Method for in-situ glyoxylation of polyacrylamide

By using discontinuous intermittent glyoxylation in paper mills and simplifying alkali consumption and pH control, the problem of insufficient strength properties and gel formation of glyoxylated polyacrylamide in humid conditions is solved, improving the performance of paper and board. Strength and folding resistance, reducing production complexity and cost.

CN115151694BActive Publication Date: 2024-10-18KEMIRA OY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202180016148.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-17
Publication Date
2024-10-18
Estimated Expiration
2041-03-17

AI Technical Summary

Technical Problem

In the existing technology, the in-situ preparation of glyoxylated polyacrylamide in paper mills or cardboard mills has complexity and storage stability problems, resulting in insufficient strength properties under humid conditions, and high molecular weight polyacrylamide is not suitable for use in applications. It is easy to form gel, affecting the production efficiency and quality of paper and cardboard.

Method used

By using discontinuous intermittent glyoxylation reactions in paper or cardboard mills, control the pH and temperature of the reaction mixture, measure the viscosity to regulate the reaction process, simplify the prediction and addition of alkali consumption, avoid online pH measurements, and shorten the reaction time , ensuring the cross-linking level and performance of glyoxylated polyacrylamide.

Benefits of technology

It is possible to improve the short-span compressive strength and tensile energy absorption of paper and cardboard under humid conditions, reduce the risk of cracks, simplify the process, reduce production costs, and improve the overall strength performance of paper and cardboard.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004546264360000161
    Figure GDA0004546264360000161
  • Figure GDA0004546264360000181
    Figure GDA0004546264360000181
  • Figure GDA0004546264360000192
    Figure GDA0004546264360000192
Patent Text Reader

Abstract

The present invention relates to a method for in-situ glyoxylation of polyacrylamide in a paper mill, a board mill, etc., wherein a discontinuous batch glyoxylation reaction of an aqueous reaction mixture is carried out in a reaction vessel equipped with a driven agitator to form an aqueous polymer composition comprising glyoxylated polyacrylamide for use in the manufacturing process of paper, board, etc. The method comprises forming or obtaining an aqueous reaction mixture comprising a polyacrylamide base polymer and glyoxal, determining the alkali consumption of the reaction mixture, and adding a predetermined amount of alkali required to adjust the pH value of the reaction mixture to 8-10, preferably 8.5-9.5, to the reaction mixture based on the determined alkali consumption. The temperature of the reaction mixture is optionally adjusted to a temperature range of 15-40°C, more preferably 20-30°C, and the in-situ glyoxylation reaction of the polyacrylamide base polymer is allowed to proceed in the reaction mixture. The viscosity of the reaction mixture and / or process variables related to the viscosity of the reaction mixture are determined, and when a predetermined final viscosity value is obtained, an acid is added to the reaction mixture to reduce the pH value of the reaction mixture to <8, preferably <7, and the aqueous polymer composition comprising glyoxylated polyacrylamide is removed from the reaction vessel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for on-site glyoxylation of polyacrylamide in paper mills, board mills and the like. Background Art

[0002] Board, especially corrugated container board, is one of the most used packaging materials in the world due to its low price, lightweight structure and recyclability. However, container board also has limitations. One of the main disadvantages of container board is its poor water and moisture resistance. The main building block of container board is amphiphilic cellulose-based fibers, whose hydrophilic hydroxyl groups give the fibers mechanical strength but at the same time make them susceptible to moisture. This means that under humid conditions, the strength of the board may decrease rapidly.

[0003] Nowadays, many goods are produced in countries with humid environmental conditions, for example, in Southeast Asia, from where they are shipped all over the world. Corrugated board is also used to package humid or moisture-producing goods, such as fruits, vegetables or frozen foods, and / or are stored in humid environments, such as cold storage spaces. As the packaging is exposed to moisture in the environment or the packaged goods during transportation and / or storage, the strength of the packaging can be reduced. Ultimately, this can even lead to the collapse of the packaging. Therefore, there is an increasing need to provide improved strength properties for carton board and equivalent fiber products, even under humid conditions.

[0004] Another challenge for packaging produced from corrugated paperboard is the so-called score cracking. Score cracking refers to the misalignment of fibers along the score line on the outside of the paperboard in the edge area of ​​the package. When folded along the score line, the outer surface of the paperboard is stretched. Surface sizing can increase the tensile strength of the paperboard, but since the strain is not increased, the paperboard may become brittle. Score cracking is a quality defect that should be minimized when manufacturing packaging from paperboard.

[0005] Glyoxylated polyacrylamide (GPAM) and compositions containing glyoxylated polyacrylamide are often used to make paper, paperboard, etc. to improve the properties of the final product. Polyacrylamide polymers can be formed by polymerization of acrylamide and cationic monomers, which can produce ionic bonds with anionic fiber surfaces. The molecular weight (i.e., length) of the polyacrylamide backbone is an important parameter for polymer functionality because a long backbone provides sufficient size, which allows bonding and connection between fiber surfaces. Glyoxylation crosslinks the polyacrylamide polymer. The crosslinked structure improves the drainage and dehydration capabilities of the polyacrylamide, and has less negative impact on sheet formation than linear polyacrylamide polymers of similar molecular weight.

[0006] Glyoxylated polyacrylamide is a reactive polymer that can covalently bond with cellulose, and thus can provide improvements in, for example, strength properties. For example, the dry strength and / or wet strength properties of paper and paperboard can be improved by adding glyoxylated polyacrylamide to the stock suspension. In general, the good forming and good bonding capabilities provided by glyoxylated polyacrylamide contribute to the strength properties of the final paper or paperboard, which are measured by the ring crush test (RCT), bursting strength, and Concora medium test (CMT). These strength description parameters are particularly important when manufacturing liner, testliner, or fluting board grades.

[0007] High molecular weight glyoxylated polyacrylamide, especially if the paper or paperboard is made from a furnish containing recycled fibers, contributes to the strength properties of the paper or paperboard. In these cases, one of the challenges is often the high ash content of the furnish, which requires the backbone of the polyacrylamide polymer to have a sufficiently high molecular weight. Otherwise, inorganic particles between the fibers may hinder bond formation, and the glyoxylated polyacrylamide cannot effectively contact the fibers and form bonds between them. Therefore, the physical size of the glyoxylated polyacrylamide polymer, i.e., the molecular weight, is of great significance for the strength improvement efficiency.

[0008] However, glyoxylated polyacrylamide compositions, especially high molecular weight polyacrylamide compositions, present challenges in their commercial applications. It is known that glyoxylated polyacrylamide may have insufficient storage stability. As mentioned above, glyoxylated polyacrylamide is formed by crosslinking a polyacrylamide-based polymer using glyoxal. The resulting glyoxylated polyacrylamide polymer is not fully stable because the glyoxal in the polymer aqueous solution tends to continue to crosslink with the polyacrylamide base polymer. This means that the viscosity of the GPAM aqueous solution usually increases during storage as the crosslinking reaction proceeds. Finally, the continued crosslinking reaction may even lead to gel formation and make the glyoxylated polyacrylamide unsuitable for the manufacture of paper, paperboard, etc. Therefore, the shelf life of the glyoxylated polyacrylamide and its aqueous solution is limited.

[0009] Increasing the molecular weight of the polyacrylamide base polymer to obtain the desired strength properties may result in extensive gel formation. In order to reduce the risk of crosslinking and gel formation, the glyoxylated polyacrylamide polymer is therefore often prepared, transported and stored in the form of an aqueous solution with a relatively low concentration, for example, 5 wt%-7 wt% of active glyoxylated polyacrylamide polymer. This means that the transportation and storage costs of the glyoxylated polyacrylamide composition are relatively high due to the large volumes involved.

[0010] Due to its storage stability limitations, glyoxylated polyacrylamide polymers, especially high molecular weight glyoxylated polyacrylamide polymers, are sometimes prepared in situ at a paper mill or board mill immediately before being added to the process. Some continuous and discontinuous processes for the in situ preparation of glyoxylated polyacrylamide have been proposed. However, the in situ preparation of glyoxylated polyacrylamide has proven to be complicated in practice. There are challenges in a continuous process for producing glyoxylated polyacrylamide with consistent acceptable quality while keeping the throughput of the process at an appropriate level, i.e., keeping the reaction time short enough for industrial production. In particular, the control of various process parameters and conditions has been very complex. Summary of the invention

[0011] It is an object of the present invention to minimize or possibly even eliminate the disadvantages present in the prior art.

[0012] Another object of the present invention is to provide a simple and effective method for in situ production of glyoxylated polyacrylamide.

[0013] Still another object of the present invention is to provide a method for in-situ production of glyoxylated polyacrylamide, which can be used to improve the strength properties of paper, paperboard, etc., especially under wet conditions.

[0014] The embodiments mentioned in this text relate, where applicable, to all aspects of the invention, even if this is not always mentioned individually.

[0015] In a typical process according to the present invention for in-situ glyoxylation of polyacrylamide in a paper mill, board mill, etc., wherein a discontinuous batch glyoxylation reaction of an aqueous reaction mixture is carried out in a reaction vessel equipped with a driven agitator to form an aqueous polymer composition comprising glyoxylated polyacrylamide for use in a paper, board, etc. manufacturing process, the process comprises:

[0016] - forming or obtaining an aqueous reaction mixture comprising a polyacrylamide base polymer and glyoxal;

[0017] - determining the base consumption of the reaction mixture;

[0018] - adding a predetermined amount of base to the reaction mixture, according to the determined base consumption, which amount is required to adjust the pH value of the reaction mixture to a range of 8-10, preferably 8.5-9.5;

[0019] - optionally adjusting the temperature of the reaction mixture to a temperature range of 15-40°C, more preferably 20-30°C;

[0020] - allowing the polyacrylamide base polymer in the reaction mixture to undergo an in situ glyoxylation reaction;

[0021] - measuring the viscosity of the reaction mixture and / or a process variable related to the viscosity of the reaction mixture;

[0022] - when a predetermined final viscosity value is reached, adding an acid to the reaction mixture to reduce the pH of the reaction mixture to <8, preferably <7; and

[0023] - removing the aqueous polymer composition comprising the glyoxylated polyacrylamide from the reaction vessel.

[0024] The typical use of the glyoxylated polyacrylamide prepared according to the method of the present invention is in the manufacture of paper and paperboard, and the preferred dosage is 0.5-3 kg / t.

[0025] Now, surprisingly, it has been found that a complex and / or time-consuming online pH measurement is not required for proper control of the in-situ glyoxylation of polyacrylamide. By actively determining the alkali consumption of the reaction mixture before the start of the glyoxylation reaction, it is possible, for example, by mathematical calculation, to predetermine the necessary amount of alkali to be added to the reaction mixture with sufficient accuracy. In this way, the in-situ glyoxylation process of polyacrylamide can be made simple and efficient, the reaction time being kept within reasonable limits while achieving the desired crosslinking level. It has been found that the reaction time can be significantly shortened without reducing the properties of the glyoxylated polyacrylamide polymer. On the contrary, the present invention provides the possibility of producing a glyoxylated polyacrylamide polymer, which provides enhanced strength properties for the final product, especially under humid conditions. The progress of the glyoxylation process can be effectively controlled by using simple measurements of viscosity and / or viscosity-related parameters without the need for complex measurement schemes involving various parameters and / or online sensors such as pH meters. The method can be implemented by using equipment that is usually already present in paper and board mills, which makes the method applicable and easy to modify in practice.

[0026] The aqueous polymer composition comprising glyoxylated polyacrylamide obtainable by the present invention is able to increase the short span compressive strength (SCT strength) of paper, paperboard, etc. under high humidity conditions. Thus, the present invention is able to provide a final paper or paperboard having properties that make it suitable for use in demanding environments and / or demanding packaging of goods such as fruit or frozen foods. The use of the aqueous polymer composition comprising glyoxylated polyacrylamide obtainable by the present invention can also help to reduce the weight of the package, thereby reducing CO2 emissions associated with packaging and transportation. Fluting particularly requires SCT strength under high humidity conditions to reduce the risk of package collapse during storage and / or transportation.

[0027] The aqueous polymer composition comprising glyoxylated polyacrylamide obtainable by the present invention also reduces the risk of score cracking. It has been observed that the aqueous polymer composition comprising glyoxylated polyacrylamide obtainable by the present invention is able to significantly increase the tensile energy absorption (TEA) of paper, board, etc. In this way, it is possible to produce liners and / or test liners having improved strength properties and capable of withstanding stretching when the board is folded along the score line during packaging production.

[0028] In this document, the terms "humid conditions" and "high humidity conditions" are used interchangeably, and both refer to environmental conditions with high humidity, wherein the relative humidity is ≥80%, preferably ≥85%, and more preferably ≥90%. For example, under high humidity conditions, the relative humidity (RH) may be 80%-100%. Tests for evaluating high humidity performance, such as SCT strength under high humidity conditions, may be performed, for example, with test strips air conditioned at 85% RH and 23°C for at least 4 hours. High humidity conditions typically increase the moisture content of a paper or paperboard web to >7%, which reduces the amount of hydrogen bonding between web components. This may result in reduced web strength if no countermeasures are taken, such as the present invention.

[0029] In the present invention, the in-situ glyoxylation reaction of polyacrylamide in paper mills, paperboard mills, etc. is carried out in a discontinuous intermittent glyoxylation reaction of an aqueous reaction mixture in a reaction vessel equipped with a driven agitator. The term "discontinuous intermittent glyoxylation reaction" means that the reaction mixture materials, for example, polyacrylamide base polymer, glyoxal, water, etc. are introduced into the reaction vessel at the beginning of the glyoxylation process, and the formed reaction mixture is retained in the reaction vessel until the reaction ends. During the glyoxylation reaction, an aqueous polymer composition comprising glyoxylated polyacrylamide is formed. The formed polymer composition comprising glyoxylated polyacrylamide polymer is then taken out from the reaction vessel. The reaction cycle of the discontinuous intermittent glyoxylation reaction begins when a batch of reaction mixture materials is introduced into the reaction vessel, including possible temperature adjustment time, etc., and ends the reaction cycle when the reaction vessel is ready to receive the next batch of reaction mixture materials after the aqueous polymer composition is taken out from the reaction vessel (including necessary emptying time and flushing time). In the present invention, the reaction cycle (reaction cycle) can be less than 130 minutes, preferably less than 100 minutes. For example, the reaction cycle time may be 35-130 minutes, preferably 45-100 minutes or 45-90 minutes, sometimes even 45-75 minutes, which enables efficient production of glyoxylated polyacrylamide for use in paper mills, board mills, and the like.

[0030] At the beginning of the glyoxylation reaction, an aqueous reaction mixture comprising at least polyacrylamide base polymer and glyoxal is obtained or formed in the reaction vessel. According to one embodiment, the reaction mixture is formed by metering or dosing into the reaction vessel an appropriate amount of reaction mixture material comprising polyacrylamide base polymer, glyoxal and dilution water respectively. Alternatively, a premix comprising polyacrylamide base polymer and glyoxal can be used. It may be more convenient to use a premix sometimes, because it is possible to avoid processing glyoxal concentrated solution.

[0031] The alkali consumption of the reaction mixture is measured before the alkali is added to the reaction mixture. The alkali consumption of the polyacrylamide base polymer can be measured before forming or obtaining the reaction mixture. The alkali consumption is measured to provide the amount of alkali required to adjust the pH of the reaction mixture to a pH range of 8-10. The alkali consumption can be, for example, determined by theoretically calculating and / or estimating the alkali consumption based on the properties of the base polymer or premix, such as the structure of the base polymer or other available information. Alternatively, the alkali consumption can be, for example, determined by titrating a diluted sample of the polyacrylamide base polymer with an alkaline solution to a feasible final level. The feasible final level of the titration of the diluted sample of the polyacrylamide base polymer may be higher than the target range of pH 8-10 of the reaction mixture, because the pH value of the basic polyacrylamide base polymer is generally reduced after the addition of glyoxal. Preferably, when determining the alkali consumption of the polyacrylamide base polymer, the same base polymer concentration and the same alkali concentration as in the glyoxal acidification reaction are used. If a premix comprising a polyacrylamide base polymer and glyoxal is used for the reaction mixture, the alkali consumption of the premix is ​​determined, for example, by titration.

[0032] Based on the determined alkali consumption, a predetermined amount of alkali required to adjust the pH of the reaction mixture to a range of 8-10, preferably 8.5-9.5, sometimes 8.7-9.5 is added to the reaction mixture. This means that the measured value of the alkali consumption of the polyacrylamide base polymer or premix is ​​used, for example, by calculation, to predetermine the amount of alkali required to adjust the pH of the reaction mixture to a suitable level. Since the alkali consumption of the polyacrylamide base polymer / premix is ​​used to predetermine the amount of alkali required to adjust the pH, it is possible to avoid the problems associated with the use of online pH meters, whose reliability may sometimes be insufficient and / or unreliable. In addition, since the glyoxylation reaction is not controlled by pH measurement, the reaction cycle time can be significantly shortened, thereby providing an improved efficiency of the online glyoxylation.

[0033] The addition of the base results in the pH of the reaction mixture being adjusted from the starting pH to a reaction pH in the range of pH 8-10, preferably 8.5-9.5, sometimes 8.7-9.5, without pH control or pH measurement. Typically, NaOH is used as the base. In the present invention, the predetermined amount of base is preferably added based only on the base consumption of the polyacrylamide base polymer / premix, and there is no online pH control of the reaction mixture during the addition of the base or the glyoxylation reaction. Since the amount of base is predetermined (e.g., based on calculations), rather than based on a pH value continuously measured from the reaction mixture during the addition, the reaction cycle time can be significantly shortened without reducing the properties of the glyoxylated polyacrylamide polymer obtained.

[0034] When a predetermined amount of base is added to the reaction mixture, the reaction mixture is effectively mixed by the driven agitator and continues to be mixed throughout the glyoxylation reaction. The reaction vessel typically has a volume of <6 m 3 , preferably <5m 3 , more preferably <4m 3 The reactor volume may, for example, be in the range of 0.5 to 6 m 3 , preferably 0.75-4m 3 , more preferably 1-3m 3 The relatively small reactor volume makes it possible to provide effective mixing of the reaction mixture using conventional driven agitators used in industry. In addition, the relatively small reaction vessel is easier to install on site at a paper mill or board mill. It is even possible to make the reaction vessel mobile. For example, it can be mounted on a transport pallet and moved with a forklift.

[0035] Preferably, the reaction vessel does not contain any bypass circuit for circulating the reaction mixture or part thereof outside the reaction vessel before the end of the glyoxylation reaction. The reaction vessel is thus free of bypass circuits and the like. It is possible to carry out the required measurements (if any) from the reaction mixture residing in the reaction vessel, which means that no bypass circuit is required for removing process samples. This is a clear advantage, since in the industrial production of glyoxylated polyacrylamide polymers, the maintenance of bypass circuits and the like is usually complicated.

[0036] The temperature of the reaction mixture can be optionally adjusted to a temperature range of 15-45°C or 15-40°C, preferably 20-40°C, more preferably 20-35°C or 20-30°C. The adjustment of the reaction mixture temperature can be carried out before the addition of the base, i.e. before the start of the glyoxylation reaction, and / or during the glyoxylation reaction. Temperature adjustment can be achieved by using a reaction vessel that can be cooled / heated. Another option for adjusting the temperature of the reaction mixture is to add hot water or cold water to the reaction mixture. For example, the water used to form the reaction mixture can be heated or cooled to a suitable temperature. According to one embodiment of the present invention, during the glyoxylation reaction, for example, by using a standard temperature sensor installed in a suitable position in the reaction vessel, the temperature of the reaction mixture is measured. The temperature of the reaction mixture can preferably be measured and adjusted during the entire glyoxylation reaction.

[0037] When the pH value of the reaction mixture is adjusted to pH 8-10 with a predetermined amount of alkali, the glyoxylation reaction, i.e., the crosslinking of the polyacrylamide base polymer, will begin. During the glyoxylation reaction, the pH of the reaction mixture is preferably maintained at a level of pH 8-10, preferably 8.5-9.5, and sometimes 8.7-9.5. Too low a pH value of the reaction mixture may reduce the reaction rate of the glyoxylation reaction, while too high a pH value of the reaction mixture may increase the risk of gelation during the glyoxylation process.

[0038] According to a preferred embodiment of the present invention, an additional alkali stream can be fed into the reaction mixture during the glyoxylation reaction. In practice, this means that the pH value of the reaction mixture is first adjusted to pH 8-10, preferably 8.5-9.5, and sometimes a pH value in the range of 8.7-9.5 with a predetermined amount of alkali. When the glyoxylation reaction is carried out, the pH value of the reaction mixture will usually decrease, which may cause the glyoxylation reaction rate to decrease. This can be effectively offset by adding a small amount of additional alkali stream to the reaction mixture. The amount of alkali added to the reaction mixture by the additional alkali stream is usually less than the calculated amount of alkali added to the reaction mixture. Generally speaking, the amount of alkali added by the additional alkali stream can be 5vol%-50vol%, preferably 10vol%-30vol% of the calculated amount of alkali.

[0039] The effects of the pH and temperature of the reaction mixture on the glyoxylation reaction are at least sometimes interrelated. High reaction pH, e.g., pH>10 and high temperature, e.g.,>40°C, may result in almost immediate gelation of the reaction mixture. According to one embodiment of the present invention, during the glyoxylation reaction, a reaction temperature in the range of 20-25°C and a reaction mixture pH in the range of 8.5-9.5 are preferred.

[0040] During the glyoxylation reaction, the viscosity of the reaction mixture and / or process variables related to the viscosity of the reaction mixture are measured and tracked. The measurement can be continuous, or can be performed at preselected preferably short time intervals. The measured values ​​obtained are used to determine the appropriate endpoint of the glyoxylation reaction, i.e. when the desired crosslinking level is reached. According to a preferred embodiment of the present invention, the viscosity of the reaction mixture is measured indirectly. The viscosity of the reaction mixture can be estimated, measured or determined by measuring the torque and / or power consumption of the motor-driven agitator of the reaction vessel, preferably the torque of the driven agitator. When the viscosity of the reaction mixture increases, the power consumption and torque of the driven agitator increase. Measuring the power consumption and / or torque of the driven agitator provides a simple and reliable method to indirectly monitor and measure the viscosity changes of the reaction mixture without the need for complex sensor systems, etc.

[0041] Alternatively or additionally, the viscosity of the reaction mixture can be measured from the reaction mixture using a rotational viscometer, an oscillation viscometer or a vibration viscometer. By using one of the viscometers, it is possible to measure the power consumption or torque driving the stirrer and the viscosity of the reaction mixture.

[0042] The in-situ glyoxylation of the polyacrylamide base polymer in the reaction mixture is allowed to proceed until a predetermined final viscosity value or viscosity level is reached. The calculated amount of alkali, the temperature of the reaction mixture and / or the additional alkali flow are selected so that the reaction time of the glyoxylation reaction is at most 120 minutes. The reaction time of the glyoxylation reaction refers to the time from the addition of the calculated amount of alkali to the reaction mixture to the addition of acid to the reaction mixture to reduce the pH value of the reaction mixture <8, preferably <7 when the reaction mixture ends. During the reaction time, the reaction mixture obtains the desired glyoxylation level, i.e. the crosslinking level of the polyacrylamide base polymer, and forms an aqueous polymer composition comprising glyoxylated polyacrylamide. It is generally desirable that the reaction time is not too long, which can achieve an effective industrial online process. The reaction time of the in-situ glyoxylation reaction can be in the range of 10-120 minutes or 10-100 minutes, preferably 15-80 minutes, more preferably 20-60 minutes, and even more preferably 20-50 minutes. One skilled in the art will be able to theoretically calculate or estimate, based on his or her experience and / or a small amount of experimentation (if necessary), the combination of base amount, reaction mixture temperature, and / or additional base flow that is required to obtain the desired reaction time.

[0043] The optional feed of the additional alkali stream can be interrupted when the viscosity of the reaction mixture has reached a certain predetermined level, close to the predetermined final viscosity, before reaching a predetermined final viscosity value or level. After the alkali feed is interrupted, the glyoxylation reaction rate is reduced. This is beneficial in the later stages of the glyoxylation reaction because it provides more time for the rapid increase in the viscosity of the reaction mixture that occurs at the end of the glyoxylation reaction to react and makes the final viscosity measurement or estimate more accurate.

[0044] When a predetermined final viscosity value or level is reached, an acid is added to the reaction mixture to reduce the pH of the reaction mixture to a pH of ≤8, preferably ≤7, more preferably ≤5. This means that when the viscosity of the reaction mixture reaches a predetermined final viscosity, the pH is reduced to ≤8. The reduction in pH effectively terminates the glyoxylation reaction and stops the crosslinking of the polyacrylamide chains. The pH of the reaction mixture can be reduced to a pH range of 2.5-5, preferably 3-4. The pH is reduced by adding an acid such as formic acid or sulfuric acid to the reaction mixture.

[0045] The predetermined final viscosity value of the reaction mixture can be 20-60cP or 20-45cP, preferably 25-40cP, more preferably 25-35cP. Usually the final viscosity value is selected to provide a suitable crosslinking level without taking any risk of gel formation. The final viscosity value of the reaction mixture is at least twice the initial viscosity of the reaction mixture and at most nine times the initial viscosity of the reaction mixture. Preferably, the predetermined final viscosity value can be 2-7 times, preferably 2-5 times, more preferably 2.5-5 times, of the initial viscosity of the reaction mixture. The initial viscosity of the reaction mixture can be determined before the alkali of the calculated amount is added to the reaction mixture by one of the measuring methods known per se and / or described elsewhere in the application. According to one embodiment of the present invention, the initial viscosity of the reaction mixture can be 4-15cP, preferably 6-12cP, more preferably 7-10cP.

[0046] After the addition of acid, the aqueous polymer composition comprising the glyoxylated polyacrylamide is removed from the reaction vessel. The formed polymer composition comprising the glyoxylated polyacrylamide can be removed from the reaction vessel immediately or after a suitable storage time, preferably immediately. The glyoxylated polyacrylamide can be used to produce paper, paperboard, etc. immediately after the glyoxylation reaction ends, or the glyoxylated polyacrylamide can be first stored in a reaction vessel or in a separate storage container. According to one embodiment of the present invention, the glyoxylated polyacrylamide can be stored for 0.1-100 hours, preferably 0.5-10 hours before it is used to produce paper, paperboard, etc.

[0047] According to a preferred embodiment of the present invention, the aqueous polymer composition comprising glyoxylated polyacrylamide is transferred from the reaction vessel via a pipeline via an optional storage container, preferably directly to a process for the manufacture of paper, board, etc. after the glyoxylation reaction is completed. The aqueous polymer composition comprising glyoxylated polyacrylamide obtained is used in a process for the manufacture of paper, board, etc. by metering it into a fiber suspension before forming a web of paper, board, tissue, etc. Preferably, the polymer composition is transferred directly to the fiber suspension by pumping through a pipeline, which fiber suspension forms one or more layers of the final fiber product. The ability to use the obtained polymer composition directly is advantageous because it minimizes the risk of gel formation that may occur during long-term storage.

[0048] By using the present invention, glyoxal is effectively consumed in the glyoxylation reaction, and the obtained aqueous polymer composition contains low amounts of residual glyoxal. The aqueous polymer composition containing glyoxylated polyacrylamide preferably contains 0.1wt%-1.5wt%, preferably 0.2wt%-1wt%, more preferably 0.2wt%-0.99wt% of residual glyoxal, calculated based on the total weight of the aqueous polymer composition.

[0049] The aqueous polymer composition comprising glyoxylated polyacrylamide obtained by the present process may have a viscosity of >20 mPas, preferably >25 mPas and / or <50 mPas, preferably <35 mPas, measured at 25°C using a Brookfield viscometer.

[0050] The present method can use polyacrylamide base polymers with higher molecular weight. According to one embodiment of the present invention, the polyacrylamide base polymer can have a weight average molecular weight in the range of 50 000-300 000g / mol, preferably 90 000-250 000g / mol, more preferably 100 000-200 000g / mol or 110 000-200000g / mol, sometimes 155 000-200 000g / mol. The weight average molecular weight of the base polymer can be, for example, 115 000-190 000g / mol, preferably 120 000-170000g / mol, more preferably 130 000-160 000g / mol. As mentioned above, the use of high molecular weight polyacrylamide base polymers is usually associated with a huge risk of gel formation during the glyoxylation reaction, but the present method reduces or eliminates this risk. The higher the molecular weight of the base polymer, the larger the molecular size of the final cross-linked structure, in this case the base polymer chains are cross-linked with glyoxal. Larger structures provide improved strength and dewatering properties, especially for furnishes containing recycled fibers and / or having high ash content.

[0051] Preferably, the polyacrylamide base polymer is cationic. The polyacrylamide base polymer can be obtained by polymerization of acrylamide and 7mol%-50mol%, preferably 7mol%-30mol%, more preferably 11mol%-16mol% of hydrolytically stable cationic monomers. According to one embodiment, the polyacrylamide base polymer can be obtained by polymerization of acrylamide and 6mol%-8mol% or 11mol%-14mol% of hydrolytically stable cationic monomers. For example, the polyacrylamide base polymer can be obtained by polymerization of acrylamide and 11mol%-17mol%, preferably 11mol%-15mol% of hydrolytically stable cationic monomers. It has been observed that when the amount of the cationic monomer is about 10mol%, the ash retention in the produced paper or paperboard will increase, which will reduce the strength effect obtained. According to one embodiment, the cationic monomer can be selected from diallyldimethylammonium chloride (DADMAC), 3-(acrylamidopropyl)-trimethyl-ammonium chloride (APTAC), 3-(methacrylamidopropyl) trimethyl-ammonium chloride (MAPTAC) or any combination thereof. Preferably the cationic monomer is diallyldimethylammonium chloride (DADMAC).These cationic monomers, especially in the amounts described, can provide hydrolytic stability to the reaction mixture.

[0052] According to one embodiment, the reaction mixture may have a solid content of 2wt%-8wt%, preferably 3wt%-7wt%, preferably 4wt%-6wt%, calculated by the gross weight of the reaction mixture. The solid content of the reaction mixture may be, for example, 4.1wt%-6.5wt%, preferably 4.4wt%-6.5wt%, more preferably 4.4wt%-6.0wt%. The solid content of the reaction mixture may be adjusted to a suitable level by adding water to the reaction mixture, preferably before adding a calculated amount of alkali. A minimum solid content, i.e., the concentration of the polyacrylamide base polymer, is necessary for the viscosity increase, which provides a preferred signal for terminating the glyoxylation reaction.

[0053] Before adding the base, the pH value of the reaction mixture may be in the range of 2-8, preferably 3-7, more preferably 3-6.

[0054] According to one embodiment of the present invention, polyacrylamide base polymer and glyoxal are provided as an acidic premix for forming a reaction mixture. This means that there is no need to mix a separate base polymer and glyoxal, thereby reducing the treatment of harmful glyoxal in a factory environment, thereby improving occupational safety. For example, the premix may include a polyacrylamide base polymer containing at least 5mol% of a cationic monomer and having a weight-average molecular weight MW in the range of 50 000-350 000g / mol and 0.1wt%-2wt% of glyoxal, and these amounts are calculated according to the gross weight of the aqueous prepolymer composition. Generally speaking, the pH value of the premix is ​​in the range of 2-4, preferably 2.2-3.5, more preferably 2.5-3.3. When the pH of the reaction mixture is adjusted to an alkaline pH, the cross-linking reaction of the premix is ​​activated.

[0055] According to one aspect, the present invention also relates to an aqueous reaction mixture or reaction composition comprising a polyacrylamide base polymer and glyoxal. The composition comprises a polyacrylamide base polymer obtained by polymerization of (meth)acrylamide with 10 mol% to 25 mol% or 10 mol% to 18 mol%, preferably 11 mol% to 17 mol%, more preferably 11 mol% to 15 mol% of a hydrolytically stable monomer, the base polymer having a weight average molecular weight of 115 000 to 200 000 g / mol, preferably 115 000 to 190 000 g / mol, more preferably 120 000 to 170 000 g / mol or 130 000 to 160 000 g / mol; and 6 wt% to 25 wt%, preferably 10 wt% to 20 wt%, more preferably 12 wt% to 18 wt% of glyoxal, calculated based on the dry weight of the prepolymer composition. Suitable hydrolytically stable cationic monomers have been defined elsewhere in this application. The reaction mixture or reaction composition is suitable for the method of the present invention and provides an improvement in strength and / or dehydration effect. The reaction mixture or reaction composition may have a solid content of 3wt%-7wt%, preferably 4wt%-6.5wt%, more preferably 4.5wt%-6.5wt% or 4.5wt%-6.0wt%.

[0056] The aqueous polymer composition comprising glyoxylated polyacrylamide prepared by the present invention is particularly suitable for use as a dry strength and / or dewatering agent in paper or paperboard manufacturing. The aqueous polymer composition comprising glyoxylated polyacrylamide prepared by the present invention provides good dry strength and / or dewatering results, especially when used to make paper or paperboard containing recycled fibers.

[0057] According to a preferred embodiment, the aqueous polymer composition can be used to manufacture paper or paperboard to improve the strength properties of the paper or paperboard under high humidity conditions. The composition is particularly suitable for improving the SCT strength or tensile energy absorption of paper or paperboard.

[0058] According to one embodiment, the aqueous polymer composition comprising glyoxylated polyacrylamide prepared by the present invention is particularly suitable for the manufacture of fiber webs having a basis weight (dry weight) of at least 20 g / m 2 , preferably at least 60g / m 2 , more preferably at least 80 g / m 2 , more preferably at least 100 g / m 2 For example, the basis weight of the fiber web when dry may be in the range of 20-500 g / m 2 , preferably 50-400g / m 2 , preferably 60-350g / m 2 Or sometimes even 100-200g / m 2 within the range.

[0059] According to one embodiment, the present invention is suitable for manufacturing a fiber web, which forms a layer in a multi-layer paperboard selected from waste paper liner corrugated paper, kraft corrugated paper or corrugated medium. The waste paper liner corrugated paper may include a layered structure comprising two to four layers, and / or having a thickness of 80-350 g / m 2 The corrugated paper core can have a single-layer structure. The basis weight can be between 110-180g / m 2 within the range.

[0060] Some embodiments of the invention are more closely described in the following non-limiting examples. DETAILED DESCRIPTION

[0061] Example

[0062] Example 1: Determination of the amount of alkali required

[0063] A series of diluted polyacrylamide base polymer samples were titrated with sodium hydroxide (5.0 wt%) to determine the amount of sodium hydroxide required to adjust the pH of the reaction mixture to the target pH level required in the glyoxylation reaction. Each polyacrylamide base polymer was diluted to a concentration of 4.0 wt%. 1000 g of the diluted polyacrylamide base polymer sample was taken for titration test. Each sample was titrated to a pH value of 9.5 at 25°C, and the amount of alkali required was recorded. Then 9.65 g of glyoxal (40%) was added to the polyacrylamide base polymer sample at pH 9.5. The reaction mixture was mixed for 1 minute at 25°C and the pH was recorded. The titration test results are shown in Table 1.

[0064] Table 1 Results of Example 1

[0065]

[0066] The results in Table 1 show that after the addition of glyoxal, the pH of the reaction mixture is in the desired range of 8-10. By titrating the polyacrylamide base polymer with a NaOH solution, it is possible to determine the amount of alkali required. The pH of the reaction mixture containing a polyacrylamide base polymer at a concentration of 4.0 wt% was adjusted to 9.5, and after the addition of glyoxal, the pH was adjusted to 8.6-8.9. One reason for the difference in pH before and after the addition of glyoxal is that the pH meter requires a stabilization time of at least about 1 minute after the addition of glyoxal. However, alkaline glyoxal solutions containing polyacrylamide base polymers are not stable because glyoxal begins to react with the polyacrylamide base polymer, whereby the pH begins to decrease.

[0067] Example 2: In situ glyoxylation of polyacrylamide base polymer

[0068] The in-situ glyoxylation process of polyacrylamide polymer is carried out in a 30-liter pilot reactor. The pilot reactor is protected by an insulating fabric to keep the temperature in the pilot reactor stable. The pilot reactor is equipped with a first agitator (Heidolph RZR 2102), the speed is adjusted to 200 rpm, and a second agitator (Heidolph Hei-TorquePrecision 400), with torque monitoring, the speed is adjusted to 80 rpm. The pilot reactor is also equipped with an online viscometer (Anton Paar, L-Vis 510), a metering pump for adding alkali to the reaction mixture, and a pH meter for monitoring the pH value during the glyoxylation reaction.

[0069] The polyacrylamide base polymer BP3 from Example 1 is a copolymer of acrylamide (77 mol %) and DADMAC (23 mol %).

[0070] 21.7kg tap water (25°C) and 2.89kg polyacrylamide base polymer (34%, 25°C) were metered into the pilot reactor and mixed for 2 minutes. The concentration of polyacrylamide base polymer in the reaction mixture was 4.0wt%. 238g glyoxal (40%, 25°C) was metered into the pilot reactor and mixed for 2 minutes. The temperature of the reaction mixture was 25°C. 65.4g NaOH solution (5%) was added within 1 minute. The reaction time started after the metering of alkali was completed. During the reaction, the temperature, online viscosity (Anton Paar viscometer), torque of the agitator and pH value were monitored. Samples were also taken from the reaction mixture and the viscosity was measured by using a Brookfield DV1+ viscometer. After the metering of alkali was completed for 5 minutes, NaOH (5%) was pumped, and the flow rate was 1.74mL / min to prevent the pH value of the reaction mixture from decreasing. After 32 minutes of the reaction time, the additional NaOH flow was stopped. 54 minutes after the reaction started, 22g of sulfuric acid (30%) was added to the reaction mixture to stop the glyoxylation reaction. The viscosity of the final glyoxylated polyacrylamide product was measured by an Anton Paar viscometer to be 33cP and by a Brookfield DV1+ viscometer to be 35cP. The test values ​​of the pilot reactor experiment of the process are shown in Table 2.

[0071] Table 2 Detection values ​​of pilot reactor experiment

[0072]

[0073]

[0074] The values ​​in Table 1 show that glyoxylated polyacrylamide can be produced online by adjusting the pH using the determined alkali analysis value. An online viscometer can be used to control the glyoxylation rate and viscosity. The torque level of the agitator can track the viscosity value and is therefore suitable for monitoring the reaction rate of the glyoxylated reaction mixture.

[0075] Example 3: In-situ glyoxylation, preparation of glyoxylated polyacrylamide with different viscosities

[0076] The in-situ glyoxylation process was carried out using the same pilot reactor as in Example 2. The glyoxylation process was the same as in Example 2, except that the reaction temperature was 30°C.

[0077] The polyacrylamide base polymer BP4 from Example 1 is a copolymer of acrylamide (77 mol %) and DADMAC (23 mol %).

[0078] When the viscosity of the reaction mixture (measured online with Anton Paar viscometer) reached the desired predetermined target values ​​of 22.5 cP and 33.2 cP, 200 g samples were taken from the reaction mixture. The samples taken from the reaction mixture were acidified with sulfuric acid (30%). When the viscosity of the reaction mixture (measured online with Anton Paar viscometer) reached a final value of 46.9 cP, the reaction in the pilot reactor was stopped by adding sulfuric acid to the reaction mixture. Concentration, Brookfield viscosity and pH were determined from the samples as well as the reaction mixture. The results are shown in Table 3.

[0079] Table 3 Results of Example 3

[0080]

[0081] The results in Table 3 show that glyoxylated polyacrylamides with different viscosities can be produced using the in-line process of the present invention.

[0082] Example 4: Application example to evaluate the paperboard properties that can be obtained when using in situ produced glyoxylated polyacrylamide

[0083] In Example 4 the effect of the addition of the glyoxylated polyacrylamide prepared in situ according to the invention on SCT (Short Span Compression Strength), bursting strength, crush resistance (Corrugating Medium Test (CMT30)) and beta formation was tested.

[0084] The furnish is made of fluting sheet made from recycled European fibers. Sheet (110g / m 2 ) was formed using a Rapid Koethen sheet former (RK) as follows: the batch was wet disintegrated using a pulper (Noviprofiber, France) at 70°C at 3% consistency at 500 rpm for 30 seconds and at 1000 rpm for 25 minutes without soaking. The wet disintegrated slurry was further diluted to 0.6% with tap water, the pH was adjusted to pH 6.8, and the conductivity was adjusted to 3.5 mS / cm. The salt used to adjust the conductivity consisted of 70% calcium acetate, 20% sodium sulfate and 10% sodium bicarbonate.

[0085] Chemical additions for batching were made to a dynamic drain tank type mixing vessel with a mixing speed of 1000 rpm.

[0086] GPAM sample 1, GPAM sample 2 and GPAM sample 3 from Example 3 were used as strength additives in the experiments. The metering amounts of dry additives per ton of dry batch were 1.2 and 2.4 kg / t.

[0087] The retention rate was kept constant in each test and an ash content of 16% was reached in the board. Cationic polyacrylamide CPAM (FennoPol K 3500P, Kemira Oyj) was dissolved to 0.5% and further diluted to a concentration of 0.05% and added as a retention aid 15 seconds before drainage. At test 0, the amount of cationic polyacrylamide was 400 g / t and the amount was adjusted according to the desired retention level in the other tests 1-6. Silica (FennoSil 2180, Kemira Oyj) was diluted to a concentration of 0.1% and metered in at 400 g / t (dry) 10 seconds before drainage as a retention aid.

[0088] Chemical additions are shown in Table 5.

[0089] After adding the chemicals, the batch was poured into the RK board former and the water was drained through the pipeline by suction. The board was removed from the pipeline and dried in a vacuum dryer (93°C, 10 minutes). Before laboratory testing, the boards were preconditioned for 24 hours at 23°C and 50% relative humidity according to ISO 187 standard. The method and equipment for board testing are shown in Table 4. The index strength value is calculated as the strength value divided by the basis weight. Beta formation was measured according to the instructions of the Ambertec equipment. The normalized beta formation is the same as the formation index of the Ambertec equipment.

[0090] The results of Example 4 are shown in Table 6.

[0091] As can be seen from Table 5, the GPAM samples produced according to the present invention significantly reduce the amount of cationic polyacrylamide required to obtain the desired retention level. This means that the retention polymer consumption is significantly and unexpectedly reduced. As can be seen from Table 6, SCT and burst index, which are important parameters for liner corrugated paper, are improved in all GPAM samples. The SCT value of GPAM sample 3 is the highest at 1.2 kg / t of measurement. CMT strength, which is an important parameter of fluted board (flutingboard) in addition to SCT, is also improved. Due to good forming, GPAM sample 1 obtains the highest CMT improvement. Low normalized forming indicates that forming is improved.

[0092] Table 4 Methods and equipment used to test the produced panels

[0093] Measurement equipment standard Basis Weight Mettler Toledo ISO 536 Short Span Compression Test (SCT) Lorentzen & Wettre ISO 9895 Bursting strength Lorentzen & Wettre ISO 2758 Corrugated paper core test (CMT30) Lorentzen & Wettre ISO 7263 Beta Forming Ambertec, Finland

[0094] Table 5 Chemical additions in Example 4

[0095]

[0096] Table 6 Results of Example 4.

[0097]

[0098] Example 5: Application example of evaluating the effect of different base polymers and glyoxal amounts on board properties

[0099] In Example 5, the effects of different polyacrylamide base polymers and glyoxal dosages on SCT (short span compressive strength), burst strength and compression resistance (corrugated core test (CMT30)) were tested.

[0100] The polyacrylamide base polymer used is a copolymer of acrylamide and DADMAC. Information on the molecular weight and amount of DADMAC in the base polymer is provided in Tables 7-9.

[0101] Use the pilot reactor identical with embodiment 2 to implement the in-situ glyoxylation process.The concentration of polyacrylamide base polymer in the reaction mixture is 4.4wt%, and various glyoxal amounts that can be seen from Tables 7-9 are tested.The initial glyoxal amount is 0.44wt% (10wt% dry state), 0.66 (15wt% dry state) and 0.88wt% (20wt% dry state) of the reaction mixture weight percentage.The glyoxylation reaction is started by adding the NaOH that is calculated to provide pH 9.1 for the reaction mixture.When measuring 33mPas Brookfield viscosity at 25 ℃, sulfuric acid (30%) is added to the reaction mixture to stop the glyoxylation reaction, so that the pH drops to 3-4.

[0102] Handsheets were prepared in the same manner as in Example 4 by using European recycled fiber for furnish. Glyoxylated polyacrylamide was added to the mixing vessel 60 seconds before board preparation. The ash content in the prepared board was 17%.

[0103] Table 7 Effect of glyoxal dosage

[0104]

[0105] As can be seen from Table 7, the GPAM produced provides relatively good results regardless of the amount of glyoxal used. It is expected that an amount of glyoxal of 10 wt% to 20 wt% may provide the best results.

[0106] Table 8 Effect of base polymer charge

[0107]

[0108] As can be seen from Table 8, Tests 10-13 provided better SCT index and burst strength values. This suggests that GPAM produced using a polyacrylate base polymer having a cationicity of 6 mol% to 18 mol% cationic units may be preferred.

[0109] Table 9 Effect of base polymer molecular weight

[0110]

[0111] As can be seen from Table 9, Run 18 and Run 19 provide better SCT index and burst strength values. This suggests that GPAM produced using a polyacrylate base polymer having a weight average molecular weight of 135,000-185,000 may be preferred.

[0112] Example 6: Application example to evaluate the effect of different base polymers and glyoxal amounts on strength and risk of score cracking at high humidity

[0113] The effects of different polyacrylamide base polymers and glyoxal amounts on SCT (short span compressive strength), SCT at 85% relative humidity (RH), and tensile energy absorption (TEA) were tested in Example 6. An increase in TEA indicates a lower risk of scarring.

[0114] The polyacrylamide base polymer used is a copolymer of acrylamide and DADMAC. Information on the molecular weight of the base polymer and the amount of DADMAC (base polymer loading) is provided in Table 10.

[0115] The in-situ glyoxylation process was carried out by using the same pilot reactor as in Example 2. The glyoxylation reaction was started by adding NaOH calculated to provide the reaction mixture with a pH of 9.1. The glyoxylation reaction was terminated by adding sulfuric acid (30%) to the reaction mixture when the Brookfield viscosity was 25-35 mPas measured at 25°C, whereby the pH dropped to 3-4.

[0116] Handsheets were prepared in the same general manner as in Example 4 by using European recycled fiber for furnish. The furnish was wet disintegrated at 70°C at 3% consistency using a pulper (Noviprofiber, France) at 500 rpm for 30 seconds and wet disintegrated at 1000 rpm for 25 minutes without soaking. The wet disintegrated pulp was further diluted to 0.6% consistency with tap water, the pH was adjusted to 6.8 and the conductivity was adjusted to 3.0 mS / cm. The salt used to adjust the conductivity consisted of 70% calcium acetate, 20% sodium sulfate and 10% sodium bicarbonate. Glyoxylated polyacrylamide was added to the mixing container 60 seconds before board preparation. The ash content in the prepared board was 16%. The glyoxylated polyacrylamide dosage used in the preparation of handsheets for each experiment is shown in Table 10.

[0117] TEA values ​​were measured from the air-conditioned sheets using a Lorenzen & Wettre tensile tester at 50% RH and 23°C according to ISO standard 1924-3. For SCT measurements at 85% RH, the test strips were air-conditioned at 85% RH and 23°C for at least 4 hours and then transferred in a plastic bag to the Lorenzen & Wettre SCT (STFI) measurement. The SCT measurement was performed immediately after the sample was removed from the plastic bag. No moisture correction of the test equipment was used to verify the actual strength at high humidity.

[0118] The SCT, SCT at 85% RH, and TEA results were indexed by dividing the measured strength results by the basis weight of the board to improve the accuracy of the comparison.

[0119] The results are shown in Table 10. Tests 32, 35, 36 and 37 were implemented for a 14 mol% loading level in the base polymer. Tests 34-38 using high molecular weight base polymers significantly reduced the amount of glyoxal added in the solution (<1%) compared to tests 32 and 33. This has a significant safety advantage in manufacturing, as well as an advantage when the final paper or paperboard is specifically used for food contact purposes. The test results of tests 35-37 show that the high molecular weight of the base polymer and the dry solids content of the reaction mixture increase the values ​​of TEA, SCT and SCT under high humidity. Tests 33 and 38 were completed with a 23 mol% loading in the base polymer, while test 34 was completed with a 5.5 mol% loading. The results of test 38 show that TEA, SCT and SCT values ​​under high humidity are particularly improved with the high molecular weight of the base polymer and the higher base polymer charge. The results in Table 10 generally show that when the aqueous reaction mixture described in the present application is used for in-situ glyoxylation, SCT under high humidity can be surprisingly improved. Increasing the dosage of glyoxylated polyacrylamide to 3 kg / t even further improved the SCT at high humidity. It can also be seen from Table 10 that the scarring can be reduced when the molecular weight and base polymer loading (charge) are properly selected based on the measured TEA results. The tested glyoxal levels of 9%-20% work well in this application.

[0120] Table 10 Basic polymer properties, glyoxylation reaction parameters and final viscosity of the obtained polymer compositions

[0121]

[0122]

[0123] It is obvious to a person skilled in the art that the invention is not limited to the embodiments described above, but that the invention can be varied within the scope of the appended claims.

Claims

1. A method for in-situ glyoxylation of polyacrylamide in a paper or board mill, wherein a discontinuous batch glyoxylation reaction of an aqueous reaction mixture is carried out in a reaction vessel equipped with a driven stirrer to form an aqueous polymer composition comprising glyoxylated polyacrylamide for use in the paper or board manufacturing process, said method include: - forming or obtaining an aqueous reaction mixture comprising a polyacrylamide base polymer and glyoxal; - Determining the base consumption of the reaction mixture by titration, wherein the polyacrylamide base polymer is diluted, an alkaline solution is added and titrated to the target pH at 25°C and the amount of base required is recorded, then glyoxal is added to the polyacrylamide base polymer, the reaction mixture is mixed for 1 minute at 25°C and the pH is recorded; - adding to the reaction mixture a predetermined amount of base required to adjust the pH value of the reaction mixture to a range of 8-10 based on the determined base consumption; - optionally adjusting the temperature of the reaction mixture to a temperature range of 15-40°C; - allowing the polyacrylamide base polymer in the reaction mixture to undergo an in situ glyoxylation reaction; - measuring the viscosity of the reaction mixture and / or a process variable related to the viscosity of the reaction mixture; - when a predetermined final viscosity value is reached, adding an acid to the reaction mixture to reduce the pH of the reaction mixture to <8; and - Removing the aqueous polymer composition comprising the glyoxylated polyacrylamide from the reaction vessel.

2. The method according to claim 1, It is characterized in that The aqueous polymer composition is transferred from the reaction vessel to the paper or paperboard manufacturing process via a pipeline via an optional storage container.

3. The method according to claim 1 or 2, It is characterized in that The weight average molecular weight of the polyacrylamide base polymer is in the range of 50 000-300 000 g / mol.

4. The method according to claim 1 or 2, It is characterized in that The polyacrylamide base polymer is obtained by polymerization of acrylamide and 7 mol % to 50 mol % of a hydrolytically stable cationic monomer.

5. The method according to claim 1 or 2, It is characterized in that The reaction mixture has a solid content of 2 wt% to 8 wt%.

6. The method according to claim 1 or 2, It is characterized in that The reaction time of the in-situ glyoxylation reaction is in the range of 10-120 minutes.

7. The method according to claim 1 or 2, It is characterized in that The polyacrylamide base polymer and glyoxal are provided as an acidic premix for forming the reaction mixture.

8. The method according to claim 1 or 2, It is characterized in that During the glyoxylation an additional stream of base is fed to the reaction mixture.

9. The method according to claim 1 or 2, It is characterized in that The temperature of the reaction mixture is measured and regulated during the entire glyoxylation reaction.

10. The method according to claim 1 or 2, It is characterized in that The viscosity of the reaction mixture was measured by measuring the torque of the electric stirrer.

11. The method according to claim 1 or 2, It is characterized in that The viscosity of the reaction mixture is measured from the reaction mixture by using a rotational viscometer, an oscillation viscometer, or a vibration viscometer.

12. The method according to claim 1 or 2, It is characterized in that The initial viscosity of the reaction mixture was in the range of 4-15 cP.

13. The method according to claim 1 or 2, It is characterized in that The predetermined final viscosity value is in the range of 20-60 cP.

14. The method according to claim 1 or 2, It is characterized in that The predetermined final viscosity value is 2-7 times the initial viscosity of the reaction mixture.

15. The method according to claim 1 or 2, It is characterized in that The aqueous polymer composition comprises 0.1 wt% to 1.5 wt% of residual glyoxal, calculated based on the total weight of the aqueous polymer composition.

Citation Information

Patent Citations

  • High Molecular Weight and High Cationic Charge Glyoxalated Polyacrylamide Copolymers and Their Methods of Manufacture and Use

    US20160201269A1

  • An On-Line Control and Reaction Process for pH Adjustment

    US20170342663A1