A testing method for silicone leather
By testing the bonding properties of silicone leather in the tensile state, the problem that existing methods cannot accurately determine the bonding properties under high temperature boiling is solved, and a more accurate and efficient test method is provided to ensure production and Performance consistency on the application side.
Patent Information
- Application Number
- CN202210778112.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-04
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-07-04
AI Technical Summary
The existing testing methods cannot effectively test the bonding performance of silicone leather in the tensile state, resulting in inconsistent determination of bonding performance between the production end and the application end, especially the problem of peeling and delamination after boiling at high temperature.
A test method is adopted, which involves cutting a rectangular silicone leather sample and folding it in half, stretching and slashing the silicone material layer perpendicular to the tensile direction on one side of the clamp, and heating it in water at 95-105°C for 4-6 hours. The shrinkage and/or delamination are observed and the graded judgment is made based on the peeling situation.
This method can more accurately simulate the use state of silicone leather at the application end, improve the determination consistency and testing efficiency of adhesive performance, and avoid deviations from traditional methods.
Smart Images

Figure CN115097113B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of synthetic leather, and in particular relates to a testing method for organic silicon leather. Background Art
[0002] Globally, concerns about environmental protection and animal welfare are rapidly reshaping the leather industry - especially in China, the world's largest leather market. At the same time, both regular leather and current synthetic alternatives fail to meet the growing requirements of products such as automobiles and wearable electronics in terms of weather resistance, stain resistance, odor and sustainability. Leather is known for its soft touch and breathability, providing premium texture and comfort. However, it also has some significant disadvantages, including weak UV resistance, poor crack and aging resistance, and brittleness. In contrast, other types of synthetic leather, while durable, have problems with dangerous, irritating odors that come from complex chemical reagents and pose a threat to human health.
[0003] The unique molecular structure of silicone can meet consumers' demands for leather in terms of softness, moisture permeability, stability and environmental protection. However, silicone leather usually has the problem of easy peeling and delamination after high-temperature boiling, which requires manufacturers to always pay attention to the boiling resistance of silicone leather products during the research and development process.
[0004] The existing testing method usually directly puts the product in water and continuously heats it to observe whether it peels off. However, silicone leather is often in a stretched state at the application end, and its bonding performance will change due to stretching, resulting in inconsistent bonding performance judgments at the production end and the application end. In view of this, providing an efficient silicone leather boiling resistance test method is a technical problem that needs to be solved urgently in the field of synthetic leather. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for testing silicone leather, especially to test and characterize the bonding performance of silicone leather products under tension.
[0006] The technical solution adopted by the present invention to solve the above problems is:
[0007] A method for testing silicone leather comprises the following steps:
[0008] S1. Cut the silicone leather test sample into a rectangular shape, fold the sample in half at the midpoint of the long side and fix it;
[0009] S2. The fixed silicone leather test sample is stretched and loaded into a fixture, and the silicone material layer is cut perpendicular to the stretching direction on at least one side of the fixture;
[0010] S3. The silicone leather test sample scratched by S2 is placed in 95-105°C water and heated for 4-6 hours;
[0011] S4. Observe the shrinkage and / or delamination of the silicone leather test sample after treatment in S3, and scrape the sample to observe the peeling condition.
[0012] Furthermore, the organic silicone leather test sample is a composite layer of a silicone material layer and a base material layer formed by coating a silicone material on a base material.
[0013] Furthermore, the base material is PET or TPU.
[0014] Furthermore, the rectangle in step S1 is a rectangle with a long side of 200-500 mm and a short side of 20-50 mm, preferably a rectangle with a long side of 300 mm and a short side of 30 mm.
[0015] Furthermore, the fixing in step S1 is to take the folded part as the starting point and fix it at 50-200 mm along the long side. Preferably, the fixing is to take the folded part as the starting point and fix it at 100 mm along the long side.
[0016] Furthermore, when the silicone leather test sample is scratched in step S2, the silicone material layer is completely scratched, and the test sample is not completely disconnected. Preferably, the silicone material layer is completely scratched, and the base material layer is not disconnected.
[0017] Furthermore, the stretching in step S2 is stretching in the long side direction to 120-140% of the original length. Preferably, the stretching is 130% of the original length.
[0018] Furthermore, when the silicone leather test sample is scratched in step S2, the interval between two adjacent scratches is 20-30 mm. Preferably, the interval is 20 mm.
[0019] Furthermore, step S4 also includes grading according to the peeling condition of the sample, and the grading standard is:
[0020] If there is no obvious shrinkage and / or delamination at the cut of the sample, and there is no delamination between the silicone material layer and the base material layer after scraping the sample, or the delamination area is less than 5% of the total area of the sample, it is judged that there is no delamination;
[0021] If there is slight shrinkage and / or delamination at the cut of the sample, and after scraping the sample, the silicone material layer and the base material layer are delaminated and the delamination area is 10-30% of the total area of the sample, it is judged as moderate delamination;
[0022] Obvious peeling is judged to be present when obvious shrinkage and / or delamination occurs at the cut of the sample, and when the silicone material layer and the base material layer are completely peeled off / fall off after scraping the sample.
[0023] The beneficial effects of the present invention are:
[0024] The test method provided by the present invention is a boiling water test under a stretched state, which can better simulate the use of silicone leather materials at the application end and determine the bonding performance of the material when used compared to traditional test methods. Other conventional methods in the field do not stretch or scratch the test object, and there is a certain deviation in the performance judgment of the material.
[0025] The test method provided by the present invention performs a scratching operation on the organic silicon leather test sample, and integrates the method of the hundred-grid test. Since the organic silicon leather test sample is a silicone product, the traditional hundred-grid test is not applicable. The present invention applies the advantages of the hundred-grid test to the test of organic silicon leather by reasonably setting the steps, which is simple and efficient. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0027] Figure 1 This is a rendering of the treated silicone leather test sample in Example 1;
[0028] Figure 2 This is a rendering of the treated silicone leather test sample in Example 2;
[0029] Figure 3 This is a rendering of the effect of the treated silicone leather test sample in Example 3. DETAILED DESCRIPTION
[0030] The present invention is described in detail below with reference to the examples. The examples are only preferred embodiments of the present invention and are not intended to limit the present invention.
[0031] Embodiment 1: A method for testing silicone leather, comprising the following steps:
[0032] S1. Cut the silicone leather test sample into a rectangle with a long side of 300 mm and a short side of 30 mm, and fold the sample in half at the midpoint of the long side, and measure 100 mm from the fold to fix it; the silicone leather test sample is a composite layer of a silicone material layer and a base material layer formed by coating a silicone material on a base material, and the base material is TPU;
[0033] S2. Stretch the fixed silicone leather test sample to 130% of its original length and place it in a fixture. Scratch the silicone material layer on one side of the fixture perpendicular to the stretching direction, with the interval between two adjacent scratches being 20 mm.
[0034] S3. The silicone leather test sample after being scratched in S2 was placed in water at 100°C and heated for 4 hours;
[0035] S4. Observe the shrinkage and / or delamination of the silicone leather test sample after treatment in S3, and scrape the sample to observe the peeling. It was observed that there was no shrinkage or delamination between the silicone material layer and the TPU, and no peeling occurred after scraping. Figure 1 , it was judged as no peeling.
[0036] Embodiment 2: A method for testing silicone leather, comprising the following steps:
[0037] S1. Cut the silicone leather test sample into a rectangle with a long side of 200 mm and a short side of 20 mm, and fold the sample in half at the midpoint of the long side, and measure 70 mm from the fold to fix it; the silicone leather test sample is coated with a silicone material on a base material to form a composite layer of a silicone material layer and a base material layer, and the base material is PET;
[0038] S2. The fixed silicone leather test sample is stretched to 130% of its original length and placed in a fixture. The silicone material layer is scratched perpendicular to the stretching direction on one side of the fixture, with the interval between two adjacent scratches being 25 mm.
[0039] S3. The silicone leather test sample after being scratched in S2 was placed in water at 100°C and heated for 4 hours;
[0040] S4. Observe the shrinkage and / or delamination of the silicone leather test sample after treatment in S3, and scrape the sample to observe the peeling condition. It was observed that the silicone material layer and PET had slight shrinkage and delamination, and the peeling area after scraping was about 10%. Figure 2 , judged as moderate peeling.
[0041] Embodiment 3: A method for testing silicone leather, comprising the following steps:
[0042] S1. Cut the silicone leather test sample into a rectangle with a long side of 500 mm and a short side of 50 mm, and fold the sample in half at the midpoint of the long side, and measure 200 mm from the fold to fix it; the silicone leather test sample is a composite layer of a silicone material layer and a base material layer formed by coating the silicone material on a base material, and the base material is PET;
[0043] S2. The fixed silicone leather test sample is stretched to 130% of its original length and placed in a fixture. The silicone material layer is scratched perpendicular to the stretching direction on one side of the fixture, with the interval between two adjacent scratches being 30 mm.
[0044] S3. The silicone leather test sample after being scratched in S2 was placed in water at 100°C and heated for 4 hours;
[0045] S4. Observe the shrinkage and / or delamination of the silicone leather test sample after treatment in S3, and scrape the sample to observe the peeling condition. It was observed that the silicone material layer and TPU were severely delaminated and the whole piece was peeled off. Figure 3 , judged as obvious peeling.
[0046] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0047] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0048] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for testing silicone leather, characterized in that: The following steps are involved: S1. Cut the silicone leather test sample into a rectangular shape, fold the sample in half at the midpoint of the long side and fix it; S2. The fixed silicone leather test sample is stretched and loaded into a fixture, and the silicone material layer is cut perpendicular to the stretching direction on at least one side of the fixture; S3. The silicone leather test sample after being scratched in S2 is heated in water at 95-105°C for 4-6 hours; S4. Observe the shrinkage and / or delamination of the silicone leather test sample after treatment in S3, and scrape the sample to observe the peeling condition.
2. The method for testing silicone leather according to claim 1, characterized in that: The organic silicon leather test sample is a composite layer of a silicone material layer and a base material layer formed by coating a silicone material on a base material.
3. The method for testing silicone leather according to claim 2, characterized in that: The base material is PET or TPU.
4. The method for testing silicone leather according to claim 1, characterized in that: The rectangle in step S1 is a rectangle with a long side of 200-500 mm and a short side of 20-50 mm.
5. The method for testing silicone leather according to claim 1, characterized in that: The fixing in step S1 is to take the folded part as the starting point and fix at 50-200 mm along the long side direction.
6. The method for testing silicone leather according to claim 1, characterized in that: When the silicone leather test sample is scratched in step S2, the silicone material layer is completely cut, but the test sample is not completely cut.
7. The method for testing silicone leather according to claim 1, characterized in that: The stretching in step S2 is stretching in the long side direction to 120-140% of the original length.
8. The method for testing silicone leather according to claim 1, characterized in that: When the silicone leather test sample is scratched in step S2, the interval between two adjacent scratches is 20-30 mm.
9. The method for testing silicone leather according to claim 1, characterized in that: Step S4 also includes grading the samples according to their peeling conditions, and the grading standard is: If there is no obvious shrinkage and / or delamination at the cut of the sample, and there is no delamination between the silicone material layer and the base material layer after scraping the sample, or the delamination area is less than 5% of the total area of the sample, it is judged that there is no delamination; If there is slight shrinkage and / or delamination at the cut of the sample, and after scraping the sample, the silicone material layer and the base material layer are delaminated and the delamination area is 10-30% of the total area of the sample, it is judged as moderate delamination; Obvious peeling is judged to be present when obvious shrinkage and / or delamination occurs at the cut of the sample, and when the silicone material layer and the base material layer are completely peeled off / fall off after scraping the sample.
Citation Information
Patent Citations
Leather shoe peeling strength test machine
CN201083674Y
Textile yarn scratch resistance detection device
CN214374018U
High-temperature tensile testing jig
JP2007285703A
Heat-shrinkable polyolefin film and its manufacturing process
JP2009045920A
Testing the Adhesion of Elastic Adhesives or Elastic Sealing Materials on Surfaces of Components