriazole structure is 500 or less.
[0069] (21) A microcapsule containing a coloring agent,
[0070] The coloring agent is selected from the group consisting of a compound represented by the general formula (1) described below and a compound having an indole structure,
[0071] The microcapsules further contain a compound having a benzotriazole structure and an aromatic solvent, wherein the aromatic solvent includes a compound having at least one aromatic ring and no aromatic condensed ring.
[0072] Effects of the Invention
[0073] According to the present invention, it is possible to provide a pressure measurement sheet set and a pressure measurement sheet having excellent storage stability.
[0074] Furthermore, according to the present invention, it is possible to provide a method for producing a pressure measurement sheet set, a method for producing a pressure measurement sheet, a sheet, a dispersion, a dispersion set, and microcapsules. BRIEF DESCRIPTION OF THE DRAWINGS
[0075] Figure 1 This is a cross-sectional view of one embodiment of a pressure measurement sheet set.
[0076] Figure 2 This is a diagram for explaining how to use the pressure measurement sheet set.
[0077] Figure 3 This is a cross-sectional view of one embodiment of a pressure measurement sheet. DETAILED DESCRIPTION
[0078] Hereinafter, the present invention will be described in detail.
[0079] In addition, in this specification, the numerical range expressed using "to" means a range including the numerical values described before and after "to" as the lower limit and the upper limit.
[0080] Furthermore, in the numerical ranges described in this specification, the upper limit or lower limit described in a certain numerical range may be replaced by the upper limit or lower limit of the numerical range described in another stage. Furthermore, in the numerical ranges described in this specification, the upper limit or lower limit described in a certain numerical range may be replaced by the value shown in the embodiments.
[0081] The various components described below may be used alone or in combination of two or more. For example, the polyisocyanate described below may be used alone or in combination of two or more.
[0082] In the present specification, when simply referred to as a substituent, examples of the substituent include the following substituent T.
[0083] (Substituent T)
[0084] Examples of the substituent T include a halogen atom (a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc.), an alkyl group, a cycloalkyl group, an alkenyl group, a cycloalkenyl group, an alkynyl group, an aryl group, a heterocyclic group, a cyano group, a hydroxyl group, a nitro group, a carboxyl group, an alkoxy group, an aryloxy group, a silyloxy group, a heterocyclic group, an acyloxy group, a carbamoyloxy group, an amino group (including an alkylamino group and a phenylamino group), an acylamino group, an aminocarbonylamino group, an alkoxycarbonylamino group, an aryloxycarbonylamino group, a sulfamoylamino group, an alkyl or arylsulfonylamino group, a mercapto group, an alkylthio group, an arylthio group, a heterocyclicthio group, a sulfamoyl group, a sulfonic acid group, an alkyl or arylsulfinyl group, an alkyl or arylsulfonyl group, an acyl group, an aryloxycarbonyl group, an alkoxycarbonyl group, a carbamoyl group, an aryl or heterocyclic azo group, an imide group, a phosphinyl group, a phosphinyloxy group, a phosphinylamino group, a silyl group, and a polymerizable group.
[0085] Among the above-mentioned substituents, the hydrogen atoms in the substituent having hydrogen atoms may be substituted by any of the above-mentioned substituents.
[0086] The characteristics of the pressure measuring sheet set and the pressure measuring sheet of the present invention include the use of microcapsules containing a predetermined coloring agent, a compound having a benzotriazole structure, and a predetermined aromatic solvent.
[0087] According to the research of the inventors, it is known that during the above-mentioned storage, external light affects the coloring agent in the pressure measuring sheet set and the pressure measuring sheet, resulting in a decrease in the coloring concentration. That is, if the pressure measuring sheet set and the pressure measuring sheet are irradiated with light such as external light during storage, the light-based coloring agent deteriorates over time, and the coloring property of the pressure measuring sheet set and the pressure measuring sheet becomes insufficient. On the other hand, the microcapsules used in the present invention can suppress the degradation of the coloring agent by combining a prescribed coloring agent and a compound having a benzotriazole structure. As a result, it is estimated that a pressure measuring sheet set and a pressure measuring sheet with excellent storage stability can be obtained.
[0088] Furthermore, it is presumed that the microcapsules used in the present invention can improve the solubility of the compound having a benzotriazole structure and provide more excellent storage stability by containing a predetermined aromatic solvent.
[0089] [First embodiment]
[0090] Figure 1 This is a cross-sectional view of one embodiment of a pressure measurement sheet set.
[0091] The pressure measurement sheet set 10 includes a first sheet 16 and a second sheet 22, wherein the first sheet 16 has a first support 12 and a first layer 14 disposed on the first support 12 and containing microcapsules 13, and the second sheet 22 has a second support 18 and a second layer 20 disposed on the second support 18 and containing a color developer.
[0092] like Figure 2 As shown, when the pressure measurement sheet set 10 is used, the first sheet 16 and the second sheet 22 are stacked so that the first layer 14 in the first sheet 16 and the second layer 20 in the second sheet 22 face each other. By applying pressure from at least one of the first support 12 side of the first sheet 16 and the second support 18 side of the second sheet 22 in the obtained stacked body, the microcapsules 13 are ruptured in the pressurized area, and the coloring agent contained in the microcapsules 13 flows out of the microcapsules 13 and reacts with the coloring agent in the second layer 20. As a result, coloring is performed in the pressurized area.
[0093] As described later, the first sheet 16 may have the first layer 14 or the first support 12 . Also, the second sheet 22 may have the second layer 20 or the second support 18 .
[0094] In addition, Figure 1 In the embodiment, the first support 12 and the first layer 14 are directly stacked, but the present invention is not limited to this embodiment. As described later, another layer (for example, an easy-adhesion layer) may be arranged between the first support 12 and the first layer 14. Figure 1 In the embodiment, the second support 18 and the second layer 20 are directly stacked, but the present invention is not limited to this embodiment, and as described later, another layer (for example, an easy-adhesion layer) may be arranged between the second support 18 and the second layer 20.
[0095] Hereinafter, the structures of the first sheet 16 and the second sheet 22 constituting the pressure measurement sheet set 10 will be described in detail.
[0096] <<1st sheet>>
[0097] Figure 1 The first sheet 16 described in has a first support 12 and a first layer 14 including microcapsules 13 containing a color developer.
[0098] Hereinafter, each component will be described in detail.
[0099] <First Support>
[0100] The first support is a member for supporting the first layer. In addition, when the first layer itself can be handled, the first sheet may not have the first support.
[0101] The first support may be in any shape of a sheet or a plate.
[0102] Examples of the first support include resin films and synthetic papers.
[0103] Examples of the resin film include polyester films such as polyethylene terephthalate films, cellulose derivative films such as cellulose triacetate, polyolefin films such as polypropylene and polyethylene, and polystyrene films.
[0104] Examples of synthetic paper include paper obtained by biaxially stretching polypropylene or polyethylene terephthalate to form multiple micropores (Yupo, etc.), paper made from synthetic fibers such as polyethylene, polypropylene, polyethylene terephthalate and polyamide, and paper obtained by layering these on a portion, one side or both sides of the paper.
[0105] Among them, from the viewpoint of better storage stability (hereinafter also referred to as "the viewpoint of better effect of the present invention") and from the viewpoint of further improving the color development concentration by pressurization, a resin film or a synthetic paper is preferred, and a resin film is more preferred. From the viewpoint of being able to visually recognize the color development property when visually recognized from the support side, the support is preferably transparent.
[0106] From the viewpoint of achieving more excellent effects of the present invention, the thickness of the first support is preferably 10 to 200 μm.
[0107] <1st floor>
[0108] The first layer includes microcapsules containing a predetermined coloring agent, a compound having a benzotriazole structure, and an aromatic solvent.
[0109] Hereinafter, first, the materials constituting the microcapsules will be described in detail.
[0110] Microcapsules generally have a core and a capsule wall for containing a core material constituting the core (a substance contained (also referred to as an included component)).
[0111] In the present invention, the microcapsule contains a coloring agent as a core material (inner component). Since the coloring agent is contained in the microcapsule, the coloring agent can exist stably until the microcapsule is ruptured by applying pressure.
[0112] Microcapsules have a capsule wall containing a core material.
[0113] As the material of the capsule wall of the microcapsule (wall material), there can be mentioned known resins which have been used as wall materials of microcapsules containing coloring agents in the applications of pressure-sensitive copy paper or thermal recording paper. Specifically, there can be mentioned polyurethane, polyurea, polyurethane urea, melamine-formaldehyde resin and gelatin.
[0114] Among them, from the viewpoint of achieving more excellent effects of the present invention, it is preferred that the capsule wall of the microcapsule contains at least one resin selected from the group consisting of polyurethaneurea, polyurethane, and polyurea.
[0115] The capsule wall of the microcapsule is preferably substantially composed of a resin. Substantially composed of a resin means that the content of the resin relative to the total mass of the capsule wall is 90% by mass or more, preferably 100% by mass. That is, the capsule wall of the microcapsule is preferably composed of a resin.
[0116] In addition, polyurethane refers to a polymer having a plurality of urethane bonds, and is preferably a reaction product formed from raw materials containing a polyol and a polyisocyanate.
[0117] Furthermore, polyurea refers to a polymer having a plurality of urea bonds, and is preferably a reaction product formed from raw materials including polyamines and polyisocyanates. In addition, polyurea can be synthesized using polyisocyanates instead of polyamines by reacting a portion of polyisocyanates with water to form polyamines.
[0118] Furthermore, polyurethane urea refers to a polymer having a carbamate bond and a urea bond, and is preferably a reaction product formed from raw materials including polyols, polyamines, and polyisocyanates. In addition, when polyols and polyisocyanates are reacted, sometimes a part of the polyisocyanates reacts with water to form polyamines, and as a result, polyurethane urea can be obtained.
[0119] Furthermore, the melamine-formaldehyde resin is preferably a reaction product formed by the polycondensation of melamine and formaldehyde.
[0120] The polyisocyanate is a compound having two or more isocyanate groups, and examples thereof include aromatic polyisocyanates and aliphatic polyisocyanates. Examples of the polyisocyanate include adducts of polyols such as trimethylolpropane and bifunctional polyisocyanates.
[0121] Furthermore, the above-mentioned polyol refers to a compound having two or more hydroxyl groups, for example, low molecular weight polyols (e.g., aliphatic polyols, aromatic polyols. In addition, "low molecular weight polyols" refer to polyols with a molecular weight of 400 or less), polyvinyl alcohol, polyether polyols, polyester polyols, polylactone polyols, castor oil polyols, polyolefin polyols and hydroxyl-containing amine compounds (for example, amino alcohols. As amino alcohols, for example, propylene oxide or ethylene oxide adducts of amino compounds such as ethylenediamine, namely N,N,N',N'-tetrakis[2-hydroxypropyl]ethylenediamine, etc. can be mentioned.).
[0122] Furthermore, the above-mentioned polyamine refers to a compound having two or more amino groups (primary or secondary amino groups), for example, aliphatic polyamines such as diethylenetriamine, triethylenetetramine, 1,3-propylenediamine and hexamethylenediamine; epoxy compound adducts of aliphatic polyamines; alicyclic polyamines such as piperazine; heterocyclic diamines such as 3,9-bis-aminopropyl-2,4,8,10-tetraoxospiro-(5,5)undecane.
[0123] The glass transition temperature of the capsule wall of the microcapsule is not particularly limited, but is preferably 50 to 160° C., more preferably 80 to 150° C., from the viewpoint of facilitating the formation of microcapsules in the first layer when the first layer is formed.
[0124] The glass transition temperature of the capsule wall is measured as follows.
[0125] Prepare 50 sheets of the first layer (microcapsule layer) of 1 cm in length and 1 cm in width, immerse all of them in 10 ml of water and let stand for 24 hours to obtain an aqueous dispersion of microcapsules. Alternatively, when the first sheet includes the first support, 50 sheets of the first sheet of 1 cm in length and 1 cm in width may be prepared and immersed.
[0126] The obtained aqueous dispersion of microcapsules was centrifuged at 15000 rpm for 30 minutes to separate microcapsules. Ethyl acetate was added to the separated microcapsules, and further stirred at 25°C for 24 hours. Thereafter, the obtained solution was filtered, and the obtained residue was vacuum dried at 60°C for 48 hours, thereby obtaining microcapsules containing no substance inside (hereinafter also referred to as "measurement material"). That is, the capsule wall material of the microcapsule to be measured for the glass transition temperature can be obtained.
[0127] Next, the thermal decomposition temperature of the obtained measurement material was measured using a thermogravimetric differential thermal analyzer TG-DTA (device name: DTG-60, Shimadzu Corporation). In addition, the thermal decomposition temperature refers to the temperature at which the measurement material is heated from room temperature at a constant heating rate (10°C / min) and the mass of the measurement material before heating is reduced by 5% by mass as the thermal decomposition temperature (°C) in a thermogravimetric analysis (TGA) in an atmospheric environment.
[0128] Next, the glass transition temperature of the material was measured using a differential scanning calorimeter DSC (device name: DSC-60a Plus, Shimadzu Corporation) in a closed pan at a heating rate of 5°C / min within a range of 25°C to (thermal decomposition temperature (°C) - 5°C).
[0129] As the glass transition temperature of the capsule wall of the microcapsule, the value at the time of the second cycle of temperature increase was used.
[0130] The volume-based median diameter (D50) of the microcapsule is not particularly limited, but is preferably 1 to 80 μm, more preferably 5 to 70 μm, and further preferably 10 to 50 μm.
[0131] The volume-based median diameter of the microcapsules can be controlled by adjusting the production conditions of the microcapsules and the like.
[0132] Here, the volume-based median diameter of the microcapsule refers to the diameter at which the total volume of the particles on the larger diameter side and the smaller diameter side is equal when the entire microcapsule is divided into two using the particle diameter at which the cumulative volume is 50% as the threshold value. That is, the median diameter corresponds to the so-called D50.
[0133] This is a value calculated by photographing the surface of the first layer of the first sheet having the first layer containing microcapsules at 1000 times with an optical microscope and measuring the sizes of all microcapsules within a range of 500 μm×500 μm.
[0134] The volume-based median diameter of the microcapsules contained in the dispersion can be measured by a laser diffraction / scattering particle size distribution measuring apparatus (LA-960, manufactured by HORIBA).
[0135] The number average wall thickness of the capsule wall of the microcapsule is not particularly limited, but is preferably 0.01 to 2 μm, more preferably more than 0.02 μm and less than 2 μm, and further preferably 0.05 to 1.5 μm.
[0136] In addition, the wall thickness of the microcapsule refers to the thickness (μm) of the capsule wall of the capsule particles forming the microcapsule, and the number average wall thickness refers to the average value of the thickness (μm) of each capsule wall of 5 microcapsules obtained by scanning electron microscopy (SEM) and averaged. More specifically, a cross-sectional slice of the first sheet having the first layer containing microcapsules is prepared, and the cross section is observed at 200 times by SEM, and on the basis of selecting any 5 microcapsules having a long diameter in the range of (the value of the median diameter (D50) based on the volume of the microcapsule) × 0.9 to (the value of the median diameter (D50) based on the volume of the microcapsule) × 1.1, the cross section of each selected microcapsule is observed at 15000 times, and the thickness of the capsule wall is obtained and the average value is calculated. In addition, the long diameter refers to the longest diameter when observing the microcapsule.
[0137] The ratio (δ / Dm) of the number average wall thickness δ of the microcapsules to the volume-based median diameter (D50) Dm of the microcapsules is not particularly limited, but is often 0.001 or more. From the viewpoint of achieving more excellent effects of the present invention, it is preferred that the relationship of formula (1) is satisfied.
[0138] Formula (1) 0.100>δ / Dm>0.001
[0139] That is, the ratio (δ / Dm) is preferably greater than 0.001 and less than 0.100. If the relationship of the formula (1) is satisfied, the color density level can be set to a range in which the color development level can be easily recognized according to the pressure.
[0140] (Coloring Agent)
[0141] The microcapsules contain a coloring agent selected from the group consisting of compounds represented by the general formula (1) and compounds having an indole structure.
[0142] The coloring agent refers to a compound that develops color from a colorless state by contact with a color developer described later. As the coloring agent, an electron donating dye precursor (precursor of a color-developing dye) is preferred. That is, as the coloring agent, an electron donating colorless dye is preferred.
[0143] [Compound represented by general formula (1)]
[0144] [Chemical formula 1]
[0145]
[0146] In the general formula (1), R 1 and R 3 Each independently represents an oxygen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent.
[0147] By R 1 and R 3The number of carbon atoms in the alkyl group represented by is not particularly limited, but is preferably 1 to 10, more preferably 1 to 5, from the viewpoint of further improving the effects of the present invention.
[0148] The type of the substituent that the alkyl group or the aryl group may have is not particularly limited, and the substituents exemplified in the substituent T described above may be mentioned.
[0149] Among them, from the viewpoint of more excellent effect of the present invention, as R 1 and R 3 , are preferably each independently an alkyl group which may have a substituent or an aryl group which may have a substituent, more preferably an alkyl group which may have a substituent, and still more preferably an unsubstituted alkyl group.
[0150] R 2 and R 4 Each independently represents an alkyl group which may have a substituent or an aryl group which may have a substituent.
[0151] By R 2 and R 4 The number of carbon atoms in the alkyl group represented by is not particularly limited, but is preferably 1 to 10, more preferably 1 to 5, from the viewpoint of further improving the effects of the present invention.
[0152] By R 2 and R 4 The aryl group represented may be a monocyclic structure or a bicyclic structure.
[0153] The type of the substituent that the alkyl group and the aryl group may have is not particularly limited, and the groups exemplified in the substituent T described above can be mentioned.
[0154] Among them, from the viewpoint of more excellent effect of the present invention, as R 2 and R 4 , are each independently preferably an alkyl group which may have a substituent, and more preferably an unsubstituted alkyl group.
[0155] Among them, all R 1 ~R 4 Preferred are unsubstituted alkyl groups, and more preferred are the same unsubstituted alkyl groups.
[0156] X 1 Indicates -O- or -NR 5 Among them, from the viewpoint of more excellent effect of the present invention, -NR 5 -.
[0157] R 5 represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent.
[0158] By R 5The number of carbon atoms in the alkyl group represented by is not particularly limited, but is preferably 1 to 10, more preferably 1 to 5, from the viewpoint of further improving the effects of the present invention.
[0159] By R 5 The aryl group represented may be a monocyclic structure or a bicyclic structure.
[0160] The type of the substituent that the alkyl group and the aryl group may have is not particularly limited, and the groups exemplified in the substituent T described above can be mentioned.
[0161] Among them, from the viewpoint of more excellent effect of the present invention, as R 5 , preferably an aryl group which may have a substituent, more preferably an aryl group substituted with a group selected from a halogen atom, a cyano group, a nitro group and a carboxyl group.
[0162] The molecular weight of the compound represented by the general formula (1) is not particularly limited, but is preferably 300 or more, more preferably 500 or more. The upper limit is not particularly limited, but is preferably 2000 or less, more preferably 1000 or less.
[0163] [Compounds having an indole structure]
[0164] The compound having an indole structure is a compound having an indole structure as a partial structure. In addition, as described above, the compound having an indole structure functions as a coloring agent. That is, the compound is equivalent to a coloring agent having an indole structure.
[0165] The number of indole structures in the compound having an indole structure is not particularly limited, and may be one or more. Among them, from the viewpoint of achieving a more excellent effect of the present invention, the number of indole structures is preferably two or more, and more preferably two.
[0166] The compound having an indole structure is preferably a compound represented by the general formula (2) or a compound represented by the general formula (3), and more preferably a compound represented by the general formula (3).
[0167] [Chemical formula 2]
[0168]
[0169] In the general formula (2), R 6 and R 7 Each independently represents a hydrogen atom or an alkyl group which may have a substituent.
[0170] By R 6 The number of carbon atoms in the alkyl group represented is not particularly limited, but is preferably 1 to 30, more preferably 1 to 20, further preferably 1 to 12, and particularly preferably 5 to 10 from the viewpoint of further improving the effects of the present invention.
[0171] By R 7 The number of carbon atoms in the alkyl group represented is not particularly limited, but is preferably 1 to 10, more preferably 1 to 5, and even more preferably 1 to 3 from the viewpoint of further improving the effects of the present invention.
[0172] The type of the substituent that the alkyl group may have is not particularly limited, and the substituents exemplified in the substituent T described above can be mentioned.
[0173] Among them, from the viewpoint of more excellent effect of the present invention, R 6 and R 7 Preferably, it represents an alkyl group which may have a substituent, and more preferably, it represents an unsubstituted alkyl group.
[0174] R 8 represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent.
[0175] By R 8 The number of carbon atoms in the alkyl group represented by is not particularly limited, but is preferably 1 to 10, more preferably 1 to 5, from the viewpoint of further improving the effects of the present invention.
[0176] By R 8 The aryl group represented may be a monocyclic structure or a bicyclic structure.
[0177] The type of the substituent that the alkyl group and the aryl group may have is not particularly limited, and the groups exemplified in the substituent T described above can be mentioned.
[0178] Among them, from the viewpoint of more excellent effect of the present invention, as R 8 , preferably an aryl group which may have a substituent, more preferably an aryl group which has a substituent.
[0179] X 2 Indicates -O- or -NR 9 -.
[0180] Among them, from the viewpoint of more excellent effects of the present invention, as X 2 , preferably -O-.
[0181] R 9 represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent.
[0182] By R 9 The number of carbon atoms in the alkyl group represented by is not particularly limited, but is preferably 1 to 10, more preferably 1 to 5, from the viewpoint of further improving the effects of the present invention.
[0183] By R 9 The aryl group represented may be a monocyclic structure or a bicyclic structure.
[0184] The type of the substituent that the alkyl group and the aryl group may have is not particularly limited, and the groups exemplified in the substituent T described above can be mentioned.
[0185] The molecular weight of the compound represented by the general formula (2) is not particularly limited, but is preferably 300 or more, more preferably 500 or more. The upper limit is not particularly limited, but is preferably 2000 or less, more preferably 1000 or less.
[0186] [Chemical formula 3]
[0187]
[0188] In the general formula (3), R 10 ~R 13 Each independently represents a hydrogen atom or an alkyl group which may have a substituent.
[0189] By R 10 and R 12 The number of carbon atoms in the alkyl group represented is not particularly limited, but is preferably 1 to 30, more preferably 1 to 20, further preferably 1 to 12, and particularly preferably 5 to 10 from the viewpoint of further improving the effects of the present invention.
[0190] By R 11 and R 13 The number of carbon atoms in the alkyl group represented is not particularly limited, but is preferably 1 to 10, more preferably 1 to 5, and even more preferably 1 to 3 from the viewpoint of further improving the effects of the present invention.
[0191] The type of the substituent that the alkyl group may have is not particularly limited, and the substituents exemplified in the substituent T described above can be mentioned.
[0192] Among them, from the viewpoint of more excellent effect of the present invention, as R 10 ~R 13 , preferably an alkyl group which may have a substituent, and more preferably an unsubstituted alkyl group.
[0193] X 3 Indicates -O- or -NR 14 -.
[0194] Among them, from the viewpoint of more excellent effects of the present invention, as X 3 , preferably -O-.
[0195] R 14 represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent.
[0196] By R 14The number of carbon atoms in the alkyl group represented by is not particularly limited, but is preferably 1 to 10, more preferably 1 to 5, from the viewpoint of further improving the effects of the present invention.
[0197] By R 14 The aryl group represented may be a monocyclic structure or a bicyclic structure.
[0198] The type of the substituent that the alkyl group and the aryl group may have is not particularly limited, and the groups exemplified in the substituent T described above can be mentioned.
[0199] The molecular weight of the compound represented by the general formula (3) is not particularly limited, but is preferably 300 or more, more preferably 500 or more. The upper limit is not particularly limited, but is preferably 2000 or less, more preferably 1000 or less.
[0200] The coloring agent may be used alone or in combination of two or more.
[0201] Furthermore, as the coloring agent, a compound represented by the general formula (1) and a compound having an indole structure may be used in combination.
[0202] As the coloring agent, a coloring agent other than the compound represented by the general formula (1) and the compound having an indole structure may be used in combination.
[0203] The content of the color former selected from the compound represented by the general formula (1) and the compound having an indole structure is preferably 20 to 100% by mass, more preferably 40 to 100% by mass, based on the total mass of the color former.
[0204] The content of the coloring agent in the first layer is not particularly limited, but is usually 0.05 to 2.00 g / m 2 From the viewpoint of more excellent effects of the present invention, it is preferably 0.10 to 1.20 g / m 2 , more preferably 0.20 to 0.80 g / m 2 .
[0205] (Compound having a benzotriazole structure)
[0206] The microcapsule contains a compound having a benzotriazole structure. The compound having a benzotriazole structure is preferably a UV absorber. That is, the compound is preferably a UV absorber having a benzotriazole structure.
[0207] The ultraviolet absorber is an organic compound having a function of absorbing ultraviolet rays irradiated from the outside.
[0208] The number of benzotriazole structures in the compound having a benzotriazole structure is not particularly limited, and may be one or more.
[0209] As the compound having a benzotriazole structure, a compound represented by the general formula (4) is preferred.
[0210] [Chemical formula 4]
[0211]
[0212] In the general formula (4), R 15 ~R 18 Each independently represents a hydrogen atom or a substituent.
[0213] As R 15 ~R 18 The substituent represented by is not particularly limited, and the groups exemplified in the substituent T described above can be mentioned.
[0214] Among them, R 15 ~R 18 When it is a substituent, from the viewpoint of excellent effect of the present invention, R 15 ~R 18 At least one of them is a halogen atom.
[0215] R 19 represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent.
[0216] By R 19 The aryl group represented may be a monocyclic structure or a bicyclic structure.
[0217] The type of the substituent that the alkyl group and the aryl group may have is not particularly limited, and the groups exemplified in the substituent T described above can be mentioned.
[0218] Among them, from the viewpoint of excellent effect of the present invention, as R 19 , preferably an aryl group which may have a substituent, and more preferably an aryl group substituted with at least one hydroxyl group.
[0219] The molecular weight of the compound having a benzotriazole structure is not particularly limited, but from the viewpoint of achieving a more excellent effect of the present invention, it is preferably 500 or less, more preferably 400 or less, and further preferably 350 or less. The lower limit is not particularly limited, but is often 100 or more. When the molecular weight of the compound having a benzotriazole structure is small, it is easily dissolved in the aromatic solvent described later, resulting in better storage stability.
[0220] The compound having a benzotriazole structure is not particularly limited, and examples thereof include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-5'-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-dodecane-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-5'-(1,1,3,3-tetramethylbutyl)phenyl)benzotriazole, 2-(2'-hydroxy-4'-octyloxyphenyl)benzotriazole, 2-(2'-hydroxy-3'-(3,4,5,6-tetrahydrophthalimidomethyl)-5'-methylbenzylphenyl)benzotriazole, 2-(3'-sec-butyl-5'-tert-butyl-2'-hydroxyphenyl)benzotriazole, 2-(3',5'-bis-(α,α-dimethylbenzyl)-2'-hydroxyphenyl)benzotriazole 2-(3'-tert-butyl-2'-hydroxy-5'-(2-octyloxycarbonylethyl)phenyl)-5-chloro-benzotriazole, 2-(3'-tert-butyl-5'-[2-(2-ethylhexyloxy)-carbonylethyl]-2'-hydroxyphenyl)-5-chloro-benzotriazole, 2-(3'-tert-butyl-2'-hydroxy-5'-(2-methoxycarbonylethyl)phenyl)-5-chloro-benzotriazole, 2-(3'-tert-butyl-2'-hydroxy-5'-(2-methoxycarbonylethyl)phenyl)benzotriazole, 2-(3'-tert-butyl phenyl)benzotriazole, 2-(3'-tert-butyl-2'-hydroxy-5'-(2-octyloxycarbonylethyl)phenyl)benzotriazole, 2-(3'-tert-butyl-5'-[2-(2-ethylhexyloxy)carbonylethyl]-2'-hydroxyphenyl)benzotriazole, 2-(3'-dodecane-2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(3'-tert-butyl-2'-hydroxy-5'-(2-isooctyloxycarbonylethyl)phenyl)benzotriazole and 2,2'-methylene-bis[4-(1,1,3,3-tetramethylbutyl)-6-benzotriazol-2-ylphenol].
[0221] Among them, from the viewpoint of more excellent effects of the present invention, the compound having a benzotriazole structure is preferably 2-(2'-hydroxy-5'-methylphenyl)benzotriazole or 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole.
[0222] The compound having a benzotriazole structure may be used alone or in combination of two or more.
[0223] The content of the compound having a benzotriazole structure in the microcapsule is not particularly limited, but is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more relative to the coloring agent from the viewpoint of achieving better effects of the present invention.
[0224] The upper limit is not particularly limited, but is preferably 500% by mass or less, more preferably 300% by mass or less, and further preferably 100% by mass or less, from the viewpoint of the solubility of the compound having a benzotriazole structure.
[0225] As the ultraviolet absorber, an ultraviolet absorber other than the compound having a benzotriazole structure may be used.
[0226] The content of the ultraviolet absorber other than the compound having a benzotriazole structure is preferably 0 to 50% by mass, more preferably 0 to 25% by mass, based on the total mass of the compound having a benzotriazole structure.
[0227] (Aromatic solvents)
[0228] The microcapsules contain aromatic solvents.
[0229] The aromatic solvent is a solvent having an aromatic ring. The aromatic solvent is preferably in a liquid state at 25° C. The specific compound described below is also preferably in a liquid state at 25° C.
[0230] The aromatic solvent includes a compound having at least one aromatic ring and no aromatic condensed ring (hereinafter also referred to as a "specific compound"). That is, the aromatic solvent includes a solvent having at least one aromatic ring and no aromatic condensed ring.
[0231] The number of aromatic rings contained in the specific compound is not particularly limited, but is preferably 1 or more from the viewpoint of achieving a better effect of the present invention. The upper limit is not particularly limited, but is preferably 5 or less, more preferably 3 or less, and further preferably 1 or 2.
[0232] Furthermore, the aromatic ring may have a substituent. Examples of the substituent that the aromatic ring may have include the groups exemplified as the substituent T described above.
[0233] Furthermore, the specific compound does not have an aromatic condensed ring. An aromatic condensed ring refers to a ring formed by condensing two or more aromatic rings.
[0234] The aromatic solvent preferably contains a compound represented by the general formula (5).
[0235] [Chemical formula 5]
[0236]
[0237] In the general formula (5), R 20 ~R 24 Each independently represents a hydrogen atom, an alkyl group which may have a substituent, or a monocyclic aromatic group which may have a substituent.
[0238] By R 20 ~R 24 The number of carbon atoms in the alkyl group represented is not particularly limited, but is preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 5 from the viewpoint of further improving the effects of the present invention.
[0239] By R 20 ~R 24 The monocyclic aromatic group represented by means a monocyclic aromatic group, and examples thereof include a benzene ring group and a monocyclic aromatic heterocyclic group.
[0240] Among them, from the viewpoint of excellent effect of the present invention, as R 20 ~R 24 , preferably a hydrogen atom or an alkyl group which may have a substituent.
[0241] The type of the substituent that the alkyl group and the monocyclic aromatic group may have is not particularly limited, and the groups exemplified in the substituent T described above can be mentioned.
[0242] L represents a single bond or an alkylene group which may have a substituent.
[0243] The number of carbon atoms of the alkylene group represented by L is not particularly limited, but is preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 5 from the viewpoint of further improving the effects of the present invention.
[0244] Among them, from the viewpoint of achieving more excellent effects of the present invention, L is preferably an alkylene group which may have a substituent.
[0245] The type of the substituent that the alkylene group may have is not particularly limited, and the groups exemplified in the substituent T described above can be mentioned.
[0246] R 25 represents a hydrogen atom or a monocyclic aromatic group which may have a substituent.
[0247] By R 25 The monocyclic aromatic group represented by means a monocyclic aromatic group, and examples thereof include a benzene ring group and a monocyclic aromatic heterocyclic group.
[0248] Among them, from the viewpoint of excellent effect of the present invention, as R 25 , preferably a monocyclic aromatic group which may have a substituent.
[0249] The specific compound is not particularly limited, and examples thereof include alkylbenzene compounds, diarylalkane compounds such as 1,1-diphenylethane and 1-phenyl-1-(2,3-silyl)ethane, alkylbiphenyl compounds such as isopropylbiphenyl, triarylmethane compounds, diarylalkylene compounds, and aromatic hydrocarbons such as arylindane compounds.
[0250] Among them, the aromatic solvent is preferably an alkylbenzene compound or a diarylalkane compound from the viewpoint of excellent solubility of the compound having a benzotriazole structure.
[0251] The aromatic solvent may be used alone or in combination of two or more.
[0252] Among them, from the viewpoint of achieving more excellent effects of the present invention, it is preferred to use two or more aromatic solvents, and more preferably to use a mixture of 2 to 5 aromatic solvents.
[0253] Aromatic solvents other than the specific compound may be used in combination.
[0254] The content of the specific compound is preferably 50 to 100% by mass, more preferably 75 to 100% by mass, based on the total mass of the aromatic solvent.
[0255] The content of the aromatic solvent in the microcapsule is not particularly limited, but is preferably 20 to 80% by mass, more preferably 30 to 70% by mass, based on the total mass of the microcapsule, from the viewpoint of excellent desired effects of the present invention.
[0256] (Other ingredients)
[0257] The microcapsule may contain other components besides the above-mentioned predetermined coloring agent, the compound having a benzotriazole structure and the aromatic solvent.
[0258] The microcapsules may contain aliphatic solvents.
[0259] The aliphatic solvent refers to a solvent containing a compound having an aliphatic group, that is, a solvent containing a compound having no aromatic ring.
[0260] There is no particular limitation on the aliphatic solvent, and examples thereof include aliphatic hydrocarbons such as isoparaffin and dibutyl phthalate; natural animal and plant oils such as soybean oil, corn oil, cottonseed oil, rapeseed oil, olive oil, coconut oil, castor oil and fish oil; and high-boiling-point fractions of natural products such as mineral oil.
[0261] Among them, from the viewpoint of achieving more excellent effects of the present invention, the aliphatic solvent is preferably an aliphatic hydrocarbon, and more preferably an isoalkane.
[0262] The aliphatic solvent may be used alone or in combination of two or more.
[0263] The content of the aliphatic solvent in the microcapsule is not particularly limited, but is preferably 5 to 40% by mass, more preferably 10 to 30% by mass, based on the total mass of the aromatic solvent, from the viewpoint of excellent desired effects of the present invention.
[0264] In addition to the above-mentioned components, the microcapsules may contain one or more solvents other than the above-mentioned solvents, light stabilizers, antioxidants, waxes, deodorants and other additives as necessary.
[0265] (Method for producing microcapsules)
[0266] The method for producing microcapsules is not particularly limited, and examples thereof include a method comprising a step of forming microcapsules using the above-mentioned coloring agent, the above-mentioned compound having a benzotriazole structure, the above-mentioned aromatic solvent, and a capsule wall material. Specifically, examples thereof include known methods such as interfacial polymerization, internal polymerization, phase separation, external polymerization, and coacervation. Among them, interfacial polymerization is preferred.
[0267] Hereinafter, the interfacial polymerization method will be described by taking as an example a method for producing microcapsules whose capsule walls are polyurea or polyurethaneurea.
[0268] The interfacial polymerization method includes a step of dispersing an oil phase containing a predetermined coloring agent, a compound having a benzotriazole structure, an aromatic solvent and a capsule wall material (for example, a raw material containing at least one selected from polyisocyanate, polyol and polyamine. In addition, when polyamine is produced in a reaction system by reacting polyisocyanate with water, polyol and polyamine may not be used) in an aqueous phase containing an emulsifier to prepare an emulsion (emulsification step) and a step of polymerizing the capsule wall material at the interface between the oil phase and the aqueous phase to form a capsule wall and form microcapsules containing the coloring agent (encapsulation step).
[0269] The mass ratio of the total amount of polyol and polyamine to the amount of polyisocyanate in the raw materials (total amount of polyol and polyamine / amount of polyisocyanate) is not particularly limited, but is preferably 0.1 / 99.9 to 30 / 70, and more preferably 1 / 99 to 25 / 75.
[0270] In addition, the type of the emulsifier used in the emulsification step is not particularly limited, and examples thereof include a dispersant and a surfactant.
[0271] As a dispersant, polyvinyl alcohol is mentioned, for example.
[0272] The first layer may contain other components (eg, a binder, a surfactant) in addition to the above-mentioned microcapsules.
[0273] Furthermore, the mass per unit area of the first layer (g / m 2 ) is not particularly limited, but is preferably 0.5 to 30 g / m from the viewpoint of achieving a more excellent effect of the present invention. 2 .
[0274] <Method for Forming the First Layer>
[0275] The method for forming the first layer is not particularly limited, and examples include a method having a step of applying a first layer-forming composition containing microcapsules to form the first layer. Specifically, examples include a method in which a first layer-forming composition containing microcapsules is applied to a first support and dried as needed.
[0276] The first layer forming composition preferably contains at least microcapsules and a solvent. Alternatively, a microcapsule dispersion obtained by the above-mentioned interfacial polymerization method may be used as the first layer forming composition.
[0277] The first layer forming composition may contain other components that can be contained in the above-mentioned first layer.
[0278] The method for coating the first layer forming composition is not particularly limited. Examples of the coater used for coating include an air knife coater, a rod coater, a bar coater, a curtain coater, a gravure coater, an extrusion coater, a die coater, a slide bead coater, and a knife coater.
[0279] After the first layer-forming composition is applied onto the first support, the coating film may be dried as necessary. Examples of the drying treatment include heating treatment.
[0280] In the above, a method of forming the first layer on the first support is described, but the method is not limited to the above method. For example, the first layer may be formed on a temporary support and then the temporary support may be peeled off to form a first sheet composed of the first layer.
[0281] The temporary support is not particularly limited as long as it is a releasable support.
[0282] <Packaging>
[0283] The first sheet may be contained in the package.
[0284] The package may be a bag or a container including a container body having an opening and a lid for closing the opening.
[0285] The total light transmittance of the package is not particularly limited, but is preferably less than 5.0%, more preferably less than 4.0%, and further preferably less than 1.0% from the viewpoint of achieving better effects of the present invention. The lower limit is not particularly limited, and may be 0%.
[0286] The diffusion transmittance of the package is not particularly limited, but is preferably less than 5.0%, more preferably less than 4.0%, and further preferably less than 1.0% from the viewpoint of achieving more excellent effects of the present invention. The lower limit is not particularly limited, and may be 0%.
[0287] The parallel light transmittance of the package is not particularly limited, but is preferably less than 5.0%, more preferably less than 4.0%, and further preferably less than 1.0% from the viewpoint of achieving a more excellent effect of the present invention. The lower limit is not particularly limited, and may be 0%.
[0288] The haze of the package is not particularly limited, but is preferably less than 5.0%, more preferably less than 4.0%, and further preferably less than 1.0% from the viewpoint of achieving a more excellent effect of the present invention. The lower limit is not particularly limited, and may be 0.0%.
[0289] The total light transmittance, diffuse transmittance, parallel light transmittance and haze of the package can be measured, for example, using a haze meter (HGM-2DP, manufactured by Suga Test Instruments Co., Ltd.) by a method in accordance with JIS-K-7361.
[0290] The total light transmittance, diffuse transmittance, parallel light transmittance and haze of the package are preferably all less than 5.0%, more preferably less than 4.0%, and further preferably less than 1.0%. The lower limit is not particularly limited, and may be 0%.
[0291] The thickness of the package is not particularly limited, but is preferably 20 μm or more, more preferably 50 μm or more, and further preferably 100 μm or more. The upper limit is not particularly limited, but is preferably 1000 μm or less, and more preferably 500 μm or less.
[0292] The material constituting the package body is not particularly limited, and examples thereof include resins, and more specifically, polyolefin resins, polyethylene resins, and polypropylene resins.
[0293] The resins may be used alone or in combination of two or more.
[0294] The color of the package is not particularly limited, and examples thereof include transparent, brown, and black. Among them, brown or black is preferred, and black is more preferred, from the viewpoint of achieving a more excellent effect of the present invention.
[0295] In addition, when adjusting the color tone of the package, the package may contain a colorant.
[0296] The package preferably contains carbon black. From the viewpoint of achieving more excellent effects of the present invention, the content of carbon black is preferably 1.0% by mass or more, more preferably 3.0% by mass or more, and even more preferably 5.0% by mass or more relative to the total mass of the package.
[0297] The carbon black is not particularly limited, and examples thereof include gas black, furnace black, channel black, anthracene black, acetylene black, Ketjen black, thermal black, lamp black, lampblack, pine smoke, bone black, and vegetable black.
[0298] The carbon black may be used alone or in combination of two or more.
[0299] <Other parts>
[0300] The first sheet may have other members in addition to the above-mentioned first support and first layer.
[0301] For example, the first sheet may include an easily adhesive layer between the first support and the first layer for improving the adhesion between the two.
[0302] The thickness of the easy-adhesion layer is not particularly limited, but is preferably 0.005 to 2 μm, and more preferably 0.01 to 1 μm.
[0303] <<Second Sheet>>
[0304] Figure 1 The second sheet 22 described in has a second support 18 and a second layer 20 disposed on the second support 18 and containing a color developer.
[0305] Hereinafter, each component will be described in detail.
[0306] <Second Support>
[0307] The second support is a member for supporting the second layer. In addition, when the second layer itself can be handled, the second sheet may not have the second support.
[0308] The configuration of the second support is the same as that of the first support described above, and therefore description thereof will be omitted.
[0309] <Level 2>
[0310] (Developer)
[0311] The second layer is a layer containing a color developer.
[0312] The color developer is a compound that has no color-developing function itself but has the property of causing the color-developing agent to develop color when in contact with the color-developing agent. The color developer is preferably an electron-accepting compound.
[0313] As the developer, inorganic compounds and organic compounds can be cited, preferably the inorganic compounds and organic compounds described in paragraphs 0055 to 0056 of International Publication No. 2009 / 008248. From the viewpoint of better color concentration and image quality after color development, the inorganic compound is preferably an inorganic particle (for example, acidic clay, activated clay), and the organic compound is preferably a metal salt of an aromatic carboxylic acid. The developer can be appropriately selected by the pressure band or coating method to be measured. In particular, in a pressure band of 500 MPa or less, from the viewpoint of better color concentration and image quality after color development, acidic clay or activated clay is preferred.
[0314] The content of the color developer in the second layer is not particularly limited, but is preferably 20 to 95% by mass, more preferably 30 to 90% by mass, based on the total mass of the second layer from the viewpoint of achieving more excellent effects of the present invention.
[0315] The color developer may be used alone or in combination of two or more.
[0316] The content of the color developer in the second layer is not particularly limited, but is preferably 0.1 to 30 g / m 2 When the developer is an inorganic compound, the content of the developer is preferably 3 to 20 g / m 2 , more preferably 5 to 15 g / m 2 When the developer is an organic compound, the content of the developer is preferably 0.1 to 5 g / m 2 , more preferably 0.2 to 3 g / m 2 .
[0317] (pH adjuster)
[0318] The second layer preferably contains a pH adjuster. If the second layer contains a pH adjuster, the color developer becomes easy to be evenly arranged without aggregation, so the image quality after color development becomes better. When the color developer is acidic, the pH adjuster is preferably an alkaline pH adjuster.
[0319] The alkaline pH adjuster refers to a compound that exhibits alkalinity to such an extent that the pH can be adjusted.
[0320] The pH adjuster may be an organic base or an inorganic base, and among these, an inorganic base is preferred from the viewpoint of achieving a more excellent effect of the present invention.
[0321] The alkaline pH adjuster is not particularly limited, and examples thereof include sodium hydroxide, potassium hydroxide, lithium hydroxide, sodium carbonate, potassium carbonate, ammonium carbonate, and combinations thereof.
[0322] The pH adjuster may be used alone or in combination of two or more.
[0323] The content of the pH adjuster contained in the second layer is preferably 0.1 to 5.0% by mass, more preferably 0.5 to 2.0% by mass, based on the total mass of the developer.
[0324] (Other ingredients)
[0325] The second layer may contain other components in addition to the above-mentioned developer.
[0326] Examples of other components include polymer binders, pigments, fluorescent whitening agents, defoaming agents, penetrants, ultraviolet absorbers, surfactants, and preservatives.
[0327] Examples of polymer binders include synthetic polymers and natural polymers such as styrene-butadiene copolymers, polyvinyl acetate, polyacrylates, polyvinyl alcohol, polyacrylic acid, maleic anhydride-styrene copolymers, olefin resins, modified acrylate copolymers, starch, casein, gum arabic, gelatin, carboxymethyl cellulose or its salts, and methyl cellulose.
[0328] Examples of the pigment include heavy calcium carbonate, light calcium carbonate, talc, and titanium dioxide.
[0329] The thickness of the second layer is not particularly limited, but is preferably 1 to 50 μm, more preferably 2 to 30 μm, from the viewpoint of achieving more excellent effects of the present invention.
[0330] And, the mass per unit area of the second layer (g / m 2 ) is not particularly limited, but from the viewpoint of more excellent effects of the present invention, it is preferably 0.5 to 30 g / m 2 .
[0331] <Method for Forming the Second Layer>
[0332] The method for forming the second layer is not particularly limited.
[0333] For example, there can be mentioned a method in which a second layer-forming composition containing a color developer is applied onto the second support and the obtained coating film is dried as necessary.
[0334] The second layer forming composition may be a dispersion obtained by dispersing the developer in water or the like. When the developer is an inorganic compound, the developer dispersion may be prepared by mechanically dispersing the inorganic compound in water. When the developer is an organic compound, the developer dispersion may be prepared by mechanically dispersing the organic compound in water or dissolving it in an organic solvent.
[0335] The second layer forming composition may contain other components that can be contained in the above-mentioned second layer.
[0336] The method of applying the second layer forming composition is not particularly limited, and examples thereof include a method using a coater used when applying the above-mentioned first layer forming composition.
[0337] After the second layer-forming composition is applied onto the second support, the coating film may be dried as necessary. Examples of the drying treatment include heating treatment.
[0338] In addition, although the method of forming the second layer on the second support is described above, it is not limited to the above method. For example, the second layer may be formed on a temporary support and then the temporary support may be peeled off to form a second sheet composed of the second layer.
[0339] The temporary support is not particularly limited as long as it is a releasable support.
[0340] From the viewpoint of excellent color density and image quality, the pH value of the extract obtained by immersing the second sheet having a size of 10 cm in length and 10 cm in width in 50 mL of water at 25° C. for 10 minutes is preferably in the range of 6.0 to 9.0 at 25° C. When the pH range is 9.0 or less, when the coloring agent selected from the compound represented by the general formula (1) and the compound having an indole structure moves from the first layer to the second layer to develop color, the coloring reaction of the coloring agent proceeds smoothly, and thus the color density becomes better.
[0341] In measuring the pH value of the extract of the second sheet, the second sheet cut into 10 cm in length by 10 cm in width was immersed in 50 mL of water at 25°C for 10 minutes, and then the pH value of the extract obtained by filtration was measured at 25°C using a pH meter (COMPACT pH METER B-212 manufactured by HORIBA).
[0342] Examples of methods for adjusting the pH include a method of selecting a color developer having an appropriate acid value, a method of changing the type and amount of the pH adjuster, and a combination thereof.
[0343] <Packaging>
[0344] The second sheet may be contained in the package.
[0345] Examples of the package include a package used when the above-mentioned first sheet is contained therein.
[0346] <Other parts>
[0347] The second sheet may have other members in addition to the above-mentioned second support and second layer.
[0348] For example, the second sheet may include an easily adhesive layer between the second support and the second layer for improving the adhesion between the two.
[0349] The aspect of the easy-adhesion layer may be the aspect of the easy-adhesion layer which the above-mentioned 1st sheet|seat may have.
[0350] As described above, the first sheet and the second sheet are stacked in a manner such that the first layer of the first sheet and the second layer of the second sheet are opposed to each other to obtain a laminate, and the laminate is pressurized for use. That is, the first sheet is equivalent to a sheet for measuring pressure together with the second sheet.
[0351] When the laminate is subjected to pressure to develop color, the L of the color developing portion * a * b * The chromaticity in the color system is not particularly limited, but is preferably chromaticity a from the viewpoint of easy visual recognition of the color. * More than 30 and less than 80, preferably chromaticity b * It is greater than -50 and not more than 50. When a coloring agent selected from the compound represented by the general formula (1) and a compound having an indole structure is used, it is easy to fall within the above range.
[0352] In addition, when measuring the above-mentioned chromaticity, after the first sheet and the second sheet of the laminated body after applying pressure are peeled off, the chromaticity of the color-developing part of the second sheet is measured using a densitometer RD-19 (GretagMacbeth). In the case where the second sheet includes a transparent second support, the chromaticity of the above-mentioned color-developing part is measured from the second support side.
[0353] [Second embodiment]
[0354] Figure 3 This is a cross-sectional view of one embodiment of a pressure measurement sheet.
[0355] The pressure measurement sheet 30 includes a support 32 , a second layer 20 containing a color developer, and a first layer 14 containing predetermined microcapsules 13 in this order.
[0356] When the pressure measurement sheet 30 is used, by applying pressure from at least one of the support body 32 side and the first layer 14 side, the microcapsules 13 are ruptured in the pressurized area, and the coloring agent contained in the microcapsules 13 flows out of the microcapsules 13, thereby reacting with the coloring agent in the second layer 20. As a result, coloring occurs in the pressurized area.
[0357] As will be described later, the pressure measurement sheet 30 only needs to include the first layer 14 and the second layer 20 , and may not include the support 32 .
[0358] In addition, Figure 3In the embodiment, the support 32 and the second layer 20 are directly stacked, but the present invention is not limited to this embodiment, and as described later, another layer (for example, an easy-adhesion layer) may be disposed between the support 32 and the second layer 20.
[0359] And, in Figure 3 2 discloses a pressure measuring sheet 30 including a support 32, a second layer 20, and a first layer 14 in this order, but the invention is not limited to this embodiment, and a pressure measuring sheet may also include a support 32, a first layer 14, and a second layer 20 in this order.
[0360] The first layer 14 and the second layer 20 in the pressure measurement sheet 30 are the same as the first layer 14 and the second layer 20 described in the first embodiment, and thus description thereof is omitted.
[0361] Hereinafter, the support body 32 will be mainly described in detail.
[0362] <Support>
[0363] The support is a member for supporting the first layer and the second layer. In addition, when the laminate of the first layer and the second layer can be processed by itself, the pressure measurement sheet may not have a support.
[0364] A preferred embodiment of the support body is the same as the preferred embodiment of the first support body described above, and therefore the description thereof is omitted.
[0365] <Method for Manufacturing Pressure Measurement Sheet>
[0366] The method for producing the pressure measurement sheet is not particularly limited, and a known method may be used.
[0367] For example, the following method can be mentioned: after the second layer is formed on the support, a composition for forming the second layer containing a developer is applied to the support and dried as needed, and then a composition for forming the first layer containing predetermined microcapsules is applied to the second layer and dried as needed to form the first layer. In addition, the method for forming the microcapsules is as described above.
[0368] The method for forming the first layer using the first layer forming composition is as described in the first embodiment. Furthermore, the method for forming the second layer using the second layer forming composition is also as described in the first embodiment.
[0369] <Packaging>
[0370] The pressure measurement sheet may be contained in a package.
[0371] As the package body, there can be mentioned the package body used when the first sheet material described in the above-mentioned first embodiment is contained.
[0372] <Other parts>
[0373] The pressure measurement sheet may include other members in addition to the support body, the second layer, and the first layer.
[0374] For example, the pressure measurement sheet may include an easy-adhesion layer between the support and the second layer for improving the adhesion between the two.
[0375] The aspect of the easy-adhesion layer may be the aspect of the easy-adhesion layer which the above-mentioned 1st sheet|seat may have.
[0376] There is no particular limitation on the uses of the pressure measuring sheet set and pressure measuring sheet of the present invention, and examples thereof include pressure measurement during the manufacture of electronic parts (pressure measurement during the bonding process of liquid crystal panels, confirmation of pressure distribution during the solder printing process of printed circuit boards, confirmation of pressure distribution during the crimping process of integrated circuits or wiring, etc.), and pressure measurement during the manufacture of automobiles (pressure measurement of the surface of the cylinder gasket of the engine, pressure measurement of the flange surfaces of various sealing parts, and confirmation of the ground contact and ground contact pressure of tires).
[0377] [Third embodiment]
[0378] As a third embodiment of the present invention, there is mentioned a dispersion (hereinafter also referred to as "first dispersion") (dispersion for forming a pressure measurement layer) which is used to form a layer used in combination with a layer containing a color developer for pressure measurement and contains microcapsules containing a color developer.
[0379] In the first dispersion, the coloring agent is selected from the group consisting of the compound represented by the above general formula (1) and a compound having an indole structure.
[0380] The microcapsules further contain a compound having a benzotriazole structure and an aromatic solvent, wherein the aromatic solvent includes a compound having at least one aromatic ring and no aromatic condensed ring.
[0381] The details of the components contained in the first dispersion are as described above.
[0382] Examples of the first dispersion include the above-mentioned first layer-forming composition.
[0383] The first dispersion generally contains a solvent. The type of the solvent contained in the first dispersion is not particularly limited, and examples thereof include water and organic solvents.
[0384] The first dispersion is used to form a layer for pressure measurement (corresponding to the first layer described above) similarly to the first layer-forming composition.
[0385] The first dispersion liquid may be used in combination with a dispersion liquid used to form a layer containing a color developer (hereinafter, also referred to as a "second dispersion liquid"). That is, the first dispersion liquid and the second dispersion liquid may be used as a set (dispersion liquid set).
[0386] The second dispersion liquid is a dispersion liquid containing a color developer.
[0387] Examples of the second dispersion include the above-mentioned second layer forming composition.
[0388] As an aspect of the color developer contained in the second dispersion, an aspect of the color developer contained in the second layer forming composition can be mentioned.
[0389] The second dispersion generally contains a solvent. The type of the solvent contained in the second dispersion is not particularly limited, and examples thereof include water and organic solvents.
[0390] In addition, the first dispersion preferably does not contain coarse particles because the first dispersion can be applied to a curved surface without irregularities and does not cause clogging in a spray or other application method.
[0391] Furthermore, for the same reason as above, the volume-based median diameter (D50) of the microcapsule is preferably 1 to 50 μm.
[0392] Furthermore, for the same reason as described above, it is preferred that the second dispersion does not contain coarse particles.
[0393] Furthermore, for the same reasons as above, the color developer contained in the second dispersion is preferably an organic compound. The organic compound is preferably a metal salt of an aromatic carboxylic acid, more preferably a metal salicylate, and still more preferably a zinc salicylate.
[0394] The first dispersion can also be applied to an object that is difficult to measure pressure in a sheet such as a pressure measurement sheet set or a pressure measurement sheet. More specifically, a required amount of the first dispersion is applied to an area where pressure measurement of the pressure measurement object is required, and a layer containing the microcapsules is formed in the area, without being affected by the surface shape of the pressure measurement object, thereby enabling pressure measurement. In particular, it can be preferably applied to a case where pressure on a curved surface is measured. More specifically, the first dispersion is applied to a curved surface portion to form a layer containing microcapsules, thereby enabling pressure measurement.
[0395] In addition, as described above, the layer formed of the first dispersion is used in combination with the layer containing the developer for pressure measurement. Therefore, as in the case of using the first dispersion, a required amount of the second dispersion is applied to a region where pressure measurement of the pressure measurement object is required, and the layer containing the developer is disposed adjacent to the layer containing the microcapsules, thereby enabling pressure measurement.
[0396] In addition, the layer containing microcapsules and the layer containing the developer are usually stacked and arranged in the area where the pressure measurement object needs to be measured, but either layer may be arranged on the side of the pressure measurement object. In other words, either the first dispersion or the second dispersion may be applied first in the area where the pressure measurement object needs to be measured.
[0397] As described above, by applying pressure from the other side to the surface coated with the first dispersion and the second dispersion, the microcapsules are ruptured in the pressurized area, and the coloring agent contained in the microcapsules flows out of the microcapsules, contacts the coloring agent, and reacts with the coloring agent to develop color. As a result, color is developed in the pressurized area.
[0398] The method of applying the first dispersion liquid and the second dispersion liquid is not particularly limited, and examples thereof include roll coating, spray coating, brush coating, and dip coating.
[0399] The first dispersion liquid and the second dispersion liquid may be applied directly to the measurement surface of the measurement object, or may be applied via a film, paper, or the like.
[0400] The application amount of the first dispersion and the second dispersion can be set according to the measurement purpose, but from the viewpoint of obtaining good color development and color development distribution, for example, it is preferably 2 to 40 g / m2 in terms of solid content. 2 .
[0401] [Fourth embodiment]
[0402] As a fourth embodiment of the present invention, there is mentioned a dispersion liquid (hereinafter also referred to as "third dispersion liquid") containing microcapsules containing a color former and a color developer (a dispersion liquid for forming a pressure measurement layer), which is used to form a layer for pressure measurement.
[0403] In the third dispersion, the coloring agent is selected from the group consisting of the compound represented by the above general formula (1) and a compound having an indole structure.
[0404] The microcapsules further contain a compound having a benzotriazole structure and an aromatic solvent, wherein the aromatic solvent includes a compound having at least one aromatic ring and no aromatic condensed ring.
[0405] As an aspect of the microcapsules contained in the third dispersion, the aspect of the microcapsules contained in the first layer forming composition can be mentioned.
[0406] As an aspect of the color developer contained in the third dispersion, the aspect of the color developer contained in the second layer forming composition can be mentioned.
[0407] The third dispersion generally contains a solvent. The type of the solvent contained in the first dispersion is not particularly limited, and examples thereof include water and organic solvents.
[0408] The third dispersion may be a mixture of the above-mentioned first layer forming composition with a color developer, or a mixture of the above-mentioned second layer forming composition with the first layer forming composition.
[0409] In addition, the third dispersion preferably does not contain coarse particles because the coating can be applied to a curved surface without irregularities and clogging is not caused in a coating method such as spraying.
[0410] Furthermore, for the same reason as above, the volume-based median diameter (D50) of the microcapsule is preferably 1 to 50 μm.
[0411] Furthermore, for the same reasons as above, the color developer contained in the third dispersion is preferably an organic compound. The organic compound is preferably a metal salt of an aromatic carboxylic acid, more preferably a metal salicylate, and still more preferably a zinc salicylate.
[0412] Since the third dispersion liquid contains microcapsules containing a color former and a color developer, pressure measurement can be performed only with the layer formed by applying the third dispersion liquid.
[0413] That is, like the first dispersion and the second dispersion, the third dispersion can also be applied to an object whose pressure is difficult to measure in a sheet such as a pressure measurement sheet set or a pressure measurement sheet. More specifically, the pressure can be measured by applying a required amount of the third dispersion to an area where pressure measurement of the pressure measurement object is required, without being affected by the surface shape of the pressure measurement object, and forming a layer in the area.
[0414] Examples of the coating method and coating conditions of the third dispersion include the coating method and coating conditions of the above-mentioned first dispersion and second dispersion.
[0415] The first dispersion liquid, the second dispersion liquid, and the third dispersion liquid described above can be used for various purposes.
[0416] For example, the following can be mentioned: confirmation of pressure distribution in the forming process of various components, main bodies, etc. or the assembly process of components in the manufacture of vehicles such as automobiles or aircraft, confirmation of pressure distribution in the assembly process of building materials, confirmation of pressure distribution in processes such as curved surface processing of electronic products, confirmation of impact force applied to goods accompanying transportation, confirmation of each mold in the manufacture of metal products, confirmation of each mold during the molding process of resin products, confirmation of pressure distribution in the tableting of pharmaceutical tablets, confirmation of pressure distribution on the surface of furniture such as sofa seats, confirmation of grip force applied to stationery, etc., confirmation of pressure on stationery, confirmation of impact force applied to sports equipment such as balls made of elastic materials, and confirmation of the gap (clearance) between upper and lower teeth in dental products.
[0417] Example
[0418] Below, the present invention is further described in detail based on examples. The materials, usage, ratios, processing contents and processing sequences shown in the following examples, as long as they do not depart from the gist of the present invention, can be appropriately changed. Therefore, the scope of the present invention should not be interpreted in a limited manner by the examples shown below. In addition, as long as there is no special explanation, the following "parts" and "%" are mass references.
[0419] [Example 1]
[0420] <Preparation of Microcapsules Containing Coloring Agent>
[0421] In 50 parts of 1,1-diphenylethane (manufactured by JXTG Energy Co., Ltd., SAS-296) were dissolved 3 parts of 3',6'-bis(diethylamino)-2-(4-nitrophenyl)spiro[isoindol-1,9'-xanthene]-3-one (manufactured by Hodogaya Chemical Co., Ltd., Pink-DCF) as a coloring agent, 4 parts of 6'-(diethylamino)-1',3'-dimethylfluoran (manufactured by Hodogaya Chemical Co., Ltd., Orange-DCF) and 3 parts of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole (JOHOKU CHEMICAL CO., LTD, JF-77-P) as an ultraviolet absorber to obtain a solution A.
[0422] Next, 13 parts of synthetic isoalkane (Idemitsu Kosan Co., Ltd., IP Solvent 1620) and 0.3 parts of N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine (ADEKA CORPORATION, ADEKA POLYETHER EDP-300) dissolved in 2.5 parts of methyl ethyl ketone were added to the stirred solution A to obtain solution B. Furthermore, 2.5 parts of trimethylolpropane adduct of toluene diisocyanate (DIC CORPORATION, BURNOCK D-750) dissolved in 6 parts of ethyl acetate were added to the stirred solution B to obtain solution C. Furthermore, the above solution C was added to a solution in which 7 parts of polyvinyl alcohol (PVA-217E, Kuraray Co., Ltd.) were dissolved in 140 parts of water to perform emulsification dispersion. 200 parts of water was added to the emulsified liquid after emulsification and dispersion, and the mixture was heated to 70°C while being stirred, stirred for 1 hour, and then cooled. Furthermore, water was added to adjust the concentration to obtain a microcapsule liquid containing a coloring agent having a solid content concentration of 20%.
[0423] The volume-based median diameter (D50) of the obtained color forming agent-containing microcapsules was 20 μm. The volume-based median diameter (D50) was measured by the above-mentioned method using an optical microscope.
[0424] <Pressure Measurement Sheet Set Production>
[0425] (Preparation of the first sheet)
[0426] 18 parts of the obtained microcapsule liquid containing a coloring agent, 10 parts of water, 1.8 parts of colloidal silica (Nissan Chemical Industries, LTD., SNOWTEX30, solid content 30%), 2 parts of a 1% aqueous solution of sodium carboxymethylcellulose (DKS Co. Ltd., SEROGEN 5A), 4.5 parts of a 1% aqueous solution of sodium carboxymethylcellulose (DKS Co. Ltd., SEROGEN EP), 1 part of a 15% aqueous solution of a side chain alkylbenzene sulfonic acid amine salt (DKS Co. Ltd., NEOGEN T), 0.2 parts of a 1% aqueous solution of polyoxyethylene polyoxypropylene lauryl ether (DKS Co. Ltd., NOIGEN LP-70) and 0.2 parts of a 1% aqueous solution of sodium-bis(3,3,4,4,5,5,6,6,6-nonafluorohexyl)-2-sulfonyloxysuccinate (FUJIFILM The mixture was mixed with 0.2 parts of a 1% aqueous solution of 1% AHE (W-AHE) to obtain a composition for forming the first layer.
[0427] The obtained first layer forming composition was applied on a polyethylene terephthalate (PET) sheet having a thickness of 75 μm by a bar coater so that the mass after drying would be 6.0 g / m 2 Next, the obtained coating film was heated to form a first layer, thereby producing a first sheet.
[0428] (Preparation of the Second Sheet)
[0429] 100 parts of activated clay (Shilton F-242, Mizusawa Industrial Chemicals, Ltd.), 0.5 parts of sodium hexametaphosphate (sodium hexametaphosphate, Nippon Chemical Industry Co., Ltd.), 15 parts of a 10% sodium hydroxide aqueous solution and 240 parts of water were added as a developer to obtain a dispersion containing a developer. The obtained dispersion was mixed with 30 parts of an olefin resin (ARAKAWA CHEMICAL INDUSTRIES, LTD., Polymaron 482, solid content concentration 25 mass%), 35 parts of a modified acrylate copolymer (Zeon Corporation, Nippon LX814, solid content concentration 46 mass%), 80 parts of a 1% aqueous solution of sodium carboxymethylcellulose (DKS Co. Ltd., SEROGEN EP), 18 parts of a 15% aqueous solution of sodium alkylbenzenesulfonate (DKS Co. Ltd., NEOGEN T), 20 parts of a 1% aqueous solution of polyoxyethylene polyoxypropylene lauryl ether (DKS Co. Ltd., NOIGEN LP-70), and sodium-bis(3,3,4,4,5,5,6,6,6-nonafluorohexyl)-2-sulfonyloxysuccinate (FUJIFILM A second layer-forming composition containing a color developer was prepared by adding 20 parts of a 1% aqueous solution of W-AHE (Corporation Corporation).
[0430] The second layer-forming composition containing a color developer was applied on a PET sheet having a thickness of 75 μm so that the solid content applied amount became 7.0 g / m 2 Next, the obtained coating film was dried to form a second layer, thereby obtaining a second sheet.
[0431] [Examples 2 to 18, Comparative Examples 1 to 3]
[0432] As shown in Table 1, the first sheet and the second sheet were produced in the same procedure as in Example 1 except that various conditions such as the materials and the contents of the materials were changed.
[0433] 〔Measurement and Evaluation〕
[0434] <Storage stability evaluation>
[0435] Evaluation of the pressure measurement sheet set was performed using the first sheet and the second sheet produced in each of the examples and comparative examples.
[0436] Specifically, the first sheet and the second sheet cut into a size of 5 cm in length and 5 cm in width were overlapped so that the surface of the first layer of the first sheet was in contact with the surface of the second layer of the second sheet, thereby obtaining a laminate. Next, the laminate was pressed at a pressure of 1.0 MPa by a pressurizing punch (DSF-C1-A, manufactured by AIDA ENGINEERING, LTD.) to cause it to develop color. Afterwards, the first sheet and the second sheet constituting the laminate were peeled off, and the concentration (DA) of the coloring portion formed on the second sheet was measured from the support (PET sheet) surface side using a densitometer RD-19 (manufactured by GretagMacbeth).
[0437] Furthermore, after the first sheet was added to the package shown in Table 1, it was treated at 70,000 Lux for 24 hours using a weather tester (Super Xenon Weather Meter SX75, manufactured by Suga Test Instruments Co., Ltd.) according to JEITA CP-3901 (Digital Color Photo Print Image Preservation Test Method), and then it was colored in the same manner as above, and the concentration (DB) of the colored portion was measured.
[0438] Furthermore, the rate of change in color density DC (DB / DA) was calculated and evaluated according to the following evaluation criteria.
[0439] "A": DC is 0.9 or more (almost no change in color is observed).
[0440] "B": DC is 0.6 or more and less than 0.9 (a slight change in color is observed).
[0441] "C": DC is 0.4 or more and less than 0.6 (change in color development is observed).
[0442] "D": DC is less than 0.4 (change in hair color is clearly observed).
[0443] <Color density evaluation>
[0444] In the same manner as described in <Storage Stability Evaluation>, the first sheet and the second sheet produced in each embodiment and comparative example were used to carry out the evaluation of the sheet group for pressure measurement, and the concentration (DA) of the color-developing portion formed on the second sheet was measured from the surface side of the support body (PET sheet).
[0445] In addition, the initial density (DB) of the unused second sheet was measured from the support (PET sheet) surface side using a densitometer RD-19 (manufactured by GretagMacbeth).
[0446] Then, the color development density ΔD was obtained by subtracting the initial density DB from the color development density DA, and the evaluation was performed according to the following evaluation criteria.
[0447] "A": ΔD is 0.7 or more (color development is clearly observed).
[0448] "B": ΔD is 0.4 or more and less than 0.7 (color development is observed).
[0449] "C": ΔD is 0.2 or more and less than 0.4 (color development is slightly observed).
[0450] "D": ΔD is less than 0.2 (color development is hardly observed).
[0451] <Color Measurement>
[0452] The pressure measurement sheet set was colored in the same manner as described in <Color density evaluation>, and then color was measured using a spectrophotometer (CM-3700A, manufactured by Konica Minolta, Inc.). * a * b * Chroma a in the color system * and chromaticity b * .
[0453] <Measurement of total light transmittance>
[0454] The total light transmittance of the packaging bodies shown in Table 1 was measured using a haze meter (HGM-2DP, manufactured by Suga Test Instruments Co., Ltd.) by a method in accordance with JIS-K-7361.
[0455] In addition, the diffuse transmittance, parallel light transmittance and haze of the packaging bodies used in Examples 1, 4, 6 to 9 and 12 to 18 were all 0.0%.
[0456] <Image quality evaluation>
[0457] A copper wire of 0.5 mm in diameter and 3 cm in length was sandwiched between the first sheet and the second sheet and pressed at 1.0 MPa to develop color in a linear form, and the length d of the widest line width was evaluated.
[0458] "A": d≤2mm
[0459] "B": 2mm<d≤3mm
[0460] "C": 3mm<d
[0461] In Table 1, the materials are as follows.
[0462] <Ultraviolet light absorber>
[0463] JF-77-P: 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, manufactured by JOHOKU CHEMICAL CO., LTD.
[0464] Tinuvin326: Bumetrizole, manufactured by BASF
[0465] Tinuvin PA 144: Phenol, 2-(5-chloro-2H-benzotriazol-2-yl)-6-(1,1-dimethylethyl)-4-methyl, manufactured by BASF
[0466] <Coloring Agent>
[0467] Orange-DCF: 6'-(diethylamino)-1',3'-dimethylfluoran, manufactured by Hodogaya Chemical Co., Ltd.
[0468] Pink-DCF: 3',6'-bis(diethylamino)-2-(4-nitrophenyl)spiro[isoindol-1,9'-xanthene]-3-one, manufactured by Hodogaya Chemical Co., Ltd.
[0469] Coloring agent A: 3,3-bis(2-methyl-1-octyl-3-indolyl)phthalide
[0470] <Solvent>
[0471] SAS-296: 1,1-Diphenylethane, manufactured by JXTG Energy
[0472] Olefin L: Linear alkylbenzene, manufactured by JXTG Energy
[0473] IP Solvent 1620: Synthetic isoalkane, manufactured by Idemitsu Kosan Co., Ltd.
[0474] Tricresyl phosphate: manufactured by DAIHACHI CHEMICAL INDUSTRY CO., LTD.
[0475] <Developer>
[0476] Active clay: Shilton F-242, manufactured by Mizusawa Industrial Chemicals, Ltd. In Table 1, in the column "Ratio [%]", the ratio (%) of the content of the ultraviolet absorber to the content of the coloring agent {(content of ultraviolet absorber / content of coloring agent) × 100}
[0477]
[0478] As shown in Table 1, when the pressure measurement sheet set of the present invention was used, it was confirmed that the desired effect was obtained.
[0479] From the comparison between Examples 1 and 2 and Example 3, it was confirmed that when the total light transmittance of the package body was less than 5.0%, a more excellent desired effect could be obtained.
[0480] From the comparison between Example 1 and Example 8, it was confirmed that when the content of the coloring agent was 0.10 to 1.20 g / m 2 In the case of , a better color concentration can be obtained.
[0481] From the comparison between Example 2 and Example 5, it was confirmed that when the content of the ultraviolet absorber was 10% by mass or more relative to the content of the coloring agent, a more excellent desired effect was obtained.
[0482] From the comparison between Examples 3 and 10 to 11, it was confirmed that when a compound having one or two aromatic rings and no aromatic condensed ring is used as the aromatic solvent, a more excellent effect is achieved.
[0483] Comparison between Examples 1 and 14 to 16 and Examples 17 to 18 confirmed that when the pH value of the extract obtained by immersing the second sheet (10 cm×10 cm) in 50 mL of water at 25°C for 10 minutes was 6.0 to 9.0 at 25°C, more excellent color density or image quality could be obtained.
[0484] In addition, the above shows a method of using a pressure measuring sheet group having a first sheet and a second sheet, but a pressure measuring sheet is made by stacking the second layer and the first layer in sequence on a supporting body, and the same test as above is carried out, and the same results as those in each embodiment are obtained.
[0485] Specifically, the second layer and the first layer produced in the above-mentioned Example 1 are arranged in sequence on a polyethylene terephthalate sheet to produce a pressure measurement sheet having a support body, a second layer and a first layer in sequence, and the results of the above-mentioned evaluations (storage stability evaluation, color concentration evaluation and image quality evaluation, etc.) are carried out, and the same results as in Example 1 are obtained.
[0486] [Example 19]
[0487] The dispersion group was spray-coated on a curved surface member, and storage stability evaluation and color development density evaluation were performed.
[0488] Specifically, the microcapsule liquid containing the color former prepared in the above Example 1 was prepared as the first dispersion liquid, and the dispersion liquid containing the color developer prepared in the above Example 1 was prepared as the second dispersion liquid.
[0489] <Storage stability evaluation and color development concentration evaluation>
[0490] The first dispersion was applied to a metal plate (concave mirror / convex mirror (R=100 mm) made of stainless steel (SUS304)) as a coated object by brushing, and after drying for 24 hours to form a first layer, the second dispersion was applied to the first layer by brushing to form a second layer. The same metal plate was placed on the coated surface so as to cover the coated area, and a press machine (product name: H1F35-1, manufactured by Komatsu Ltd.) was used to press for 120 seconds at a pressure of 10 MPa. After the pressurization was completed, the metal plate placed on the upper part was removed, and the color development and color distribution of the coated area were confirmed by visual observation, and it was confirmed that the color development was being carried out at a sufficient concentration that could be visually recognized and the color development distribution could be visually recognized with a sufficient color development concentration difference.
[0491] Furthermore, the first dispersion was applied to a metal plate (concave mirror / convex mirror (R=100 mm) made of stainless steel (SUS304)) as a coated object by brushing to form the first layer, and then added to the same black polyethylene bag as in Example 1, and treated at 70000 Lux for 24 hours by a weathering tester (Super Xenon Weather Meter SX75, manufactured by Suga Test Instruments Co., Ltd.) and according to JEITA CP-3901 (Digital Color Photo Print Image Preservation Test Method). Thereafter, the second dispersion was applied to the first layer by brushing to form the second layer. Next, in the same order as above, the coated area was colored by pressure treatment using a metal plate, and the color and color distribution of the coated area were confirmed by visual observation. As a result, almost no color change was observed compared to the case where no light irradiation was performed.
[0492] (Example 20)
[0493] The developer-containing dispersion prepared in Example 1 was changed to a 3,5-bis(α-methylbenzyl)salicylate zinc dispersion (LR-220 manufactured by SANKO CO., LTD., solid content concentration 41%) diluted with water to a solid content concentration of 20%, and the brush application was changed to spray application. The storage stability evaluation and the color development density evaluation were performed in the same manner as in Example 19. As a result, it was confirmed that the color was developed at a sufficient concentration to be visually recognized, the color development distribution was visually recognized at a sufficient color development density difference, and almost no change in color development was observed compared to the case where light irradiation was not performed.
[0494] 〕Example 21〕
[0495] As a result of color development density evaluation carried out in the same manner as in Example 20 except that the order of applying the first dispersion and the second dispersion was changed, it was confirmed that color was developed at a sufficient density to be visually recognized and that color development distribution was visually recognized with a sufficient color development density difference, as in Example 20.
[0496] [Example 22]
[0497] As a result of color development density evaluation in the same manner as in Example 20, except that the first dispersion and the second dispersion were preliminarily mixed to prepare the third dispersion and the third dispersion was used for coating at a predetermined position, it was confirmed that, similarly to Example 20, color development was achieved at a sufficient concentration to be visually recognized and that color development distribution was visually recognized with a sufficient color development density difference.
[0498] [Comparative Example 4]
[0499] The storage stability evaluation and color development concentration evaluation were performed in the same manner as in Example 19, except that the first dispersion liquid was the microcapsule liquid containing the coloring agent prepared in Comparative Example 1. As a result, it was confirmed that the color was developed at a sufficient concentration to be visually recognized and the color development distribution was visually recognized with a sufficient color development concentration difference, but the color development was insufficient in the case of light irradiation compared to the case of no light irradiation.
[0500] Explanation of symbols
[0501] 10-sheet group for pressure measurement, 12-1st support, 14-1st layer, 16-1st sheet, 18-2nd support, 20-2nd layer, 22-2nd sheet, 30-sheet for pressure measurement, 32-support, 20-2nd layer, 22-2nd sheet, 30-sheet for pressure measurement, 32-support.
Claims
1. A pressure measurement sheet set, comprising: A first sheet having a first layer, wherein the first layer comprises microcapsules containing a coloring agent; and a second sheet having a second layer containing a developer, The coloring agent comprises a compound selected from the group consisting of a compound represented by the general formula (1) and a compound having an indole structure, The microcapsule also contains a compound having a benzotriazole structure and an aromatic solvent. The content of the compound having a benzotriazole structure is 10% by mass or more and 100% by mass or less relative to the content of the coloring agent, The coloring agent may include a coloring agent other than the compound represented by the general formula (1) and the compound having an indole structure. The aromatic solvent includes a compound having one or two aromatic rings and no aromatic condensed ring, and the compound having one or two aromatic rings and no aromatic condensed ring is a compound represented by general formula (5), R 1 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, R 2 and R 4 Each independently represents an alkyl group having 1 to 5 carbon atoms or an aryl group having a monocyclic structure or a bicyclic structure, X 1 Indicates -O- or -NR 5 -, R 5 represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or an aryl group having a monocyclic structure or a bicyclic structure, In the general formula (5), R 20 ~R 24 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, L represents a single bond or an alkylene group having 1 to 5 carbon atoms, R 25 represents a hydrogen atom or a monocyclic aromatic group.
2. The pressure measurement sheet set according to claim 1, wherein: The pH value of the extract obtained by immersing the second sheet having a size of 10 cm in length and 10 cm in width in 50 mL of water at 25° C. for 10 minutes was in the range of 6.0 to 9.0 at 25° C.
3. The pressure measurement sheet set according to claim 1 or 2, wherein: The second layer further comprises a pH adjuster.
4. The pressure measurement sheet set according to claim 1 or 2, wherein: The molecular weight of the compound having a benzotriazole structure is 500 or less.
5. The pressure measurement sheet set according to claim 1 or 2, wherein: The content of the coloring agent is 0.10 g / m 2 ~1.20g / m 2 .
6. The pressure measurement sheet set according to claim 1 or 2, wherein: The first sheet and the second sheet are stacked so that the first layer of the first sheet and the second layer of the second sheet face each other to form a stacked body, and a pressure is applied to the stacked body to cause the color developing portion L to develop color. * a * b * Chroma a in the color system * More than 30 and less than 80, chromaticity b * Over -50 and below 50.
7. The pressure measurement sheet set according to claim 1 or 2, wherein: The first sheet material is contained in a packaging body.
8. The pressure measurement sheet set according to claim 7, wherein: The total light transmittance of the packaging body is less than 5.0%.
9. The pressure measurement sheet set according to claim 7, wherein: The packaging body has a thickness of 20 μm or more.
10. A pressure measuring sheet, comprising: The first layer comprises microcapsules containing a coloring agent; and The second layer comprises a developer, The coloring agent comprises a compound selected from the group consisting of a compound represented by the general formula (1) and a compound having an indole structure, The microcapsule also contains a compound having a benzotriazole structure and an aromatic solvent. The content of the compound having a benzotriazole structure is 10% by mass or more and 100% by mass or less relative to the content of the coloring agent, The coloring agent may include a coloring agent other than the compound represented by the general formula (1) and the compound having an indole structure. The aromatic solvent includes a compound having one or two aromatic rings and no aromatic condensed ring, and the compound having one or two aromatic rings and no aromatic condensed ring is a compound represented by general formula (5), R 1 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, R 2 and R 4 Each independently represents an alkyl group having 1 to 5 carbon atoms or an aryl group having a monocyclic structure or a bicyclic structure, X 1 Indicates -O- or -NR 5 -, R 5 represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or an aryl group having a monocyclic structure or a bicyclic structure, In the general formula (5), R 20 ~R 24 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, L represents a single bond or an alkylene group having 1 to 5 carbon atoms, R 25 represents a hydrogen atom or a monocyclic aromatic group.
11. A method for manufacturing a pressure-measuring sheet set, which is the method for manufacturing a pressure-measuring sheet set according to any one of claims 1 to 9, comprising: A step of forming the microcapsules using the coloring agent, the compound having a benzotriazole structure, the aromatic solvent and a capsule wall material; and A step of applying a first layer-forming composition containing the microcapsules to form a first layer.
12. A method for manufacturing a pressure measuring sheet, which is the method for manufacturing a pressure measuring sheet according to claim 10, comprising: A step of forming the microcapsules using the coloring agent, the compound having a benzotriazole structure, the aromatic solvent and a capsule wall material; and A step of applying a first layer-forming composition containing the microcapsules to form a first layer.
13. A sheet material having a layer comprising microcapsules containing a coloring agent, The coloring agent comprises a compound selected from the group consisting of a compound represented by the general formula (1) and a compound having an indole structure, The microcapsule also contains a compound having a benzotriazole structure and an aromatic solvent. The content of the compound having a benzotriazole structure is 10% by mass or more and 100% by mass or less relative to the content of the coloring agent, The coloring agent may include a coloring agent other than the compound represented by the general formula (1) and the compound having an indole structure. The aromatic solvent includes a compound having one or two aromatic rings and no aromatic condensed ring, and the compound having one or two aromatic rings and no aromatic condensed ring is a compound represented by general formula (5), R 1 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, R 2 and R 4 Each independently represents an alkyl group having 1 to 5 carbon atoms or an aryl group having a monocyclic structure or a bicyclic structure, X 1 Indicates -O- or -NR 5 -, R 5 represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or an aryl group having a monocyclic structure or a bicyclic structure, In the general formula (5), R 20 ~R 24 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, L represents a single bond or an alkylene group having 1 to 5 carbon atoms, R 25 represents a hydrogen atom or a monocyclic aromatic group.
14. A dispersion liquid for forming a layer used in combination with a layer containing a color developer for pressure measurement and comprising microcapsules containing a color developer, The coloring agent comprises a compound selected from the group consisting of a compound represented by the general formula (1) and a compound having an indole structure, The microcapsule also contains a compound having a benzotriazole structure and an aromatic solvent. The content of the compound having a benzotriazole structure is 10% by mass or more and 100% by mass or less relative to the content of the coloring agent, The coloring agent may include a coloring agent other than the compound represented by the general formula (1) and the compound having an indole structure. The aromatic solvent includes a compound having one or two aromatic rings and no aromatic condensed ring, and the compound having one or two aromatic rings and no aromatic condensed ring is a compound represented by general formula (5), R 1 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, R 2 and R 4 Each independently represents an alkyl group having 1 to 5 carbon atoms or an aryl group having a monocyclic structure or a bicyclic structure, X 1 Indicates -O- or -NR 5 -, R 5 represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or an aryl group having a monocyclic structure or a bicyclic structure, In the general formula (5), R 20 ~R 24 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, L represents a single bond or an alkylene group having 1 to 5 carbon atoms, R 25 represents a hydrogen atom or a monocyclic aromatic group.
15. The dispersion according to claim 14, wherein The molecular weight of the compound having a benzotriazole structure is 500 or less.
16. A dispersion set comprising: The dispersion according to claim 14 or 15; and A dispersion liquid containing a developer used to form a layer containing a developer.
17. A dispersion liquid for forming a layer for pressure measurement, comprising microcapsules containing a color former and a color developer, The coloring agent comprises a compound selected from the group consisting of a compound represented by the general formula (1) and a compound having an indole structure, The microcapsule also contains a compound having a benzotriazole structure and an aromatic solvent. The content of the compound having a benzotriazole structure is 10% by mass or more and 100% by mass or less relative to the content of the coloring agent, The coloring agent may include a coloring agent other than the compound represented by the general formula (1) and the compound having an indole structure. The aromatic solvent includes a compound having one or two aromatic rings and no aromatic condensed ring, and the compound having one or two aromatic rings and no aromatic condensed ring is a compound represented by general formula (5), R 1 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, R 2 and R 4 Each independently represents an alkyl group having 1 to 5 carbon atoms or an aryl group having a monocyclic structure or a bicyclic structure, X 1 Indicates -O- or -NR 5 -, R 5 represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or an aryl group having a monocyclic structure or a bicyclic structure, In the general formula (5), R 20 ~R 24 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, L represents a single bond or an alkylene group having 1 to 5 carbon atoms, R 25 represents a hydrogen atom or a monocyclic aromatic group.
18. The dispersion according to claim 17, wherein The molecular weight of the compound having a benzotriazole structure is 500 or less.
19. A microcapsule containing a coloring agent, The coloring agent comprises a compound selected from the group consisting of a compound represented by the general formula (1) and a compound having an indole structure, The microcapsule also contains a compound having a benzotriazole structure and an aromatic solvent. The content of the compound having a benzotriazole structure is 10% by mass or more and 100% by mass or less relative to the content of the coloring agent, The coloring agent may include a coloring agent other than the compound represented by the general formula (1) and the compound having an indole structure. The aromatic solvent includes a compound having one or two aromatic rings and no aromatic condensed ring, and the compound having one or two aromatic rings and no aromatic condensed ring is a compound represented by general formula (5), R 1 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, R 2 and R 4 Each independently represents an alkyl group having 1 to 5 carbon atoms or an aryl group having a monocyclic structure or a bicyclic structure, X 1 Indicates -O- or -NR 5 -, R 5 represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or an aryl group having a monocyclic structure or a bicyclic structure, In the general formula (5), R 20 ~R 24 Each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, L represents a single bond or an alkylene group having 1 to 5 carbon atoms, R 25 represents a hydrogen atom or a monocyclic aromatic group.