A method for regenerating water glass casting waste sand and obtained regenerated sand
By roasting, alkali washing and dehydrating rice husk and foundry water glass waste sand, the problem of low waste sand recycling rate and high energy consumption in the foundry industry is solved, and the comprehensive utilization of rice husk ash and foundry waste sand is achieved. It reduces process energy consumption, improves the quality and stability of recycled sand, and achieves clean production.
Patent Information
- Application Number
- CN202210738870.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-06-27
AI Technical Summary
In the existing technology, the recycling rate of waste sand in the foundry industry is low and the energy consumption is high, resulting in resource waste and environmental pollution, and the potential value of rice husk ash has not been fully utilized.
By mixing rice husk and used foundry water glass waste sand for roasting, alkali washing, dehydration and drying, the comprehensive utilization of rice husk ash and foundry waste sand is achieved, the energy consumption of the process is reduced, and the regenerated sand is restored through the NaOH aqueous solution reaction activity, reducing energy consumption and pollution in the process.
It achieves comprehensive utilization of solid waste resources such as foundry waste sand and rice husks, reduces process energy consumption, improves the quality and stability of recycled sand, reduces the discharge of liquid tailings, and achieves clean production.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of resource recovery, and in particular to a method for regenerating water glass casting waste sand and the obtained regenerated sand. Background Art
[0002] According to relevant statistics, at present, for every ton of qualified castings produced, about 1~1.3t of waste sand and 300kg of waste slag are discharged. Based on this calculation, my country's foundry industry discharges 30 million tons of waste sand and 9 million tons of waste slag every year. The recycling rate of waste sand is less than 30%, resulting in great waste of resources and environmental pollution. The key reason is that the technology of waste sand recycling is backward, the energy consumption is high, and the quality of recycled sand is low, which makes it difficult to reuse waste sand resources.
[0003] According to relevant statistics, my country produces nearly 40 million tons of rice husks every year. Generally, rice husks are treated as general solid waste or used as simple fuel, with a very low comprehensive utilization rate. In addition, the rice husk ash after burning is discharged as waste, polluting the ecological environment, and the potential value of rice husk ash has not been fully utilized.
[0004] Industrial green development is not only a problem of energy consumption, but also a problem of production methods. Promoting industrial green development requires not only the transformation and upgrading of energy utilization methods, utilization efficiency and consumption structure, but also optimization and innovation in product design, production technology and other aspects. In terms of green manufacturing, typical demonstrations should be used to drive the green transformation of production models and promote low-carbon development of the entire industrial chain. Therefore, rice husk ash and foundry waste sand need to be put back into production to achieve waste utilization.
[0005] Based on the above practical situation and needs, the present invention is specially proposed. Summary of the invention
[0006] The object of the present invention is to provide a method for regenerating water glass waste sand for casting. The method comprises mixing rice husk and used water glass waste sand for casting, and then sequentially performing roasting, alkali washing, dehydration and drying, so as to realize the comprehensive utilization of rice husk ash and waste sand for casting, and reduce process energy consumption while enhancing performance.
[0007] To achieve the above object, the technical solution of the present invention is as follows:
[0008] The present invention relates to a method for regenerating water glass casting waste sand, comprising the following steps:
[0009] (1) Crushing the bulk of the waste sand from foundry water glass;
[0010] Preferably, the blocky waste sand of foundry water glass is crushed into single grains of sand by screening.
[0011] (2) roasting the rice husk and the crushed foundry water glass waste sand to obtain a roasting product;
[0012] Preferably, the mass ratio of the rice husk to the waste sand is 1:(8-10).
[0013] Preferably, the calcination temperature is 200-400° C., and the calcination time is 1-2 h.
[0014] (3) mixing the calcined product with an aqueous NaOH solution and stirring, and performing solid-liquid separation after the reaction is completed to obtain wet sand and an aqueous sodium silicate solution;
[0015] Preferably, the mass fraction of the NaOH aqueous solution is 10-15%.
[0016] Preferably, the mixing is carried out in a closed mixer, and the mass ratio of the calcined product to the NaOH aqueous solution is (2-5):1, preferably 3:1.
[0017] Preferably, during the mixing and stirring, the temperature of the mixture is 90-100° C. and the reaction time is 1-3 hours.
[0018] (4) The wet sand is washed with clean water, dehydrated and dried in sequence to obtain finished regenerated sand.
[0019] The present invention also relates to the regenerated sand obtained by the above regeneration method.
[0020] Beneficial effects of the present invention:
[0021] The present invention provides a method for regenerating water glass casting waste sand, which comprises mixing rice husks and used casting water glass waste sand, and then sequentially performing roasting, alkali washing, dehydration and drying. Compared with the prior art, the method has the following advantages:
[0022] 1) Comprehensive utilization of solid waste resources such as foundry waste sand and rice husks is achieved. Even water glass that has lost its activity on the surface of waste sand can be reused after the method is used;
[0023] 2) Since rice husks are added during the roasting process, the process energy consumption is low, reducing energy and emissions;
[0024] 3) There are few residual ions on the surface of the regenerated sand, the conductivity is low, and the quality of the regenerated sand is stable;
[0025] 4) The collected liquid tailings are new sodium silicate solution and raw materials that can be used to prepare sodium hydroxide aqueous solution, without additional discharge, thus achieving clean production. DETAILED DESCRIPTION
[0026] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0027] The embodiment of the present invention relates to a method for regenerating water glass casting waste sand, comprising the following steps:
[0028] (1) Crushing the bulk of the waste sand from foundry water glass;
[0029] In one embodiment of the present invention, the massive waste sand of foundry water glass is crushed into single particles by screening, so as to make the subsequent reaction more complete.
[0030] (2) roasting the rice husk and the crushed foundry water glass waste sand to obtain a roasting product;
[0031] In one embodiment of the present invention, the mass ratio of rice husk to waste sand is 1:(8-10). If the amount of rice husk added is too large, the content of SiO2 in the mixture of rice husk and waste sand will be high. In the process of subsequent chemical reaction between the roasted product and NaOH to generate water glass, the modulus of water glass (the chemical formula of water glass is Na2O·nSiO2, where n is the modulus of water glass) will exceed 3.5. Water glass with a large modulus needs to be dissolved in a steam environment and is not suitable for use as a casting binder; secondly, if the amount of rice husk added is too large, the calorific value temperature generated is high, resulting in heat waste; if the amount of rice husk added is too small, the heat provided by the joint roasting of rice husk and waste sand is insufficient, and the energy consumption of the heat source that needs to be supplemented increases, which is not conducive to energy conservation and emission reduction.
[0032] In one embodiment of the present invention, the roasting temperature is 200-400°C and the roasting time is 1-2 hours. The roasting process includes: using the burning rice husk to provide heat value to remove low melting point substances in the waste sand, mainly the glue binder used in the sand core assembly; and adding NaOH solution in the next step to heat the solution, thereby further reducing energy consumption.
[0033] (3) mixing the calcined product with an aqueous solution of NaOH and stirring, and performing solid-liquid separation after the reaction is completed to obtain wet sand and an aqueous solution of sodium silicate;
[0034] In one embodiment of the present invention, the mass fraction of the NaOH aqueous solution is 10-15%. Since the waste sand and rice husk ash after roasting will absorb some water, the mass fraction of the NaOH aqueous solution should not be too high, otherwise it will lead to high acid consumption value and pH value of the regenerated sand, reducing the strength of the sand core.
[0035] In one embodiment of the present invention, the mixing is carried out in a closed mixer, and the mass ratio of the calcined product to the NaOH aqueous solution is (2-5):1, preferably 3:1.
[0036] In one embodiment of the present invention, during mixing and stirring, the temperature of the mixture is 90-100° C. and the reaction time is 1-3 hours. If the reaction time is too long or the concentration of the NaOH aqueous solution is too high, SiO2 in the regenerated sand will react with NaOH, destroying the morphology of the sand surface.
[0037] The main chemical components of rice husk ash are shown in Table 1, among which the main component is SiO2, with a content of more than 90%.
[0038] Table 1
[0039]
[0040] The chemical reactions involved in steps (2) and (3) are as follows:
[0041] ① The water glass sand is dehydrated during the core making and pouring process, losing its adhesiveness and causing the reaction shown in formula (I), that is, the water glass on the surface of the old sand is dehydrated to generate sodium oxide and silicate.
[0042] (Na2O mSiO2nH2O) Na2SiO3·nH2O→Na2O+ H2SiO3 (I)
[0043] ② After the roasted product is mixed with an aqueous NaOH solution, in an alkaline environment, the silica on the surface of the old sand and the silicon dioxide mainly from the rice husk ash absorb water and recover their activity, and the reactions shown in formulas (II) and (III) occur.
[0044] H2SiO3+2NaOH → Na2SiO3+H2O (II)
[0045] SiO2+2NaOH →Na2SiO3+ H2O (III)
[0046] It can be seen from formula (II) and formula (III) that the sodium silicate on the surface of the waste sand that has lost water is reactivated in an alkaline aqueous solution environment and is regenerated into sodium silicate, which is continued to be used as a binder in casting production.
[0047] The conventional water glass wet regeneration process includes the following steps: using the acid-base neutralization principle, adding acid (such as oxalic acid, hydrochloric acid, etc.) to the aqueous solution to react chemically with the sodium silicate on the surface of the waste sand to generate water-soluble salt, separating the waste sand from the sewage and drying it as regenerated sand, and recycling the sewage after treatment. The disadvantage of this process is that the ion concentration in the circulating water is getting higher and higher, resulting in high conductivity of the regenerated sand, or it is necessary to regularly discharge sewage and add clean water, otherwise the conductivity of the regenerated sand will increase.
[0048] It should be noted that the conductivity of an aqueous solution is related to the concentration of solute salts or other chemical impurities that decompose into electrolytes. The conductivity of a water sample is an important indicator for measuring the salt content, ion content, and impurity content of the water. The purer the water, the lower the conductivity and the higher the corresponding resistivity.
[0049] The higher the conductivity of the regenerated sand, the higher the ion content on the sand surface. These ions will accelerate the chemical reaction of the binder. When used in core making, it is easy to cause problems such as rapid solidification (that is, a single grain of sand solidifies and cannot bond with the surrounding sand particles) and low strength. Therefore, the conductivity of the regenerated sand should be reduced as much as possible.
[0050] In addition, in step (3), the SiO2 powder in the rice husk will react with NaOH. After the wet sand is dehydrated by negative pressure, the resulting aqueous solution is a new sodium silicate solution (sodium silicate aqueous solution is commonly known as water glass, and the obtained water glass can be used to derive and prepare silicon series products according to standard GB / T4029-1996). The modulus of the water glass is between 2 and 3, and it can continue to be used as a binder in casting production, thereby realizing the comprehensive utilization of rice husks without additional discharge.
[0051] (4) The wet sand is washed with clean water, dehydrated and dried in sequence to obtain finished regenerated sand.
[0052] Among them, after the wet sand is washed with clean water and dehydrated, the collected water mainly contains Na + OH - , a small amount of SiO3 2- The plasma can be used to prepare the NaOH solution in the subsequent step (3).
[0053] The embodiment of the present invention also relates to the regenerated sand obtained by the above regeneration method, which has low loss on ignition and can be used directly instead of the original sand.
[0054] Example 1
[0055] A method for regenerating water glass casting waste sand comprises the following steps:
[0056] (1) crushing the bulk foundry water glass waste sand by screening to obtain single-grain sand;
[0057] (2) mixing rice husk and crushed foundry water glass waste sand in a mass ratio of 1:9 and then roasting them at a roasting temperature of 300° C. for 1 h to obtain a roasted product;
[0058] (3) Mixing the calcined product with a 12% NaOH aqueous solution in a closed mixer, wherein the mass ratio of the calcined product to the NaOH aqueous solution is 3:1, the temperature of the mixture is 95°C, and the reaction time is 2 hours. After the reaction is completed, solid-liquid separation is performed to obtain wet sand and sodium silicate aqueous solution;
[0059] (4) The wet sand is washed with clean water, dehydrated and dried in sequence to obtain finished regenerated sand.
[0060] According to the methods described in GBT 7143-2010 Chemical Analysis Methods of Silica Sand for Foundry and GBT 26659-2011 Regenerated Silicon for Foundry, the performance of the regenerated sand obtained in Example 1 was tested. The results are shown in Table 2.
[0061] Table 2
[0062]
[0063] The results show that the physical and chemical properties of the regenerated sand obtained by the method of the present invention are close to those of the original sand, wherein the water content and mud content are low, and the loss on ignition is low, and the regenerated sand can be directly used in production instead of the original sand.
[0064] The modulus of water glass in the obtained sodium silicate aqueous solution is between 2 and 3, and the water glass can be further used as a binder in casting production.
[0065] The reaction conditions in Examples 2 to 8 and Comparative Examples 1 and 2 were changed, and the specific settings are shown in Table 3. The performance test results are shown in Table 4.
[0066] Table 3
[0067]
[0068] *Except for the parameters recorded in Table 1, the other parameters of each embodiment are the same as those of Embodiment 1.
[0069] Table 4
[0070]
[0071] From the above test results, it can be seen that in Example 1, no rice husk is added, and the gas consumption is too high, which will increase the production cost and is inconsistent with the policy of environmental protection and energy conservation.
[0072] Comparative Example 2 replaces the sodium hydroxide solution with calcium hydroxide solution. Since calcium hydroxide has low solubility, the residual calcium hydroxide will remain on the surface of the wet sand, causing a sharp increase in the acid consumption value.
[0073] In Example 1 of the present invention, rice husks are added during the waste sand roasting process, and the natural gas consumption of the regeneration process is significantly reduced. In Examples 3 and 4, the amount of rice husks is further increased, and it is found that after excessive addition of rice husks, although the natural gas consumption can be further reduced, when NaOH is quantitatively added, excess SiO2 in the rice husk ash will remain on the surface of the wet sand, thereby causing the fine powder mud content of the regenerated sand to directly increase.
[0074] In Examples 7 and 8, if NaOH is added in excess, NaOH will remain on the surface of the wet sand, resulting in a direct increase in the acid consumption value and conductivity of the regenerated sand. In Example 6, if the amount of NaOH added is too little, SiO2 will remain on the surface of the wet sand. Since SiO2 is insoluble in water, these micropowders cannot be removed in the subsequent clean water rinse, resulting in a direct increase in the micropowder mud content of the regenerated sand, which will sharply reduce the strength of the sand core.
[0075] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for regenerating water glass casting waste sand, characterized in that: The following steps are involved: (1) crushing the bulk of the waste water glass sand; wherein: the crushing is performed by screening to crush the bulk of the waste water glass sand into single particles of sand; (2) roasting the rice husk and the crushed waste water glass sand to obtain a roasting product; wherein: The mass ratio of the rice husk to the waste sand is 1:9; the roasting temperature is 300° C., and the roasting time is 1 hour; (3) mixing and stirring the calcined product with a NaOH aqueous solution, and performing solid-liquid separation after the reaction is completed to obtain wet sand and a sodium silicate aqueous solution; wherein: the mass fraction of the NaOH aqueous solution is 12%; the mass ratio of the calcined product to the NaOH aqueous solution is 3:1; during the mixing and stirring, the temperature of the mixture is 95° C., and the reaction time is 2 h; (4) The wet sand is washed with clean water, dehydrated and dried in sequence to obtain finished regenerated sand.
2. The regenerated sand obtained by the method according to claim 1.