Polyester, adhesives and films
By using a high-content condensation polymer of naphthalene dicarboxylic acid and dimer diol in polyester, adhesives and films with excellent dielectric properties are prepared, which solves the problem that the dielectric properties of polyester in the existing technology are not suitable for high frequencies. The problem of insufficient heat resistance of FPC and adhesives has been achieved, and the applicability and heat resistance in high-frequency areas have been achieved.
Patent Information
- Application Number
- CN202180019416.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-30
- Filing Date
- 2021-03-26
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-03-26
AI Technical Summary
The relative dielectric constant and dielectric loss tangent of existing polyester resins are high, making them unsuitable for flexible printed wiring boards (FPCs) in high-frequency areas, and the heat resistance of existing adhesives is insufficient.
By using a polycondensate of polycarboxylic acid and polyol, containing more than 50 mol% of naphthalenedicarboxylic acid and more than 20 mol% of dimer diol, a polyester with a relative dielectric constant ≤3.0 and a dielectric loss tangent ≤0.008 is prepared. esters and used in the preparation of adhesives and films.
It realizes adhesives and films with excellent solvent solubility, heat resistance and viscosity of polyester and good dielectric properties, which are suitable for FPC in high-frequency areas.
Smart Images

Figure BDA0003834427450000111
Abstract
Description
Technical Field
[0001] The present invention relates to a polyester, an adhesive and a film, and more particularly to a polyester having excellent dielectric properties and an adhesive and a film containing the polyester. Background Art
[0002] Polyester is widely used as a raw material for resin compositions used in coating agents, inks, adhesives, etc., and is generally composed of polycarboxylic acids and polyols. Since the flexibility and molecular weight can be freely controlled by the selection and combination of polycarboxylic acids and polyols, it is widely used in various applications, including coating agents and adhesives.
[0003] Among them, polyester has excellent adhesion to metals including copper, and is used as an adhesive for flexible printed circuit boards (FPCs) and the like when mixed with a curing agent such as epoxy resin (for example, Patent Document 1).
[0004] FPC has excellent bending property, can cope with the multifunctionalization and miniaturization of personal computer (PC), smart phone etc., therefore, it is mostly used to assemble electronic circuit substrate in narrow and complex interior. In recent years, the miniaturization, lightness, high density and high power development of electronic equipment, along with the popularity of these, the performance requirements for circuit board (electronic circuit substrate) are getting higher and higher. Especially along with the high speed of signal transmission in FPC, the high frequency of signal is developing. Then, the requirement of low dielectric properties (low dielectric constant, low dielectric loss tangent) in high frequency region of FPC is gradually improved. In addition, for the substrate for FPC, not only polyimide (PI) and polyethylene terephthalate (PET) in the past, substrate films such as liquid crystal polymer (LCP) and syndiotactic polystyrene (SPS) with low dielectric properties are also proposed. In order to realize low dielectric properties, the policy of reducing the dielectric loss of substrate and adhesive of FPC is proposed. As adhesive, the combination of polyolefin and epoxy resin (patent document 2) etc. is being developed.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Publication No. 6-104813
[0008] Patent Document 2: International Publication No. WO2016 / 047289 Summary of the invention
[0009] Problems to be solved by the invention
[0010] However, the polyester resin described in Patent Document 1 has high relative dielectric constant and dielectric loss tangent, does not have the above-mentioned low dielectric properties, and is not suitable for FPC in high-frequency regions. In addition, the adhesive described in Patent Document 2 cannot be said to have excellent heat resistance as an adhesive for reinforcing plates or between layers.
[0011] The present invention is accomplished against the background of the above-mentioned problems in the prior art. That is, the object of the present invention is to provide a polyester having excellent solvent solubility, heat resistance, and viscosity, low relative dielectric constant and dielectric loss tangent, and excellent dielectric properties, and an adhesive containing the polyester.
[0012] Means for solving problems
[0013] As a result of intensive studies, the present inventors have found that the above-mentioned problems can be solved by the means shown below, and have completed the present invention.
[0014] That is, the present invention has the following configurations.
[0015] A polyester having a polycarboxylic acid component and a polyol component as structural units, containing 50 mol % or more of a naphthalene dicarboxylic acid component based on 100 mol % of the polycarboxylic acid component, and containing 20 mol % or more of a dimer diol component based on 100 mol % of the polyol component.
[0016] The polyester preferably has a glass transition temperature of -30°C or higher.
[0017] A polyester having a relative dielectric constant (εc) of 3.0 or less and a dielectric loss tangent (tanδ) of 0.008 or less at 10 GHz.
[0018] An adhesive comprising the above polyester.
[0019] A film comprising the above polyester.
[0020] Effects of the Invention
[0021] The polyester of the present invention has excellent solvent solubility, heat resistance, and viscosity, and also has excellent dielectric properties, and is therefore suitable as an adhesive and film for FPC in a high-frequency region. DETAILED DESCRIPTION
[0022] Hereinafter, one embodiment of the present invention will be described in detail below. However, the present invention is not limited thereto, and can be implemented in various modified forms within the scope of the description.
[0023] The polyester of the present invention is composed of a chemical structure obtainable by a polycondensate of a polycarboxylic acid component and a polyol component, and is composed of one or more components selected from each of a polycarboxylic acid component and a polyol component.
[0024] The polyester of the present invention contains 50 mol% or more of naphthalene dicarboxylic acid components in 100 mol% of the total polycarboxylic acid components, preferably 70 mol% or more, more preferably 80 mol% or more, particularly preferably 90 mol% or more, and may be 100 mol%. By using a large amount of naphthalene dicarboxylic acid components, the dielectric properties of the polyester are improved.
[0025] Examples of the naphthalene dicarboxylic acid component include 2,6-naphthalene dicarboxylic acid, 2,7-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 2,3-naphthalene dicarboxylic acid, and 1,8-naphthalene dicarboxylic acid, and any of these can be used, or two or more of these can be used. Among them, 2,6-naphthalene dicarboxylic acid is preferred because of its excellent reactivity and availability during polymerization.
[0026] The polyester of the present invention may contain a polycarboxylic acid component other than the naphthalene dicarboxylic acid component. The polycarboxylic acid component other than the naphthalene dicarboxylic acid component is not particularly limited, and the polycarboxylic acid component is preferably an aromatic polycarboxylic acid component or an alicyclic polycarboxylic acid component, and more preferably an aromatic dicarboxylic acid component or an alicyclic dicarboxylic acid component. By using an aromatic polycarboxylic acid component or an alicyclic polycarboxylic acid component as a copolymerization component, excellent dielectric properties can be exerted.
[0027] The aromatic dicarboxylic acid component is not particularly limited, and terephthalic acid, isophthalic acid, phthalic acid, 4,4′-dicarboxybiphenyl, 5-sodium sulfoisophthalate, or esters thereof, etc. can be used.
[0028] The alicyclic dicarboxylic acid component is not particularly limited, and 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, tetrahydrophthalic acid, methyltetrahydrophthalic acid, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hydrogenated naphthalene dicarboxylic acid, and the like can be used.
[0029] The polyester of the present invention contains 20 mol% or more of dimer diol in 100 mol% of the total polyol component, preferably 30 mol% or more, and more preferably 40 mol% or more. By using a large amount of dimer diol, the dielectric properties and solvent solubility of the polyester are improved.
[0030] The dimer diol is obtained by reducing the carboxyl group of a dimer acid having 20 to 48 carbon atoms obtained by dimerizing unsaturated fatty acids having C10 to 24 and a saturated dimer acid obtained by hydrogenating the dimer acid. In addition, a vegetable oil can be used as a raw material for the dimer diol. Furthermore, the dimer diol may include a trimer that is a trimer of unsaturated fatty acids having C10 to 24 and a saturated trimer obtained by hydrogenating the trimer.
[0031] The polyester of the present invention may contain a polyol component other than the dimer diol. The polyol other than the dimer diol is not particularly limited, and ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 2-methyl-1,3-propanediol, neopentyl glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 2-methyl-2-ethyl-1,3-propanediol, 2,2-diethyl-1,3-propanediol, 2-ethyl-2- Aliphatic polyols such as n-propyl-1,3-propanediol, 2,2-di-n-propyl-1,3-propanediol, 2-n-butyl-2-ethyl-1,3-propanediol, 2,2-di-n-butyl-1,3-propanediol, 2,4-diethyl-1,5-pentanediol, and 2-ethyl-1,3-hexanediol, alicyclic polyols such as 1,4-cyclohexanedimethanol and tricyclodecanedimethanol, polyalkylene ether glycols such as polytetramethylene glycol and polypropylene glycol, etc., can be used alone or in combination. Among them, tricyclodecanedimethanol is preferred.
[0032] The polyester of the present invention can also be copolymerized with a trivalent or higher polycarboxylic acid component and / or a trivalent or higher polyol component. As a trivalent or higher polycarboxylic acid component, for example, aromatic carboxylic acids such as trimellitic acid, pyromellitic acid, benzophenonetetracarboxylic acid, trimesic acid, trimellitic anhydride (TMA), pyromellitic anhydride (PMDA), and aliphatic carboxylic acids such as 1,2,3,4-butanetetracarboxylic acid can be cited, and these can use one or more than two kinds. As a trivalent or higher polyol component, for example, glycerol, trimethylolpropane, trimethylolethane, pentaerythritol, α-methyl glucose, mannitol, sorbitol can be cited, and one or more than two kinds can be used from these. However, if the copolymerization amount of a trivalent or higher polycarboxylic acid component and / or a trivalent or higher polyol component is large, the dielectric properties of the polyester may deteriorate, so it is not preferred. When a trivalent or higher polycarboxylic acid component and / or a trivalent or higher polyol component is copolymerized, the content is preferably 5 mol% or less, more preferably 4 mol% or less, out of 200 mol% of the total of the polycarboxylic acid component and the polyol component.
[0033] The dielectric loss tangent of the polyester of the present invention at 10 GHz is preferably 0.008 or less, more preferably 0.005 or less. A polyester having a low dielectric loss tangent can provide an adhesive composition having excellent low dielectric properties.
[0034] The relative dielectric constant of the polyester of the present invention at 10 GHz is preferably 3.0 or less, more preferably 2.6 or less. The polyester having a low relative dielectric constant can provide an adhesive composition having excellent low dielectric properties.
[0035] The glass transition temperature of the polyester of the present invention is preferably above -30°C, more preferably above -20°C. By setting the glass transition temperature to a range of above -30°C, good dielectric properties are exhibited. And the stickiness (adhesiveness) of the resin surface tends to be suppressed, and the handleability of the resin is improved. In addition, the glass transition temperature is preferably below 100°C. By setting the glass transition temperature to below 100°C, lamination can be performed even at a low temperature of about 80°C. In addition, the lower the glass transition temperature, the better the bonding strength tends to be.
[0036] As the polycondensation reaction method for producing the polyester of the present invention, there are, for example: 1) a method of heating a polycarboxylic acid and a polyol in the presence of a known catalyst, and performing a polyol removal and polycondensation reaction via a dehydration esterification step; 2) a method of heating an alcohol ester of a polycarboxylic acid and a polyol in the presence of a known catalyst, and performing a polyol removal and polycondensation reaction via an ester exchange reaction; 3) a method of performing depolymerization; etc. In the above methods 1) and 2), a part or all of the acid components may be replaced by anhydrides.
[0037] When producing the polyester of the present invention, a conventionally known polymerization catalyst can be used, for example, titanium compounds such as tetra-n-butyl titanate, tetraisopropyl titanate, and titanium acetylacetonate, antimony compounds such as antimony trioxide and antimony tributoxy, germanium compounds such as germanium oxide and tetra-n-butoxygermanium, and other catalysts such as acetates of magnesium, iron, zinc, manganese, cobalt, and aluminum can be used. These catalysts can be used alone or in combination of two or more.
[0038] The number average molecular weight of the polyester of the present invention is preferably 5000 or more, more preferably 10000 or more. In addition, it is preferably 100000 or less, more preferably 50000 or less, and further preferably 30000 or less. If it is within the above range, the handling when dissolved in a solvent is easy, the adhesive strength is good, and the dielectric properties are excellent, so it is preferred.
[0039] The acid value of the polyester of the present invention is preferably 200 eq / 10 6 g or less, more preferably 100 eq / 10 6 g or less, more preferably 50eq / 10 6 g or less, particularly preferably 40eq / 10 6 g or less, and most preferably 30eq / 10 6 When the resin acid value is within the above range, low dielectric properties and excellent pot life are achieved, and in an isocyanate curing system, effects of improving substrate adhesion and crosslinking properties can also be expected.
[0040] As a method for increasing the acid value of the polyester of the present invention, for example, there are: (1) a method of adding a trivalent or higher polycarboxylic acid and / or a trivalent or higher polycarboxylic acid anhydride to react after the polycondensation reaction is completed (acid addition); (2) a method of intentionally modifying the resin by the action of heat, oxygen, water, etc. during the polycondensation reaction. These methods can be carried out arbitrarily. The polycarboxylic anhydride used in the acid addition in the above-mentioned acid addition method is not particularly limited, and examples thereof include trimellitic anhydride, pyrophthalic anhydride, hexahydrophthalic anhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 3,3,4,4-biphenyltetracarboxylic dianhydride, ethylene glycol ditriphthalic anhydride, etc., and one or more of these can be used. Triphthalic anhydride is preferred.
[0041] The polyester of the present invention can be used as an adhesive. In particular, the polyester of the present invention has excellent dielectric properties and is therefore suitable for an adhesive for FPC in a high-frequency range.
[0042] When the polyester of the present invention is used as an adhesive, a curing agent can also be included to make an adhesive composition. As a curing agent, epoxy resin, polyisocyanate, polycarbodiimide, etc. can be used. By cross-linking with these curing agents, the cohesive force of the resin can be improved and the heat resistance can be improved. Polyisocyanates are preferred due to the small influence on heat resistance and dielectric properties. Relative to 100 parts by mass of polyester, the content of the curing agent is preferably more than 0.1 parts by mass, more preferably more than 0.5 parts by mass, further preferably more than 1 part by mass, and particularly preferably more than 2 parts by mass. By being above the above lower limit, a sufficient curing effect can be obtained, and excellent adhesion and solder heat resistance can be exerted. In addition, it is preferably less than 30 parts by mass, more preferably less than 20 parts by mass, further preferably less than 15 parts by mass, and particularly preferably less than 10 parts by mass. By being below the above upper limit, the shelf life and low dielectric properties become good. That is, by being within the above range, in addition to being able to obtain adhesion, solder heat resistance and shelf life, an adhesive composition with excellent low dielectric properties can also be obtained.
[0043] The polyester of the present invention can be used as a film. When the polyester of the present invention is used as a film, the polyester can be directly processed into a film for use, or a material further dispersed with various fillers such as glass fiber and silica can be processed into a film for use. The thickness and shape of the film of the present invention are not particularly limited, and also include the form generally referred to as a sheet.
[0044] The film of the present invention is excellent in dielectric properties and is therefore suitable as a rigid substrate for high-speed transmission or a CCL base film of an FPC.
[0045] Example
[0046] Hereinafter, the present invention will be specifically described with reference to Examples. In the Examples and Comparative Examples, the abbreviation "part" means part by mass.
[0047] (1) Determination of polyester composition
[0048] Using 400MHz 1 The molar ratio of the polycarboxylic acid component and the polyol component constituting the polyester was quantitatively determined by H-nuclear magnetic resonance spectrometry (hereinafter sometimes referred to as NMR). Deuterated chloroform was used as a solvent. In addition, when the acid value of the polyester was increased by acid post-addition, the total amount of the acid components other than the acid components used for acid post-addition was set to 100 mol % and the molar ratio of each component was calculated.
[0049] (2) Determination of glass transition temperature
[0050] The measurement was performed using a differential scanning calorimeter (DSC-200, SII Company). 5 mg of the sample (polyester) was placed in an aluminum lid-type container and sealed, and cooled to -50°C using liquid nitrogen. Then, the temperature was raised to 150°C at a heating rate of 20°C / min. In the endothermic curve obtained during the heating process, the temperature of the intersection of the extension line of the baseline before the endothermic peak appeared (below the glass transition temperature) and the tangent line of the endothermic peak (the tangent line with the largest slope from the rising section of the peak to the peak apex) was taken as the glass transition temperature (Tg, unit: °C).
[0051] (3) Determination of number average molecular weight
[0052] The polyester sample was dissolved and / or diluted in tetrahydrofuran in such a way that the resin concentration was about 0.5% by weight, and filtered through a polytetrafluoroethylene membrane filter with a pore size of 0.5 μm as a sample for measurement. The molecular weight was measured by gel permeation chromatography (GPC) using tetrahydrofuran as the mobile phase and a differential refractometer as the detector. The flow rate was 1 mL / min and the column temperature was 30°C. The chromatographic columns used were KF-802, 804L, and 806L manufactured by Showa Denko. Monodisperse polystyrene was used as the molecular weight standard.
[0053] (4) Determination of acid value
[0054] 0.2 g of polyester sample was dissolved in 40 ml of chloroform and titrated with 0.01 N potassium hydroxide ethanol solution. 6 g polyester equivalent (eq / 10 6 g). Use phenolphthalein as an indicator.
[0055] Hereinafter, production examples of the polyester of the present invention and polyester serving as comparative examples are shown.
[0056] (Example 1)
[0057] Production Example of Polyester (a1)
[0058] In a reaction vessel equipped with a stirrer, a condenser, and a thermometer, 326 parts of dimethyl 2,6-naphthalene dicarboxylate, 1520 parts of dimer diol (Croda, Pripol 2033), and 0.03 mol% of tetrabutyl titanate as a catalyst were added, and the temperature was raised from 160°C to 220°C over 4 hours, and an esterification reaction was carried out while undergoing a dehydration process. Then, the system was depressurized to 5 mmHg over 20 minutes, and the temperature was further raised to 250°C for a polycondensation reaction process. Then, the pressure was reduced to less than 0.3 mmHg, and after a polycondensation reaction for 60 minutes, it was taken out. The composition of the obtained polyester (a1) was analyzed by NMR, and the result was 2,6-naphthalene dicarboxylic acid / dimer diol = 100 / 100 [molar ratio] in terms of molar ratio. In addition, the glass transition temperature was -17°C. The obtained polyester (a1) was subjected to evaluations of solvent solubility, viscosity, heat resistance, relative dielectric constant, and dielectric loss tangent. The evaluation results are shown in Table 1.
[0059] (Examples 2 to 8, Comparative Examples 1 to 7)
[0060] Production Examples of Polyesters (a2) to (a14)
[0061] According to the production example of polyester (a1), the types and mixing ratios of raw materials were changed to synthesize polyesters (a2) to (a14). Physical properties and evaluation results are shown in Table 1. PTMG1000 is polytetramethylene ether glycol (average molecular weight 1000).
[0062] Relative dielectric constant (ε c ) and dielectric loss tangent (tanδ)
[0063] The polyester dissolved in toluene in such a manner that the solid content concentration becomes 30% by mass is applied to a Teflon (registered trademark) sheet with a thickness of 100 μm in an amount to give a thickness of 25 μm after drying, and dried at 130°C for 3 minutes. Then, the Teflon (registered trademark) sheet is peeled off to obtain a test resin sheet. Then, the obtained test resin sheet is cut into strip samples of 8 cm × 3 mm to obtain a test sample. Relative dielectric constant (ε c ) and dielectric loss tangent (tan δ) were measured using Network Analyzers (manufactured by Anritsu Corporation) by using a resonant cavity perturbation method at a temperature of 23° C. and a frequency of 10 GHz.
[0064] <Evaluation Criteria of Relative Dielectric Constant>
[0065] ◎: 2.3 or less
[0066] ○: More than 2.3 and less than 3.0
[0067] ×: more than 3.0
[0068] <Evaluation criteria for dielectric loss tangent>
[0069] ◎: 0.005 or less
[0070] ○: more than 0.005 and less than 0.008
[0071] ×: more than 0.008
[0072] viscosity
[0073] A polyester varnish dissolved in toluene in such a way that the solid content concentration becomes 30% by mass is applied to a polyester film (Toyobo E5101, thickness 50 μm, corona treated surface) in an amount to make the thickness after drying 25 μm, and dried at 130°C for 3 minutes. The dried adhesive sheet is cut into a width of 25 mm and a length of 200 mm at room temperature (23°C), and the surface of the adhesive layer is attached to a rolled copper foil substrate (JX Metal Co., Ltd., BHY series), and the adhesive sheet is pressed from above using a 2kg rubber roller at a speed of 20 mm / second twice. Then, 180° peeling is performed under the condition of a peeling speed of 300 mm / min to confirm the state of the peeled substrate. The substrate has no residual glue and the interface peeling is evaluated as ○, and the adhesive layer is transferred to the substrate side as ×.
[0074] <Evaluation criteria for viscosity>
[0075] ○: No residual adhesive and interface peeling
[0076] ×: There is residual adhesive, or the adhesive layer is transferred to the substrate side
[0077] Solvent solubility
[0078] The polyester was stirred at 80° C. for 6 hours and dissolved in toluene so that the solid content concentration became 60% by mass or 50% by mass, and the solubility at this time was evaluated according to the following criteria.
[0079] <Evaluation Criteria for Solvent Solubility>
[0080] ◎: Solid content concentration is 60% by mass, completely dissolved without any dissolved residue
[0081] ○: Solid content concentration is 50% by mass, completely dissolved without any dissolved residue
[0082] ×: Solid content concentration is 50% by mass, and there is dissolved residue of resin
[0083] Heat resistance
[0084] The measurement was performed using a differential thermal and thermogravimetric simultaneous measuring device (Shimadzu Corporation, DTG-60). 50 mg of polyester was placed in a platinum bath and heated to 1000°C at a rate of 5°C / min in a nitrogen atmosphere with a flow rate of 20 ml / min. Decomposition was performed at high temperature, and the temperature at which the weight became 95% of the initial weight was taken as the 5% weight loss temperature, which was used as an indicator of heat resistance.
[0085] <Evaluation criteria for heat resistance>
[0086] ○: 5% weight loss temperature is 300°C or higher
[0087] ×: 5% weight loss temperature is lower than 300°C
[0088]
[0089] Industrial Applicability
[0090] The polyester of the present invention is excellent in solvent solubility, heat resistance and viscosity, has a low relative dielectric constant and dielectric loss tangent, and is useful as an adhesive and film for FPC in a high-frequency range.
Claims
1. A polyester having a polycarboxylic acid component and a polyol component as structural units, wherein the polyester contains 60 mol % or more of a naphthalene dicarboxylic acid component when the polycarboxylic acid component is 100 mol %, and contains 25 mol % or more of a dimer diol component when the polyol component is 100 mol %, The dimer diol is obtained by reducing the carboxyl group of a dimer acid having 20 to 48 carbon atoms obtained by dimerizing an unsaturated fatty acid having 10 to 24 carbon atoms and a saturated dimer acid obtained by hydrogenating the dimer acid. The polyol other than the dimer diol is selected from ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 2-methyl-1,3-propylene glycol, neopentyl glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 2-methyl-2-ethyl-1,3-propanediol, 2,2-diethyl-1,3-propanediol, 2-ethyl-2-n-propyl-1,3-propanediol, 2,2-di-n-propyl One or more of 1,3-propanediol, 2-n-butyl-2-ethyl-1,3-propanediol, 2,2-di-n-butyl-1,3-propanediol, 2,4-diethyl-1,5-pentanediol, 2-ethyl-1,3-hexanediol, 1,4-cyclohexanedimethanol, tricyclodecane dimethanol, polytetramethylene glycol, polypropylene glycol, glycerol, trimethylolpropane, trimethylolethane, pentaerythritol, α-methylglucose, mannitol, and sorbitol. 2 . The polyester according to claim 1 , wherein the content of the dimer diol component is 40 mol % or more.
3. The polyester according to claim 1, which has a glass transition temperature of -30°C or higher. The polyester according to any one of claims 1 to 3, which has a relative dielectric constant εc of 3.0 or less and a dielectric loss tangent tanδ of 0.008 or less at 10 GHz. 5 . An adhesive comprising the polyester according to claim 1 . 6 . A film comprising the polyester according to claim 1 .