A testing device and method for friction and wear performance between high-performance fiber bundle and heddle eye
By designing a testing device that includes a heddle eye clamp, a spring end clamp, and a fiber end clamp, and combining it with the UMT-Tribolab friction and wear testing machine, the friction and wear performance test between the fiber bundle and the heddle eye under periodic alternating tension conditions was realized. This solves the problem that the existing technology can only test under constant tension conditions and provides more accurate test results.
Patent Information
- Application Number
- CN202210708565.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-22
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-06-22
AI Technical Summary
Existing fiber bundle-healing eye friction and wear testing devices can only be used under constant tension conditions, which cannot simulate the periodic alternating tension friction between the fiber bundle and the healing eye during actual weaving, resulting in inaccurate test results.
Design a high-performance test device for the tribological wear performance between fiber bundles and heddle eyes, including heddle eye clamps, spring end clamps, fiber end clamps, and microscope clamps. In conjunction with the UMT-Tribolab tribological testing machine, tribological wear tests are conducted by setting periodic alternating tension conditions. The test parameters include preload force, loading force, friction frequency, and friction time.
It enables accurate testing of the friction and wear performance between fiber bundles and heddle holes under periodic alternating tension. The device is simple and efficient, and the test results are stable and reliable. The experimental conditions can be adjusted according to the needs of different weaving processes.
Smart Images

Figure CN115096734B_ABST
Abstract
Description
Technical Field
[0001] The invention patent relates to fiber bundle friction and wear testing, and specifically to a testing device and method for the friction and wear performance between a high-performance fiber bundle and a heddle eye. Background Art
[0002] The rapid development of my country's defense, aerospace and other fields has made fiber-reinforced composite materials an important direction for the development of new materials in the future. Woven fabrics have become a widely used reinforcement material due to their simple structure and good stability in the warp and weft directions. However, during the weaving opening movement, the warp yarn will repeatedly rub against the heddle eye under the action of alternating tension. This friction phenomenon often causes severe wear of the fiber bundles, accompanied by the generation of hairiness, resulting in unclear openings, which not only affects production efficiency, but may also reduce the performance of the fabric preform and even the final composite product. Therefore, the study of the friction and wear law between the fiber bundle and the heddle eye during the opening movement has important scientific significance and engineering practical value.
[0003] The Chinese patent "An experimental method for simulating the friction between fiber bundles and reeds in weaving" (application number CN201910602534.4) discloses a device and test method for simulating the friction between fiber bundles and reeds in actual weaving. The invention method can realize the reciprocating friction between the fiber bundle and the reed teeth under constant tension conditions under suspended working conditions by using a friction and wear tester, and can measure the values of friction force and friction coefficient. In addition, the Chinese patent "A device for simulating damage to fiber bundles in the weaving process, its method and application" (application number CN202110007201.4) discloses a device and test method for simulating damage to fiber bundles in different weaving areas of the weaving process. The device contains a reciprocating friction test module between the fiber bundle and the heddle eye during the simulated opening process. The module can only realize the wear resistance test of the fiber bundle under constant tension conditions.
[0004] In summary, the existing testing technology can only realize the friction and wear experiment between the high-performance fiber bundle and the moving components of the loom under constant tension conditions. However, in the research of Bessette et al. (Bessette C, Decrette M, Tourlonias M, et al. In-situ measurement of tension and contact forces for weaving process monitoring: Application to 3D interlock [J]. Composites: Part A, Applied Science &, 126 (C): 105604-105604.), it has been confirmed that in the actual weaving process, the reciprocating friction between the high-performance fiber bundle and the heddle eye is carried out under the action of periodic alternating tension on the fiber bundle. Therefore, in order to more accurately test the friction and wear performance between the high-performance fiber bundle and the heddle eye under actual weaving conditions, the present invention proposes a testing device and a testing method for the friction and wear performance between the high-performance fiber bundle and the heddle eye under periodic alternating tension conditions, which can realize the test of the friction and wear performance of the fiber bundle by setting variables such as the contact force between the fiber bundle and the heddle eye, the fiber bundle tension, the reciprocating motion frequency, and the reciprocating friction motion distance. Summary of the invention
[0005] The present invention aims to solve the deficiencies of the prior art and to provide a testing device and method for the friction and wear performance between a high-performance fiber bundle and a heddle eye.
[0006] In order to achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a high-performance fiber bundle-heald eye friction and wear performance testing device is designed, and the heald eye clamp, the fiber end lower clamp, the spring end lower clamp and the microscope clamp cooperate to evaluate the fiber bundle friction and wear, wherein:
[0007] The heddle eye clamp comprises a fastening structure and a connecting structure. The fastening structure comprises a first heddle eye clamp fixing column and a second heddle eye clamp fixing column; the connecting structure comprises a channel connecting the heddle eye clamp and the heddle eye grinding head.
[0008] Particularly, the heddle eye clamp connection structure and the fastening structure are connected as one body.
[0009] The spring end lower clamp comprises a supporting structure, a fastening structure and a connecting structure. The supporting structure comprises a spring end lower clamp fixing base; the fastening structure is a spring end lower clamp limiting hole; the connecting structure comprises a spring end lower clamp spring limiting groove, a spring end lower clamp spring connecting rod and a spring end lower clamp spring.
[0010] Particularly, there are four limiting holes of the spring end lower clamp, which are located on the fixing base of the spring end lower clamp, and the positions of the limiting holes of the spring end lower clamp match the fixing platform of the friction and wear tester.
[0011] Particularly, the spring limiting groove of the spring end lower clamp is located on the center line of the spring end lower clamp fixed base, and the length and width of the limiting groove are used in conjunction with the specifications of the spring of the spring end lower clamp.
[0012] Particularly, one end of the spring of the spring end lower clamp is connected to the spring limiting groove of the spring end lower clamp through a spring connecting rod.
[0013] Particularly, the spring of the clamp under the spring end is a tension spring, and springs of different specifications can be used according to experimental requirements.
[0014] The fiber end lower clamp comprises a supporting structure, a fastening structure and a connecting structure. The supporting structure comprises a fiber end lower clamp fixing base; the fastening structure is a fiber end lower clamp limiting groove; the connecting structure comprises a fiber end lower clamp fixing screw channel and a fiber end lower clamp fixing screw.
[0015] Particularly, there are two limit grooves of the fiber end lower clamp, which are symmetrically distributed on the fixed base of the fiber end lower clamp, and the size of the limit grooves matches the linear reciprocating module of the friction and wear tester.
[0016] Particularly, the internal thread of the fixing screw channel of the clamp under the fiber end is engaged with the fixing thread.
[0017] In particular, the sample fiber bundle is fixed in a fixing screw channel of the clamp below the fiber end.
[0018] The microscope fixture comprises a supporting structure and a fastening structure. The supporting structure comprises a microscope bracket; and the fastening structure is a microscope fixture limiting groove.
[0019] Particularly, the microscope fixture has two limiting grooves which are symmetrically distributed on the microscope bracket and are connected to the fixed platform of the friction and wear testing machine via fixing screws.
[0020] Particularly, the digital microscope is fixed on a microscope stand, perpendicular to the sample fiber bundle.
[0021] The present invention also provides a method for using the above-mentioned testing device, characterized in that the method comprises the following steps:
[0022] S1. The heddle eye grinding head is glued to the heddle eye clamp connection structure and fixed to the heddle eye clamp, and the heddle eye grinding head is checked to see whether it is tightly connected to the heddle eye clamp.
[0023] In particular, the heald eye grinding heads of different materials and specifications can be replaced according to experimental needs.
[0024] S2. Insert the first and second fixing columns of the heddle eye fixture into the sensor of the UMT-Tribolab friction and wear testing machine, and fix them with the fixing screws on the sensor.
[0025] The UMT-Tribolab friction and wear testing machine sensor has a loading force parameter range of 0.23-20N.
[0026] S3. Fix the spring end lower clamp and the fiber end lower clamp fastening structure with screws and screw holes on the reciprocating linear module of the friction and wear testing machine.
[0027] S4. Connect the two ends of the sample fiber bundle to the spring end lower clamp and the fiber end lower clamp respectively. Pass one end of the sample fiber bundle through the spring and fix the sample fiber bundle with a heat shrink tube. Pass the other end of the sample fiber bundle through the fiber end lower clamp to fix the fiber bundle channel, hang the weight, adjust the tension, suspend for 1 minute, and tighten the fiber bundle with the fixing screw.
[0028] The outer layer of the heat shrink tube is made of radiation cross-linked polyethylene, and the inner layer is hot melt adhesive. A hot air gun is used to shrink it quickly to fix the sample fiber bundle.
[0029] S5. Set test parameter values.
[0030] The test parameter values include preload force, load force, friction frequency, friction time, and friction stroke.
[0031] S6. Start the program to conduct the test. After the test, derive the relationship curve between the friction force, friction coefficient, loading force, horizontal stroke, test chamber temperature and time in the loading stage.
[0032] S7. Photograph the sample fiber bundle after friction. Use a digital microscope to observe the surface hairiness of the sample fiber bundle after friction.
[0033] The present invention can achieve the following beneficial effects: the testing device provided by the present invention can test the friction and wear between the high-performance fiber bundle and the heddle eye under periodic alternating tension conditions on the basis of the original friction and wear testing method, the device is simple and efficient, and the test results are stable and reliable. The testing method provided by the present invention can change the experimental conditions such as heddle specifications, horizontal stroke, loading force, friction times, etc. according to different requirements of the weaving process for testing, providing a basis for subsequent related research.
[0034] The embodiments of the present invention use carbon fiber bundle samples as test objects, and conduct experimental tests on the effects of normal load, fiber bundle pre-tension, and friction frequency on the friction between the fiber bundle and the heddle eye. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1A schematic diagram of the use of a fixture for testing the friction and wear performance between a high-performance fiber bundle and a heddle eye according to the present invention;
[0036] Figure 2 A schematic diagram of a heddle eye fixture for testing a high-performance fiber bundle-heddle eye friction and wear performance test device and a test method of the present invention;
[0037] Figure 3 The experimental curve of time versus fiber bundle friction coefficient COF as described in Example 1 of a testing device and testing method for friction and wear performance between a high-performance fiber bundle and a heddle eye of the present invention;
[0038] Figure 4 The present invention is a high-performance fiber bundle-heddle eye friction and wear performance testing device and testing method embodiment 1 of the ... f The experimental curve of
[0039] Figure 5 This is a surface morphology diagram of the fiber bundle after the friction test described in Example 1 of a testing device and testing method for friction and wear performance between a high-performance fiber bundle and a heddle eye of the present invention;
[0040] Numbers shown in the accompanying drawings: 1-heald eye fixture fixing column 1; 2-heald eye fixture fixing column 2; 3-heald eye grinding head; 4-spring connecting rod; 5-spring; 6-spring limiting groove; 7-spring end lower fixture fixing base; 8-spring end lower fixture limiting hole; 9-fiber end lower fixture fixing base; 10-fixing screw; 11-fiber end lower fixture limiting groove; 12-heat shrink tube; 13-fiber bundle channel; 14-sample fiber bundle; 15-microscope bracket; 16-microscope bracket limiting groove; 17-digital microscope; DETAILED DESCRIPTION
[0041] The technical solution of the present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0042] The technical solution of the present invention to solve the technical problem is to invent a test method for the friction and wear performance between a high-performance fiber bundle and a heddle eye, and the test method adopts the following steps:
[0043] S1: The heddle eye grinding head is glued to the heddle eye clamp connection structure and fixed to the heddle eye clamp, and whether the heddle eye grinding head is tightly connected to the heddle eye clamp is detected.
[0044] In particular, the heald eye grinding heads of different materials and specifications can be replaced according to experimental needs.
[0045] S2. Insert the first and second fixing columns of the heddle eye fixture into the sensor of the UMT-Tribolab friction and wear testing machine, and fix them with the fixing screws on the sensor.
[0046] The UMT-Tribolab friction and wear testing machine sensor has a loading force parameter range of 0.23-20N.
[0047] S3. Fix the spring end lower clamp and the fiber end lower clamp fastening structure with screws and screw holes on the reciprocating linear module of the friction and wear testing machine.
[0048] S4. Connect the two ends of the sample fiber bundle to the spring end lower clamp and the fiber end lower clamp respectively. Pass one end of the sample fiber bundle through the spring and fix the sample fiber bundle with a heat shrink tube. Pass the other end of the sample fiber bundle through the fiber end lower clamp to fix the fiber bundle channel, hang the weight, adjust the tension, suspend for 1 minute, and tighten the fiber bundle with the fixing screw.
[0049] The outer layer of the heat shrink tube is made of radiation cross-linked polyethylene, and the inner layer is hot melt adhesive. A hot air gun is used to shrink it quickly to fix the sample fiber bundle.
[0050] S5. Set test parameter values.
[0051] The test parameter values include preload force, load force, friction frequency, friction time, and friction stroke.
[0052] S6. Start the program to conduct the test. After the test, derive the relationship curve between the friction force, friction coefficient, loading force, horizontal stroke, test chamber temperature and time in the loading stage.
[0053] S7. Photograph the sample fiber bundle after friction. Use a digital microscope to observe the surface hairiness of the sample fiber bundle after friction.
[0054] Example 1
[0055] This embodiment designs a test of the friction and wear performance between the carbon fiber bundle and the heddle eye under different loading forces, and includes the following steps when used:
[0056] S1. The heddle eye grinding head is glued to the heddle eye clamp connection structure and fixed to the heddle eye clamp, and the heddle eye grinding head is checked to see whether it is tightly connected to the heddle eye clamp.
[0057] S2. Insert the first and second fixing columns of the heddle eye fixture into the sensor of the UMT-Tribolab friction and wear testing machine, and fix them with the fixing screws on the sensor.
[0058] S3. Fix the spring end lower clamp and the fiber end lower clamp fastening structure with screws and screw holes on the reciprocating linear module of the friction and wear testing machine.
[0059] S4. Connect the two ends of the sample fiber bundle to the spring end lower clamp and the fiber end lower clamp respectively. Pass one end of the sample fiber bundle through the spring and fix the sample fiber bundle with a heat shrink tube. Pass the other end of the sample fiber bundle through the fiber end lower clamp to fix the fiber bundle channel, hang an 80g weight, adjust the tension, suspend for 1 minute, and tighten the fiber bundle with the fixing screw.
[0060] S5. Set the test parameter values. Use the 20N sensor of the UMT-Tribolab friction and wear tester, set the preload force to 0.4N, the load force to 0.5N, the friction time to 300s, the friction frequency to 3Hz, and the friction stroke to 4mm.
[0061] S6. Start the program to conduct the test, and after the test, export the relationship curve between the friction force, friction coefficient and time in the loading stage.
[0062] S7. Photograph the sample fiber bundle after friction. Use a digital microscope to observe the surface hairiness of the sample fiber bundle after friction.
[0063] S8. Repeat the test steps and change the loading force parameters set in S5 to 0.3N and 0.7N respectively.
[0064] The degree of fiber bundle damage is characterized by counting the hairiness area. The higher the degree of fiber bundle surface damage, the more hairiness is produced, and the more obvious the decline in the mechanical properties of the fiber bundle. According to the test, the hairiness area is 1.242mm when the loading force is 0.3N. 2 When the loading force is 0.5N, the hairiness area is 1.606mm 2 When the loading force is 0.7N, the hairiness area is 2.14mm 2 The increase of loading force increases the degree of damage to the fiber bundle.
[0065] Example 2
[0066] This embodiment designs a test of the friction and wear performance between the carbon fiber bundle and the heddle eye under different pre-tensions, and includes the following steps when used:
[0067] S1. The heddle eye grinding head is glued to the heddle eye clamp connection structure and fixed to the heddle eye clamp, and the heddle eye grinding head is checked to see whether it is tightly connected to the heddle eye clamp.
[0068] S2. Insert the first and second fixing columns of the heddle eye fixture into the sensor of the UMT-Tribolab friction and wear testing machine, and fix them with the fixing screws on the sensor.
[0069] S3. Fix the spring end lower clamp and the fiber end lower clamp fastening structure with screws and screw holes on the reciprocating linear module of the friction and wear testing machine.
[0070] S4. Connect the two ends of the sample fiber bundle to the spring end lower clamp and the fiber end lower clamp respectively. Pass one end of the sample fiber bundle through the spring and fix the sample fiber bundle with a heat shrink tube. Pass the other end of the sample fiber bundle through the fiber end lower clamp to fix the fiber bundle channel, hang an 80g weight, adjust the tension, suspend for 1 minute, and tighten the fiber bundle with the fixing screw.
[0071] S5. Set the test parameter values. Use the 20N sensor of the UMT-Tribolab friction and wear tester, set the preload force to 0.4N, the load force to 0.5N, the friction time to 300s, the friction frequency to 3Hz, and the friction stroke to 4mm.
[0072] S6. Start the program to conduct the test, and after the test, export the relationship curve between the friction force, friction coefficient and time in the loading stage.
[0073] S7. Photograph the sample fiber bundle after friction. Use a digital microscope to observe the surface hairiness of the sample fiber bundle after friction.
[0074] S8. Repeat the test steps and change the weight of the hanging weight in S4 to 40g and 120g respectively.
[0075] After testing, the hairiness area is 1.03mm when the weight is 40g 2 , when the weight is 80g, the hairiness area is 1.606mm 2 , when the weight is 120g, the hairiness area is 2.436mm 2 The increase of pre-tension increases the degree of damage to the fiber bundle.
[0076] Example 3
[0077] This embodiment is designed to test the friction and wear performance between the carbon fiber bundle and the heddle eye under different friction frequencies, and the following steps are included when used:
[0078] S1. The heddle eye grinding head is glued to the heddle eye clamp connection structure and fixed to the heddle eye clamp, and the heddle eye grinding head is checked to see whether it is tightly connected to the heddle eye clamp.
[0079] S2. Insert the first and second fixing columns of the heddle eye fixture into the sensor of the UMT-Tribolab friction and wear testing machine, and fix them with the fixing screws on the sensor.
[0080] S3. Fix the spring end lower clamp and the fiber end lower clamp fastening structure with screws and screw holes on the reciprocating linear module of the friction and wear testing machine.
[0081] S4. Connect the two ends of the sample fiber bundle to the spring end lower clamp and the fiber end lower clamp respectively. Pass one end of the sample fiber bundle through the spring and fix the sample fiber bundle with a heat shrink tube. Pass the other end of the sample fiber bundle through the fiber end lower clamp to fix the fiber bundle channel, hang an 80g weight, adjust the tension, suspend for 1 minute, and tighten the fiber bundle with the fixing screw.
[0082] S5. Set the test parameter values. Use the 20N sensor of the UMT-Tribolab friction and wear tester, set the preload force to 0.4N, the load force to 0.5N, the friction time to 300s, the friction frequency to 3Hz, and the friction stroke to 4mm.
[0083] S6. Start the program to conduct the test, and after the test, export the relationship curve between the friction force, friction coefficient and time in the loading stage.
[0084] S7. Photograph the sample fiber bundle after friction. Use a digital microscope to observe the surface hairiness of the sample fiber bundle after friction.
[0085] S8. Repeat the test steps and change the friction frequency parameter set in S5 to 1Hz and 5Hz respectively.
[0086] After testing, the hairiness area is 2.731mm when the reciprocating friction frequency is 1Hz 2 When the reciprocating friction frequency is 3Hz, the hairiness area is 1.606mm 2 When the reciprocating friction frequency is 5Hz, the hairiness area is 0.709mm 2 The increase in reciprocating friction frequency reduces the degree of damage to the fiber bundle.
[0087] The above-described embodiments are merely descriptions of preferred implementations of the present invention and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, ordinary technicians in this field may make various modifications and improvements to the technical solutions of the present invention, which should all fall within the scope of protection determined by the claims of the present invention.
Claims
1. A testing device for friction and wear performance between high-performance fiber bundles and heald eyes, characterized in that: It includes a heald eye fixture, a spring end lower fixture, a fiber end lower fixture and a microscope fixture; The heddle eye clamp comprises a fastening structure and a connecting structure; the fastening structure comprises a heddle eye clamp fixing column 1 (1) and a heddle eye clamp fixing column 2 (2); the connecting structure comprises a connecting channel between the heddle eye clamp and the heddle eye grinding head (3); the heddle eye grinding head (3) and the heddle eye clamp fixing column (2) are glued and connected to form a whole; The spring end lower clamp comprises a supporting structure, a fastening structure and a connecting structure; the supporting structure comprises a spring end lower clamp fixed base (7); the fastening structure is a limiting hole (8) located on the fixed base (7) and fixed to the reciprocating linear module of the friction and wear testing machine by screws; the connecting structure comprises a spring connecting rod (4), a spring limiting groove (6) and a spring (5); the spring (5) passes through the spring connecting rod (4) and is fixed on the fixed base (7); The fiber end lower clamp comprises a supporting structure, a fastening structure and a connecting structure; the supporting structure comprises a fiber end lower clamp fixing base (9); the fastening structure is a limiting groove (11) located on the fixing base (9), connected to a fixing platform of a friction and wear testing machine via screws; the connecting structure comprises a fiber end lower clamp fixing screw channel (13) and a fiber end lower clamp fixing screw (10); the fiber bundle channel (13) is perpendicular to the fixing screw (10); The microscope fixture comprises a supporting structure and a fastening structure; the supporting structure is a microscope bracket (15), and the fastening structure is a microscope bracket limiting groove (16), which is connected to a fixed platform of a friction and wear testing machine via screws; and a digital microscope (17) is fixed on the microscope bracket (15).
2. A high-performance fiber bundle-heald eye friction and wear performance testing device according to claim 1, characterized in that: The fiber bundle includes but is not limited to various high-performance fibers such as carbon fiber, quartz fiber, alumina fiber, silicon nitride fiber, silicon carbide fiber, etc.
3. A high-performance fiber bundle-heald eye friction and wear performance testing device according to claim 1, characterized in that: The heald eye grinding head (3) of different materials and specifications can be replaced according to experimental requirements.
4. The testing device for friction and wear performance between high-performance fiber bundles and heald eyes according to claim 1, characterized in that: The spring (5) of the lower clamp at the spring end is a tension spring, and tension springs of different specifications can be replaced to change the tension variation range during the fiber bundle testing process.
5. The testing device for friction and wear performance between high-performance fiber bundle and heald eye according to claim 1, characterized in that: The initial tension of the fiber bundle can be adjusted by hanging weights of different masses.
6. The testing device for friction and wear performance between high-performance fiber bundles and heald eyes according to claim 1, characterized in that: The heald eye fixture is perpendicular to the fiber bundle and is matched with a friction and wear testing machine to evaluate the friction and wear performance between the fiber bundle and the heald eye.
7. A method for testing friction and wear between a high-performance fiber bundle and a heddle eye, using the testing device for friction and wear performance between a high-performance fiber bundle and a heddle eye according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: S1, gluing the heddle eye grinding head (3) to the heddle eye clamp connection structure and fixing it to the heddle eye clamp, and checking whether the heddle eye grinding head is tightly connected to the heddle eye clamp; S2, insert the heddle eye fixture fixing column 1 (1) and the heddle eye fixture fixing column 2 (2) into the UMT-Tribolab friction and wear testing machine sensor and fix them with screws; S3, fix the spring end lower clamp and the fiber end lower clamp fastening structure with screws and screw holes on the reciprocating linear module of the friction and wear testing machine; S4, pass one end of the sample fiber bundle (14) through the spring (5), use the heat shrink tube (12) to fix the sample fiber bundle (14), pass the other end of the sample fiber bundle (14) through the fiber end lower clamp fixing fiber bundle channel (13), hang weights, adjust the tension, suspend for 1 minute, and tighten the fiber bundle with the fixing screw (10); S5, setting test parameter values; S6, start the program to conduct the test, and after the test, derive the relationship curve between the friction force, friction coefficient, loading force, horizontal stroke, test chamber temperature, and time during the loading stage; S7. Use a digital microscope (17) to observe the surface hairiness of the sample fiber bundle (14) after friction.