A high reliability low temperature curing silver paste for ferrite and preparation method thereof
By optimizing the silver paste formula and process, the problem of poor adhesion and conductivity of low-temperature curing silver paste on ferrite materials has been solved, and the preparation of high-reliability low-temperature curing silver paste has been achieved. It is suitable for high temperature and high humidity environments, and its performance is close to that of sintering. type silver paste.
Patent Information
- Application Number
- CN202210790485.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-05
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-07-05
AI Technical Summary
The existing low-temperature curing silver paste has low adhesion and poor conductivity on ferrite materials, making it difficult to use in high-temperature scenes and high-humidity environments. There is also a lack of low-temperature curing silver paste suitable for ferrite substrates.
By optimizing the ratio of resin, curing agent, defoaming agent, dispersant and solvent, combined with adjusting the ratio of spherical and flaky silver powder, a tight overlap is formed to achieve the preparation of highly reliable low-temperature curing silver paste, with a use temperature of only 150°C. Ready to cure.
It achieves higher bonding force and conductivity than sintered silver paste, and is resistant to solvents, acid washing, alkali washing, boiling, soldering, and hot and cold shock. It is suitable for high-humidity environments, and its performance is close to that of sintered silver paste. Silver paste.
Smart Images

Figure CN115188520B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of conductive silver paste, and in particular to a high-reliability, low-temperature curing silver paste for ferrite and a preparation method thereof. Background Art
[0002] Driven by high-tech such as 5G, the electronic information industry has developed rapidly. The low operating temperature (below 200°C) makes low-temperature curing silver paste widely used in printed circuits, solar cells, membrane switches, electrode leads, flexible devices and other fields. In application scenarios such as 5G base stations, higher requirements are placed on the weather resistance and high temperature resistance of electronic components. However, the existing low-temperature curing silver paste is not moisture-resistant, has poor thermal stability, low adhesion, and poor conductivity, making it difficult to be further applied.
[0003] Since ferrite has gyromagnetism and high magnetic permeability, ferrite is widely used in electronic components such as circulators and chip inductors. Existing conductive silver pastes used for ferrite are mostly sintering pastes, which generally require high temperatures above 500°C for sintering and are complicated to operate. For example, patent CN110164585A discloses a method for preparing a high-conductivity and high-adhesion conductive paste for ferrite core inductors. The paste is composed of silver powder and an organic carrier. The mass of the silver powder is 1-20 times that of the organic carrier. The content of the high molecular polymer in the organic carrier is 6-32wt%, and the content of the organic additive is 68-94wt%. The silver paste described in the patent has high conductivity and good adhesion on the ferrite substrate, but its sintering temperature is too high (500-1500°C), and it cannot be used in some high-temperature-resistant scenes such as resin.
[0004] Based on the above description, the existing low-temperature curing paste has not been applied in large quantities on ferrite materials due to low adhesion and poor conductivity on ferrite ceramics, etc. Moreover, there is no patent report on the use of low-temperature curing silver paste on ferrite substrates.
[0005] Therefore, it is necessary to develop a low-temperature curing silver paste with high reliability for use on ferrite, which has become an urgent problem to be solved. Summary of the invention
[0006] According to the above technical problem of lack of high conductivity and high adhesion conductive paste for low temperature process scenarios, a high reliability low temperature curing silver paste for ferrite and a preparation method thereof are provided. The present invention mainly achieves a higher binding force than sintered silver paste by optimizing the ratio of resin, curing agent, defoaming agent, dispersant and solvent; at the same time, by adjusting the ratio of flaky metal and spherical metal, a close overlap is formed between the silver powders, achieving conductivity comparable to that of sintered silver paste.
[0007] The technical means adopted by the present invention are as follows:
[0008] A high-reliability low-temperature curing silver paste for ferrite, characterized in that the low-temperature curing silver paste consists of the following components in percentage by mass:
[0009] Silver powder 65-75%,
[0010] Resin 17-27%,
[0011] Defoaming agent 0.5~1.5%,
[0012] Dispersant 0.5~1.2%,
[0013] Curing agent 1.6~3.2%,
[0014] Solvent 2.4~4%,
[0015] The sum of the mass percentages of the various components is 100%.
[0016] Furthermore, the silver powder is formed by mixing spherical silver powder and flaky silver powder, wherein the mass ratio of the spherical silver powder to the flaky silver powder is between 0.5 and 2.
[0017] Furthermore, the average particle size of the spherical silver powder is 0.5-0.8 μm, and the tap density is greater than 4.9 g / cm 3 , purity>99%, oxygen content<1%, preferably 99.99% powder.
[0018] Furthermore, the average particle size of the flaky silver powder is 2.0-5.0 μm, and the tap density is greater than 3.4 g / cm 3 , purity>99%, oxygen content<1%, preferably 99.99% powder.
[0019] Further, the resin is selected from epoxy resin (EP), which is bisphenol A epoxy resin or novolac epoxy resin. Preferred novolac epoxy compounds, particularly those obtained by the reaction of epichlorohydrin and / or methyl epichlorohydrin with phenolic novolac, are obtained by the reaction of phenols (such as phenol, cresol, halogenated phenol and alkylphenol) with formaldehyde in the presence of an acidic catalyst. Such resins generally have a large molecular weight and a high Tg value, and the coating film has the characteristics of high dry film strength, high temperature resistance, and good solvent resistance after curing. Specific examples of such suitable phenolic epoxy compounds include N-738, N-740, N-770, N-775, N-865 manufactured by Dainippon Ink & Chemicals Co., Ltd., PNE-177, CNE-200 manufactured by Changchun Artificial Resin Factory, PFNE7300 manufactured by Hunan Jiashengde Material Technology Co., Ltd., DEN431, DEN438, DEN439, DEN444 manufactured by Dow Chemical, PY-307-1, EPN1179, EPN1180, EPN1183, EPN9880, GY289 manufactured by Huntsman Advanced Materials Co., Ltd., Epikote 155 manufactured by Shell, ESN-138 manufactured by Sanwa Chemical Co., Ltd., YDPN-631, YDPN-638, One or more of YDPN-641, YDPN-644, NPPN-631, NPPN-638, NPPN-638S manufactured by Nan Ya Plastics Industry Co., Ltd., F-51, F-44, F-43 manufactured by Bluestar Chemical New Materials Co., Ltd., SQPN638, SQPN048, SQPN051 manufactured by Shandong Shengquan Chemical.
[0020] Furthermore, the curing agent is an amine curing agent, which is one or a mixture of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, dipropylenetriamine, dimethylaminopropylamine, polyethylenepolyamine, diethylaminopropylamine, trimethylhexamethylenediamine, dihexyltriamine, hexamethylenediamine, trimethylhexamethylenediamine, diethylamine, polyetherdiamine, diaminomethylcyclohexane, menthanediamine, diaminocyclohexylmethane, and metaphenylenediamine.
[0021] Furthermore, the dispersant is one or a mixture of aminoacrylate copolymers, phosphates, and polyacid homopolymers, preferably EFKA-4580.
[0022] Furthermore, the defoaming agent is one or both of polysiloxanes and mineral oils, preferably Agitan315.
[0023] Furthermore, the solvent is one or a mixture of ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, diethylene glycol methyl ether acetate, propylene glycol methyl ether acetate, dipropylene glycol methyl ether acetate, propylene glycol methyl ether propionate, propylene glycol butyl ether acetate, and a mixture of dibasic esters, preferably ethylene glycol ethyl ether acetate.
[0024] The present invention also discloses a method for preparing the above-mentioned high-reliability, low-temperature curing silver paste for ferrite, which is characterized in that the components of the slurry except the defoamer are weighed into the same open container according to the mass fraction, and stirred evenly at a speed of 300r / min with a high-speed disperser, then the defoamer is added and stirred evenly again with a high-speed disperser at a speed of 500r / min, and finally ground on a three-roll grinder for 4 to 8 times to make the slurry reach a uniform dispersion state, and the grinding is stopped when the slurry fineness is detected to be less than 5.5μm, and the viscosity is detected at 25°C and 10r / min to be 35.0-45.0Pa·s.
[0025] Compared with the prior art, the present invention has the following advantages:
[0026] 1. By optimizing the ratio of resin, curing agent, defoamer, dispersant and solvent, a higher bonding force than sintered silver paste is achieved;
[0027] 2. By adjusting the ratio of sheet metal and spherical metal, a close overlap is formed between the silver powders, achieving conductivity comparable to that of sintered silver paste;
[0028] 3. Compared with the sintered silver paste used for ferrite, the low-temperature curing silver paste developed by the present invention has a low use temperature and can be cured into a film at only 150°C and 30 minutes, forming a strong bond on the ferrite substrate. In addition, the low-temperature curing silver paste developed by the present invention has high reliability: it has the characteristics of resistance to solvents, acid washing, alkali washing, boiling, soldering, and cold and hot shocks, and is also suitable for use in high-humidity environments. The performance is comparable to that of existing sintered silver pastes.
[0029] Based on the above reasons, the present invention can be applied to scenarios such as circulators that require printing conductive circuits on ferrite substrates, and can be widely promoted in this field. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0031] Figure 1 This is a metallographic microscope photograph (500 times) of the film layer after the slurry formula in Example 1 of the present invention is cured. It can be seen from the figure that the flaky silver powder has achieved a close overlap, and the spherical silver powder has filled the gap, and the entire film layer is in a dense state.
[0032] Figure 2 This is a metallographic microscope photograph (500 times) of the film layer after the slurry formula in Example 2 of the present invention is cured. It can be seen from the figure that the flaky silver powder has achieved a close overlap, and the spherical silver powder has filled the gap, and the entire film layer is in a dense state.
[0033] Figure 3 This is a metallographic microscope photo (500 times) of the film layer after curing of the slurry formula in Comparative Example 1 of the present invention. It can be seen from the figure that the powder in the film layer is loose and the overlapping path formed is small. This shows that the increase in resin content will affect the overlapping between powders, thereby increasing the resistivity of the film layer. DETAILED DESCRIPTION
[0034] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0035] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0037] Example 1
[0038] The present embodiment provides a high-reliability, low-temperature curing silver paste for ferrite, which is specifically prepared as follows: 70 parts of silver powder are weighed in a total amount by mass and put into an open container, wherein the mass ratio of spherical silver powder to flaky silver powder is 2:1, and then 22 parts of resin, 1.2 parts of dispersant, 2.4 parts of curing agent and 3.2 parts of solvent are added in sequence, and stirred at a speed of 300r / min for 10 minutes using a high-speed disperser, and then 1.2 parts of defoaming agent are added, and the high-speed disperser is used again to stir at 500r / min for 5 minutes, and the mixture is ground with a three-roll mill for 4-8 times to obtain a low-temperature curing silver paste.
[0039] Example 2
[0040] The present embodiment provides a high-reliability, low-temperature curing silver paste for ferrite, which is specifically prepared as follows: 65 parts of silver powder in total are weighed by mass into an open container, wherein the mass ratio of spherical silver powder to flaky silver powder is 1:2, and then 27 parts of resin, 1.2 parts of dispersant, 1.6 parts of curing agent and 4 parts of solvent are added in sequence, and stirred at a speed of 300r / min for 10 minutes using a high-speed disperser, and then 1.2 parts of defoaming agent are added, and the high-speed disperser is used again to stir at 500r / min for 5 minutes, and the mixture is ground with a three-roll mill for 4-8 times to obtain a low-temperature curing silver paste.
[0041] Example 3
[0042] The present embodiment provides a high-reliability, low-temperature curing silver paste for ferrite, which is specifically prepared as follows: 75 parts of silver powder are weighed in a total amount by mass and put into an open container, wherein the mass ratio of spherical silver powder to flaky silver powder is 2:1, and then 17 parts of resin, 1.2 parts of dispersant, 3.2 parts of curing agent and 2.4 parts of solvent are added in sequence, and stirred at a speed of 300r / min for 10 minutes using a high-speed disperser, and then 1.2 parts of defoaming agent are added, and the high-speed disperser is used again to stir at 500r / min for 5 minutes, and the mixture is ground with a three-roll mill for 4-8 times to obtain a low-temperature curing silver paste.
[0043] Example 4
[0044] The present embodiment provides a high-reliability, low-temperature curing silver paste for ferrite, which is specifically prepared as follows: 70 parts of silver powder are weighed in a total amount by mass and put into an open container, wherein the mass ratio of spherical silver powder to flaky silver powder is 1:1, and then 22 parts of resin, 1.2 parts of dispersant, 2.4 parts of curing agent and 3.2 parts of solvent are added in sequence, and stirred at a speed of 300r / min for 10 minutes using a high-speed disperser, and then 1.2 parts of defoaming agent are added, and the high-speed disperser is used again to stir at 500r / min for 5 minutes, and the mixture is ground with a three-roll mill for 4-8 times to obtain a low-temperature curing silver paste.
[0045] Comparative Example 1
[0046] On the basis of Example 1, 10 parts of silver powder were removed, the ratio of ball powder to flake powder remained unchanged, and its amount was transferred to resin (22 parts → 32 parts), and the rest remained unchanged.
[0047] Comparative Example 2
[0048] On the basis of Example 1, the mass fraction of silver powder is kept unchanged, the flaky silver powder is removed, and all spherical silver powder is used, and the rest remains unchanged.
[0049] Comparative Example 3
[0050] On the basis of Example 1, 1.2 parts of the curing agent were removed and transferred to the solvent (3.2 parts → 4.4 parts), and the rest remained unchanged.
[0051] Table 1: Formula ingredients list
[0052]
[0053]
[0054] The low-temperature curing silver paste prepared above was printed on a 2mm thick ferrite substrate to form a layer of 80 microns thick paste, and then placed in a blast oven, baked at 150°C for 30 minutes, and then taken out and cooled for performance testing. The test contents are as follows:
[0055] (1) Pencil hardness: pencil hardness tester, 6H pencil;
[0056] (2) Adhesion: 100-grid test;
[0057] (3) Solvent resistance: Soak in 25℃ alcohol for 20 minutes;
[0058] (4) Acid resistance: 25℃, 10vol%H 2 SO 4 Soak for 20 minutes;
[0059] (5) Alkali resistance: 25°C, soaked in 10wt% NaOH for 20 minutes;
[0060] (6) Boiling water resistance: soak in 100℃ boiling water for 30 minutes;
[0061] (7) Solder resistance: Place in 288℃ solder bath for 10 seconds, repeat 3 times;
[0062] (8) Thermal shock resistance: Heat the sample to 150°C in a blast drying oven, quickly place it in cold water and let it stand for 1 minute. Repeat this three times and observe the film shedding.
[0063] (9) Conductivity: Use a component analyzer to test the film thickness, then substitute the correction factor based on the film thickness and use a four-probe tester to test the square resistance.
[0064] Table 2: Test results
[0065]
[0066] The above test results show that the resin content and the ball powder-sheet powder mass ratio have a great influence on the resistivity of the film layer. The more resin content, the greater the ball powder-sheet powder mass ratio, and the lower the resistivity of the slurry after curing. The curing agent content has a great influence on the adhesion and reliability of the film layer. When the curing agent content is lower than a certain value, the adhesion of the slurry on the ferrite surface decreases, and the reliability of solvent resistance, alkali resistance, solder resistance, and thermal shock resistance is significantly deteriorated.
[0067] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A high reliability low temperature curing silver paste for ferrite, characterized in that: The low temperature curing silver paste is composed of the following components in percentage by weight: Silver powder 65-75%, Resin 17-27%, Defoaming agent 0.5~1.5%, Dispersant 0.5~1.2%, Curing agent 1.6~3.2%, Solvent 2.4~4%, Among them, the sum of the mass percentage of each component is 100%; The silver powder is formed by mixing spherical silver powder and flaky silver powder, and the mass ratio of the spherical silver powder to the flaky silver powder is between 0.5 and 2.
2. The high reliability low temperature curing silver paste for ferrite according to claim 1, characterized in that: The average particle size of the spherical silver powder is 0.5-0.8 μm, and the tap density is >4.9 g / cm 3 , purity>99%, oxygen content<1%.
3. The high reliability low temperature curing silver paste for ferrite according to claim 1, characterized in that: The average particle size of the flaky silver powder is 2.0-5.0 μm, and the tap density is greater than 3.4 g / cm 3 , purity>99%, oxygen content<1%.
4. The high reliability low temperature curing silver paste for ferrite according to claim 1, characterized in that: The resin is epoxy resin, which is bisphenol A epoxy resin or phenolic epoxy resin.
5. The high reliability low temperature curing silver paste for ferrite according to claim 1, characterized in that: The curing agent is an amine curing agent, which is one or a mixture of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, dipropylenetriamine, dimethylaminopropylamine, polyethylenepolyamine, diethylaminopropylamine, trimethylhexamethylenediamine, dihexyltriamine, hexamethylenediamine, trimethylhexamethylenediamine, diethylamine, polyetherdiamine, diaminomethylcyclohexane, menthanediamine, diaminocyclohexylmethane, and metaphenylenediamine.
6. The high reliability low temperature curing silver paste for ferrite according to claim 1, characterized in that: The dispersant is one or a mixture of aminoacrylate copolymers, phosphates, and polyacid homopolymers.
7. The high reliability low temperature curing silver paste for ferrite according to claim 1, characterized in that: The defoaming agent is one or both of polysiloxanes and mineral oils.
8. The high reliability low temperature curing silver paste for ferrite according to claim 1, characterized in that: The solvent is one or a mixture of ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, diethylene glycol methyl ether acetate, propylene glycol methyl ether acetate, dipropylene glycol methyl ether acetate, propylene glycol methyl ether propionate, propylene glycol butyl ether acetate, and a mixture of dibasic acid esters.
9. A method for preparing a high-reliability, low-temperature curing silver paste for ferrite according to any one of claims 1 to 8, characterized in that: Weigh each component of the slurry except the defoamer according to the mass fraction into the same open container, stir evenly with a high-speed disperser at a speed of 300r / min, then add the defoamer and stir evenly with the high-speed disperser again at a speed of 500r / min, finally grind on a three-roll grinder 4 to 8 times to make the slurry reach a uniform dispersion state, stop grinding when the slurry fineness is detected to be <5.5μm, and the viscosity at 25℃ and 10r / min is 35.0-45.0Pa·s.