Metallic H x MoO3 nanoribbon electrode material
The electrochemical activation method is used to embed protons to form metallic HxMoO3 nanobelt electrode material, which solves the problem of low α-MoO3 conductivity leading to battery capacity attenuation, achieves the high specific capacity and energy density of proton batteries, and significantly improves the circulation stability of the material Sex and application potential.
Patent Information
- Application Number
- CN202210754011.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-06-29
Smart Images

Figure 220629161201 
Figure 220629161204 
Figure 220629161206
Abstract
Description
Technical Field
[0001] The invention provides a new electrode material, specifically a HxMoO3 nanobelt electrode of metallic titanium, belonging to the technical field of new batteries. Background Art
[0002] An ideal energy storage device needs to store more energy in a shorter time with less weight. Based on the calculation of the theoretical capacity of the electrode, the lower the atomic mass of the charge carrier, the greater the theoretical energy density. In recent years, a lot of research work has focused on batteries with metal elements as current carriers, such as Li + 、Na + 、Zn 2+ and Al 3+ Etc. However, less attention has been paid to non-metallic ions, especially proton ions. Compared with metal ions, proton ions are not only abundant in resources and have very small ionic radius, but also can be transported by proton hopping / Grotthuss free diffusion, and are considered to be ideal charge carriers. Proton batteries are expected to become ideal devices for large-scale energy storage in the future. High-performance electrode materials are the key to realizing the application of proton batteries. Molybdenum trioxide materials are widely used in positive electrode materials of various charge and discharge batteries due to their low cost and high capacity.
[0003] Protons are considered to be the most ideal energy storage charge carriers in "rocking chair" batteries due to their small ion size and light weight. Compared with other metal cations, proton batteries with hydrogen ions as charge carriers show high safety and excellent cycle stability, and have great application prospects. At present, the research on proton batteries is still in its infancy, and there are few reports on positive electrode materials that can be used for proton batteries. Therefore, it is of great significance to develop new high-performance positive electrode materials for proton batteries.
[0004] In recent years, α-MoO3 has also been studied as the positive electrode of proton batteries to achieve highly reversible proton storage. However, the low conductivity of α-MoO3 often causes the battery capacity to decay rapidly. Summary of the invention
[0005] In view of the above technical problems, the present invention provides a novel metallic HxMoO3 nanobelt as a proton storage electrode material developed and designed by using MoO3 nanobelt as a raw material through electrochemical activation. 1.75 MoO3 nanobelts, as the positive electrode material of proton batteries, effectively enhance the rate performance of proton batteries.
[0006] Metallic H x MoO3 nanobelt electrode material, the H x In MoO3 nanobelt electrode materials, 0.5≤x≤2.0.
[0007] As a preferred embodiment, 1.0≤x≤2.0.
[0008] Furthermore, as a preferred embodiment, x is 1.0, 1.25, 1.5, 1.75, or 2.0.
[0009] Through theoretical calculations, in-situ Raman and ex-situ XRD, it can be found that when the X value is low (less than 1), H x MoO3 maintains the semiconductor energy band of α-MoO3 and its orthorhombic structure. With the insertion of more hydrogen ions, such as 1.0≤x≤2.0, H x The gap between the conduction band and the valence band of MoO3 is getting smaller and smaller. When X=1.75, the metallic H 1.75 MoO3.
[0010] For a metallic H provided by the present invention x The preparation method of MoO3 nanobelt electrode material comprises the following steps: assembling an α-MoO3 electrode sheet, a graphite rod and a saturated Ag / AgCl as a working electrode, a counter electrode and a reference electrode respectively into a three-electrode battery, and performing CV cycles at -0.38V to 0.7V in an H2SO4 aqueous solution to achieve proton embedding to obtain HxMoO3 nanobelts, wherein 0.5≤x≤2.0 in the HxMoO3 nanobelt electrode material.
[0011] The α-MoO3-containing electrode sheet is prepared by mixing α-MoO3 nanobelts, carbon black and polyvinylidene fluoride in a mass ratio of 6-7:2-3:1-2 to obtain a slurry, which is dripped onto carbon fiber paper and dried to obtain the α-MoO3-containing electrode sheet.
[0012] The concentration of the H2SO4 aqueous solution is 5-10M.
[0013] After 5-20 cycles of CV at -0.38V~0.7V, H x MoO3 nanobelt, wherein 1.0≤x≤2.0.
[0014] In 7-9M H2SO4 aqueous solution, CV cycles were performed at -0.38V~0.7V for 10-20 cycles to obtain H with x of 1.0, 1.25, 1.5, 1.75, or 2.0. x MoO3 nanoribbon products.
[0015] A symmetrical full battery, comprising the metallic H prepared above x MoO3 nanobelt electrode material.
[0016] The technical solution of the present invention uses α-MoO3 nanobelts as precursors to perform proton insertion and synthesize metallic H by electrochemical activation. x MoO3 nanoribbons. After electrochemical activation, H x MoO3 nanobelts still maintain an orthorhombic structure. Compared with α-MoO3 nanobelts, due to the embedding of protons, H x The (020) diffraction peak of MoO3 nanobelts shifts to a lower angle, indicating an increase in interlayer spacing. At the same time, high-angle annular dark field (HAADF) STEM and selected area electron diffraction (SAED) were also used to further study the H x Changes in the structure of MoO3 nanoribbons. x The SAED pattern of MoO3 nanobelts further proves that H1.75MoO3 still maintains an orthorhombic structure after proton insertion. There are three oxygen environments in MoO3, namely asymmetric bridging O1, symmetric bridging O2 and terminal O3. After proton intercalation, the interaction between O3 p orbital and intercalated proton ions promotes the positive shift of Mo d orbital, and the symmetric degenerate state undergoes Jahn-Teller distortion, which leads to the transition from semimetal to metal.
[0017] During the first discharge process, protons are embedded in MoO3, causing local Jahn-Teller distortion of the conduction band electrons, forming metallic H1.75MoO3 nanobelts. The electrochemically pre-intercalated protons can not only directly connect to the terminal oxygen through OH bonds, but also interact with the oxygen in the adjacent layer through hydrogen bonds to form a hydrogen bond network, which promotes the rapid transfer of protons and is beneficial to enhancing the rate performance of the material. As the positive electrode material of the proton battery, at an ultra-high current density of 500 mA / g, as in one case, the metallic H 1.75 MoO3 nanobelts exhibited a high specific capacity of 111 mAh / g with a charging time of less than 1 s. At the same time, H 1.75 The MoO3 symmetric battery exhibits a high energy density of 59 Wh / kg; even at a power density of 12.7 kW / kg, it can still achieve an energy density of 14.7 Wh / kg, which has great application potential. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is the XRD pattern of the α-MoO3 nanobelt prepared in Example 1.
[0019] Figure 2 These are SEM images of the α-MoO3 nanobelts prepared in Example 1, wherein a is a picture taken at a magnification of 15,000, and b is a picture taken at a magnification of 100,000.
[0020] Figure 3This is the TEM image of the α-MoO3 nanobelt prepared in Example 1.
[0021] Figure 4 This is the HRTEM image of the α-MoO3 nanobelt prepared in Example 1.
[0022] Figure 5 This is the EDS element distribution diagram of the α-MoO3 nanobelt prepared in Example 1.
[0023] Figure 6 α-MoO3 and H 1.75 XRD pattern of MoO3 nanoribbons.
[0024] Figure 7 This is the band structure of α-MoO3.
[0025] Figure 8 H 1.75 Energy band structure of MoO3.
[0026] Fig. 9 is the electronic state density of α-MoO3.
[0027] Fig.10 H 1.75 Electronic state density of MoO3.
[0028] Fig.11 High-resolution HAADF STEM image of MoO3 nanobelts.
[0029] Fig.12 This is the SAED pattern of MoO3 nanobelt on the zoon axis
[100] .
[0030] Fig.13 Intensity line scan of the blue and pink dashed lines in the HAADF pattern of the SAED pattern of MoO3 nanoribbons.
[0031] Fig.14 MoO3 crystal observed along the
[001] direction of MoO3 nanobelt.
[0032] Fig.15 H 1.75 High-resolution HAADF STEM image of MoO3 nanoribbons.
[0033] Fig.16 H 1.75 SAED pattern of MoO3 nanoribbons on the zoon axis
[100] .
[0034] Fig.17 H 1.75 Intensity line scan of the blue and pink dashed lines in the HAADF pattern of the SAED pattern of MoO3 nanoribbons.
[0035] Fig.18 H 1.75 MoO3 nanoribbons MoO3 crystals observed along the
[001] direction.
[0036] Fig.19 H 1.75 CV curves of MoO3 nanobelts at a scan rate of 10 mV / s.
[0037] Fig. 20 H 1.75 Cycling stability of the MoO3 nanobelt battery at a current density of 100 A / g, and the inset is the corresponding charge / discharge curve.
[0038] Fig.21 H 1.75 Charge and discharge curves of MoO3 nanobelt batteries at different current densities.
[0039] Fig. 22 H 1.75 The performance of MoO3 nanobelts is compared with that of previously reported proton batteries. In the figure, Ref.14 shows the performance of α-MoO3 ammonium ion batteries; Ref.15 shows the performance of bodhislan analogs as proton batteries; Ref.16 shows the performance of α-MoO3 under lower concentration sulfuric acid conditions at -0.5-0.3V; Ref.17 shows the performance of diquinoxaline [2,3-a:2′, 3′-c]benazine polymer as a proton battery; Ref.18 shows the performance of high-load α-MoO3 as a proton battery at -0.5-0.3V; Ref.19 shows the performance of MnO2 / / α-MoO3 proton battery under low temperature conditions.
[0040] Fig.23 H 1.75 Cycling stability of MoO3 nanoribbon batteries at a current density of 500 A / g.
[0041] Fig.24 CV curve of the MoO3-based symmetric proton-ion full battery.
[0042] Fig.25 is the cycling performance of the full battery at a current density of 20 A / g.
[0043] Fig.26 The rate performance of the full battery (a) and its corresponding charge and discharge curve (b). DETAILED DESCRIPTION
[0044] Example 1
[0045] Preparation method of α-MoO3 nanobelt
[0046] α-MoO3 nanobelts were prepared by a hydrothermal method. 0.196 g of ammonium molybdate was dissolved in 55 ml of deionized water, and then 5 ml of HNO3 (65 wt.%) was added dropwise. After stirring for 10 min, the solution was transferred to a stainless steel autoclave and kept at 200°C for 24 h and cooled naturally. Then, the white product was harvested by centrifugation, washed with water three times and dried at 70°C overnight, which was α-MoO3 nanobelts.
[0047] The following examples all use α-MoO3 nanobelts as raw materials to prepare proton-type H x MoO3 nanoribbons.
[0048] The prepared α-MoO3 exhibits characteristic diffraction peaks of orthorhombic MoO3 crystals (JCPDF: 00-035-0609) at 12.77°, 23.28°, 25.57°, 27.45°, 33.50°, 38.97°, 46.17° and 58.99° ( Figure 4 ), corresponding to the (020), (110), (040), (021), (111), (060), (061) and (081) crystal planes respectively. Figure 2 a and b in Figure 3 As shown in the figure, α-MoO3 presents a uniform nanobelt morphology with a width of 100-500 nm and a length of 10-50 μm. At the same time, the SADE image shows that the prepared α-MoO3 nanobelt is a single crystal. Figure 4 The interlayer spacings of the (110) and (021) planes in the HRTEM image are 0.38 and 0.33 nm, respectively, which further proves that the prepared α-MoO3 is an orthorhombic phase. EDS image ( Figure 5 ) also further proves that Mo and O elements are uniformly distributed in the prepared α-MoO3 nanobelts.
[0049] Example 2
[0050] The α-MoO3 nanobelts, carbon black and polyvinylidene fluoride (PVDF) prepared in Example 1 were mixed uniformly in a mass ratio of 7:2:1, and the slurry was dripped onto carbon fiber paper and dried at 60°C to obtain an α-MoO3 electrode sheet. A three-electrode cell was assembled with the α-MoO3 electrode sheet, graphite rod and saturated Ag / AgCl as the working electrode, counter electrode and reference electrode, respectively, and tested in 8 MH2SO4 aqueous solution. By performing CV cycles from -0.38 to 0.7 V, after the first discharge to -0.38 V, protons were embedded in α-MoO3 to form H 1.75 MoO3 nanoribbons.
[0051] The method steps are the same as those in Example 2, except that the use of alkaline electrolyte will not allow the production of proton-embedded nanobelt products.
[0052] The method and steps are the same as those in Example 2. After one cycle at -0.38 to 0.7 V, H is prepared by discharging to 0.1 V. 0.5 MoO3 nanoribbons.
[0053] The method and steps are the same as those in Example 2. After one cycle at -0.38 to 0.7 V, H is prepared by discharging to 0.05 V. 1.0 MoO3 nanoribbons.
[0054] The method and steps are the same as those in Example 2. After cycling once at -0.38 to 0.7 V and then discharging to -0.15 V, H 1.25 MoO3 nanoribbons.
[0055] The method and steps are the same as those in Example 2. After one cycle at -0.38~0.7 V, H is obtained by discharging to -0.38 V. 1.5 MoO3 nanoribbons.
[0056] The method and steps are the same as those in Example 2. After one cycle at -0.38-0.7 V, H was prepared by discharging to -0.42 V. 2.0 MoO3 nanoribbons.
[0057] The method and steps are the same as those in Example 2. After one cycle at -0.38-0.7 V, H was prepared by discharging to -0.45 V. 2.2 MoO3 nanoribbons.
[0058] The present invention synthesizes α-MoO3 nanobelts by a one-step hydrothermal method, and uses the α-MoO3 nanobelts as precursors to perform proton embedding and synthesize metallic H by an electrochemical activation method. 1.75 MoO3 nanobelts. Figure 6 As shown in the figure, the α-MoO3 nanobelts exhibit characteristic diffraction peaks of orthorhombic MoO3 crystals (JCPDF: 04-008-4311) at 12.69°, 23.28°, 25.57°, 27.45°, 38.97°, 46.17° and 58.99°, corresponding to the (020), (101), (400), (210), (600), (002) and (810) crystal planes, respectively. After electrochemical activation, the H1.75MoO3 nanobelts still maintain the orthorhombic structure. Compared with the α-MoO3 nanobelts, due to the embedding of protons, the (020) crystal plane diffraction peak of the H1.75MoO3 nanobelts shifts to the low-angle direction, showing an increased interlayer spacing. At the same time, high-angle annular dark field (HAADF) STEM test and selected area electron diffraction (SAED) were also used to further study the H during the electrochemical activation process. 1.75 Changes in the structure of MoO3 nanobelts. Fig.12 and14 As shown, MoO3 and H 1.75 The zigzag array of Mo atoms in MoO3 nanoribbons propagates preferentially along the
[001] direction, and there is an obvious van der Waals gap between the zigzag arrays of Mo atoms, indicating that MoO3 and H 1.75 MoO3 nanobelts are all layered structures. 1.75 The SAED pattern of MoO3 nanoribbons further proves that after proton insertion, H 1.75 MoO3 still maintains an orthorhombic structure ( Fig.16 In addition, the spacing between Mo atoms along the
[010] and
[001] directions can also be further characterized by scanning the intensity of the blue and pink dashed lines in the HAADF map. Fig.16 and 18 As shown in the figure, the average spacing of α-MoO3 along the
[010] and
[001] directions is 0.69 and 0.33 nm, respectively. 1.75 The average spacings of MoO3 along the
[010] and
[001] directions are 0.73 and 0.41 nm, respectively, indicating that proton insertion causes structural changes. Fig.14 and 18 As shown in Figure 2, the inserted protons bond with the terminal oxygen of the MoO6 octahedron (the top O atom pointing to the van der Waals gap), resulting in elongated Mo-O bonds and extended (001) planes; and due to the formation of hydrogen bonds, the distance between the protons and the terminal oxygen in the adjacent layers is about 0.219 nm. At the same time, DFT calculations were used to study the molecular dynamics of MoO3 and H 1.75 The band structure of MoO3. Figure 7 As shown, the band gap of MoO3 is 1.9 eV; while in H 1.75 No obvious band gap is observed in MoO3 ( Figure 8 ), indicating that H 1.75 MoO3 has metallic properties. There are three oxygen environments in MoO3, namely asymmetric bridging O1, symmetric bridging O2 and terminal O3 ( Fig. 9 and 10 ). After proton intercalation, the interaction between the O3 p orbital and the intercalated proton ion promotes the positive shift of the Mod orbital, and the symmetric degenerate state undergoes Jahn-Teller distortion, which leads to the transition from semimetal to metal.
[0059] Example 3
[0060] In order to evaluate H 1.75 Proton storage properties of MoO3 nanoribbons based on H 1.75 The three-electrode Swagelok cell of MoO3 nanoribbons was tested using the method of reference 14.
[0061] In order to evaluate H 1.75 Proton storage properties of MoO3 nanoribbons based on H 1.75 The three-electrode Swagelok cell of MoO3 nanoribbons was tested. Fig.19 As shown in Figure 2, two pairs of redox peaks can be observed at 0.23 / -0.019 V and -0.22 / -0.33 V, which are attributed to the protons in H 1.75 Reversible insertion / extraction in MoO3. At a current density of 100 A / g, H 1.75 The MoO3 nanobelts exhibited a high reversible specific capacity of 188 mAh / g, and after 50 cycles, they could still reach 153 mAh / g, with a capacity retention rate of about 81% ( Fig. 20 ).
[0062] For H 0.5 MoO3、H 1.0 MoO3、H 1.25 MoO3、H 1.5 MoO3、H 2.0 For the proton-embedded MoO3 nanobelt product, at a current density of 100 A / g, H 0.5 MoO3、H 1.0 MoO3、H 1.25 MoO3、H 1.5 MoO3、H 2.0 MoO3 nanobelts exhibit high reversible specific capacities of 53.7 mAh / g, 107.4 mAh / g, 134.3 mAh / g, 161.1 mAh / g, and 214.9 mAh / g. After 50 cycles, they can still reach 43.7 mAh / g, 87.4 mAh / g, 109.3 mAh / g, 131.1 mAh / g, and 174.9 mAh / g, all with ultra-high capacity retention rates.
[0063] At a high current density of 600 A / g, H 1.75 The discharge capacity of MoO3 nanobelts can still reach 115 mAh / g, showing excellent rate performance ( Fig.21 ). Compared with previously reported proton ion batteries, H 1.75 MoO3 nanoribbons not only exhibit high reversible capacity, but also can achieve a charging time of less than 1 s ( Fig. 22 ). At the same time, at a high current density of 500 A / g, H 1.75 MoO3 nanoribbons can provide an initial specific capacity of 111 mAh / g in a charging time of less than 1 s, and the capacity retention rate can still reach 80% after 5000 cycles ( Fig.23 ), showing significantly enhanced cycling stability.
[0064] Fig. 22 The references in are as follows:
[0065] (Compared literature:
[14] G. Liang, Y. Wang, Z. Huang, F. Mo, X. Li, Q. Yang, D. Wang, H. Li, S. Chen, C. Zhi, Advanced Materials 2020, 32, 1907802.
[0066]
[15] X. Wu, JJ Hong,W. Shin, L. Ma, T. Liu, X. Bi, Y. Yuan, Y. Qi,TW Surta, W. Huang, Nature Energy 2019, 4, 123.
[0067]
[16] X. Wang, Y. Xie, K.Tang, C. Wang, C. Yan, Angewandte ChemieInternational Edition 2018, 57, 11569.
[0068]
[17] Z. Tie, L. Liu, S. Deng, D. Zhao, Z. Niu, Angewandte Chemie International Edition 2020, 59, 4920.
[0069]
[18] Z. Su, W. Ren, H.Guo, X. Peng, X. Chen, C. Zhao, Advanced Functional Materials 2020, 2005477.
[0070]
[19] L. Yan, J. Huang, Z.Guo, X. Dong, Z. Wang, Y. Wang, ACS EnergyLetters 2020, 5, 685.)
[0071] Example 4
[0072] H 1.75 Symmetric full cell composed of MoO3 nanobelts as electrode materials and its electrochemical performance test. The full cell is assembled with 2036 button cells and H 1.75MoO3 was used as the positive electrode, α-MoO3 as the negative electrode, glass fiber film as the separator, and 8M sulfuric acid solution as the electrolyte. The button cells were assembled and the electrochemical performance was tested in the voltage range of 0-1V.
[0073] In H 1.75 Electrochemical performance and testing of symmetrical full-cell composed of MoO3 nanobelts as electrode materials. Fig.25 As shown in the figure, under the condition of current density of 20 A / g, the capacity retention rate of the full battery can still reach 75% after 1000 cycles, showing excellent cycle stability. At the same time, the reversible capacity of the full battery can still reach 138 and 120 mAh / g (based on the mass of the positive electrode material) under the conditions of 20 and 100 A / g. Fig.26 (a and b) show excellent rate performance. The full battery can achieve a high energy density of 59 Wh / kg at 8.7 kW / kg; and at a power density of 12.7 kW / kg, the energy density can still reach 14.7 Wh / kg, which has great application potential.
[0074] In fact, for H 0.5 MoO3、H 1.0 MoO3、H 1.25 MoO3、H 1.5 MoO3、H 2.0 For the full cell prepared by the above method, the proton-embedded MoO3 nanobelt product has a current density of 20 A / g. 0.5 MoO3、H 1.0 MoO3、H 1.25 MoO3、H 1.5 MoO3、H 2.0 The reversible capacity of MoO3 nanobelts can reach high reversible specific capacities of 39.4 mAh / g, 78.9 mAh / g, 98.6 mAh / g, 118.3 mAh / g, and 157.7 mAh / g.
Claims
1. A metallic H 1.75 The method for preparing MoO3 nanobelt electrode material is characterized in that: α-MoO3 nanobelts were prepared by a hydrothermal method: 0.196 g ammonium molybdate was dissolved in 55 ml deionized water, and then 5 ml HNO3 65 wt.% was added dropwise. After stirring for 10 minutes, the solution was transferred to a stainless steel autoclave and kept at 200 °C for 24 h, cooled naturally, and then the white product was harvested by centrifugation, washed with water three times and dried at 70 °C overnight to obtain α-MoO3 nanobelts. H 1.75 Preparation of MoO3 nanobelts: The prepared α-MoO3 nanobelts, carbon black and polyvinylidene fluoride (PVDF) were mixed uniformly in a mass ratio of 7:2:
1. The slurry was dripped onto carbon fiber paper and dried at 60°C to obtain α-MoO3 electrode sheets. A three-electrode cell was assembled with α-MoO3 electrode sheets, graphite rods and saturated Ag / AgCl as working electrode, counter electrode and reference electrode, respectively. The cell was tested in 8M H2SO4 aqueous solution. By performing CV cycles from -0.38 to 0.7 V, protons were embedded in α-MoO3 to form H after the first discharge to -0.38 V. 1.75 MoO3 nanoribbons.