Polyimide COF material containing porphyrin unit, electrode and preparation method

By preparing polyimide COF materials containing porphyrin units, the stability problems of inorganic electrode materials and the performance problems of traditional organic electrode materials have been solved, and electrode materials with high specific capacity and good conductivity have been achieved, which are suitable for lithium-ion batteries.

CN119019685AActive Publication Date: 2024-11-26JIANGXI NORMAL UNIV

Patent Information

Application Number
CN202411119848.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

Existing inorganic electrode materials suffer from irreversible phase transitions, high costs, and significant regional variations, while traditional organic electrode materials suffer from low specific capacity and poor conductivity, all of which affect the stability and performance of batteries.

Method used

Polyimide COF materials containing porphyrin units were prepared by polymerizing 5,10,15,20-tetra(4-aminophenyl)porphyrin with acid anhydride to form an organic covalent framework, which was then combined with conductive carbon black and polyvinylidene fluoride and coated onto copper foil to prepare electrodes.

Benefits of technology

It improves charge transport efficiency, enhances the contact between electrode materials and electrolyte, and improves the specific capacity and stability of the battery, making it suitable for high-performance lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019685A_ABST
    Figure CN119019685A_ABST
Patent Text Reader

Abstract

The invention discloses a porphyrin unit-containing polyimide COF material, an electrode and a preparation method, and relates to the technical field of battery electrode materials.The preparation method comprises the steps that 5, 10, 15, 20-tetra (4-aminophenyl) porphyrin and an anhydride-containing solvent are subjected to a polymerization reaction and transferred into a hydrothermal reaction kettle for a reaction, and porphyrin unit-containing polyimide COF of an organic covalent framework is obtained; and washing, removing the solvent, and drying to obtain the porphyrin unit-containing polyimide COF material. And adding the porphyrin unit-containing polyimide COF material, conductive carbon black and polyvinylidene fluoride into N-methyl pyrrolidone, stirring, and smearing on a copper foil to obtain the electrode. The porphyrin unit-containing polyimide COF material has the beneficial effects that the porphyrin unit-containing polyimide COF material contains a large number of active sites, the charge transfer efficiency of the material can be effectively improved, the problems that small organic molecules are easily dissolved in an electrolyte material, the specific capacity is low, the conductivity is poor and the like are solved, and the specific capacity and the capacity retention rate are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery electrode materials, and in particular relates to a polyimide COF material containing a porphyrin unit, an electrode and a preparation method. Background Art

[0002] With the increasing depletion of fossil energy and the intensification of environmental pollution, energy and environmental issues have become two key challenges facing mankind, and secondary batteries have become one of the important ways to solve the problem. At present, the electrode materials of secondary batteries are mainly concentrated in inorganic materials. These materials use the valence change of transition metals to achieve ion storage, but at the same time they are prone to irreversible phase change, which seriously affects the stability and rate performance of the battery. In addition, inorganic electrode materials are heavily dependent on transition metal resources, have high costs and regional distribution differences, which is not conducive to long-term environmentally friendly development. Therefore, it is urgent to develop clean and replaceable electrode materials. Organic electrode materials have shown broad application prospects with their excellent performance and environmental friendliness. In particular, organic materials rich in conjugated structures have become an important direction for future electrode material research due to their efficient charge transfer ability and structural diversity. Through molecular design, these materials can achieve structural controllability, thereby optimizing battery performance and meeting the needs of different application scenarios. With the continuous advancement of energy technology and the enhancement of environmental awareness, clean and efficient organic electrode materials will play an increasingly important role in lithium-ion batteries and other energy storage devices, providing a solid guarantee for achieving a sustainable energy future. Summary of the invention

[0003] The purpose of the present invention is to solve at least one of the technical problems existing in the prior art, and to provide a polyimide COF material, electrode and preparation method containing porphyrin units, aiming to overcome the technical difficulties such as low specific capacity and poor conductivity of traditional organic electrode materials. The present invention prepares a series of polyimide COF materials containing porphyrin units, and the polyimide COF materials containing porphyrin units can not only provide abundant redox sites, but also significantly improve the charge transfer efficiency of the material. The present invention effectively solves the problems of small organic molecules being easily soluble in electrolytes, low specific capacity of organic electrode materials and poor conductivity. The porous structure of the COF material can also make the electrode material fully contact with the electrolyte, so that the material shows excellent performance and stability in secondary batteries. The organic electrode material of the present invention has high specific capacity and good conductivity, and can be widely used in high-performance lithium-ion batteries.

[0004] The technical solution of the present invention is as follows: In a first aspect, the present invention provides a method for preparing a polyimide COF material containing a porphyrin unit, comprising the following steps: The 5,10,15,20-tetrakis(4-aminophenyl)porphyrin is polymerized with a solvent containing anhydride to obtain a polyamic acid solution containing porphyrin units; The polyamic acid solution containing porphyrin units is transferred to a hydrothermal reactor for reaction to obtain an organic covalent framework polyimide COF containing porphyrin units; The polyimide COF containing porphyrin units of the organic covalent framework is cleaned with a solvent, and then the solvent is removed and dried to obtain a polyimide COF material containing porphyrin units.

[0005] Optionally, the acid anhydride includes at least one of BPDA, PMDA, and NTCDA.

[0006] Optionally, the molar ratio of the 5,10,15,20-tetrakis(4-aminophenyl)porphyrin to the acid anhydride is 0.5-1.5:1.5-2.5, preferably 0.7-1.3:1.7-2.3, and more preferably 0.9-1.1:1.9-2.1.

[0007] Optionally, the mass fraction of the porphyrin unit-containing polyamic acid solution is 0.5% to 5%, preferably 1% to 5%, and more preferably 2% to 5%.

[0008] Optionally, the solvent is N,N-dimethylacetamide.

[0009] Optionally, the amount of the solvent added is 27.7-290 times the mass of 5,10,15,20-tetrakis(4-aminophenyl)porphyrin.

[0010] Optionally, the polymerization reaction is carried out at -5 to 5°C for 3 to 6 hours, preferably at -4 to 4°C for 4 to 6 hours, and more preferably at -3 to 3°C for 4 to 5 hours.

[0011] Optionally, the reaction temperature of the porphyrin unit-containing polyamic acid solution in the hydrothermal reactor is 140-200°C, and the reaction time is 64-96 hours. Preferably, the reaction temperature is 160-200°C, and the reaction time is 68-96 hours; more preferably, the reaction temperature is 180-200°C, and the reaction time is 72-96 hours.

[0012] Optionally, the polyimide COF containing porphyrin units is centrifuged 3-5 times with N,N-dimethylacetamide until the eluate is colorless and transparent, and then ultrasonically treated with deionized water for 0.5-1.5 hours to replace the high-boiling point DMAC, and freeze-dried to obtain a polyimide COF material containing porphyrin units.

[0013] In a second aspect, the present invention provides a polyimide COF material containing a porphyrin unit, which is prepared by the above method.

[0014] In a third aspect, the present invention provides a method for preparing an electrode, wherein the porphyrin unit-containing polyimide COF material prepared by the above method or the porphyrin unit-containing polyimide COF material and the above porphyrin unit-containing polyimide COF material are added with N-methylpyrrolidone, wherein the amount of conductive carbon black added is 5%-30% of the mass of the porphyrin unit-containing polyimide COF material, and the amount of polyvinylidene fluoride added is 5%-20% of the mass of the porphyrin unit-containing polyimide COF material, stirred for 5-10 hours, and then applied on copper foil with a thickness of 30-80 mm to obtain an electrode.

[0015] Preferably, the amount of conductive carbon black added is 5%-20% of the mass of the polyimide COF material containing porphyrin units, and the amount of polyvinylidene fluoride added is 5%-15% of the mass of the polyimide COF material containing porphyrin units; more preferably, the amount of conductive carbon black added is 5%-15% of the mass of the polyimide COF material containing porphyrin units, and the amount of polyvinylidene fluoride added is 5%-10% of the mass of the polyimide COF material containing porphyrin units. In a fourth aspect, the present invention provides an electrode, which is prepared using the above method.

[0016] The present invention has at least one of the following beneficial effects: The porphyrin unit-containing polyimide COF material prepared by the present invention contains a large number of active sites, which can effectively improve the charge transfer efficiency of the material. The porous structure of the COF material can also enable the electrode material to fully contact the electrolyte, so that the material exhibits excellent performance and stability in the secondary battery; and can simultaneously solve the problems of small organic molecules being easily soluble in the electrolyte material, the low specific capacity and poor conductivity of the organic electrode material, and can be used as a high-performance organic electrode material for secondary batteries.

[0017] The electrode prepared by the porphyrin unit-containing polyimide COF material prepared by the present invention can be used in lithium-ion batteries. Compared with the prior art, the specific capacity and capacity retention rate of the battery prepared by the electrode of the present invention are significantly higher than those of the PI material with the same structural unit. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 Example 1 at 0.1A·g -1 Capacity retention rate test chart after 10 cycles at a current density of; Figure 2 Example 4 at 5A·g -1 Capacity retention rate test chart of 10,000 cycles at a current density of; Figure 3 For comparative examples 1 to 2 at 0.5 A·g -1 Specific capacity test diagram at current density. DETAILED DESCRIPTION

[0019] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0020] The present invention is further described in detail below with specific examples, but the present invention is not limited to the following specific examples.

[0021] Example 1 5,10,15,20-tetrakis(4-aminophenyl)porphyrin (TAPP) (67.47 mg, 0.1 mmol) and biphenyltetracarboxylic acid dianhydride (BPDA) (59.42 mg, 0.2 mmol) were dissolved in N,N-dimethylacetamide (DMAC) (14.036 g, 15 mL) and reacted at -1 °C for 4.5 hours to obtain a polyamic acid solution containing porphyrin units. The polyamic acid containing porphyrin units was transferred to a reactor and continued to react at 140 °C for 72 hours to obtain a polyacrylic COF containing porphyrin units. After the reaction was completed, DMAC was centrifuged for 3-5 times for washing until the eluate was colorless and transparent, and then deionized water was ultrasonically treated for 1 hour to replace the high-boiling point DMAC, and finally COF powder was obtained by freeze drying.

[0022] The prepared polyimide COF powder containing porphyrin units, 10% conductive carbon black, and 10% polyvinylidene fluoride were added with 4.5 g of N-methylpyrrolidone, stirred for 10 hours, and then coated on copper foil with a coating thickness of 75 mm to obtain an electrode.

[0023] The electrodes were assembled into button cells, where the negative electrode material of the battery was polyimide COF, and the counter electrode was metallic lithium. The separator material of the battery was Celgard 2300, and the electrolyte was 1M LiPF6 dissolved in EC:DMC:EMC with a volume ratio of 1:1:1. In an argon-filled glove box, the button half-cells were assembled in the order from the negative electrode shell to the positive electrode, and after being pressed with a sealing machine, a testable finished battery was obtained. Figure 1 As shown, when the current density is set to 0.1 A g -1 After 10 cycles of charge and discharge, the specific capacity of the polyimide COF containing porphyrin units is 967.12 mAh·g -1 .

[0024] Example 2 5,10,15,20-tetrakis(4-aminophenyl)porphyrin (TAPP) (67.47 mg, 0.1 mmol) and biphenyltetracarboxylic acid dianhydride (BPDA) (59.42 mg, 0.2 mmol) were dissolved in N,N-dimethylacetamide (DMAC) (14.036 g, 15 mL) and reacted at -1 °C for 4.5 hours to obtain a polyamic acid solution containing porphyrin units. The polyamic acid containing porphyrin units was transferred to a reactor and continued to react at 140 °C for 72 hours to obtain a polyacrylic COF containing porphyrin units. After the reaction was completed, DMAC was centrifuged for 3-5 times for washing until the eluate was colorless and transparent, and then deionized water was ultrasonically treated for 1 hour to replace the high-boiling point DMAC, and finally COF powder was obtained by freeze drying.

[0025] The prepared polyimide COF powder containing porphyrin units, 10% conductive carbon black, and 10% polyvinylidene fluoride were added with 4.5 g of N-methylpyrrolidone, stirred for 5-10 hours, and then coated on copper foil with a coating thickness of 75 mm to obtain an electrode.

[0026] The above electrodes were assembled into a button cell, in which the negative electrode material of the battery was polyimide COF, and the counter electrode was metallic lithium. The separator material of the battery was Celgard 2300, and the electrolyte was 1M LiPF6 dissolved in EC:DMC:EMC with a volume ratio of 1:1:1. In an argon-filled glove box, the button half-cells were assembled from the negative electrode shell to the positive electrode, and after being pressed with a sealing machine, a testable finished battery was obtained. When the current density was set to 0.5 A·g -1 After 10 cycles of charge and discharge, the specific capacity of the polyimide COF containing porphyrin units is 897.03 mAh·g -1 .

[0027] Example 3 5,10,15,20-tetrakis(4-aminophenyl)porphyrin (TAPP) (67.47 mg, 0.1 mmol) and biphenyltetracarboxylic acid dianhydride (BPDA) (59.42 mg, 0.2 mmol) were dissolved in N,N-dimethylacetamide (DMAC) (14.036 g, 15 mL) and reacted at -1 °C for 4.5 hours to obtain a polyamic acid solution containing porphyrin units. The polyamic acid containing porphyrin units was transferred to a reactor and continued to react at 140 °C for 72 hours to obtain a polyacrylic COF containing porphyrin units. After the reaction was completed, DMAC was centrifuged for 3-5 times for washing until the eluate was colorless and transparent, and then deionized water was ultrasonically treated for 1 hour to replace the high-boiling point DMAC, and finally COF powder was obtained by freeze drying.

[0028] The prepared polyimide COF powder containing porphyrin units, 10% conductive carbon black, and 10% polyvinylidene fluoride were added with 4.5 g of N-methylpyrrolidone, stirred for 10 hours, and then coated on copper foil with a coating thickness of 75 mm to obtain an electrode.

[0029] The above electrodes were assembled into a button cell, in which the negative electrode material of the battery was polyimide COF, and the counter electrode was metallic lithium. The separator material of the battery was Celgard 2300, and the electrolyte was 1M LiPF6 dissolved in EC:DMC:EMC with a volume ratio of 1:1:1. In an argon-filled glove box, the button half-cells were assembled from the negative electrode shell to the positive electrode, and after being pressed with a sealing machine, a testable finished battery was obtained. When the current density was set to 1.0 A·g -1 After 10 cycles of charge and discharge, the specific capacity of the porphyrin-containing polyimide COF is 818.13 mAh·g -1 .

[0030] Example 4 5,10,15,20-tetrakis(4-aminophenyl)porphyrin (TAPP) (67.47 mg, 0.1 mmol) and biphenyltetracarboxylic acid dianhydride (BPDA) (59.42 mg, 0.2 mmol) were dissolved in N,N-dimethylacetamide (DMAC) (14.04 g, 15 mL) and reacted at -1 °C for 4.5 hours to obtain a polyamic acid solution containing porphyrin units. The polyamic acid containing porphyrin units was transferred to a reactor and continued to react at 140 °C for 72 hours to obtain a polyacrylic COF containing porphyrin units. After the reaction was completed, DMAC was centrifuged for 3-5 times for washing until the eluate was colorless and transparent, and then deionized water was ultrasonically treated for 1 hour to replace the high-boiling point DMAC, and finally COF powder was obtained by freeze drying.

[0031] The prepared polyimide COF powder containing porphyrin units, 10% conductive carbon black, and 10% polyvinylidene fluoride were added with 4.5 g of N-methylpyrrolidone, stirred for 10 hours, and then coated on copper foil with a coating thickness of 75 mm to obtain an electrode.

[0032] The above electrodes were assembled into a button cell. When the current density was set to 5.0 A·g -1The negative electrode material of the battery is polyimide COF, and the counter electrode is metallic lithium. The separator material of the battery is Celgard 2300, and the electrolyte is 1M LiPF6 dissolved in EC:DMC:EMC with a volume ratio of 1:1:1. In an argon-filled glove box, it is assembled into a button half-cell in the order from the negative electrode shell to the positive electrode, and after being pressed with a sealing machine, a testable finished battery is obtained. After 10 cycles of corresponding charge and discharge, the specific capacity of the polyimide COF containing porphyrin units is 677.6 mAh·g -1 .

[0033] like Figure 2 The results are shown for Example 4 at 5A·g -1 The capacity retention rate test diagram under the current density of Figure 2 It can be seen that the button cell prepared in Example 4 has a -1 The capacity retention rate after 10,000 cycles at a current density of 1.5877 W was as high as 71.92%.

[0034] Comparative Example 1 The difference from Example 2 is that "5-(4-aminophenyl)-10,15.20-triphenylporphyrin (TPPNH2)" is used instead of "COF powder", and the method for preparing the electrode includes: adding 4.5 grams of N-methylpyrrolidone to TPPNH2, conductive carbon black (added amount is 10% of the mass of TPPNH2), and polyvinylidene fluoride (added amount is 10% of the mass of TPPNH2), stirring for 10 hours, and then applying it on copper foil with a coating thickness of 75 mm to obtain a TPPNH2 electrode.

[0035] The electrodes were assembled into button cells, where the negative electrode material of the battery was TPPNH2 electrode, and the counter electrode was metallic lithium. The separator material of the battery was Celgard 2300, and the electrolyte was 1M LiPF6 dissolved in EC:DMC:EMC with a volume ratio of 1:1:1. In an argon-filled glove box, the button half-cells were assembled in the order from the negative electrode shell to the positive electrode, and after being pressed with a sealing machine, a testable finished battery was obtained. Figure 3 As shown in Figure 2, when the current density is set to 0.5 A·g-1, the battery has a specific capacity of 344.9 mAh·g after 10 cycles of charge and discharge. -1 .

[0036] Comparative Example 2 The difference from Example 2 is that "biphenyltetracarboxylic dianhydride (BPDA)" is used instead of "COF powder", and the method for preparing the electrode includes: adding BPDA, conductive carbon black (the addition amount is 10% of the mass of BPDA), and polyvinylidene fluoride (the addition amount is 10% of the mass of BPDA) to 4.5 grams of N-methylpyrrolidone, stirring for 10 hours, and then applying it on copper foil to obtain a coating with a thickness of 75 mm to obtain a BPDA electrode.

[0037] The electrodes were assembled into button cells, where the negative electrode material of the battery was BPDA electrode, and the counter electrode was metallic lithium. The separator material of the battery was Celgard 2300, and the electrolyte was 1M LiPF6 dissolved in EC:DMC:EMC with a volume ratio of 1:1:1. In an argon-filled glove box, the button half-cells were assembled in the order from the negative electrode shell to the positive electrode, and after being pressed with a sealing machine, a testable finished battery was obtained. Figure 3 As shown in Figure 2, when the current density is set to 0.5 A·g-1, the battery has a specific capacity of 573.6 mAh·g after 10 cycles of charge and discharge. -1 .

[0038] Results Analysis Comparing Example 2 with Comparative Examples 1 and 2, it can be seen that the battery prepared in Example 2 has a high -1 The specific capacity after 10 cycles of charge and discharge at the current density is 897.03 mAh g -1 , while the batteries prepared in Comparative Example 1 (TPPNH2) and Comparative Example 2 (BPDA) were -1 The specific capacity after 10 cycles of discharge at the current density is 344.9 mAh·g -1 and 573.6 mAh g -1 , the specific capacity of Example 2 is significantly higher than that of Comparative Example 1 (TPPNH2) and Comparative Example 2 (BPDA); therefore, compared with TPPNH2 and BPDA materials, the specific capacity of the polyimide COF material containing porphyrin units of the present invention is significantly improved. Therefore, the present invention can improve the specific capacity of the battery by preparing the polyimide COF material containing porphyrin units.

[0039] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a polyimide COF material containing a porphyrin unit, characterized in that: The following steps are involved: The 5,10,15,20-tetrakis(4-aminophenyl)porphyrin is polymerized with a solvent containing anhydride to obtain a polyamic acid solution containing porphyrin units; The obtained polyamic acid solution containing porphyrin units is transferred to a hydrothermal reactor for reaction to obtain an organic covalent framework polyimide COF containing porphyrin units; The obtained organic covalent framework polyimide COF containing porphyrin units is washed with a solvent, and then the solvent is removed and dried to obtain a polyimide COF material containing porphyrin units.

2. The preparation method according to claim 1, characterized in that: The acid anhydride includes at least one of BPDA, PMDA and NTCDA.

3. The preparation method according to claim 1, characterized in that: The molar ratio of the 5,10,15,20-tetrakis(4-aminophenyl)porphyrin to the acid anhydride is 0.5-1.5:1.5-2.

5.

4. The preparation method according to claim 1, characterized in that: The mass fraction of the polyamic acid solution containing porphyrin units is 0.5%-5%; the solvent is N,N-dimethylacetamide, and the added amount of the solvent is 27.7-290 times the mass of 5,10,15,20-tetrakis(4-aminophenyl)porphyrin.

5. The preparation method according to claim 1, characterized in that: The polymerization reaction conditions are: reacting at -5~5°C for 3-6 hours.

6. The preparation method according to claim 1, characterized in that: The reaction temperature of the porphyrin unit-containing polyamic acid solution in the hydrothermal reactor is 140-200° C., and the reaction time is 64-96 hours.

7. The preparation method according to claim 1, characterized in that: The polyimide COF containing porphyrin units is centrifuged 3-5 times with N,N-dimethylacetamide until the eluate is colorless and transparent, and then ultrasonically treated with deionized water for 0.5-1.5 hours to displace the high-boiling point N,N-dimethylacetamide, and freeze-dried to obtain a polyimide COF material containing porphyrin units.

8. A polyimide COF material containing porphyrin units, characterized in that: The method is prepared by any one of claims 1 to 7.

9. A method for preparing an electrode, characterized in that: Add N-methylpyrrolidone to the porphyrin unit-containing polyimide COF material prepared by the method of any one of claims 1 to 7 or the porphyrin unit-containing polyimide COF material described in claim 8, conductive carbon black and polyvinylidene fluoride, wherein the amount of conductive carbon black added is 5%-30% of the mass of the porphyrin unit-containing polyimide COF material, and the amount of polyvinylidene fluoride added is 5%-20% of the mass of the porphyrin unit-containing polyimide COF material, stir for 5-10 hours, and then apply on copper foil with a thickness of 30-80 mm to obtain an electrode.

10. An electrode, characterized in that: The method according to claim 9 is used to prepare the product.

Citation Information

Patent Citations

  • Polyimide COF material based on ethylenediamine tetraacetic acid dianhydride as well as preparation method and application of polyimide COF material

    CN113881064A

  • Preparation method and application of three-dimensional covalent organic framework 3D COF material based on 8-connected cubic ligand

    CN116082591A

Cited By

  • Conjugated terminal group polyimide covalent organic framework material as well as preparation method and application thereof