Flame retardant epoxy resin composition, prepreg, fiber reinforced composite material and preparation thereof

Through the compounding of phosphorus-containing modified epoxy resin and halogen-free flame retardant, the problems of flammability and low flame retardant efficiency of the epoxy resin matrix are solved, and fiber-reinforced composite materials with high flame retardant efficiency and heat resistance are realized. Meet the high flame retardant grade requirements of aviation and rail transportation.

CN115197537BActive Publication Date: 2024-10-25TECHSTORM MATERIAL TECH SHANGHAI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210457230.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-27
Publication Date
2024-10-25
Estimated Expiration
2042-04-27

AI Technical Summary

Technical Problem

The existing epoxy resin matrix is ​​flammable, and the traditional flame retardant scheme has low flame retardant efficiency, high smoke density during combustion, and the addition of a large amount of flame retardant leads to poor processability and reduced mechanical properties. It cannot meet the high flame retardant levels of rail transit and aviation materials. Require.

Method used

Phosphorus-containing modified epoxy resin is compounded with halogen-free flame retardant. Phosphorus-containing modified epoxy resin accounts for 5-30% of the total mass, and the phosphorus content is 1-10wt%. It is combined with halogen-free flame retardant and epoxy. The resin curing agent is used together to prepare an epoxy resin composition with high flame retardant efficiency and heat resistance.

Benefits of technology

It has achieved high flame retardant efficiency and stable fiber-reinforced composite materials, meeting the flame retardant standards of aviation interior materials FAR25.853 and rail transit EN 45545-2R1 HL2 or above, while improving the mechanical strength and heat resistance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003619197360000061
    Figure BDA0003619197360000061
  • Figure BDA0003619197360000071
    Figure BDA0003619197360000071
  • Figure BDA0003619197360000072
    Figure BDA0003619197360000072
Patent Text Reader

Abstract

The present invention relates to the technical field of fiber-reinforced thermosetting resin composite material applications, and more specifically, to a flame-retardant epoxy resin composition, a prepreg, a fiber-reinforced composite material and its preparation. The flame-retardant epoxy resin composition is prepared by raw materials including phosphorus-modified epoxy resin, epoxy resin, halogen-free flame retardant, and epoxy resin curing agent; the phosphorus-modified epoxy resin accounts for 5-30% of the total mass of the raw materials, the mass ratio of the phosphorus-modified epoxy resin to the halogen-free flame retardant is 1:(1-3), and the phosphorus content in the phosphorus-modified epoxy resin is 1-10wt%. The flame-retardant epoxy composition of the present invention has a high carbonization rate, a low heat release rate, low smoke release and low smoke toxicity, and a halogen-free flame-retardant epoxy prepreg is obtained by impregnating reinforcing fibers such as carbon fiber, glass fiber, basalt fiber, and aramid fiber, and a fiber-reinforced composite material with excellent flame retardant properties prepared by the epoxy prepreg, which meets the flame retardant requirements of rail transit and aviation interior materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of application of fiber-reinforced thermosetting resin composite materials, and more specifically, to a flame-retardant epoxy resin composition, a prepreg, a fiber-reinforced composite material and a preparation method thereof. Background Art

[0002] Since most epoxy resin matrices are flammable materials, they are extremely easy to cause fires, which limits their development. In addition, the epoxy groups of traditional flame-retardant composite materials mostly use halogen-containing flame retardant solutions such as bromine-containing epoxy, which have the disadvantages of low flame retardant efficiency, high smoke density and high smoke toxicity during combustion. At the same time, ordinary red phosphorus, phosphonate, metal hydride and ammonium polyphosphate are added. In order to meet the flame retardant grade requirements of rail transit EN45545-2 HL2 or above or aviation interior materials FAR25.853, the amount of flame retardant added is large, resulting in poor processability of the epoxy resin matrix, reduced mechanical properties, and reduced glass transition temperature, which cannot give full play to the lightweight advantages of low density and high strength of fiber-reinforced composite materials. For example, CN201410157894 uses ATN series epoxy resin, micronized dicyandiamide, urea accelerator, hydrated aluminum oxide and white carbon black to obtain resin impregnated in the carbon fiber layer, but the flame retardant and mechanical properties of the prepreg cannot meet the requirements at the same time. Summary of the invention

[0003] In view of some problems existing in the prior art, the first aspect of the present invention provides a flame retardant epoxy resin composition, the preparation raw materials include phosphorus-modified epoxy resin, epoxy resin, halogen-free flame retardant, epoxy resin curing agent; the phosphorus-modified epoxy resin accounts for 5-30% of the total mass of the preparation raw materials, and the mass ratio of the phosphorus-modified epoxy resin to the halogen-free flame retardant is 1: (1-3).

[0004] Preferably, the phosphorus-modified epoxy resin accounts for 10-20% of the total mass of the raw materials.

[0005] The phosphorus-modified epoxy resin in the present invention includes commercially available phosphorus-modified epoxy resin, or phosphorus-modified epoxy resin obtained by reacting a phosphorus-containing reactive flame retardant with an epoxy resin, and the reaction is a conventional method well known to those skilled in the art.

[0006] In one embodiment, the phosphorus content in the phosphorus-containing modified epoxy resin is 1-10 wt %, preferably 3-8 wt %.

[0007] The inventor unexpectedly discovered in the experiment that when the phosphorus content in the phosphorus-modified epoxy resin used in the present invention is 1-10wt%, especially 3-8wt%, the cured epoxy resin composition obtained has high flame retardant efficiency, and the prepreg-cured fiber-reinforced composite material prepared by the epoxy composition has good flame retardant properties, and the fiber-reinforced composite material has good heat resistance. However, if the phosphorus content is too high, the cross-linking density of the cured epoxy resin composition may be reduced, the glass transition temperature may be reduced, and the heat resistance of the fiber-reinforced composite material may be reduced.

[0008] In one embodiment, the phosphorus-modified epoxy resin has a viscosity of 2000-90000 mPa.s at 75°C.

[0009] In a preferred embodiment, the phosphorus-modified epoxy resin is selected from one or more of Clariant EP-360, Clariant EP-390, DPO-128 resin, and DPO-638 resin.

[0010] Clariant EP-360 in the present invention is a solid phosphorus-modified epoxy resin, with a phosphorus content of 6.4 wt %, an epoxy equivalent weight of EEW=500 g / eq., and a viscosity of 19000 mPa.s at 75° C.

[0011] Clariant EP-390: solid phosphorus-modified epoxy resin, phosphorus content: 9.7wt%, epoxy equivalent weight: EEW>>500g / eq., viscosity at 75℃: 24000mPa.s.

[0012] DPO-128 resin: prepared by reacting the phosphorus-containing reactive flame retardant diphenylphosphine (DPO) with bisphenol A glycidyl ether epoxy resin NPEL-128 (sourced from Daosheng Tianhe Materials Technology (Shanghai) Co., Ltd.), phosphorus content 5.4wt%, epoxy equivalent: EEW=540g / eq., 75℃ viscosity: 2000mPa.s.

[0013] DPO-638 resin: prepared by reacting the phosphorus-containing reactive flame retardant diphenylphosphine oxide (DPO) with the phenolic epoxy resin NPPN-638S (sourced from Daosheng Tianhe Materials Technology (Shanghai) Co., Ltd.), phosphorus content 3.8wt%, epoxy equivalent: EEW=330g / eq., 75℃ viscosity: 86000mPa.s.

[0014] In one embodiment, the epoxy equivalent of the epoxy resin is 100-500 g / eq.

[0015] In one embodiment, the epoxy resin accounts for 20-40% of the total mass of the raw materials.

[0016] Preferably, the epoxy resin is selected from one or more of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, aliphatic epoxy resin, alicyclic epoxy resin, and toughened modified epoxy resin.

[0017] Preferably, the epoxy resin is selected from one or more of NPEL-128, NPEF-170, NPES-901, NPPN-638S, Huntsman MY-0500, and DER 858.

[0018] NPEL-128 in the present invention is purchased from Nanya Electronic Materials (Kunshan) Co., Ltd., a low-viscosity liquid bisphenol A epoxy resin, epoxy equivalent weight: EEW = 184 ~ 190g / eq., 25 ° C viscosity: 12000 ~ 15000mPa.s.

[0019] NPEF-170, purchased from Nan Ya Plastics Industrial Co., Ltd., is a low-viscosity liquid bisphenol F type epoxy resin, epoxy equivalent weight: EEW = 160-180 g / eq., viscosity at 25°C: 2000-5000 mPa.s.

[0020] NPES-901, purchased from Nanya Electronic Materials (Kunshan) Co., Ltd., solid bisphenol A type epoxy resin, epoxy equivalent: EEW = 450 ~ 500g / eq., softening point: 67 ~ 74 ° C.

[0021] NPPN-638S, purchased from Nan Ya Plastics Industrial Co., Ltd., linear phenolic epoxy resin, epoxy equivalent weight: EEW = 184 ~ 190g / eq., 25 ° C viscosity: 12000-15000mPa.s.

[0022] Huntsman MY-0500 resin, glycidylamine type trifunctional epoxy resin, epoxy equivalent weight: EEW = 105 ~ 115g / eq., 25 ℃ viscosity: 2000 ~ 5000mPa.s.

[0023] DER 858, purchased from Olin Company, polyurethane modified toughened epoxy resin, epoxy equivalent weight: EEW = 380 ~ 420g / eq., softening point: 95-105 ° C.

[0024] In one embodiment, the halogen-free flame retardant accounts for 20-40% of the total mass of the raw materials for preparation, and the halogen-free flame retardant is selected from one or more of ammonium polyphosphate, piperazine pyrophosphate, melamine pyrophosphate, melamine urate, polyphosphate ester, hexaphenoxy cyclotriphosphazene, triphenylphosphine oxide, alkyl hypophosphite, aluminum hydroxide, magnesium hydroxide, and zinc borate.

[0025] Preferably, the zinc borate is hydrated zinc borate with a particle size D50≤10 μm, purchased from Hefei Wanran New Material Technology Co., Ltd.

[0026] Preferably, the aluminum hydroxide has a particle size D50≤8 μm and is purchased from Dongguan Hongtaiji Flame Retardant Materials Co., Ltd.

[0027] Preferably, the degree of polymerization of ammonium polyphosphate is greater than 1000, the particle size D50 is less than or equal to 20 μm, and the brand is Clariant AP-428.

[0028] Preferably, the alkyl phosphinate is diethyl aluminum phosphite with a particle size of D50≤7 μm, purchased from Hubei Youfeng Technology Co., Ltd.

[0029] Preferably, the brand of piperazine pyrophosphate is Guangzhou Edenda NH5500, and the particle size D50≤5 μm.

[0030] Preferably, the melamine ureate has a D50 of ≤5 μm and is purchased from Dongguan Hongtaiji Flame Retardant Materials Co., Ltd.

[0031] Preferably, the triphenylphosphine oxide has a phosphorus content of 11.1 wt %, and is purchased from Guangzhou Xijia New Materials Co., Ltd.

[0032] Preferably, the polyphosphate ester is a cyclic polyphosphate ester with a phosphorus content of 25 wt %, a brand name of TR-22, and is purchased from Guangzhou Xijia New Materials Co., Ltd.

[0033] In one embodiment, the halogen-free flame retardant includes substance (a) zinc borate, substance (b) aluminum hydroxide, and substance (c) at least one or more selected from ammonium polyphosphate, diethyl aluminum hypophosphite, piperazine pyrophosphate, melamine urate, and triphenylphosphine oxide.

[0034] Preferably, the weight ratio of substance (a), substance (b) and substance (c) is 1:(1-5):(1-3).

[0035] The epoxy resin curing agent in the present invention is not particularly limited and can be conventionally selected by those skilled in the art.

[0036] In one embodiment, the epoxy resin curing agent includes a latent curing agent and an accelerator in a weight ratio of (1-3):1, preferably 2:1.

[0037] Preferably, the latent curing agent is selected from one or more of aromatic amines, dicyandiamide, organic hydrazides, modified aromatic amines, modified dicyandiamides, modified organic hydrazides, and linear phenolic resins, and more preferably dicyandiamide.

[0038] Preferably, the accelerator is one or more of organic urea, modified organic urea, imidazole, and modified imidazole.

[0039] Preferably, the latent curing agent is Azken Chemical 100S, with a melting point of 209-212° C. and a D90 particle size of 1-10 μm.

[0040] Preferably, the accelerator is UR300 and / or 2MZ-OK produced by Azken Chemicals.

[0041] Among them, UR300 of Azken Chemical has a melting point of 125-135°C and a D90 particle size of 5-12 μm; 2MZ-OK, with a melting point of 250-260°C and a D90 particle size of 5-15 μm, was purchased from Shikoku Chemical Industry Co., Ltd. of Japan and is a modified imidazole accelerator.

[0042] In one embodiment, the flame retardant epoxy resin composition further comprises an auxiliary agent.

[0043] The auxiliary agent of the present invention is not particularly limited, and those skilled in the art can make conventional selections, such as a wetting agent, a viscosity reducer, a defoaming agent, an internal release agent, and the like.

[0044] Preferably, the auxiliary agent includes a wetting agent and a defoaming agent.

[0045] Preferably, the sizing agent is BYK-W980.

[0046] Preferably, the defoaming agent is BYK-A530.

[0047] The second aspect of the present invention provides a method for preparing a flame retardant epoxy resin composition, comprising: preheating a mixing device, sequentially adding an epoxy resin and a phosphorus-modified epoxy resin into the mixing device and mixing them evenly, then adding a halogen-free flame retardant and mixing them evenly, and then cooling the mixture and adding an epoxy resin curing agent to obtain the composition.

[0048] The preparation method of the flame retardant epoxy resin composition comprises: preheating a mixing device to 100° C., sequentially adding epoxy resin, phosphorus-containing modified epoxy resin and auxiliary agent into the mixing device and mixing them evenly, then adding halogen-free flame retardant and mixing them evenly, then cooling the temperature to 65-70° C., and adding epoxy resin curing agent to obtain the composition.

[0049] The third aspect of the present invention provides a prepreg prepared by impregnating reinforcing fibers with the flame retardant epoxy resin composition.

[0050] The reinforcing fibers in the present invention are not particularly limited, and examples thereof include carbon fibers, glass fibers, basalt fibers, aramid fibers, and the like.

[0051] A fourth aspect of the present invention provides a fiber-reinforced composite material formed by curing the prepreg.

[0052] In one embodiment, the method for preparing the fiber-reinforced composite material comprises: curing a prepreg or a prepreg and a flame-retardant epoxy resin composition to obtain the composite material.

[0053] Compared with the prior art, the present invention has the following beneficial effects:

[0054] (1) The present invention uses a phosphorus-modified epoxy resin with a phosphorus content of 1-10 wt%, which not only maintains good flame retardancy, but also has a high crosslinking density of the epoxy resin composition cured product, and the obtained fiber-reinforced composite material has good heat resistance;

[0055] (2) The present invention uses a phosphorus-modified epoxy resin with a viscosity of 2000-90000 mPa.s, so that the composition obtained with the epoxy resin raw material and the flame retardant has good flame retardant stability, reducing the precipitation problem of small molecule flame retardants;

[0056] (3) The flame-retardant epoxy resin composition provided by the present invention introduces phosphorus-modified epoxy resin, and adopts a variety of halogen-free flame retardant compounding technology to add a flame retardant content of less than 40wt% in the epoxy resin composition. The prepared carbon fiber prepreg cured composite material not only meets the flame retardant standard requirements of FAR25.853 for aviation interior materials, but also meets the flame retardant grade requirements of EN 45545-2R1 HL2 or above for rail transit, and the material has good mechanical strength and heat resistance;

[0057] (4) The flame retardant epoxy resin composition provided by the present invention has good fluidity and has good wettability to reinforcing fibers, especially carbon fibers, when preparing prepregs, and can give full play to the high strength characteristics of carbon fibers;

[0058] (5) The curing agent and accelerator of the specific particle size of the present invention can cooperate with each other, and the obtained resin has a good gel time;

[0059] (6) The flame-retardant epoxy composition of the present invention has a high carbonization rate, a low heat release rate, a low smoke release and a low smoke toxicity. It can be used to impregnate reinforcing fibers such as carbon fiber, glass fiber, basalt fiber, and aramid fiber to obtain a halogen-free flame-retardant epoxy prepreg, as well as a fiber-reinforced composite material with excellent flame retardant properties prepared from the epoxy prepreg, which can meet the flame retardant requirements of rail transit and aviation interior materials. DETAILED DESCRIPTION

[0060] The present invention is described below by specific implementation methods, but is not limited to the specific embodiments given below.

[0061] Example

[0062] For information and manufacturers of the substances involved in the embodiments, please refer to the content of the invention, wherein zinc borate is hydrated zinc borate with a particle size of D50≤10 μm, purchased from Hefei Wanran New Material Technology Co., Ltd., ATH is aluminum hydroxide with a particle size of D50≤8 μm, purchased from Dongguan Hongtaiji Flame Retardant Material Co., Ltd., ADP is diethyl aluminum hypophosphite with a particle size of D50≤7 μm, purchased from Hubei Youfeng Technology Co., Ltd., MCA is melamine urate with a particle size of D50≤5 μm, purchased from Dongguan Hongtaiji Flame Retardant Material Co., Ltd., and TOA is triphenylphosphine with a phosphorus content of 11.1 wt%, purchased from Guangzhou Xijia New Material Co., Ltd.

[0063] Examples 1-7

[0064] A flame retardant epoxy resin composition, the specific components of which are shown in Table 1 below.

[0065] Table 1

[0066]

[0067] The preparation method of the flame retardant epoxy resin composition is as follows: preheating a mixing device to 100° C., sequentially adding liquid bisphenol A epoxy resin, linear phenolic epoxy resin, bisphenol A solid epoxy resin, phosphorus-modified epoxy resin, defoamer and wetting agent into the mixing device and mixing them evenly, then adding zinc borate, aluminum hydroxide ATH and AP-428 and mixing them evenly, cooling the mixture to 65° C., adding curing agent dicyandiamide 100S and organic urea accelerator UR300 into the mixing device and mixing them evenly to obtain a flame retardant epoxy resin composition.

[0068] The flame retardant epoxy resin compositions obtained in Examples 1 to 7 were subjected to vacuum degassing and casting of resin tensile and impact test strips according to GB / T2567-2008 standard requirements, and the curing condition was 150° C. for 2 hours to obtain epoxy resin composition cured castings.

[0069] The flame retardant epoxy resin compositions of Examples 1-7 were tested as follows:

[0070] (1) Viscosity: The viscosity of the flame retardant epoxy resin composition at 70° C. was tested using a TADHR20 rheometer;

[0071] (2) Gel time: The gel time at 150°C was tested using a gel time tester;

[0072] (3) Carbonization rate: The thermal gravimetric analysis of the cured epoxy resin composition in air was performed using a TGA thermogravimetric tester. The test conditions were 40-800°C and a temperature rise rate of 10°C / min.

[0073] (4) Tg: based on the determination method using DSC (TA DSC Q2000) in GB / T 19466-2004;

[0074] (5) Mechanical properties: The tensile strength, tensile modulus, and elongation at break of the cured product of the flame-retardant epoxy resin composition were determined using an electronic universal tensile testing machine based on ISO 527-2. The simply supported beam impact strength of the cured product of the epoxy resin composition was determined using a simply supported beam impact testing machine based on GBT1043.1.

[0075] The test results are shown in Table 2.

[0076] Table 2

[0077]

[0078] Embodiment 8-14

[0079] A flame retardant epoxy resin composition, the specific components of which are shown in Table 3 below.

[0080] Table 3

[0081]

[0082]

[0083] The preparation method of the flame retardant epoxy resin composition is as follows: preheat a mixing device to 100°C, add epoxy resin, phosphorus-modified epoxy resin, defoamer, and wetting agent to the mixing device in turn and mix them evenly, then add flame retardant and mix them evenly, cool the mixture to 65°C, add curing agent to the mixing device and mix them evenly to obtain a flame retardant epoxy resin composition.

[0084] The flame-retardant epoxy resin compositions obtained in Examples 8-14 were respectively used in the same manner as in Examples 1-7 to obtain epoxy resin composition cured castings.

[0085] The flame retardant epoxy resin compositions of Examples 8-14 were tested for viscosity, gel time, carbonization rate, Tg and mechanical properties using the same testing methods as in Examples 1-7.

[0086] The test results are shown in Table 4.

[0087] Table 4

[0088]

[0089]

[0090] Preparation of flame retardant carbon cloth prepreg:

[0091] The flame retardant epoxy resin compositions obtained in Examples 8, 10, 11, 13, and 14 were coated with a hot melt prepreg coating machine to form resin films, and the surface density of the prepared resin films was 165 g / ㎡. Toray T300-12K carbon cloth fabric, with a specification of 2×2 plain carbon cloth and a surface density of 400 g / ㎡, was compositely impregnated with two layers of resin film and Toray T300 carbon cloth fabric using a hot melt prepreg impregnation machine to prepare flame retardant carbon cloth prepregs corresponding to the flame retardant epoxy resin compositions of Examples 8, 10, 11, 13, and 14, respectively, and the resin content of the carbon cloth prepreg was 45.2%.

[0092] Preparation of flame retardant carbon cloth prepreg sheet:

[0093] Preheat a flat-plate compression mold with a cavity thickness of 2.2 mm to 150°C, and then evenly spray a release agent; cut 5 pieces of the prepared flame-retardant carbon cloth prepreg, stack the 5 pieces of prepreg according to a 0° / 0° / 0° / 0° / 0° stacking structure, wherein 0° is along the warp direction of the carbon cloth prepreg, and 90° is along the weft direction of the carbon cloth prepreg, and then put them into a preheated flat-plate compression mold and pressurize them to a maximum pressure of 4.0 MPa according to the program, maintain the pressure and hot press for 30 minutes, and after the hot pressing is completed, a flame-retardant carbon cloth prepreg composite material sheet with a thickness of 2.2 mm is obtained.

[0094] Based on ISO 527-4 standard, the flame retardant carbon cloth prepreg composite material sheet was used to prepare 6 tensile test pieces with a length of 250 mm and a width of 25 mm along the 0° direction to test the tensile strength and tensile modulus of the flame retardant carbon cloth prepreg composite material.

[0095] Based on the ISO14130 standard, the obtained flame retardant carbon cloth prepreg composite material sheet was prepared into 10 short beam shear test pieces with a length of 22 mm and a width of 11 mm along the 0° direction to test the interlaminar shear strength of the flame retardant carbon cloth prepreg composite material.

[0096] Based on FAR 25.853, APP.F Part Ⅳ standard, the flame retardant carbon cloth prepreg composite material sheet obtained was used to prepare 6 heat release rate test pieces with a length of 150 mm and a width of 150 mm along the 0° direction to test the heat release rate and flame retardant properties of the flame retardant carbon cloth prepreg composite material.

[0097] Based on FAR 25.853, APP.F PartⅤ standard, the flame retardant carbon cloth prepreg composite material sheet obtained was used to prepare 6 heat release rate test pieces with a length of 75 mm and a width of 75 mm along the 0° direction to test the smoke density DS4 of the flame retardant carbon cloth prepreg composite material.

[0098] The thermal gravimetric curve of the cured flame retardant epoxy resin composition was tested by a TGA thermal gravimetric tester. The higher the residual carbon rate at 710°C, the easier it is for the flame retardant epoxy resin composition to form carbon during combustion, and the higher the stability of the carbon formed during combustion. The amount of small molecular combustibles produced by thermal decomposition is reduced, the heat release from combustion is reduced, and the flame retardant performance is improved.

[0099] The working principle of cone calorimeter for testing heat release rate: oxygen consumption principle, most solid materials completely burn and release basically the same amount of heat per unit mass of oxygen consumed (13.1mJ / kgO2±5%). The cone heater simulates the heat flux intensity in the fire, and its combustion environment is very similar to the real combustion environment. The lower the heat release rate and total heat release of the flame retardant carbon cloth prepreg, the better the flame retardant performance.

[0100] The test results are shown in Table 5.

[0101] Table 5

[0102]

[0103] The test results of Examples 1-14 show that the flame retardant epoxy resin composition has a high carbon residue rate, with a carbon residue rate of ≥30% at 710°C, and the flame retardant epoxy resin composition has good mechanical properties and good heat resistance. The prepared flame retardant carbon cloth prepreg composite material has good performance, excellent flame retardant properties, and a maximum heat release rate of ≤65kW / m 2 , the total heat release in the first 2 minutes is ≤65kW*min / m 2 The total smoke density DS4 in the first 4 minutes is ≤200, which meets the flame retardant standard requirements of FAR 25.853 for aviation interior materials.

[0104] Comparative Examples 1-6

[0105] A flame retardant epoxy resin composition, the specific ingredients are shown in Table 6 below.

[0106] Table 6

[0107]

[0108]

[0109] The preparation method of the flame-retardant epoxy resin, the preparation of the resin-cured casting body, the preparation of the flame-retardant carbon cloth prepreg and the corresponding testing methods are the same as those in Example 8.

[0110] The test results are shown in Table 7.

[0111] Table 7

[0112]

[0113] The flame retardant epoxy resin composition obtained in Comparative Example 2 adopts a flame retardant solution of phosphorus-modified epoxy resin compounded with zinc borate and aluminum hydroxide. The heat release rate and the total heat release in the first 2 minutes of the prepared flame retardant carbon cloth prepreg do not meet the flame retardant standard requirements of FAR 25.853 for aviation interior materials.

[0114] The flame retardant epoxy resin composition obtained in Comparative Example 4 adopts ammonium polyphosphate flame retardant scheme. Although the flame retardant performance meets the flame retardant standard requirements of FAR 25.853 for aviation interior materials, the amount of flame retardant powder added is large, exceeding 45%, resulting in reduced mechanical properties of the flame retardant epoxy resin composition cured product, and the performance of the prepared flame retardant carbon cloth prepreg composite material is significantly reduced.

[0115] The flame retardant epoxy resin composition obtained in Comparative Example 6 adopts a phosphorus-modified epoxy resin compounded with zinc borate, aluminum hydroxide and polyphosphate flame retardant. Although the flame retardant performance meets the FAR 25.853 flame retardant standard requirements for aviation interior materials, the glass transition temperature of the cured flame retardant epoxy resin composition is reduced by 20°C after the addition of the phosphate flame retardant, and the heat resistance of the material is reduced.

Claims

1. A flame retardant epoxy resin composition, characterized in that: The preparation raw materials include phosphorus-modified epoxy resin, epoxy resin, halogen-free flame retardant, and epoxy resin curing agent; The phosphorus-containing modified epoxy resin accounts for 5-30% of the total mass of the raw materials, the mass ratio of the phosphorus-containing modified epoxy resin to the halogen-free flame retardant is 1:(1-3), and the phosphorus content in the phosphorus-containing modified epoxy resin is 1-10wt%; The halogen-free flame retardant accounts for 20-40% of the total mass of the raw materials; The halogen-free flame retardant comprises substance (a) zinc borate, substance (b) aluminum hydroxide, and substance (c) at least one or more selected from the group consisting of ammonium polyphosphate, diethyl aluminum hypophosphite, piperazine pyrophosphate, melamine urate, and triphenylphosphine oxide; the weight ratio of the substance (a), substance (b), and substance (c) is 1:(1-5):(1-3); The viscosity of the phosphorus-modified epoxy resin at 75° C. is 2000-90000 mPa.s; The epoxy resin curing agent accounts for 5-10% of the total mass of the raw materials for preparation. The epoxy resin curing agent is a latent curing agent and an accelerator. The weight ratio of the latent curing agent to the accelerator is 2:

1.

2. The flame retardant epoxy resin composition according to claim 1, characterized in that: The phosphorus-containing modified epoxy resin accounts for 10-20% of the total mass of the raw materials.

3. The flame retardant epoxy resin composition according to claim 1 or 2, characterized in that: The phosphorus content in the phosphorus-containing modified epoxy resin is 3-8 wt %.

4. The flame retardant epoxy resin composition according to claim 1, characterized in that: The epoxy resin accounts for 20-40% of the total mass of the raw materials, and the epoxy resin is selected from one or more of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, aliphatic epoxy resin, alicyclic epoxy resin, and toughened modified epoxy resin.

5. The flame retardant epoxy resin composition according to claim 1, characterized in that: The latent curing agent is at least one of aromatic amines, dicyandiamide, organic hydrazides, modified aromatic amines, modified dicyandiamides, modified organic hydrazides, and linear phenolic resins; the accelerator is at least one of organic urea, modified organic urea, imidazole, and modified imidazole.

6. A method for preparing the flame retardant epoxy resin composition according to any one of claims 1 to 5, characterized in that: include: After preheating the mixing device, add the epoxy resin and the phosphorus-modified epoxy resin into the mixing device in turn and mix them evenly, then add the halogen-free flame retardant and mix them evenly, then cool down and add the epoxy resin curing agent to obtain the product.

7. A prepreg, characterized in that: The invention is obtained by impregnating reinforcing fibers with the flame retardant epoxy resin composition according to any one of claims 1 to 5.

8. A fiber-reinforced composite material, characterized in that: It is formed by curing the prepreg described in claim 7.