A Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array and its preparation method and application

By growing Mn-doped CoP nanowires on the carbon fiber cloth substrate and wrapping Ni(PO3)2 nanoclusters to form a dense heterojunction array, the problem of low electrocatalytic efficiency of cobalt-based phosphides is solved, and the electrocatalytic water is significantly improved Decomposition performance.

CN115161694BActive Publication Date: 2024-11-26JIANGSU QINA HYDROGEN ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210834149.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-14
Publication Date
2024-11-26
Estimated Expiration
2042-07-14

AI Technical Summary

Technical Problem

Cobalt-based phosphides are inefficient in electrocatalytic water decomposition, especially in alkaline electrolytes, and their adsorption capacity is insufficient, and their activity in a specific pH environment is incompatible, which limits their symmetric double electrodes. Overall water decomposition performance in the system.

Method used

Using Mn-doped CoP nanowire composite Ni(PO3) 2 nanocluster heterojunction array, dense heterojunction array is formed by growing Mn-doped CoP nanowires on the carbon fiber cloth substrate and wrapping Ni(PO3) 2 nanoclusters. The junction array was prepared by a hydrothermal method and a solvent thermal method combined with a one-step low-temperature phosphating process.

Benefits of technology

It achieves excellent performance in electrocatalytic HER and OER, improves the efficiency of electrocatalytic decomposition of water, and is simple in preparation and is easy to promote.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115161694B_ABST
    Figure CN115161694B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of nano-electrocatalytic materials, and in particular to a Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array, and a preparation method and application thereof. The preparation method of the heterojunction array is easy to promote, and only requires a simple chemical solution reaction combined with a one-step low-temperature phosphating treatment. The Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array includes a carbon fiber cloth substrate and a heterojunction array grown on the surface of the carbon fiber cloth, and the heterojunction array is composed of Mn-doped CoP and Ni(PO3)2. The Mn-doped CoP grows approximately vertically on the carbon fiber cloth substrate in the form of nanowires, and the surface of the nanowires is uniformly wrapped with Ni(PO3)2 nanoclusters. Thanks to the Mn element doping and the unique cobalt phosphide / phosphate heterogeneous interface, this heterojunction array has excellent performance in electrocatalytic water decomposition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of preparation and application of nano electrocatalytic materials, and in particular to a Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array and a preparation method and application thereof. Background Art

[0002] With the explosive growth of the world's population and the acceleration of industrialization, energy shortage has become a stumbling block to the further development of human society. Fossil energy, as the main body of the world's energy structure, is not only insufficient in reserves and unevenly distributed, but also causes major environmental pollution problems. Therefore, the development of renewable clean energy (such as hydrogen energy) is particularly urgent. Electrocatalytic water splitting, as an efficient and environmentally friendly method for hydrogen production, has received widespread attention in recent years. Precious metal materials (especially platinum and ruthenium / iridium) are efficient catalysts for electrocatalytic water splitting. However, due to their scarce reserves and high costs, they have great limitations in industrial use. Exploring economical and efficient electrocatalysts and optimizing their electrocatalytic performance has become a research hotspot. In recent years, transition metal oxides, sulfides, selenides, phosphides and carbides have been developed one after another. Among these catalysts, Co-based phosphides (including CoP, Co2P and CoP3) are considered to be highly competitive and promising alternatives to precious metal catalysts due to their abundant sources, good conductivity and rich redox sites. However, the weak water dissociation process and poor adsorption of reaction intermediates greatly limit the electrocatalytic efficiency of cobalt-based phosphides, especially in alkaline electrolytes. In addition, due to the incompatibility of hydrogen evolution reaction (HER) and oxygen evolution reaction (OER) activities of cobalt-based phosphides in specific pH environments, achieving efficient overall water splitting in a symmetric two-electrode system remains a challenge.

[0003] In order to overcome the above-mentioned inherent defects of Co-based phosphides, the introduction of second-phase or third-phase metal elements to construct bimetallic or trimetallic phosphides has become a common strategy. It is reported that the introduction of second-phase or third-phase metal elements (such as Fe, Ni, Mo, Cu, Mn, etc.) can effectively optimize the surface electronic structure of Co-based phosphides, making them have more active centers, thereby improving their intrinsic electrocatalytic activity. Among the various metal elements used to dope Co-based phosphides, manganese (Mn) is particularly promising because of its higher electronegativity than most metal elements, which can greatly promote electron transport and adjust the electronic structure. However, current research on Mn-doped Co-based phosphides mainly focuses on powder material systems. Due to the limitations of active center exposure and charge transfer capacity, their electrocatalytic performance is still unsatisfactory.

[0004] In addition to doping with metal elements, constructing heterointerfaces by integrating different catalysts is another effective means to improve the electrocatalytic performance of Co-based phosphide catalysts. The results show that rich heterointerfaces can not only expose more reaction sites and accelerate the electron transfer rate, but also achieve the synchronous adsorption of reaction intermediates. However, in fact, due to weak interfacial interactions and mismatched band structures, in many cases, it is difficult to form a dense and rich heterointerface between two different catalysts, which makes it difficult to achieve effective transfer of the carrier at the interface, limiting the full utilization of the efficiency of the heterointerface. Therefore, exploring cobalt-based phosphide heterostructures with dense and rich heterointerfaces remains a huge challenge. Summary of the invention

[0005] The purpose of the present invention is to provide a Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array and a preparation method thereof, so as to solve the problem of low efficiency of existing cobalt-based phosphide electrocatalytic water decomposition.

[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions.

[0007] The Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array provided by the present invention comprises a carbon fiber cloth substrate and a heterojunction array grown on the surface of the carbon fiber cloth; the heterojunction array is composed of Mn-doped CoP and Ni(PO3)2. The Mn-doped CoP grows approximately vertically on the carbon fiber cloth substrate in the form of nanowires, the nanowires have a diameter of 50 to 100 nm and a length of 1 to 5 μm, the surface of the nanowires is uniformly coated with Ni(PO3)2 nanoclusters, and the size of the nanoclusters is about 2 nm.

[0008] Preferably, the substrate is carbon fiber cloth.

[0009] The method for preparing the Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array provided by the present invention comprises the following steps:

[0010] Step (1), before growth, firstly, ultrasonically clean the carbon fiber cloth substrate in acetone, deionized water and anhydrous ethanol in sequence to remove the surface oxide layer and organic matter;

[0011] Step (2), growing CoMn double hydroxide nanowire arrays on the surface of a carbon fiber cloth substrate by a hydrothermal method; specifically, dissolving Mn(NO3)2·4H2O (manganese nitrate), Co(NO3)2·6H2O (cobalt nitrate hexahydrate), NH4F (ammonium fluoride) and urea in 70-80 mL of deionized water in a molar ratio of 1:(1.5-3):(5-10):(10-20) in sequence, and forming a uniform solution under ultrasonic treatment; transferring the solution to a 100 mL stainless steel autoclave, and then obliquely inserting the washed carbon fiber cloth substrate into the solution; maintaining the autoclave at 100-120° C. for 3-10 hours; after the reaction is completed, taking out the carbon fiber cloth, washing it alternately with deionized water and anhydrous ethanol, and finally placing the washed carbon fiber cloth in an oven and drying it at 70° C. for 2-8 hours to obtain a CoMn double hydroxide nanowire array;

[0012] Step (3), using a solvothermal method to wrap Ni(OH)2 nanosheets on the surface of the CoMn double hydroxide nanowire array to obtain a composite hydroxide heterostructure array; specifically, Ni(NO3)2·6H2O (nickel nitrate hexahydrate) and hexamethylenetetramine (HMT) are dissolved in 30 mL of ethanol at a molar ratio of 1: (5-10) to form a uniform solution, and the solution is transferred to a 100 mL stainless steel autoclave; then the double hydroxide nanowire array obtained in step (2) is inserted into the solution, and the autoclave is maintained at 120-140°C for 2-6 hours. After the reaction is completed, the carbon fiber cloth is taken out, and alternately washed with deionized water and anhydrous ethanol, and finally the washed carbon fiber cloth is placed in an oven and dried at 70°C for 2-8 hours to obtain a composite hydroxide heterostructure array.

[0013] Step (4), using a one-step low-temperature phosphating process, converts the above-mentioned composite hydroxide heterostructure array into the final product, i.e., a Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array. Specifically, the composite hydroxide heterostructure array obtained in step (3) and 0.5-1.5g of sodium hypophosphite (NaH2PO2) are placed in a quartz boat respectively, and then the quartz boats are placed in a tube furnace, set to calcine at 300°C in an argon atmosphere for 1-4 hours, to obtain a Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array.

[0014] Preferably, in step (2), the molar ratio of Mn(NO3)2·4H2O, Co(NO3)2·6H2O, NH4F and urea is 1:2:6:12.

[0015] Preferably, in step (3), the molar ratio of Ni(NO3)2·6H2O to hexamethylenetetramine (HMT) is 1:8.7.

[0016] The Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array provided by the present invention can be used as a high-efficiency electrocatalyst for electrocatalytic water decomposition reaction.

[0017] The technical effects of the present invention are: (1) The heterojunction array preparation method is easy to promote, and only requires a simple chemical solution reaction combined with a one-step low-temperature phosphating treatment; (2) The prepared phosphide / phosphate heterojunctions are arranged in an array form on a carbon fiber substrate, with good charge transfer efficiency and abundant heterogeneous interface contacts; (3) This heterojunction array enables the product Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array to have excellent performance in both electrocatalytic HER and OER. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 Scanning electron microscope (SEM) and transmission electron microscope (TEM) photographs of the Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array prepared by the present invention and comparative samples.

[0019] Figure 2 X-ray diffraction (XRD) patterns of the Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array prepared by the present invention and a comparative sample.

[0020] Figure 3 The electrocatalytic HER performance curves of the Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array prepared by the present invention and the comparative sample.

[0021] Figure 4 This is a graph showing the electrocatalytic OER performance of the Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array prepared in the present invention and a comparative sample. DETAILED DESCRIPTION

[0022] The technical solution of the present invention and its beneficial effects will be described in detail below in conjunction with the accompanying drawings and specific embodiments, aiming to help readers better understand the essence of the present invention, but shall not constitute any limitation on the implementation and protection scope of the present invention.

[0023] In the following embodiments, before the growth of Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction arrays, the carbon fiber cloth substrate required for the growth is first treated by the following steps: the carbon fiber cloth substrate is ultrasonically washed in acetone, deionized water and anhydrous ethanol in sequence to remove the surface oxide layer and organic matter.

[0024] Preparation Example 1:

[0025] First, a CoMn double hydroxide nanowire array was grown on the surface of a carbon fiber cloth substrate by a hydrothermal method; specifically, Mn(NO3)2·4H2O, Co(NO3)2·6H2O, NH4F and urea were dissolved in 80 mL of deionized water in a molar ratio of 1:2:6:12, and a uniform solution was formed under ultrasonic treatment. The solution was transferred to a 100 mL stainless steel autoclave, and then the cleaned carbon fiber cloth substrate was obliquely inserted into the solution. The autoclave was kept at 100°C for 5 hours. After the reaction was completed, the carbon fiber cloth was taken out and alternately washed with deionized water and anhydrous ethanol. Finally, the washed carbon fiber cloth was placed in an oven and dried at 70°C for 8 hours to obtain a CoMn double hydroxide nanowire array. Secondly, the Ni(OH)2 nanosheets were coated on the surface of the CoMn double hydroxide nanowire array by a solvothermal method; specifically, Ni(NO3)2·6H2O and hexamethylenetetramine (HMT) were dissolved in 30mL ethanol at a molar ratio of 1:8.7 to form a uniform solution, which was then transferred to a 100mL stainless steel autoclave. The double hydroxide nanowire array obtained in the above steps was then inserted into the solution, and the autoclave was kept at 120°C for 4h. After the reaction was completed, the carbon fiber cloth was taken out and washed alternately with deionized water and anhydrous ethanol. Finally, the washed carbon fiber cloth was placed in an oven and dried at 70°C for 8 hours to obtain a composite hydroxide heterostructure array. Finally, a one-step low-temperature phosphating process is used to convert the above-mentioned composite hydroxide heterostructure array into the final product; specifically, the composite hydroxide heterostructure array obtained in the above step and 1g of sodium hypophosphite (NaH2PO2) are placed in a quartz boat respectively, and then the quartz boat is placed in a tube furnace and calcined at 300°C in an argon atmosphere for 2 hours to obtain a Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array.

[0026] Preparation Example 2:

[0027] First, a CoMn double hydroxide nanowire array was grown on the surface of a carbon fiber cloth substrate by a hydrothermal method; specifically, Mn(NO3)2·4H2O, Co(NO3)2·6H2O, NH4F and urea were dissolved in 70 mL of deionized water in a molar ratio of 1:2:6:12, and a uniform solution was formed under ultrasonic treatment. The solution was transferred to a 100 mL stainless steel autoclave, and then the cleaned carbon fiber cloth substrate was obliquely inserted into the solution. The autoclave was kept at 110°C for 5 hours. After the reaction was completed, the carbon fiber cloth was taken out and alternately washed with deionized water and anhydrous ethanol. Finally, the washed carbon fiber cloth was placed in an oven and dried at 70°C for 6 hours to obtain a CoMn double hydroxide nanowire array. Secondly, the Ni(OH)2 nanosheets were coated on the surface of the CoMn double hydroxide nanowire array by a solvothermal method; specifically, Ni(NO3)2·6H2O and hexamethylenetetramine (HMT) were dissolved in 30mL ethanol at a molar ratio of 1:8.7 to form a uniform solution, which was then transferred to a 100mL stainless steel autoclave. The double hydroxide nanowire array obtained in the above steps was then inserted into the solution, and the autoclave was kept at 120°C for 5h. After the reaction was completed, the carbon fiber cloth was taken out and washed alternately with deionized water and anhydrous ethanol. Finally, the washed carbon fiber cloth was placed in an oven and dried at 70°C for 8 hours to obtain a composite hydroxide heterostructure array. Finally, a one-step low-temperature phosphating process is used to convert the above-mentioned composite hydroxide heterostructure array into the final product; specifically, the composite hydroxide heterostructure array obtained in the above step and 1g of sodium hypophosphite (NaH2PO2) are placed in a quartz boat respectively, and then the quartz boat is placed in a tube furnace and calcined at 300°C in an argon atmosphere for 2 hours to obtain a Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array.

[0028] Preparation Example 3:

[0029] First, a CoMn double hydroxide nanowire array was grown on the surface of a carbon fiber cloth substrate by a hydrothermal method; specifically, Mn(NO3)2·4H2O, Co(NO3)2·6H2O, NH4F and urea were dissolved in 70 mL of deionized water in a molar ratio of 1:2:6:12, and a uniform solution was formed under ultrasonic treatment. The solution was transferred to a 100 mL stainless steel autoclave, and then the cleaned carbon fiber cloth substrate was obliquely inserted into the solution. The autoclave was kept at 100°C for 6 hours. After the reaction was completed, the carbon fiber cloth was taken out and washed alternately with deionized water and anhydrous ethanol. Finally, the washed carbon fiber cloth was placed in an oven and dried at 70°C for 5 hours to obtain a CoMn double hydroxide nanowire array. Secondly, the Ni(OH)2 nanosheets were coated on the surface of the CoMn double hydroxide nanowire array by a solvothermal method; specifically, Ni(NO3)2·6H2O and hexamethylenetetramine (HMT) were dissolved in 30mL ethanol at a molar ratio of 1:8.7 to form a uniform solution, which was then transferred to a 100mL stainless steel autoclave. The double hydroxide nanowire array obtained in the above steps was then inserted into the solution, and the autoclave was kept at 130°C for 5h. After the reaction was completed, the carbon fiber cloth was taken out and washed alternately with deionized water and anhydrous ethanol. Finally, the washed carbon fiber cloth was placed in an oven and dried at 70°C for 6 hours to obtain a composite hydroxide heterostructure array. Finally, a one-step low-temperature phosphating process is used to convert the above-mentioned composite hydroxide heterostructure array into the final product; specifically, the composite hydroxide heterostructure array obtained in the above step and 1g of sodium hypophosphite (NaH2PO2) are placed in a quartz boat respectively, and then the quartz boat is placed in a tube furnace and calcined at 300°C in an argon atmosphere for 2 hours to obtain a Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array.

[0030] In the materials prepared in Preparation Examples 1 to 3, Mn-doped CoP grows approximately vertically on a carbon fiber cloth substrate in the form of nanowires, the nanowires have a diameter of 50 to 100 nm, and a length of 1 to 5 μm. The surface of the nanowires is evenly coated with Ni(PO3)2 nanoclusters, and the size of the nanoclusters is about 2 nm.

[0031] In order to confirm the unique advantages of the Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array prepared by the method of the present invention in the field of electrocatalysis, we used a similar method to synthesize two comparative materials, namely Mn-doped CoP nanowire array and Ni(PO3)2 nanocluster.

[0032] Preparation Comparative Example:

[0033] The carbon fiber cloth substrate required for growth is processed by the following steps: the carbon fiber cloth substrate is ultrasonically washed in acetone, deionized water and anhydrous ethanol in sequence to remove the surface oxide layer and organic matter.

[0034] The preparation of the comparative material Mn-doped CoP nanowire array is completed in the following steps: first, a CoMn double hydroxide nanowire array is grown on the surface of a carbon fiber cloth substrate by a hydrothermal method; specifically, Mn(NO3)2·4H2O, Co(NO3)2·6H2O, NH4F and urea are dissolved in 80mL of deionized water in a molar ratio of 1:2:6:12, and a uniform solution is formed under ultrasonic treatment. The solution is transferred to a 100mL stainless steel autoclave, and then the cleaned carbon fiber cloth substrate is obliquely inserted into the solution. The autoclave is kept at 100°C for 5h. After the reaction is completed, the carbon fiber cloth is taken out and alternately washed with deionized water and anhydrous ethanol. Finally, the washed carbon fiber cloth is placed in an oven and dried at 70°C for 8 hours to obtain a CoMn double hydroxide nanowire array. Secondly, the above-mentioned CoMn double hydroxide nanowire array is converted into the final product Mn-doped CoP nanowire array by a one-step low-temperature phosphating process. Specifically, the CoMn double hydroxide nanowire array obtained in the above steps and 1g of sodium hypophosphite (NaH2PO2) are placed in a quartz boat respectively, and then the quartz boat is placed in a tube furnace and calcined at 300°C for 2 hours in an argon atmosphere to obtain a comparison material Mn-doped CoP nanowire array.

[0035] The preparation of the comparative material Ni(PO3)2 nanoclusters was completed in the following steps: First, Ni(OH)2 nanosheets were grown on the surface of the carbon fiber cloth substrate by a solvothermal method; specifically, Ni(NO3)2·6H2O and hexamethylenetetramine (HMT) were dissolved in 30mL ethanol at a molar ratio of 1:8.7 to form a uniform solution, which was transferred to a 100mL stainless steel autoclave. The carbon fiber cloth substrate was then inserted into the solution, and the autoclave was kept at 120°C for 4h. After the reaction was completed, the carbon fiber cloth was taken out and washed alternately with deionized water and anhydrous ethanol, and finally the washed carbon fiber cloth was placed in an oven and dried at 70°C for 8 hours. Secondly, a one-step low-temperature phosphating process was used to convert Ni(OH)2 nanosheets into Ni(PO3)2 nanoclusters. Specifically, Ni(OH)2 nanosheets and 1g of sodium hypophosphite (NaH2PO2) were placed in a quartz boat respectively, and then the quartz boat was placed in a tubular furnace and calcined at 300°C for 2 hours in an argon atmosphere to obtain the comparison material Ni(PO3)2 nanoclusters.

[0036] The Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array prepared by the method of the present invention can be used as an electrocatalyst for electrocatalytic water decomposition reaction. The electrocatalytic HER and OER performances of the Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array and two comparative materials were tested, and the test technical scheme was: the electrocatalytic performance was tested using a three-electrode system of an electrochemical workstation. A graphite rod electrode was used as the counter electrode, and a saturated calomel electrode was used as the reference electrode. The heterojunction array grown on a carbon fiber cloth substrate was cut into 3mm×3mm and used as a working electrode for testing. A 1M KOH aqueous solution was used as the electrolyte. The polarization curve was measured by linear sweep voltammetry, and the scan rate was set to 0.002V / s. All measured potentials were converted into reversible hydrogen electrode potentials.

[0037] Figure 1 The following are scanning electron microscope (SEM) and transmission electron microscope (TEM) photos of the Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array prepared by the present invention and a comparative sample. Figure 1 As can be seen from (a) to (c), a uniform Mn-doped CoP nanowire array with a length of several microns and a diameter of about 50 to 100 nm is densely grown on the carbon fiber cloth substrate. The high-resolution TEM image clearly shows the lattice fringes with a lattice spacing of 0.284 nm (e.g. Figure 1 (d) corresponds to the {011} plane of orthorhombic CoP. Figure 1 (e) to (g) are morphological images of Mn-doped CoP nanowires composite Ni(PO3)2 nanocluster heterojunction arrays. It can be found that nanoclusters with a size of about 2 nm are uniformly wrapped on the surface of the nanowires to form a dense core-shell heterostructure. Figure 1 In the high-resolution TEM image shown in (h), two lattice fringes with interplanar spacings of 0.208 nm and 0.216 nm can be observed, corresponding to the (210) crystal plane of CoP and the (411) crystal plane of Ni(PO3)2, respectively. In summary, manganese doping and surface phosphate recombination can be achieved simultaneously through a simple low-temperature phosphating treatment. Figure 1 The element mapping image shown in (i) shows the uniform distribution of each element in the Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array prepared by the present invention.

[0038] Figure 2The X-ray diffraction (XRD) patterns of the Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array prepared by the present invention and the comparative sample; wherein (a) is the X-ray diffraction (XRD) pattern of the Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array, (b) is the X-ray diffraction (XRD) pattern of the comparative sample Mn-doped CoP nanowire array, and (c) is the X-ray diffraction (XRD) pattern of the comparative sample Ni(PO3)2 nanocluster. It can be seen from the spectrum that the characteristic peaks of the comparative material Mn-doped CoP nanowire array are located at 31.8°, 36.3°, 46.2°, 48.1° and 56.7°, respectively, corresponding to the (011), (111), (112), (211) and (301) crystal planes of the orthorhombic phase CoP standard card (JCPDS No.29-0497), indicating that the introduction of Mn does not form a new phase. The characteristic peaks of the comparative material Ni(PO3)2 nanoclusters are consistent with the monoclinic Ni(PO3)2 (JCPDSNo.28-0708). The strong peak near 26° corresponds to the carbon fiber cloth substrate. The XRD peaks of the heterojunction array of Mn-doped CoP nanowires composite Ni(PO3)2 nanoclusters simultaneously show typical signals of orthorhombic CoP and monoclinic Ni(PO3)2, which indicates the formation of a heterostructure.

[0039] Figure 3 The electrocatalytic HER performance curves of the Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array prepared by the present invention and the comparative sample are shown in FIG. 1 . It can be seen that the performance of the Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array is significantly better than that of the comparative material Mn-doped CoP nanowire array and the comparative material Ni(PO3)2 nanocluster. When the current density is 10 and 20 mA / cm 2 When the overpotential of Mn-doped CoP nanowires and Ni(PO3)2 nanocluster heterojunction arrays is 116 and 130 mV, respectively, which is significantly lower than that of the comparative materials. Its excellent performance comes from the synergistic effect of Mn doping and heterojunction composite.

[0040] Figure 4 The electrocatalytic OER performance curves of the Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array prepared by the present invention and the comparative sample are shown in Figure 2. 2 The overpotential value (245 mV) of the prepared material is significantly lower than that of the comparative material, indicating that it has a more excellent OER performance.

[0041] The embodiments described above are merely descriptions of preferred implementation modes of the present invention and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array, characterized in that: It includes a carbon fiber cloth substrate and a heterojunction array grown on the surface of the carbon fiber cloth; the heterojunction array is composed of Mn-doped CoP and Ni(PO3)2; the Mn-doped CoP grows approximately vertically on the carbon fiber cloth substrate in the form of nanowires, with a diameter of 50 to 100 nm and a length of 1 to 5 μm, and the surface of the nanowires is evenly coated with Ni(PO3)2 nanoclusters, and the size of the nanoclusters is about 2 nm.

2. The method for preparing the Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array according to claim 1, characterized in that: The following steps are involved: Firstly, CoMn double hydroxide nanowire arrays were grown on the surface of carbon fiber cloth substrate by hydrothermal method. Then, Ni(OH)2 nanosheets were wrapped on the surface of CoMn double hydroxide nanowire array by solvothermal method, i.e., Ni(NO3)2·6H2O and hexamethylenetetramine were dissolved in ethanol to form a uniform solution, and the solution and CoMn double hydroxide nanowire arrays were transferred to a stainless steel autoclave for reaction to obtain composite hydroxide heterostructure arrays. Finally, a one-step low-temperature phosphating process was used to place the composite hydroxide heterostructure array and sodium hypophosphite obtained above in a quartz boat, respectively, and then the quartz boat was placed in a tube furnace and calcined in an argon atmosphere to convert into the final product, i.e., a Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array; The specific steps of growing CoMn double hydroxide nanowire arrays on the surface of a carbon fiber cloth substrate by a hydrothermal method are as follows: dissolving Mn(NO3)2·4H2O, Co(NO3)2·6H2O, NH4F and urea in 70-80 mL of deionized water in a molar ratio of 1:(1.5-3):(5-10):(10-20) in sequence, and forming a uniform solution under ultrasonic treatment; transferring the solution to a 100 mL stainless steel autoclave, and then obliquely inserting the washed carbon fiber cloth substrate into the solution; maintaining the autoclave at 100-120° C. for 3-10 hours; after the reaction is completed, taking out the carbon fiber cloth, washing it alternately with deionized water and anhydrous ethanol, and finally placing the washed carbon fiber cloth in an oven and drying it at 70° C. for 2-8 hours to obtain a CoMn double hydroxide nanowire array.

3. The preparation method according to claim 2, characterized in that: The specific steps of obtaining the composite hydroxide heterostructure array by the solvothermal method are as follows: dissolving Ni(NO3)2·6H2O and hexamethylenetetramine in 30 mL of ethanol at a molar ratio of 1:(5-10) to form a uniform solution, and transferring it to a 100 mL stainless steel autoclave; then inserting the obtained CoMn double hydroxide nanowire array into the solution, and maintaining the autoclave at 120-140°C for 2-6 hours; after the reaction is completed, taking out the carbon fiber cloth, washing it alternately with deionized water and anhydrous ethanol, and finally placing the washed carbon fiber cloth in an oven and drying it at 70°C for 2-8 hours to obtain the composite hydroxide heterostructure array.

4. The preparation method according to claim 2, characterized in that: The specific steps of the one-step low-temperature phosphating process are: placing the obtained composite hydroxide heterostructure array and 0.5-1.5g of sodium hypophosphite in a quartz boat respectively, and then placing the quartz boat in a tube furnace, setting the argon atmosphere at 300°C for calcination for 1-4 hours to obtain a Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array.

5. The preparation method according to claim 2, characterized in that: The molar ratio of Mn(NO3)2·4H2O, Co(NO3)2·6H2O, NH4F and urea is 1:2:6:

12.

6. The preparation method according to claim 3, characterized in that: The molar ratio of Ni(NO3)2·6H2O to hexamethylenetetramine is 1:8.

7.

7. Application of the Mn-doped CoP nanowire composite Ni(PO3)2 nanocluster heterojunction array in electrocatalytic water decomposition according to claim 1, characterized in that: This heterojunction array material can be used as an electrocatalyst for HER and OER reactions.