Adhesive composition and optical adhesive
By adjusting the surface tension and glass transition temperature ratio of the monomer copolymer, an adhesive composition with excellent wettability and light resistance is prepared, which solves the problem of bubbles and light resistance in optical adhesives under high temperature and high humidity conditions. Floating problem, achieving the dual effects of stability and adhesion.
Patent Information
- Application Number
- CN202210267159.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-03-23
- Filing Date
- 2022-03-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-03-18
AI Technical Summary
Existing optical adhesives are prone to bubbles or floating between laminated layers under high temperature, high humidity and thermal shock conditions, making it difficult to ensure adhesion and prevent bubbles at the same time.
Using an adhesive composition containing a specific monomer copolymer, by adjusting the ratio of normal temperature surface tension and glass transition temperature, an adhesive with excellent wettability and light resistance is formed, ensuring that the adhesive performs well under high and low temperature conditions. stability and prevent bubbles.
It achieves stability under high temperature, low temperature and high humidity conditions while avoiding bubble generation and floating between laminate layers, meeting the requirements for adhesion and durability.
Smart Images

Figure CN115109545B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to an adhesive composition and an optical adhesive formed using the adhesive composition. Background Art
[0002] Optical adhesive (OCA, Optically Clear Adhesive) is an adhesive inserted to join functional layers constituting display products or products containing transparent electrodes (hereinafter referred to as transparent electrode products). In order to achieve the function, the adhesion of the optical adhesive is important. In particular, the above-mentioned functional layer is sometimes composed of two or more different materials or components. Even in this case, it is required that the adhesion on both sides is excellent. In Patent Document 1, an optical adhesive is known that uses a partially polymerized acrylic resin to ensure excellent adhesion to a glass substrate.
[0003] Display products or transparent electrode products containing optical adhesives may experience bubble generation or lamination layer damage due to various reasons such as foreign matter contained in the glass substrate or infiltrated between processes, gas generated in the optical adhesive or polarizing plate, and thermal shrinkage of the polarizing plate. In particular, the generation of bubbles or the floating phenomenon between laminated layers is mainly caused by foreign matter (defect) located between laminated layers of display products or transparent electrode products acting as a nucleus.
[0004] Conventional optical adhesives having high crosslinking density and glass transition temperature by introducing an excessive amount of a crosslinking agent and a monomer with high thermal stability exhibit excellent stability in high temperature, high temperature / high humidity, and thermal shock evaluations, but the generation of bubbles or floating between laminated layers significantly occurs.
[0005] Therefore, there is a demand for an optical adhesive that has stability and can prevent the generation of bubbles or the floating phenomenon between laminated layers.
[0006] Prior art literature
[0007] Patent Literature
[0008] (Patent Document 1) Korean Patent Publication No. 10-2016-0105354 Summary of the invention
[0009] The object of the present application is to provide an adhesive composition and an optical adhesive that can solve the above-mentioned problems.
[0010] Another object of the present application is to provide an adhesive composition for forming an optical adhesive which has excellent wettability and light resistance and can cover steps and defects.
[0011] Another object of the present application is to provide an adhesive composition for forming an optical adhesive that satisfies basic physical properties such as durability and adhesive strength and can minimize the generation of bubbles or floating between laminated layers.
[0012] In addition, the present application aims to provide an optical adhesive that can cover defects between laminated layers of a display product or a transparent electrode product.
[0013] The term "normal temperature" used in this application refers to the temperature in a natural state without any special heating or cooling, and may refer to any temperature in the range of about 10°C to 30°C, for example, a temperature above about 15°C, above about 18°C, above about 20°C, or above about 23°C, or below about 27°C.
[0014] The term "surface tension" used in this application is a force acting in a direction to minimize the surface of a liquid substance, and may be a value measured by a surface tension meter using a platinum ring according to ISO 304. In addition, the term "normal temperature surface tension" used in this application may be a value measured according to the above method under normal temperature. In addition, here, normal temperature may specifically be about 25°C.
[0015] The term "substituted" used in this application means that a hydrogen atom bonded to a carbon atom of a compound is replaced with another substituent. The substituted position is not particularly limited as long as it is a position where a hydrogen atom can be substituted, that is, a position where a substituent can be substituted. When there are more than two substitutions, the above-mentioned substituents may be the same or different from each other.
[0016] The term "substituent" used in the present application refers to an atom or an atomic group that replaces one or more hydrogen atoms on the parent chain of a hydrocarbon. In this case, in the present application, the carbon in the parent chain of the hydrocarbon to which the above-mentioned substituent is combined is defined as a substituted carbon. In addition, the substituent is described below, but is not limited thereto, and as long as there is no special record in the present application, the above-mentioned substituent may be further substituted by the substituent described below or may not be substituted by any substituent.
[0017] Unless otherwise stated, the term "alkyl or alkylene" used in the present application may be a straight or branched alkyl or alkylene group having 1 to 20 carbon atoms, or 1 to 16 carbon atoms, or 1 to 12 carbon atoms, or 1 to 8 carbon atoms, or 1 to 6 carbon atoms; or a cyclic alkyl or alkylene group having 3 to 20 carbon atoms, or 3 to 16 carbon atoms, or 3 to 12 carbon atoms, or 3 to 8 carbon atoms, or 3 to 6 carbon atoms. Here, the cyclic alkyl or alkylene group includes an alkyl or alkylene group that exists only in a ring structure and an alkyl or alkylene group that contains a ring structure. For example, cyclohexyl and methylcyclohexyl are both equivalent to cyclic alkyl groups.
[0018] Unless otherwise specified, the term "alkenyl or alkenylene" used in the present application may be a linear or branched non-cyclic alkenyl or alkenylene having 2 to 20 carbon atoms, or 2 to 16 carbon atoms, or 2 to 12 carbon atoms, or 2 to 8 carbon atoms, or 2 to 6 carbon atoms; or a cyclic alkenyl or alkenylene having 3 to 20 carbon atoms, or 3 to 16 carbon atoms, or 3 to 12 carbon atoms, or 3 to 8 carbon atoms, or 3 to 6 carbon atoms. Here, when an alkenyl or alkenylene includes a ring structure, it corresponds to a cyclic alkenyl or alkenylene.
[0019] Unless otherwise specified, the term "alkynyl or alkynylene" used in the present application may be a linear or branched non-cyclic alkynyl or alkynylene group having 2 to 20 carbon atoms, or 2 to 16 carbon atoms, or 2 to 12 carbon atoms, or 2 to 8 carbon atoms, or 2 to 6 carbon atoms; or a cyclic alkynyl or alkynylene group having 3 to 20 carbon atoms, or 3 to 16 carbon atoms, or 3 to 12 carbon atoms, or 3 to 8 carbon atoms, or 3 to 6 carbon atoms. Here, when the alkynyl or alkynylene group contains a ring structure, it corresponds to the cyclic alkynyl or alkynylene group.
[0020] The above-mentioned alkyl, alkylene, alkenyl, alkenylene, alkynyl, and alkynylene groups may be arbitrarily substituted with one or more substituents. In this case, the substituents may be one or more selected from halogen (chlorine (Cl), iodine (I), bromine (Br), fluorine (F)), aryl, heteroaryl, ether, carbonyl, carboxyl, and hydroxyl, but are not limited thereto.
[0021] The term "aryl" used in the present application refers to an aromatic ring obtained by removing a hydrogen from an aromatic hydrocarbon ring, and the aromatic hydrocarbon ring may include a monocyclic or polycyclic ring. The carbon number of the above-mentioned aryl is not particularly limited, but as long as it is not otherwise recorded, it can be an aryl with 6 to 30 carbon atoms, or 6 to 26 carbon atoms, or 6 to 22 carbon atoms, or 6 to 20 carbon atoms, or 6 to 18 carbon atoms, or 6 to 15 carbon atoms. In addition, the term "arylidene" used in the present application refers to a group with two binding positions on the aryl, i.e. a divalent group. They are each a divalent group, and in addition, the description of the above-mentioned aryl can be applied.
[0022] The term "heteroaryl" used in the present application is an aromatic ring containing one or more heteroatoms that are not carbon, specifically, the above-mentioned heteroatoms can contain one or more atoms selected from nitrogen (N), oxygen (O), sulfur (S), selenium (Se) and tellurium (Te). At this time, the atoms constituting the ring structure of the heteroaryl can be referred to as ring atoms. In addition, the heteroaryl can contain a monocyclic or polycyclic ring. The number of carbon atoms of the above-mentioned heteroaryl is not particularly limited, but as long as it is not otherwise recorded, it can be a heteroaryl with 2 to 30 carbon atoms, or 2 to 26 carbon atoms, or 2 to 22 carbon atoms, or 2 to 20 carbon atoms, or 2 to 18 carbon atoms, or 2 to 15 carbon atoms. In other examples, the number of ring atoms of the heteroaryl is not particularly limited, but can be a heteroaryl with 5 to 30, 5 to 25, 5 to 20, 5 to 15, 5 to 10 or 5 to 8 ring atoms.
[0023] In addition, the term "heteroarylene" used in the present application refers to a group having two bonding positions on a heteroaryl group, that is, a divalent group. Except that each of them is a divalent group, the above description of the heteroaryl group is applicable.
[0024] The term "acrylate compound" used in the present application refers to acrylic acid, methacrylic acid, a derivative of acrylic acid, or a derivative of methacrylic acid. In addition, the term "(meth)acryloyl" used in the present application refers to an acryloyl group or a methacryloyl group.
[0025] In one example of the present application, the adhesive composition includes a copolymer obtained by copolymerizing two or more monomers, and the monomers may include a monomer having a room temperature surface tension greater than 30 mN / m and a monomer having a room temperature surface tension less than 30 mN / m.
[0026] In addition, in one example of the present application, the room temperature surface tension of the copolymer of the adhesive composition can be less than 30 mN / m, less than 29.5 mN / m, less than 29 mN / m, less than 28.5 mN / m or less than 28 mN / m. In other examples, the room temperature surface tension of the copolymer of the above-mentioned adhesive composition can be greater than 20 mN / m, greater than 21 mN / m, greater than 22 mN / m or greater than 23 mN / m.
[0027] The room temperature surface tension of the adhesive composition can be affected by the room temperature surface tension of the copolymer included. In one example of the present application, the room temperature surface tension of the adhesive composition can be 30mN / m or less, 29.5mN / m or less, 29mN / m or less, 28.5mN / m or less, or 28mN / m or less. In other examples, the room temperature surface tension of the adhesive composition can be 20mN / m or more, 21mN / m or more, 22mN / m or more, or 23mN / m or more. When the room temperature surface tension of the adhesive composition meets the above range, the room temperature surface tension of the copolymer included in the adhesive composition can also meet the above range.
[0028] In one example of the present application, the monomers included in the adhesive composition may satisfy the following Formula 1.
[0029] [General formula 1]
[0030] 3≤A / B×100≤30
[0031] In Formula 1, A represents the weight of a monomer having a surface tension of greater than 30 mN / m at room temperature, and B represents the weight of a monomer having a surface tension of less than 30 mN / m at room temperature.
[0032] In addition, the value of A / B×100 in the general formula 1 may be 3 or more, 3.5 or more, 4 or more, 4.5 or more, 5 or more, 5.5 or more, or 6 or more. In other examples, the value of A / B×100 in the general formula 1 may be 30 or less, 28 or less, 26 or less, 24 or less, or 22 or less. In addition, the value of A / B×100 in the general formula 1 may be within a range formed by appropriately selecting the upper and lower limits listed above.
[0033] When the value of A / B×100 in General Formula 1 satisfies the above range, an adhesive composition having excellent wettability and light resistance and capable of covering steps and defects can be formed.
[0034] In one example of the present application, the monomers included in the adhesive composition may further include a monomer having a glass transition temperature greater than 10° C. and a monomer having a glass transition temperature less than 10° C.
[0035] In one example of the present application, the glass transition temperature of the copolymer of the adhesive composition can be below -25°C, below -26°C, below -27°C, below -28°C, below -29°C, below -30°C, below -31°C, below -32°C, below -33°C or below -34°C. In other examples, the glass transition temperature of the copolymer of the above-mentioned adhesive composition can be above -50°C, above -49.5°C, above -49°C or above -48.5°C.
[0036] The glass transition temperature of the adhesive composition may be affected by the glass transition temperature of the copolymer contained therein. In one example of the present application, the glass transition temperature of the adhesive composition may be below -25°C, below -26°C, below -27°C, below -28°C, below -29°C, below -30°C, below -31°C, below -32°C, below -33°C, or below -34°C. In other examples, the glass transition temperature of the adhesive composition may be above -50°C, above -49.5°C, above -49°C, or above -48.5°C. When the glass transition temperature of the adhesive composition satisfies the above range, the glass transition temperature of the copolymer contained in the adhesive composition may also satisfy the above range.
[0037] In one example of the present application, the monomers included in the adhesive composition may satisfy the following Formula 2.
[0038] [General formula 2]
[0039] 1≤C / D×100≤22
[0040] In Formula 2, C represents the weight of a monomer having a glass transition temperature greater than 10°C, and D represents the weight of a monomer having a glass transition temperature of 10°C.
[0041] In addition, the value of C / D×100 in the general formula 2 may be 1 or more, 1.5 or more, 2 or more, 2.5 or more, 3 or more, 3.5 or more, 4 or more, 4.5 or more, 5 or more, 5.5 or more, or 6 or more. In other examples, the value of C / D×100 in the general formula 2 may be 22 or less, 21 or less, 20 or less, 19 or less, or 18 or less. In addition, the value of C / D×100 in the general formula 2 may be within a range formed by appropriately selecting the upper and lower limits listed above.
[0042] When the value of C / D×100 in Formula 2 satisfies the above range, an adhesive composition having appropriate storage modulus and tensile modulus can be formed.
[0043] In another example of the present application, the adhesive composition includes a copolymer obtained by copolymerizing two or more monomers, and the copolymer has a room temperature surface tension of 30 mN / m or less and a glass transition temperature of -25°C or less.
[0044] In another example of the present application, the room temperature surface tension of the copolymer of the adhesive composition can be less than 30 mN / m, less than 29.5 mN / m, less than 29 mN / m, less than 28.5 mN / m or less than 28 mN / m. In other examples, the room temperature surface tension of the copolymer of the adhesive composition can be greater than 20 mN / m, greater than 21 mN / m, greater than 22 mN / m or greater than 23 mN / m.
[0045] The room temperature surface tension of the adhesive composition can be affected by the room temperature surface tension of the copolymer included. In one example of the present application, the room temperature surface tension of the adhesive composition can be 30mN / m or less, 29.5mN / m or less, 29mN / m or less, 28.5mN / m or less, or 28mN / m or less. In other examples, the room temperature surface tension of the above-mentioned adhesive composition can be 20mN / m or more, 21mN / m or more, 22mN / m or more, or 23mN / m or more. When the room temperature surface tension of the adhesive composition meets the above range, the room temperature surface tension of the copolymer included in the adhesive composition can also meet the above range.
[0046] In addition, the glass transition temperature of the copolymer of the adhesive composition can be below -25°C, below -26°C, below -27°C, below -28°C, below -29°C, below -30°C, below -31°C, below -32°C, below -33°C or below -34°C. In other examples, the glass transition temperature of the copolymer of the above-mentioned adhesive composition can be above -50°C, above -49.5°C, above -49°C or above -48.5°C.
[0047] The glass transition temperature of the adhesive composition may be affected by the glass transition temperature of the copolymer contained therein. In one example of the present application, the glass transition temperature of the adhesive composition may be below -25°C, below -26°C, below -27°C, below -28°C, below -29°C, below -30°C, below -31°C, below -32°C, below -33°C, or below -34°C. In other examples, the glass transition temperature of the adhesive composition may be above -50°C, above -49.5°C, above -49°C, or above -48.5°C. When the glass transition temperature of the adhesive composition satisfies the above range, the glass transition temperature of the copolymer contained in the adhesive composition may also satisfy the above range.
[0048] In another example of the present application, the monomers contained in the adhesive composition may include at least one of a first monomer or a second monomer, the first monomer includes a monomer having a surface tension greater than 30 mN / m at room temperature and a monomer having a surface tension less than 30 mN / m at room temperature; the second monomer includes a monomer having a glass transition temperature greater than 10°C and a monomer having a glass transition temperature less than 10°C.
[0049] The first monomer may satisfy the following general formula 1.
[0050] [General formula 1]
[0051] 3≤A / B×100≤30
[0052] In Formula 1, A represents the weight of a monomer having a surface tension of greater than 30 mN / m at room temperature, and B represents the weight of a monomer having a surface tension of less than 30 mN / m at room temperature.
[0053] In addition, the value of A / B×100 in the general formula 1 may be 3 or more, 3.5 or more, 4 or more, 4.5 or more, 5 or more, 5.5 or more, or 6 or more. In other examples, the value of A / B×100 in the general formula 1 may be 30 or less, 28 or less, 26 or less, 24 or less, or 22 or less. In addition, the value of A / B×100 in the general formula 1 may be within a range formed by appropriately selecting the upper and lower limits listed above.
[0054] When the value of A / B×100 in General Formula 1 satisfies the above range, an adhesive composition having excellent wettability and light resistance and capable of covering steps and defects can be formed.
[0055] The second monomer may satisfy the following general formula 2.
[0056] [General formula 2]
[0057] 1≤C / D×100≤22
[0058] In Formula 2, C represents the weight of a monomer having a glass transition temperature of more than 10°C, and D represents the weight of a monomer having a glass transition temperature of 10°C or less.
[0059] In addition, the value of C / D×100 in the general formula 2 may be 1 or more, 1.5 or more, 2 or more, 2.5 or more, 3 or more, 3.5 or more, 4 or more, 4.5 or more, 5 or more, 5.5 or more, or 6 or more. In other examples, the value of C / D×100 may be 22 or less, 21 or less, 20 or less, 19 or less, or 18 or less. In addition, the value of C / D×100 in the general formula 2 may be within a range formed by appropriately selecting the upper and lower limits listed above.
[0060] When the value of C / D×100 in Formula 2 satisfies the above range, an adhesive composition having appropriate storage modulus and tensile modulus can be formed.
[0061] In another example of the present application, the monomers contained in the adhesive composition may include monomers having a glass transition temperature greater than 10°C and a surface tension greater than 30 mN / m at room temperature, which is equivalent to a first monomer having a surface tension greater than 30 mN / m at room temperature or a second monomer having a glass transition temperature greater than 10°C.
[0062] The monomer having a glass transition temperature greater than 10°C and a room temperature surface tension greater than 30 mN / m may contain 0.5 wt% or more, 0.75 wt% or more, 1 wt% or more, 1.25 wt% or more, 1.5 wt% or more, or 1.75 wt% or more relative to the total weight of the monomer. In other examples, the monomer having a glass transition temperature greater than 10°C and a room temperature surface tension greater than 30 mN / m may contain 18 wt% or less, 17 wt% or less, 16 wt% or less, or 15 wt% or less relative to the total weight of the monomer. In addition, the monomer having a glass transition temperature greater than 10°C and a room temperature surface tension greater than 30 mN / m may be included in the range formed by appropriately selecting the upper and lower limits listed above.
[0063] In addition, in another example of the present application, the monomers contained in the adhesive composition may further include monomers having a glass transition temperature below 10°C and a surface tension below 30 mN / m at room temperature, which is equivalent to a first monomer having a surface tension below 30 mN / m at room temperature or a second monomer having a glass transition temperature below 10°C.
[0064] The monomer having a glass transition temperature of 10°C or less and a surface tension of 30 mN / m or less at room temperature may contain 450 parts by weight or more, 475 parts by weight or more, 500 parts by weight or more, 525 parts by weight or more, 550 parts by weight or more, or 575 parts by weight or more, relative to 100 parts by weight of the monomer having a glass transition temperature of greater than 10°C and a surface tension of greater than 30 mN / m at room temperature. In other examples, the monomer having a glass transition temperature of less than 10°C and a surface tension of 30 mN / m or less at room temperature may contain 6000 parts by weight or less, 5800 parts by weight or less, 5600 parts by weight or less, 5400 parts by weight or less, 5200 parts by weight or less, 5000 parts by weight or less, or 4800 parts by weight or less, relative to 100 parts by weight of the monomer having a glass transition temperature of greater than 10°C and a surface tension of greater than 30 mN / m at room temperature. Furthermore, the monomer having a glass transition temperature of 10° C. or lower and a room-temperature surface tension of 30 mN / m or lower may be included in a range formed by appropriately selecting the upper and lower limits listed above.
[0065] When the adhesive composition contains a monomer having a glass transition temperature greater than 10°C and a surface tension greater than 30 mN / m at room temperature and / or a monomer having a glass transition temperature below 10°C and a surface tension below 30 mN / m at room temperature in the above content range, excellent wettability and light resistance can be ensured.
[0066] In one example of the present application, the adhesive composition may contain a specific compound group, which means that it may contain one or more compounds that satisfy the above-mentioned specific compound group. For example, the adhesive composition contains a chain alkyl acrylate compound containing a compound represented by the following chemical formula 1, which means that the above-mentioned adhesive composition may contain one or more compounds that satisfy the structure of the compound represented by the following chemical formula 1.
[0067] In one example of the present application, the monomer having a room-temperature surface tension of 30 mN / m or less of the adhesive composition may include a chain alkyl acrylate compound.
[0068] The term "chain alkyl acrylate compound" used in the present application may refer to an acrylate compound containing a chain alkyl group. Here, the chain alkyl group may refer to a linear alkyl group or a branched alkyl group.
[0069] The chain alkyl group may be a linear or branched alkyl group having 1 to 30 carbon atoms, 1 to 25 carbon atoms, 1 to 20 carbon atoms, 1 to 15 carbon atoms, or 1 to 10 carbon atoms.
[0070] The surface tension of the linear alkyl acrylate compound at room temperature may be 30 mN / m or less, 29 mN / m or less, 28 mN / m or less, 27 mN / m or less, 26 mN / m or less, or 25 mN / m or less.
[0071] The glass transition temperature of the linear alkyl acrylate compound may be -20°C or lower, -30°C or lower, -40°C or lower, or -50°C or lower.
[0072] The linear alkyl acrylate compound may include one or more compounds represented by the following Chemical Formula 1.
[0073] [Chemical formula 1]
[0074]
[0075] In Chemical Formula 1, L1 is a linear alkylene group having 1 to 14 carbon atoms or a branched alkylene group having 2 to 14 carbon atoms, and R1 and R2 may each independently be hydrogen, a linear alkyl group having 1 to 6 carbon atoms, or a branched alkyl group having 2 to 6 carbon atoms.
[0076] In other examples, L1 may be a linear alkylene group having 1 or more, 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, or 7 or more carbon atoms, or a branched alkylene group having 2 or more, 3 or more, 4 or more, 5 or more, 6 or more, or 7 or more carbon atoms. In another example, L1 may be a linear or branched alkylene group having 14 or less, 13 or less, 12 or less, 11 or less, 10 or less, 9 or less, or 8 or less carbon atoms. L1 may be a linear or branched alkylene group having a carbon number within a range formed by appropriately selecting the upper and lower limits of the carbon number listed above.
[0077] In addition, in other examples, R1 and R2 can each independently be hydrogen, a straight-chain alkyl group having 1 to 4 carbon atoms, or a branched-chain alkyl group having 2 to 4 carbon atoms. In other examples, R1 and R2 can each independently be hydrogen or a straight-chain alkyl group having 1 to 2 carbon atoms.
[0078] The compound represented by the above Chemical Formula 1 may have a room temperature surface tension of 30 mN / m or less, 29 mN / m or less, 28 mN / m or less, 27 mN / m or less, 26 mN / m or less, or 25 mN / m or less.
[0079] In addition, the glass transition temperature of the compound represented by the above Chemical Formula 1 may be -20°C or less, -30°C or less, -40°C or less, or -50°C or less.
[0080] The compound represented by the above Chemical Formula 1 may be exemplified by isobutyl acrylate, isodecyl acrylate, isooctyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and the like, and is not particularly limited thereto as long as the above-mentioned physical properties are satisfied.
[0081] In one example of the present application, the chain alkyl acrylate compound may contain 55% by weight or more, 57.5% by weight or more, 60% by weight or more, 62.5% by weight or more, or 65% by weight or more relative to the total weight of the monomer having a surface tension of 30 mN / m or less at room temperature. In other examples, the chain alkyl acrylate compound may contain 98% by weight or less, 97% by weight or less, 96% by weight or less, or 95% by weight or less relative to the total weight of the monomer having a surface tension of 30 mN / m or less at room temperature. In addition, the chain alkyl acrylate compound may be contained within the range formed by appropriately selecting the upper and lower limits listed above.
[0082] In another example of the present application, the chain alkyl acrylate compound may contain 55% by weight or more, 57.5% by weight or more, 60% by weight or more, 62.5% by weight or more, or 65% by weight or more relative to the total weight of the monomer having a surface tension of 30 mN / m or less at room temperature. In other examples, the chain alkyl acrylate compound may contain 70% by weight or less, 69% by weight or less, or 68% by weight or less relative to the total weight of the monomer having a surface tension of 30 mN / m or less at room temperature. In addition, the chain alkyl acrylate compound may be contained within the range formed by appropriately selecting the upper and lower limits listed above.
[0083] In one example of the present application, the monomer having a room-temperature surface tension of 30 mN / m or less of the adhesive composition may include a hydroxyl-containing acrylate compound.
[0084] The room temperature surface tension of the hydroxyl-containing acrylate compound may be 30 mN / m or less, 29 mN / m or less, or 28 mN / m or less.
[0085] The glass transition temperature of the linear alkyl acrylate compound may be 0°C or lower, -5°C or lower, -10°C or lower, or -15°C or lower.
[0086] The hydroxyl-containing acrylate compound may be any acrylate compound having a hydroxyl group and satisfying the above-mentioned physical properties, and the type thereof is not particularly limited.
[0087] The hydroxyl-containing acrylate compound may include one or more compounds represented by the following Chemical Formula 2.
[0088] [Chemical formula 2]
[0089]
[0090] In Chemical Formula 2, L2 can be a linear alkylene group having 1 to 10 carbon atoms, a branched alkylene group having 2 to 10 carbon atoms, a linear or branched alkenylene group having 2 to 10 carbon atoms, or a linear or branched alkynylene group having 2 to 10 carbon atoms.
[0091] In one example, L2 may be a linear alkylene group having 1 or more, 2 or more, 3 or more, or 4 or more carbon atoms, and in another example, L2 may be a linear alkylene group having 10 or less, 9 or less, 8 or less, 7 or less, 6 or less, or 5 or less carbon atoms. L2 may be a linear alkylene group having a carbon number within a range formed by appropriately selecting the upper and lower limits of the carbon number listed above.
[0092] In another example, L2 may be a branched alkylene group having 2 or more, 3 or more, or 4 or more carbon atoms; a straight or branched alkenylene group; or a straight or branched alkynylene group. In another example, L2 may be a branched alkylene group having 10 or less, 9 or less, 8 or less, 7 or less, 6 or less, or 5 or less carbon atoms; a straight or branched alkenylene group; or a straight or branched alkynylene group. L2 may be a branched alkylene group, a straight or branched alkenylene group, or a straight or branched alkynylene group having a carbon number within the range formed by appropriately selecting the upper and lower limits of the carbon number listed above.
[0093] The surface tension of the compound represented by the above Chemical Formula 2 at room temperature may be 30 mN / m or less, 29 mN / m or less, or 28 mN / m or less.
[0094] In addition, the glass transition temperature of the compound represented by the above Chemical Formula 2 may be 0° C. or less, -5° C. or less, -10° C. or less, or -15° C. or less.
[0095] Examples of the compound represented by the chemical formula 2 include 2-hydroxyethyl acrylate, 4-hydroxybutyl acrylate, 2-hydroxypropyl acrylate, and 2-hydroxy-1-methylethyl acrylate, but are not particularly limited thereto as long as the above-mentioned physical properties are satisfied.
[0096] In one example of the present application, the hydroxyl-containing acrylate compound may contain 1% by weight or more, 2% by weight or more, 3% by weight or more, 4% by weight or more, or 5% by weight or more relative to the total weight of the monomer having a surface tension of 30 mN / m or less at room temperature. In other examples, the hydroxyl-containing acrylate compound may contain 40% by weight or less, 38.5% by weight or less, 37% by weight or less, or 35.5% by weight or less relative to the total weight of the monomer having a surface tension of 30 mN / m or less at room temperature. In addition, the above-mentioned hydroxyl-containing acrylate compound may be included in the range formed by appropriately selecting the upper and lower limits listed above.
[0097] In another example of the present application, the hydroxyl-containing acrylate compound may contain 30% by weight or more, 30.5% by weight or more, 31% by weight or more, or 31.5% by weight or more relative to the total weight of the monomer having a surface tension of 30 mN / m or less at room temperature. In other examples, the hydroxyl-containing acrylate compound may contain 40% by weight or less, 38.5% by weight or less, 37% by weight or less, or 35.5% by weight or less relative to the total weight of the monomer having a surface tension of 30 mN / m or less at room temperature. In addition, the above-mentioned hydroxyl-containing acrylate compound may be included in the range formed by appropriately selecting the upper and lower limits listed above.
[0098] In one example of the present application, the monomer having a room-temperature surface tension of 30 mN / m or less of the adhesive composition may include a chain alkyl acrylate compound and a hydroxyl-containing acrylate compound.
[0099] In this case, the weight ratio (P / R) of the linear alkyl acrylate compound (P) to the hydroxyl-containing acrylate compound (R) may be 1 or more, 1.2 or more, 1.4 or more, 1.6 or more, or 1.8 or less, 20 or less, 19.5 or less, 19 or less, or 18.5 or less. In addition, the weight ratio (P / R) of the linear alkyl acrylate compound (P) to the hydroxyl-containing acrylate compound (R) may be within a range formed by appropriately selecting the upper and lower limits listed above.
[0100] In other examples, the weight ratio (P / R) of the linear alkyl acrylate compound (P) to the hydroxyl-containing acrylate compound (R) may be 1 or more, 1.2 or more, 1.4 or more, 1.6 or more, or 1.8 or less, 3.6 or less, 3.2 or less, 2.8 or less, or 2.4 or less. In addition, the weight ratio (P / R) of the linear alkyl acrylate compound (P) to the hydroxyl-containing acrylate compound (R) may be within the range formed by appropriately selecting the upper and lower limits listed above.
[0101] When the weight ratio (P / R) of the linear alkyl acrylate compound (P) to the hydroxyl-containing acrylate compound (R) satisfies the above range, appropriate stability can be achieved and generation of bubbles or floating between laminated layers can be prevented.
[0102] In one example of the present application, the monomer having a room-temperature surface tension greater than 30 mN / m of the adhesive composition may include a cyclic alkyl acrylate compound.
[0103] The room temperature surface tension of the cyclic alkyl acrylate compound may be greater than 30 mN / m, 31 mN / m or more, 32 mN / m or more, or 33 mN / m or more.
[0104] The cyclic alkyl acrylate compound may have a glass transition temperature of 50° C. or higher, 55° C. or higher, 60° C. or higher, 65° C. or higher, 70° C. or higher, or 75° C. or higher.
[0105] The cyclic alkyl acrylate compound may be any acrylate compound having a cyclic alkyl group and satisfying the above-mentioned physical properties, and examples thereof include isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate, and tert-butylcyclohexyl (meth)acrylate, and the type thereof is not particularly limited.
[0106] In one example of the present application, the cyclic alkyl acrylate compound may include 10 to 100 wt %, 15 to 100 wt %, or 20 to 100 wt % relative to the total weight of the monomer having a surface tension greater than 30 mN / m at room temperature.
[0107] In one example of the present application, the monomer having a room temperature surface tension of 30 mN / m or less of the adhesive composition includes a hydroxyl-containing acrylate compound, and the monomer having a room temperature surface tension of the adhesive composition greater than 30 mN / m may include a cyclic alkyl acrylate compound. Here, the hydroxyl-containing acrylate compound and the cyclic alkyl acrylate compound are the same as described above.
[0108] In one example of the present application, the weight ratio (R / Q) of the hydroxyl-containing acrylate compound (R) to the cyclic alkyl acrylate compound (Q) may be 1.2 or more, 1.3 or more, 1.4 or more, 1.5 or more, 1.6 or more, 1.7 or more, or 1.8 or less, and may be 10 or less, 9 or less, 8 or less, 7 or less, or 6 or less. In addition, the weight ratio (R / Q) of the hydroxyl-containing acrylate compound (R) to the cyclic alkyl acrylate compound (Q) may be within the range formed by appropriately selecting the upper and lower limits listed above.
[0109] When the weight ratio (R / Q) of the hydroxyl-containing acrylate compound (R) to the cyclic alkyl acrylate compound (Q) satisfies the above range, the basic required physical properties such as durability and adhesion are met, and the generation of bubbles or floating between laminated layers can be minimized.
[0110] In one example of the present application, the monomer having a room-temperature surface tension greater than 30 mN / m of the adhesive composition may include an acrylate compound containing a cyclic ether group.
[0111] The room temperature surface tension of the cyclic ether group-containing acrylate compound may be greater than 30 mN / m, 30.5 mN / m or more, or 31 mN / m or more.
[0112] The glass transition temperature of the cyclic ether group-containing acrylate compound may be 10° C. or lower, 5° C. or lower, 0° C. or lower, -5° C. or lower, or -10° C. or lower.
[0113] The cyclic ether group-containing acrylate compound may include one or more compounds represented by the following Chemical Formula 3.
[0114] [Chemical formula 3]
[0115]
[0116] In Chemical Formula 3, R3 may be hydrogen or a linear alkyl group having 1 to 20 carbon atoms. In addition, L3 and L4 may each independently be a single bond or a linear alkylene group having 1 to 20 carbon atoms. In addition, L5 may be a single bond or a linear alkylene group having 1 to 8 carbon atoms. In addition, Q may be an oxygen atom or a carbon atom.
[0117] In other examples, L3 and L4 in Chemical Formula 3 may each independently be a linear alkylene group having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, 2 to 8 carbon atoms, 2 to 6 carbon atoms, or 2 to 4 carbon atoms. In addition, L5 may be a single bond or a linear alkylene group having 1 to 4 carbon atoms, for example, a single bond.
[0118] In addition, the sum of the number of carbon atoms present in L4 and L5 in Chemical Formula 3 may be in the range of 1 to 8. The sum of the number of carbon atoms may be 7 or less, 6 or less, 5 or less, 4 or less, or 3 or less, or 1 or more, 2 or more, or 3 or more. The sum of the number of carbon atoms of L4 and L5 is the number of carbon atoms of the alkylene group of L5 when L5 is an alkylene group and L4 is a single bond, and is the sum of the number of carbon atoms of the alkylene group of L5 and the number of carbon atoms of the alkylene group of L4 when L5 is an alkylene group and L4 is also an alkylene group. In addition, when a substituent is present in the alkylene group, the number of carbon atoms present in the substituent is not included in the above “and”.
[0119] The surface tension of the compound represented by the above Chemical Formula 3 at room temperature may be greater than 30 mN / m, 30.5 mN / m or more, or 31 mN / m or more.
[0120] In addition, the glass transition temperature of the compound represented by the above Chemical Formula 3 may be 10° C. or less, 5° C. or less, 0° C. or less, -5° C. or less, or -10° C. or less.
[0121] The compound represented by the above chemical formula 3 may be exemplified by oxiranyl (meth)acrylate, oxetanyl (meth)acrylate, tetrahydrofuranyl (meth)acrylate, tetrahydro-2H-pyranyl (meth)acrylate, oxiranylmethyl (meth)acrylate (or glycidyl (meth)acrylate), oxetanylethyl (meth)acrylate, and tetrahydrofuranylmethyl (meth)acrylate (or tetrahydrofurfuryl (meth)acrylate), etc., and is not particularly limited thereto as long as the above-mentioned physical properties are satisfied.
[0122] In one example of the present application, the acrylate compound containing a cyclic ether group, when included in the adhesive composition, may contain 35% by weight or more, 40% by weight or more, 45% by weight or more, 50% by weight or more, 55% by weight or more, or 60% by weight or more relative to the total weight of the monomer having a surface tension greater than 30 mN / m at room temperature. In other examples, the acrylate compound containing a cyclic ether group may contain 80% by weight or less, 75% by weight or less, 70% by weight or less, or 65% by weight or less relative to the total weight of the monomer having a surface tension greater than 30 mN / m at room temperature. In addition, the above-mentioned acrylate compound containing a cyclic ether group may be included in the range formed by appropriately selecting the upper and lower limits listed above.
[0123] In one example of the present application, the monomer having a room-temperature surface tension greater than 30 mN / m of the adhesive composition may include an acrylate compound containing a cyclic ether group and a compound containing an acrylamide group.
[0124] The room temperature surface tension of the acrylamide group-containing compound may be greater than 30 mN / m, 33 mN / m or more, 35 mN / m or more, or 37 mN / m or more.
[0125] In addition, the glass transition temperature of the acrylamide group-containing compound may be 80° C. or higher, 90° C. or higher, 100° C. or higher, or 110° C. or higher.
[0126] The acrylamide group-containing compound may be any compound having an acrylamide group and satisfying the above-mentioned physical properties, and examples thereof include N,N-dimethylacrylamide, N,N-methylethylacrylamide, and N,N-diethylacrylamide, and the type thereof is not particularly limited.
[0127] In one example of the present application, the acrylamide group-containing compound may contain more than 10 parts by weight, more than 15 parts by weight, more than 20 parts by weight, more than 25 parts by weight, or more than 30 parts by weight relative to 100 parts by weight of the acrylate compound containing a cyclic ether group. In other examples, it may contain less than 90 parts by weight, less than 80 parts by weight, less than 70 parts by weight, less than 60 parts by weight, less than 50 parts by weight, or less than 40 parts by weight.
[0128] In one example of the present application, the adhesive composition may further include a photoinitiator in order to utilize active energy rays for curing. Here, the photoinitiator may be selected in consideration of the high absorptivity near the emission spectrum of the active energy rays and the compatibility between the above-mentioned compounds. For the rapid curing of the adhesive composition, the above-mentioned active energy rays are preferably ultraviolet rays.
[0129] The photoinitiator may be one or more selected from benzophenone-based initiators and α-hydroxyketone initiators, preferably α-hydroxyketone initiators. Specifically, the photoinitiator may include at least one of 1-hydroxy-cyclohexylphenyl ketone, 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone and 1-hydroxy-1-methylethyl phenyl ketone in α-hydroxyketone initiators, but is not limited thereto.
[0130] The content of the photoinitiator is not particularly limited as long as the adhesive composition can be properly cured, but may be 0.01 wt % or more, 0.015 wt % or more, 0.02 wt % or more, or 0.025 wt % or more relative to the total weight of the adhesive composition. In other examples, it may be 0.05 wt % or less, 0.04 wt % or less, or 0.03 wt % or less.
[0131] The adhesive composition containing the photoinitiator can be cured by active energy rays. As mentioned above, the active energy rays can be ultraviolet rays. The light intensity of the ultraviolet rays can be 5 J / cm 2 Above, 6J / cm 2 Above, 7J / cm 2 Above, 8J / cm 2 Above, 9J / cm 2 Above or 10J / cm 2In other examples, it can be 20 J / cm 2 Below, 18J / cm 2 Below, 16J / cm 2 Below, 14J / cm 2 Below or 12J / cm 2 The curing time refers to the time until the adhesive composition is completely cured, and may vary depending on the thickness of the adhesive composition and the amount of light of the ultraviolet rays.
[0132] If necessary, according to the adhesive composition of the present application, a leveling agent, an adhesion imparting agent, a coupling agent and a viscosity modifier etc. may be further included. For example, a viscosity modifier may be further included in order to increase or reduce the viscosity, or in order to adjust the viscosity according to the shear force, for example, a plasticizer, a thixotropic agent, a diluent or a dispersant etc. may be included. A thixotropic agent may be used to adjust the viscosity according to the shear force of the adhesive composition. As usable thixotropic agents, fumed silica, bentonite etc. may be exemplified. As long as it is a diluent or a dispersant that is commonly used to reduce the viscosity of the adhesive composition, the diluent or dispersant that can show the effect as described above may be used in the art without limitation.
[0133] The adhesive composition may include the above-mentioned constitution and may be a solvent-based composition, a water-based composition or a solvent-free composition. However, in consideration of the convenience of the production process, a solvent-free composition may be suitable.
[0134] The adhesive composition can be formed by mixing the above-mentioned constituent elements, and the mixing order is not particularly limited as long as all the necessary components are contained.
[0135] In one example of the present application, the film may be the cured product of the above-mentioned adhesive composition itself, or may include the cured product of the above-mentioned adhesive composition. In addition, the film may have at least one of the following properties and may be used as an optically clear adhesive (OCA).
[0136] In one example of the present application, the film is used as an optical adhesive for a display product or a transparent electrode product, thereby covering defects between laminated layers of the display product or the transparent electrode product and preventing bubbles from being formed therefrom.
[0137] The following properties are independent, so that no property takes precedence over other properties, and the film may satisfy at least one or two or more of the following properties. A film satisfying at least one or more of the following properties is produced by combining the constituent elements of the adhesive composition.
[0138] The room temperature adhesive force of the film may be 0.7 kg / inch or more, 0.75 kg / inch or more, or 0.8 kg / inch or more. The room temperature adhesive force may be a value obtained by measuring the cured product of the adhesive composition on a PET (polyethylene terephthalate) film, using an adhesive force measuring device, at a peeling speed of 300 mm / min and a peeling angle of 180° at room temperature. In addition, the room temperature at this time may refer to about 25°C.
[0139] In addition, the tensile modulus of the film can be 0.002kgf / mm 2 Above, 0.003kgf / mm 2 Above, 0.004kgf / mm 2 Above, 0.005kgf / mm 2 Above or 0.006kgf / mm 2 In other examples, it can be 0.012 kgf / mm 2 Below, 0.011kgf / mm 2 Below, 0.01kgf / mm 2 Below or 0.009kgf / mm 2 In addition, the tensile modulus of the film may be within a range formed by appropriately selecting the upper and lower limits listed above. In this case, the tensile modulus may be defined as σ / ε, where σ is tensile stress / cross-sectional area, and ε may be a value from the strain at which the film breaks to the gauge length (initial strain) / gauge length.
[0140] In addition, the film may have a room temperature storage modulus of 0.1 MPa or less, and a 80° C. storage modulus of 0.055 MPa or less. That is, the film may have a room temperature storage modulus of 0.1 MPa or less, and a 80° C. storage modulus of 0.055 MPa or less.
[0141] The room temperature storage modulus of the above-mentioned film can be 0.1MPa or less, 0.09MPa or less, 0.08MPa or less, 0.07MPa or less, or 0.06MPa or less. In other examples, the room temperature storage modulus of the above-mentioned film can be 0.02MPa or more, 0.025MPa or more, 0.03MPa or more, 0.035MPa or more, 0.04MPa or more, or 0.045MPa or more. In addition, the room temperature at this time can refer to about 25°C, and the room temperature storage modulus of the above-mentioned film can be within the range formed by appropriately selecting the upper and lower limits listed above.
[0142] In addition, the 80°C storage modulus of the film may be 0.055 MPa or less, 0.0525 MPa or less, or 0.05 MPa or less. In other examples, the 80°C storage modulus of the film may be 0.005 MPa or more, 0.0075 MPa or more, 0.01 MPa or more, or 0.0125 MPa or more. In addition, the 80°C storage modulus of the film may be within a range formed by appropriately selecting the upper and lower limits listed above.
[0143] When the tensile modulus and storage modulus (normal temperature and 80° C.) of the film satisfy the above ranges, excellent stability can be ensured in high temperature, low temperature, thermal shock, and high temperature / high humidity evaluations.
[0144] The wetting time (wet-time) measured according to the wettability evaluation procedure described below for the film may be 60 seconds or less.
[0145] [Wettability evaluation process]
[0146] 1) The adhesive composition was placed between a first light release film and a heavy release film so as to have a predetermined thickness, and the adhesive composition was cured to produce a cured product sample.
[0147] 2) The first light release film of the cured sample was removed, and a second light release film was attached to one surface of the cured sample from which the first light release film was removed so as to overlap the cured sample to 0.2 cm in the length direction. Thus, an evaluation sample was prepared.
[0148] 3) The evaluation sample is gently placed on one surface of the glass substrate in such a manner that the second light peeling release film is in contact with the glass substrate, and the portion of the evaluation sample that is not attached to the second light peeling release film and is exposed is attached in such a manner that it is in contact with the glass substrate from the end of the cured sample to 0.2 cm in the length direction.
[0149] 4) The time elapsed from the time when the exposed portion of the evaluation sample is attached to the glass substrate in a manner of contacting the glass substrate from the end to about 0.5 cm in the length direction to the time when the above-mentioned exposed portion is in contact with the glass substrate from the end to about 2 cm in the length direction is measured as the wetting time.
[0150] After laminating the film and polarizing plate, even at about 830 to 1000 W / m 2 Even after being exposed to the same amount of light for about 500 hours, no bubbles will be generated.
[0151] At this time, the polarizing plate is not particularly limited as long as it is the polarizing plate mainly used in this field, and can have a structure in which a protective film, a TAC (tri-acetyl-cellulose) film, a PVA (poly vinyl alcohol) film, a TAC film, a PSA (pressure sensitive adhesives) film and a release film are stacked in this order.
[0152] In one example of the present application, a display or a transparent electrode may include the above-mentioned film as an adhesive layer. In addition, a display may include a transparent electrode including the film.
[0153] A display (or display product) or a transparent electrode product (display including a transparent electrode) includes a film covering foreign matter, thereby satisfying basic required physical properties such as durability and adhesion, and at the same time, minimizing the generation of bubbles or floating between laminated layers. Here, the display can be exemplified by CRT (cathode ray tube) display; PDP (plasma display panel), LCD (liquid crystal display), LED (light emitting diode) display; OLED (organic emitting diode) display and quantum dot display, but is not limited thereto. In addition, transparent electrode products can be exemplified as displays containing transparent electrodes, wherein the transparent electrode refers to an electrode material having high electrical conductivity and high transmittance in the visible light region formed on a transparent rigid substrate such as a glass substrate and a flexible substrate such as PET (polyethylene terephthalate), PES (polyether sulfone) and PEN (Polyethylene naphthalate).
[0154] The present application can provide an adhesive composition for forming an optical adhesive that has excellent wettability and light resistance and can cover steps and defects.
[0155] The present application can provide an adhesive composition for forming an optical adhesive that satisfies basic physical properties such as durability and adhesive strength and can minimize the generation of bubbles or floating between laminated layers.
[0156] In addition, the present application may provide a film capable of covering defects located between laminated layers of a display product or a transparent electrode product. BRIEF DESCRIPTION OF THE DRAWINGS
[0157] Figure 1 The graph shows the storage modulus, loss modulus, and tangent value (tan δ) of the cured product of the adhesive composition according to Example 1 as a function of temperature within a temperature range of -50°C to 120°C.
[0158] Figure 2 The graph shows the storage modulus, loss modulus, and tangent value (tan δ) of the cured product of the adhesive composition according to Example 2 as a function of temperature within a temperature range of -50°C to 120°C.
[0159] Figure 3 The graph shows the storage modulus, loss modulus, and tangent value (tan δ) of the cured product of the adhesive composition according to Comparative Example 1 as a function of temperature within a temperature range of -50°C to 120°C.
[0160] Figure 4 The graph shows the storage modulus, loss modulus, and tangent value (tan δ) of the cured product of the adhesive composition according to Comparative Example 3 as a function of temperature within a temperature range of -50°C to 120°C.
[0161] Figure 5 : is a photograph showing the relationship between a glass substrate and the cured adhesive composition after the light resistance evaluation of the adhesive composition according to Example 1.
[0162] Figure 6 : is a photograph showing the relationship between a glass substrate and the cured adhesive composition after the light resistance evaluation of the adhesive composition according to Example 2 was performed.
[0163] Figure 7 This is a photograph showing the relationship between a glass substrate and the cured adhesive composition after the light resistance of the adhesive composition according to Comparative Example 1 was evaluated.
[0164] Figure 8 This is a photograph showing the relationship between a glass substrate and the cured adhesive composition after the light resistance evaluation of the adhesive composition according to Comparative Example 2 was performed.
[0165] Fig. 9 This is a photograph showing the relationship between a glass substrate and the cured adhesive composition after the light resistance of the adhesive composition according to Comparative Example 3 was evaluated.
[0166] Fig.10 This is a photograph showing the relationship between a glass substrate and the cured adhesive composition after the light resistance evaluation of the adhesive composition according to Comparative Example 4 was performed. DETAILED DESCRIPTION
[0167] Hereinafter, the present application will be described by way of Examples and Comparative Examples, but the scope of the present application is not limited to the contents indicated below.
[0168] <Physical Property Measurement Methods>
[0169] 1. Tensile modulus determination method
[0170] The adhesive composition was placed between release films in a manner to have a thickness of 200 μm, and an ultraviolet lamp was used to irradiate the adhesive composition at 9 to 11 J / cm 2 The sample was cured by photocuring under a light intensity of 2.5 cm, cut into 2.5 cm wide, 7 cm long (gauge length 3.5 cm) and 200 μm thick, and then deformed in the longitudinal direction at a speed of 300 mm / min until it broke. The strain (△l), unit: mm) and tensile stress (tensile stress (F), unit: kgf) at this time were measured, and the tensile modulus (unit: kgf / mm) was calculated. 2 ).
[0171] Here, the tensile modulus is defined as σ / ε. σ is defined as F / A, where F (Tensile stress) is the tensile stress and A is the cross-sectional area. ε is defined as △l / l, where △l is the difference between the strain at which the sample breaks and the gauge length (initial strain), and l is the gauge length.
[0172] The adhesive composition was placed between the light release film and the heavy release film in a manner of having a thickness of 200 μm, and an ultraviolet lamp was used to irradiate the film at 9 to 11 J / cm 2 After the curing, the film was cut into pieces with a width of 2.5 cm, a length of 11 cm and a thickness of 325 μm, thereby manufacturing a cured product sample.
[0173] The peelable release film of the cured sample was removed, and a PET (polyethylene terephthalate) film with a width of more than 2.5 cm, a length of 25 cm, and a thickness of 75 μm was attached to the surface from which the peelable release film was removed. The cured sample with the PET film attached was cut into a width of 2.5 cm, a length of 25 cm, and a thickness of 350 μm.
[0174] Then, the cut solidified sample was attached so that the surface from which the cut solidified sample was removed was in contact with one surface of a glass substrate (Corning, product name: Eagle XG glass) having a width of 12.5 cm, a length of 12.5 cm, and a thickness of 700 μm. The glass substrate and the cut solidified sample were attached using a roller of about 2 kg, and after attachment, they were left at room temperature for about 30 minutes.
[0175] Then, the PET film was controlled by an adhesive strength measuring device (Dayuan Technology Co., Ltd., model name: TW-D2000) and peeled at a peeling speed of 300 mm / min and a peeling angle of 180° at room temperature to measure the adhesive strength. The adhesive strength measured by repeated experiments is expressed as an average value.
[0176] 2. Wettability evaluation method - wetting time measurement
[0177] Next, the wettability evaluation process was carried out under normal temperature and humidity conditions.
[0178] The adhesive composition was placed between a first light release film having a width of 42.0 cm, a length of 1000 cm, and a thickness of 50 μm and a heavy release film having a width of 42.0 cm, a length of 1000 cm, and a thickness of 75 μm in a manner of having a thickness of 200 μm. Then, an ultraviolet lamp was used to heat the film at 9 to 11 J / cm 2 The adhesive composition was cured by photocuring under a light intensity of , and the cured product sample was manufactured by cutting into a piece with a width of 2 cm, a length of 4 cm, and a thickness of 325 μm.
[0179] The first light release film was removed, and a second light release film having a width of 2.0 cm, a length of 4.0 cm, and a thickness of 50 μm was attached to one surface of the cured sample from which the first light release film was removed in an overlapping manner from the end of the cured sample to 0.2 cm in the length direction, thereby manufacturing an evaluation sample. That is, in the evaluation sample, the heavy release film was attached to the entire surface of one surface of the cured sample, and on the other surface, the second light release film was attached in an overlapping manner from the end of the cured sample to 0.2 cm in the length direction, and the portion without overlapping had a structure in which the cured sample was exposed.
[0180] The evaluation sample was gently placed on one surface of a glass substrate (Corning, product name: Eagle XG glass) cut to 12.5 cm in width, 12.5 cm in length and 700 μm in thickness, with the second light release film in contact with the glass substrate.
[0181] Then, the evaluation sample was attached so that it was in contact with the glass substrate from the end of the exposed cured sample to 0.2 cm in the length direction. That is, the exposed cured sample of the evaluation sample was attached so that it was in contact with the glass substrate from the end to about 0.2 cm.
[0182] The wet time was measured as the time from the time when the exposed portion of the evaluation sample was attached to the glass substrate in a manner of contacting the glass substrate from the end to about 0.5 cm in the length direction to the time when the exposed portion was in contact with the glass substrate from the end to 2 cm in the length direction.
[0183] Based on the measured elapsed time, wettability was evaluated according to the following criteria.
[0184] PASS: The elapsed time (wet-time) is less than 60 seconds
[0185] NG: Elapsed time (wet-time) is greater than 60 seconds
[0186] 3. Lightfastness evaluation method
[0187] The adhesive composition was placed between the light release film and the heavy release film in a manner of having a thickness of 200 μm, and an ultraviolet lamp was used to irradiate the film at 9 to 11 J / cm 2 After the curing, the film was cut into pieces with a width of 10 cm, a length of 10 cm and a thickness of 325 μm, thereby manufacturing a cured product sample.
[0188] The light release film of the cured sample was removed, and the cured sample was attached to one surface of a glass substrate (Corning, product name: Eagle XG glass) having a width of 10 cm, a length of 10 cm, and a thickness of 700 μm in such a manner that the cured sample was in contact with the surface from which the light release film was removed. A roller weighing about 2 kg was used to attach the glass substrate and the cured sample.
[0189] A polarizing plate having a structure in which a protective film, a TAC (tri-acetyl-cellulose) film, a PVA (polyvinyl alcohol) film, a TAC film, a PSA (pressure sensitive adhesives) film, and a release film are stacked in this order and having a width of 10 cm, a length of 10 cm, and a thickness of 258 μm is prepared, and the protective film is removed.
[0190] The heavy release film of the cured sample attached to the glass substrate was removed, and the samples were laminated using a nip roller so that the TAC film surface of the polarizing plate from which the protective film was removed came into contact with the surface from which the heavy release film was removed, thereby producing a laminated sample.
[0191] Then, in a vacuum lamination device (MRK company, product name: M-Tool vacuum laminator & autoclave) that can create a vacuum environment of about 97 kPa, the glass substrate of the laminated sample was placed facing the bottom, the release film of the polarizing plate was removed, and the PSA film was exposed. A glass substrate (Corning Incorporated, product name: Eagle XG glass) with a width of 10 cm, a length of 10 cm, and a thickness of 700 μm was placed on the above-mentioned exposed PSA film and placed at a temperature of about 40°C for about 30 seconds, and the laminated sample of the above-mentioned glass substrate and the release film of the polarizing plate removed was laminated.
[0192] That is, the laminated stacked sample had a structure in which the glass substrate, the polarizing plate from which the protective film and the release film were removed, the cured adhesive composition, and the glass base material were stacked in this order.
[0193] After lamination, an autoclave operation was performed at a temperature of about 50° C. and a pressure of about 0.5 MPa for about 15 minutes. Then, a light generating device (Philips, product name: Arenavision MVF403) was used to generate a light beam at about 830 to 1000 W / m 2 The light generated in the above light generating device was first brought into contact with the glass substrate of the laminated stacked sample for about 500 hours under a light amount of .
[0194] Then, it was confirmed whether bubbles were generated between the glass substrate and the cured adhesive composition, and the light resistance was evaluated according to the following criteria.
[0195] PASS: No bubbles are generated
[0196] NG: Bubbles are generated
[0197] 4. Storage Modulus Determination Method Based on Temperature
[0198] The adhesive composition was placed between release films in a manner to have a thickness of 200 μm, and an ultraviolet lamp was used to irradiate the adhesive composition at 9 to 11 J / cm 2 The solidified material was cured by photocuring under a light intensity of 100 nm, thereby forming a solidified material. The solidified materials were attached to each other and made into a thickness of 1 mm. The solidified material was cut into a diameter of 8 mm and a thickness of 1 mm, thereby manufacturing a disk-shaped measurement sample.
[0199] The storage modulus was measured using a rotational rheometer (TA, product name: ARES-G2) while applying 1% strain and 1 Hz rotation speed to the above-mentioned measurement sample in a temperature range of -50°C to 120°C. The temperature was increased from -50°C to 120°C at a rate of 5°C per minute.
[0200] In addition, the room temperature storage modulus is based on the storage modulus at 25°C.
[0201] Example 1
[0202] The glass transition temperature (T g ) greater than 10°C and a monomer (T1) having a glass transition temperature below 10°C is in a weight ratio of 15:85 (T1:T2), and a monomer (S1) having a surface tension at room temperature greater than 30mN / m and a monomer (S2) having a surface tension at room temperature below 30mN / m is in a weight ratio of 15:85 (S1:S2).
[0203] Specifically, isodecyl acrylate (IDA), isobornyl acrylate (IBOA), 2-hydroxyethyl acrylate (2-HEA) and butyl acrylate (BA) were uniformly mixed in a weight ratio of 24:15:27:34 (IDA:IBOA:2-HEA:BA), and 0.03 parts by weight of a photoinitiator (IRGCURE 184 manufactured by Ciba Corporation) was added to 100 parts by weight of the mixture to prepare an adhesive composition.
[0204] Example 2
[0205] An adhesive composition is manufactured in such a manner that the weight ratio of a monomer (T1) having a glass transition temperature (Tg) greater than 10°C and a monomer (T2) having a glass transition temperature less than 10°C is 7:93 (T1:T2), and the weight ratio of a monomer (S1) having a surface tension greater than 30 mN / m at room temperature and a monomer (S2) having a surface tension less than 30 mN / m at room temperature is 18:82 (S1:S2).
[0206] Specifically, butyl acrylate (BA), isobornyl acrylate (IBOA), tetrahydrofurfuryl acrylate (THFA), 2-ethylhexyl acrylate (2-EHA) and 2-hydroxyethyl acrylate (2-HEA) were uniformly mixed in a weight ratio of 20:7:11:34:28 (BA:IBOA:THFA:2-EHA:2-HEA), and 0.03 parts by weight of a photoinitiator (IRGCURE 184 manufactured by Ciba Corporation) was added to 100 parts by weight of the mixture to prepare an adhesive composition.
[0207] Example 3
[0208] An adhesive composition is manufactured in such a manner that the weight ratio of a monomer (T1) having a glass transition temperature (Tg) greater than 10°C and a monomer (T2) having a glass transition temperature less than 10°C is 2:98 (T1:T2), and the weight ratio of a monomer (S1) having a surface tension greater than 30 mN / m at room temperature and a monomer (S2) having a surface tension less than 30 mN / m at room temperature is 5:95 (S1:S2).
[0209] Specifically, 2-ethylhexyl acrylate (2-EHA), 2-hydroxyethyl acrylate (2-HEA), N,N-dimethylacrylamide (DMAA), isobornyl acrylate (IBOA) and tetrahydrofurfuryl acrylate (THFA) were uniformly mixed in a weight ratio of 90:5:1:1:3 (2-EHA:2-HEA:DMAA:IBOA:THFA), and 0.03 parts by weight of a photoinitiator (IRGCURE 184 manufactured by Ciba Corporation) was added to 100 parts by weight of the mixture to prepare an adhesive composition.
[0210] Comparative Example 1
[0211] An adhesive composition is manufactured in such a manner that the weight ratio of a monomer (T1) having a glass transition temperature (Tg) greater than 10°C and a monomer (T2) having a glass transition temperature less than 10°C is 19:81 (T1:T2), and the weight ratio of a monomer (S1) having a surface tension greater than 30 mN / m at room temperature and a monomer (S2) having a surface tension less than 30 mN / m at room temperature is 24:76 (S1:S2). Specifically, 2-ethylhexyl acrylate (2-EHA), 2-hydroxyethyl acrylate (2-HEA), N,N-dimethylacrylamide (DMAA), isostearyl acrylate (ISTA), isobornyl acrylate (IBOA) and tetrahydrofurfuryl acrylate (THFA) were uniformly mixed in a weight ratio of 39:17:5:20:14:5 (2-EHA:2-HEA:DMAA:ISTA:IBOA:THFA), and 0.18 parts by weight of a photoinitiator (IRGCURE 184 manufactured by Ciba Corporation) was added to 100 parts by weight of the mixture to prepare an adhesive composition.
[0212] Comparative Example 2
[0213] An adhesive composition was manufactured in such a manner that the weight ratio of a monomer (T1) having a glass transition temperature (Tg) greater than 10°C and a monomer (T2) having a glass transition temperature less than 10°C was 24:76 (T1:T2), and the weight ratio of a monomer (S1) having a surface tension greater than 30 mN / m at room temperature and a monomer (S2) having a surface tension less than 30 mN / m at room temperature was 37:63 (S1:S2).
[0214] Specifically, 2-ethylhexyl acrylate (2-EHA), 2-hydroxyethyl acrylate (2-HEA), N,N-dimethylacrylamide (DMAA), isostearyl acrylate (ISTA), isobornyl acrylate (IBOA) and tetrahydrofurfuryl acrylate (THFA) were uniformly mixed in a weight ratio of 33:14:12:17:12:12 (2-EHA:2-HEA:DMAA:ISTA:IBOA:THFA), and 0.15 parts by weight of a photoinitiator (IRGCURE 184 manufactured by Ciba Corporation) was added to 100 parts by weight of the mixture to prepare an adhesive composition.
[0215] Comparative Example 3
[0216] An adhesive composition is manufactured in such a manner that the weight ratio of a monomer (T1) having a glass transition temperature (Tg) greater than 10°C and a monomer (T2) having a glass transition temperature less than 10°C is 19:81 (T1:T2), and the weight ratio of a monomer (S1) having a surface tension greater than 30 mN / m at room temperature and a monomer (S2) having a surface tension less than 30 mN / m at room temperature is 24:76 (S1:S2).
[0217] Specifically, 2-ethylhexyl acrylate (2-EHA), 2-hydroxyethyl acrylate (2-HEA), N,N-dimethylacrylamide (DMAA), isostearyl acrylate (ISTA), isobornyl acrylate (IBOA) and tetrahydrofurfuryl acrylate (THFA) were uniformly mixed in a weight ratio of 39:17:5:20:14:5 (2-EHA:2-HEA:DMAA:ISTA:IBOA:THFA), and 0.03 parts by weight of a photoinitiator (IRGCURE 184 manufactured by Ciba Corporation) was added to 100 parts by weight of the mixture to prepare an adhesive composition.
[0218] Comparative Example 4
[0219] An adhesive composition is manufactured in such a manner that the weight ratio of a monomer (T1) having a glass transition temperature (Tg) greater than 10°C and a monomer (T2) having a glass transition temperature less than 10°C is 24:76 (T1:T2), and the weight ratio of a monomer (S1) having a surface tension greater than 30 mN / m at room temperature and a monomer (S2) having a surface tension less than 30 mN / m at room temperature is 30:70 (S1:S2).
[0220] Specifically, 2-ethylhexyl acrylate (2-EHA), 2-hydroxyethyl acrylate (2-HEA), N,N-dimethylacrylamide (DMAA), isobornyl acrylate (IBOA) and tetrahydrofurfuryl acrylate (THFA) were uniformly mixed in a weight ratio of 49:21:6:18:6 (2-EHA:2-HEA:DMAA:IBOA:THFA), and 0.03 parts by weight of a photoinitiator (IRGCURE 184 manufactured by Ciba Corporation) was added to 100 parts by weight of the mixture to prepare an adhesive composition.
[0221] The physical properties measured for the above-mentioned Examples and Comparative Examples are shown in Table 1 below.
[0222]
Table 1
[0223]
[0224] Referring to Table 1, the glass transition temperature in Examples 1 to 3 was -25°C or lower, and the surface tension at room temperature was 30 mN / m or lower.
[0225] On the contrary, Comparative Examples 1 to 3 could not satisfy the glass transition temperature of -25°C or less, and the room temperature surface tensions of Comparative Examples 1 to 4 all showed values greater than 30 mN / m.
[0226] In addition, referring to Table 1, Examples 1 to 3 have a value of 0.002 to 0.012 kgf / mm 2 The tensile modulus of Comparative Examples 1 to 4 was 0.012 kgf / mm 2 The tensile modulus is above .
[0227] In addition, referring to Table 1, Examples 1 to 3 all have storage moduli of 0.1 MPa or less at room temperature and storage moduli of 0.055 MPa or less at 80°C. Figure 1 and 2 , the storage modulus values according to temperature of Examples 1 and 2 can be confirmed.
[0228] On the contrary, in Comparative Examples 1 to 3, the storage modulus at room temperature all showed a value greater than 0.1 MPa, and the storage modulus at 80° C. all showed a value greater than 0.055 MPa. Figure 3 and 4 , the storage modulus values according to the temperature of Comparative Examples 1 and 3 can be confirmed.
[0229] In addition, referring to Table 1, the wetting time in Examples 1 to 3 was 60 seconds or less, and all of them were PASS in the wettability evaluation. In contrast, the wetting time in Comparative Examples 1 to 4 was greater than 60 seconds, and all of them were NG in the wettability evaluation.
[0230] In addition, referring to Table 1, Examples 1 to 3 did not generate bubbles in the light resistance evaluation and all were rated as PASS. Figure 5 and 6 The light resistance evaluation results of Examples 1 and 2 are shown. Figure 5 and 6 It can be seen that even if there is a foreign matter (defect), no bubbles are generated.
[0231] In contrast, Comparative Examples 1 to 4 generated bubbles in the light resistance evaluation and were all NG. Figures 7 to 10 The light resistance evaluation results of Comparative Examples 1 to 4 are shown. Figures 7 to 10 It can be seen that bubbles are generated with the foreign matter (defect) as the center.
Claims
1. An adhesive composition comprising a copolymer obtained by copolymerizing two or more monomers, The monomers include monomers having a surface tension greater than 30 mN / m at room temperature and monomers having a surface tension less than 30 mN / m at room temperature. The room temperature surface tension of the copolymer is less than 30 mN / m, in, The monomers having a room temperature surface tension of 30 mN / m or less include hydroxyl-containing acrylate compounds and chain alkyl acrylate compounds. Wherein, the monomer having a room temperature surface tension greater than 30 mN / m comprises a cyclic alkyl acrylate compound, wherein the weight ratio R / Q of the hydroxyl-containing acrylate compound R to the cyclic alkyl acrylate compound Q is in the range of 1.2 to 10, and The content of the linear alkyl acrylate compound in the monomer having a room temperature surface tension of 30 mN / m or less is 70 wt % or less.
2. The adhesive composition according to claim 1, in, The monomer satisfies the following general formula 1: Formula 1 3≤A / B×100≤30 In Formula 1, A represents the weight of the monomer having a surface tension greater than 30 mN / m at room temperature, and B represents the weight of the monomer having a surface tension less than 30 mN / m at room temperature.
3. The adhesive composition according to claim 1, in, The monomers include monomers with a glass transition temperature greater than 10°C and monomers with a glass transition temperature less than 10°C. The glass transition temperature of the copolymer is below -25°C.
4. The adhesive composition according to claim 3, in, The monomer satisfies the following general formula 2: Formula 2 1≤C / D×100≤22 In Formula 2, C represents the weight of the monomer having a glass transition temperature greater than 10°C, and D represents the weight of the monomer having a glass transition temperature less than 10°C.
5. The adhesive composition according to claim 1, in, The glass transition temperature of the linear alkyl acrylate compound is -20°C or lower.
6. The adhesive composition according to claim 1, in, The chain alkyl acrylate compound includes one or more compounds represented by the following Chemical Formula 1: Chemical formula 1 In Chemical Formula 1, L 1 is a linear alkylene group having 1 to 14 carbon atoms or a branched alkylene group having 2 to 14 carbon atoms, and R 1 and R 2 Each is independently hydrogen, a linear alkyl group having 1 to 6 carbon atoms, or a branched alkyl group having 2 to 6 carbon atoms.
7. The adhesive composition according to claim 1, in, The glass transition temperature of the hydroxyl-containing acrylate compound is 0° C. or lower.
8. The adhesive composition according to claim 1, in, The hydroxyl-containing acrylate compound includes one or more compounds represented by the following Chemical Formula 2: Chemical formula 2 In chemical formula 2, L 2 It is a straight-chain alkylene group having 1 to 10 carbon atoms, a branched-chain alkylene group having 2 to 10 carbon atoms, a straight-chain or branched-chain alkenylene group having 2 to 10 carbon atoms, or a straight-chain or branched-chain alkynylene group having 2 to 10 carbon atoms.
9. The adhesive composition according to claim 1, in, The cyclic alkyl acrylate compound has a glass transition temperature of 50° C. or higher.
10. The adhesive composition according to claim 1, in, The monomer having a room temperature surface tension greater than 30 mN / m includes an acrylate compound containing a cyclic ether group.
11. The adhesive composition according to claim 10, in, The glass transition temperature of the cyclic ether group-containing acrylate compound is 10° C. or less.
12. The adhesive composition according to claim 10, in, The acrylate compound containing a cyclic ether group includes one or more compounds represented by the following Chemical Formula 3: Chemical formula 3 In chemical formula 3, R 3 is hydrogen or a linear alkyl group having 1 to 20 carbon atoms, L 3 and L 4 are each independently a single bond or a linear alkylene group having 1 to 20 carbon atoms, L 5 is a single bond or a linear alkylene group having 1 to 8 carbon atoms, Q is an oxygen atom or a carbon atom. 13 . A film comprising a cured product of the adhesive composition according to claim 1 .
14. The film according to claim 13, in, The film has a room temperature adhesive force of 0.7 kg / inch or more, or a tensile modulus of 0.002 to 0.012 kgf / mm 2 The storage modulus at room temperature is 0.1 MPa or less and the storage modulus at 80°C is 0.055 MPa or less.
15. An adhesive composition comprising a copolymer obtained by copolymerizing two or more monomers, in, The monomers include monomers having a surface tension greater than 30 mN / m at room temperature and monomers having a surface tension less than 30 mN / m at room temperature. Wherein, the monomer having a room temperature surface tension of 30 mN / m or less comprises a hydroxyl-containing acrylate compound, The monomer having a room temperature surface tension greater than 30 mN / m includes a cyclic alkyl acrylate compound and an acrylate compound containing a cyclic ether group, and the acrylate compound containing a cyclic ether group includes one or more compounds represented by the following chemical formula 3: The weight ratio R / Q of the hydroxyl-containing acrylate compound R to the cyclic alkyl acrylate compound Q is in the range of 1.2 to 10. The room temperature surface tension of the copolymer is below 30 mN / m, and the glass transition temperature is below -25°C. Chemical formula 3 In chemical formula 3, R 3 is hydrogen or a linear alkyl group having 1 to 20 carbon atoms, L 3 and L 4 are each independently a single bond or a linear alkylene group having 1 to 20 carbon atoms, L 5 is a single bond or a linear alkylene group having 1 to 8 carbon atoms, Q is an oxygen atom or a carbon atom.
16. The adhesive composition according to claim 15, in, The monomers include monomers with a glass transition temperature greater than 10°C and monomers with a glass transition temperature less than 10°C. Wherein, the monomer satisfies the following general formula 1 and the following general formula 2: Formula 1 3≤A / B×100≤30 Formula 2 1≤C / D×100≤22 In Formula 1, A represents the weight of the monomer having a surface tension greater than 30 mN / m at room temperature, and B represents the weight of the monomer having a surface tension less than 30 mN / m at room temperature. In Formula 2, C represents the weight of the monomer having a glass transition temperature greater than 10°C, and D represents the weight of the monomer having a glass transition temperature less than 10°C.
17. The adhesive composition according to claim 16, in, The monomer having a glass transition temperature greater than 10° C. and a room temperature surface tension greater than 30 mN / m is contained in a range of 0.5 to 18% by weight relative to the total weight of the monomer.
18. The adhesive composition according to claim 17, in, The monomer having a glass transition temperature of 10° C. or less and a room temperature surface tension of 30 mN / m or less is in the range of 450 to 5500 parts by weight relative to 100 parts by weight of the monomer having a glass transition temperature of more than 10° C. and a room temperature surface tension of more than 30 mN / m.