Heat-resistant polyamide molding composition
The thermal aging resistance of the polyamide molding composition at high temperatures is solved by using high molecular weight polyols, sterically hindered phenol antioxidants and polycarboxylic acid compounds in the polyamide molding composition, combined with fibers or granular fillers. The problem of insufficient results has achieved stable performance in high temperature environments.
Patent Information
- Application Number
- CN202180017045.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-26
- Filing Date
- 2021-02-25
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-02-25
AI Technical Summary
The existing polyamide molding compositions have insufficient thermal aging resistance under long-term exposure to high temperatures, and traditional metal halide stabilizers have the risk of corrosion and failure, making it difficult to meet the high-temperature use requirements for automotive applications.
30 to 99.85% by weight of thermoplastic polyamide, 0.1 to 10% by weight of polyol, 0.05 to 3% by weight of steric hindered phenol antioxidant, 0 to 3% by weight of polycarboxylic acid compound and 0 to 50% by weight of The thermoplastic molding composition formed by fibers or granular fillers improves thermal aging resistance through high molecular weight component design.
The thermal aging performance of the polyamide molding composition is significantly improved, good mechanical properties are maintained, and the use of metal halides is avoided, and it is suitable for high temperature environments.
Smart Images

Figure BDA0003815632250000051 
Figure BDA0003815632250000052 
Figure BDA0003815632250000061
Abstract
Description
[0001] The present invention relates to thermoplastic molding compositions comprising polyamides which have improved resistance to heat aging.
[0002] The invention furthermore relates to the use of the molding compositions according to the invention for producing fibers, foils and moldings of any type, and also to the resulting fibers, foils and moldings.
[0003] Furthermore, the invention relates to mixtures comprising specific combinations of heat-resistant additives for polyamide molding compositions.
[0004] Thermoplastic polyamides such as PA6 and PA66 are often used in the form of glass-fiber-reinforced molding compositions as materials in the design of components which are exposed to high temperatures and / or elevated humidity during their lifetime and are subject to thermo-oxidative degradation.
[0005] Different heat resistant additives that resist or delay thermo-oxidative degradation are used in polyamide molding compositions, such as combinations of Cu-containing stabilizers, organic HALS (hindered amine light stabilizer) compounds or sterically hindered phenols or polyhydric alcohols. It is highly desirable to improve the heat aging resistance (HAR) of polyamides, since this can achieve a longer lifetime for components that are subject to thermal stress, or can reduce the risk of these failures. In addition, improved HAR can also permit the use of the components at higher temperatures.
[0006] US 2010 / 0028580 discloses heat resistant thermoplastic articles made from a thermoplastic, semi-aromatic polyamide composition comprising a polyol such as dipentaerythritol (DPE), a sterically hindered phenol such as 1098, Cu heat stabilizer and zinc neutralized ethylene-methacrylic acid copolymer. The heat aging properties of polyamide compositions can be improved by using these additives.
[0007] EP 2 27547 B1 describes molding compositions having enhanced flowability and thermal stability using highly branched or hyperbranched polyetheramines.
[0008] Furthermore, DE 10 2004 051 241 A1 describes molding compositions having improved flow properties and highly branched or hyperbranched polycarbonates or polyesters having a specific OH number measured with KOH.
[0009] EP 2 896 656 A1 discloses polyamide resin compositions containing hydroxyl-containing and carboxyl-containing compounds. The preferred compound is 3,5-dihydroxybenzoic acid.
[0010] WO 2012 / 106319 A2 discloses a thermoplastic melt-mixed composition with a heat stabilizer additive. The composition, for example, contains a copolymer (EPDM modified with maleic anhydride), a copper-based stabilizer system (including potassium iodide) and a low molecular weight additive (e.g., 2,6-naphthalene dicarboxylic acid). Unfortunately, the given heat aging experiment only covers a time period of 500 h, which does not represent most automotive applications.
[0011] EP 1 041 109 A2 discloses a polyamide composition having good flow properties, which comprises a polyol having a melting point of 150 to 280° C., which is intended to improve the flow properties. Examples of polyols are pentaerythritol, dipentaerythritol and trimethylolethane.
[0012] EP 3 059 283 B1 discloses polyamide resin compositions which should have improved heat aging resistance at low temperatures. These compositions comprise aliphatic compounds having three or more amino groups or three or more hydroxyl groups per molecule, and compounds having more than one functional group reacting with amino groups or hydroxyl groups per molecule. Suitable hydroxyl compounds are trimethylolpropane, pentaerythritol or dipentaerythritol, etc., see paragraphs
[0022] and
[0029] . Hydroxyl-containing aliphatic compounds can react, for example, with compounds having epoxy groups or glycidyl groups.
[0013] US2013 / 0217814 A1 discloses a flame retardant polyamide composition comprising polyamide, a halogen-free flame retardant selected from phosphorus compounds, boehmite, a polyamide having more than two hydroxyl groups and a number average molecular weight (M) of about 2000 or less. n ) of a polyol, and at least one reinforcing agent.
[0014] The heat aging resistance of the known molding compositions remains less than satisfactory, in particular with prolonged exposure to heat. In addition, due to the increasing degree of electrification, more and more applications require materials that do not contain any halogen-based stabilizer systems (e.g. copper iodide) in view of the risk of corrosion and the corresponding failures. Therefore, none of the compositions disclosed in the cited documents meet the requirement for good thermal stability, while avoiding the use of widely used combinations of metal halide stabilizers. Some additives with low molecular weight, such as dipentaerythritol, have a tendency to migrate out of the molding at elevated temperatures, resulting in a loss of mechanical properties over time.
[0015] It was therefore an object of the present invention to provide thermoplastic molding compositions comprising polyamides which have an improved HAR and which retain good mechanical properties after heat aging.
[0016] This object is achieved by a thermoplastic molding composition comprising
[0017] a) 30 to 99.85% by weight of at least one thermoplastic polyamide as component A;
[0018] b) 0.1 to 10% by weight of at least one organic compound having more than 6 hydroxyl groups and a number average molecular weight M greater than 2000 g / mol n The polyol is used as component B;
[0019] c) as component C, 0.05 to 3% by weight of at least one sterically hindered phenolic antioxidant;
[0020] d) 0 to 3% by weight of at least one organic compound having more than 3 carboxylic acid groups and / or carboxylate groups and having a number average molecular weight M greater than 300 g / mol n A polycarboxylic acid compound as component D;
[0021] e) 0 to 50% by weight of at least one fibrous and / or particulate filler as component E;
[0022] f) 0 to 25% by weight of other additives as component F;
[0023] The total weight % of components A to F is 100 weight %.
[0024] Furthermore, the object is achieved by a mixture comprising or consisting of:
[0025] b) 0.1 to 10 parts by weight of at least one polyol having more than 6 hydroxyl groups and having a number average molecular weight Mn of more than 2000 g / mol as component B;
[0026] c) 0.05 to 3 parts by weight of at least one sterically hindered phenolic antioxidant as component C;
[0027] d) 0 to 3 parts by weight of at least one polycarboxylic acid compound having more than 3 carboxylic acid groups and / or carboxylate groups and a number average molecular weight Mn greater than 300 g / mol as component D;
[0028] The total weight of components B to D is 100 parts by weight.
[0029] In this mixture, the amounts of components B, C and D listed below in % by weight may be used in parts by weight (eg, 0.5 % by weight becomes 0.5 parts by weight).
[0030] Furthermore, the object is achieved by the use of the mixture for improving the HAR of polyamides, in particular the HAR of polyamides after heat ageing.
[0031] The object is furthermore achieved by a process for producing a thermoplastic molding composition as described above, which process is carried out by mixing components A to F.
[0032] Furthermore, the object is achieved by the use of the thermoplastic molding composition for producing fibers, foils and moldings of any type, and by fibers, foils and moldings produced from the thermoplastic molding composition as defined above.
[0033] According to the present invention, it has been found that at least one hydroxyl group has more than six hydroxyl groups and has a number average molecular weight M greater than 2000 g / mol n The polyol is prepared from at least one sterically hindered phenolic antioxidant and preferably at least one polyol having more than three carboxylic acid or carboxylate groups and having a number average molecular weight M greater than 300 g / mol. n The specific combination of polycarboxylic acid compounds can act as heat stabilizers in thermoplastic polyamide molding compositions and significantly improve the heat aging resistance after prolonged exposure to heat.
[0034] The number average molecular weight and weight average molecular weight (M n , M w ) and polydispersity data can be obtained using gel permeation chromatography (GPC) with hexafluoroisopropanol as solvent using PMMA calibration.
[0035] This molecular weight determines all components useful in the thermoplastic molding compositions of the present invention.
[0036] This effect is most pronounced when the polyol component B and the polycarboxylic acid compounds of component D have a significantly high number average molecular weight so that they do not migrate from the thermoplastic molding composition during the life of the molded component at the molding temperature during production and at elevated service temperatures. This effect is most pronounced in thermoplastic molding compositions based on polyamide as the main component.
[0037] Furthermore, it is advantageous to use sterically hindered phenolic antioxidants having a sufficiently high molecular weight, preferably a molecular weight of more than 500 g / mol, in particular more than 1000 g / mol. Furthermore, they preferably exhibit a high thermal stability, measured by TGA (thermogravimetric analysis) under a nitrogen atmosphere, with a degradation of less than 2% up to 300° C.
[0038] As component A, the molding compositions of the invention comprise from 30 to 99.85% by weight, preferably from 35 to 99.4% by weight and in particular from 45 to 98.9% by weight, of at least one thermoplastic polyamide.
[0039] If components D, E or F or a combination thereof are present in the thermoplastic molding composition, the maximum amount of component A is reduced by the minimum amount of each of components D, E or F or a combination thereof.
[0040] The polyamides of the molding compositions of the invention generally have an intrinsic viscosity of 90 to 350 ml / g, preferably 110 to 240 ml / g, determined to ISO 307 at 25° C. in 0.5% strength by weight solution in 96% strength by weight sulfuric acid.
[0041] Preferred are semicrystalline or amorphous resins having a molecular weight (weight average) of at least 5000, as described, for example, in the following U.S. Patents: 2 071 250; 2 071 251; 2 130 523; 2 130 948; 2 241 322; 2 312 966; 2 512 606; and 3 393 210.
[0042] Examples of these are polyamides derived from lactams having 7 to 13 ring members, such as polycaprolactam, polycapryllactam and polylaurolactam, and polyamides obtained by reacting dicarboxylic acids with diamines.
[0043] Dicarboxylic acids which can be used are alkanedicarboxylic acids having 6 to 12, in particular 6 to 10, carbon atoms, and also aromatic dicarboxylic acids. By way of example only, mention may be made here of adipic acid, azelaic acid, sebacic acid, dodecanedioic acid and terephthalic acid and / or isophthalic acid.
[0044] Particularly suitable diamines are alkanediamines having 6 to 12, in particular 6 to 8, carbon atoms, and also meta-xylylenediamine, di(4-aminophenyl)methane, di(4-aminocyclohexyl)methane, 2,2-di(4-aminophenyl)propane, 2,2-di(4-aminocyclohexyl)propane and 1,5-diamino-2-methylpentane.
[0045] Preferred polyamides are polyhexamethylenediamide, polyhexamethylenesebacate and polycaprolactam, and also nylon-6 / 6,6 copolyamides, in particular polyamides having 5 to 95% by weight of caprolactam units (e.g. from C31 from BASF SE).
[0046] Other suitable polyamides are obtainable by so-called direct polymerization from ω-aminoalkylnitriles, for example aminocapronitrile (PA6) and adiponitrile with hexamethylenediamine (PA66) in the presence of water, as described, for example, in DE-A 10313681, EP-A 1198491 and EP 922065.
[0047] Mention may also be made of polyamides obtainable, for example, by condensation of 1,4-diaminobutane with adipic acid at elevated temperature (nylon-4,6). Processes for the preparation of polyamides of this structure are described, for example, in EP-A 38,094, EP-A 38,582 and EP-A 39,524.
[0048] Other suitable examples are polyamides obtainable via copolymerization of two or more of the above-mentioned monomers, and mixtures of two or more polyamides in any desired mixing ratios. Particularly preferred are mixtures of nylon-6,6 with other polyamides, in particular blends of nylon-6 and nylon-66, and mixtures of nylon-6 / 6,6 copolyamide and nylon-6,6 / 6 copolyamide.
[0049] Other copolyamides that have proven particularly advantageous are semiaromatic copolyamides, such as PA6 / 6T and PA66 / 6T, wherein the triamine content of these copolyamides is less than 0.5% by weight, preferably less than 0.3% by weight (see EP-A 299 444). Other high-temperature-resistant polyamides are known from EP-A 19 94 075 (PA 6T / 6I / MXD6).
[0050] The processes described in EP-A 129 195 and 129 196 can be used for preparing the preferred semiaromatic copolyamides having a low triamine content.
[0051] The following list is not comprehensive and includes the mentioned polyamides A) and other polyamides A) for the purposes of the present invention as well as the included monomers:
[0052] AB polymer:
[0053]
[0054] AA / BB polymer:
[0055]
[0056]
[0057] AA / BB polymer:
[0058]
[0059] Most preferred are PA6, PA66, PA6 / 66 and PA66 / 6.
[0060] Suitable copolyamides consist of:
[0061] A1) 20.0 to 90.0% by weight of units derived from terephthalic acid and hexamethylenediamine;
[0062] A2) 0 to 50.0% by weight of units derived from ε-caprolactam;
[0063] A3) 0 to 80.0% by weight of units derived from adipic acid and hexamethylenediamine.
[0064] A4) 0 to 40.0 wt. % of other polyamide-forming monomers;
[0065] The proportion of component A2) or A3) or A4) or a mixture thereof is at least 10.0% by weight.
[0066] Component A1) comprises from 20.0 to 90.0% by weight of units derived from terephthalic acid and hexamethylenediamine.
[0067] Besides the units derived from terephthalic acid and hexamethylenediamine, the copolyamide optionally comprises units derived from ε-caprolactam and / or units derived from adipic acid and hexamethylenediamine and / or units derived from other polyamide-forming monomers.
[0068] The aromatic dicarboxylic acids A4) contain 8 to 16 carbon atoms. Suitable aromatic dicarboxylic acids include, for example, isophthalic acid, substituted terephthalic acids and isophthalic acids such as 3-tert-butylisophthalic acid, polycyclic dicarboxylic acids such as 4,4'- and 3,3'-diphenyldicarboxylic acid, 4,4'- and 3,3'-diphenylmethanedicarboxylic acid, 4,4'- and 3,3'-sulfodiphenylcarboxylic acid, 1,4- or 2,6-naphthalenedicarboxylic acid, phenoxyterephthalic acid, isophthalic acid being particularly preferred.
[0069] Other polyamide-forming monomers A4) may be derived from dicarboxylic acids having 4 to 16 carbon atoms and aliphatic or cycloaliphatic diamines having 4 to 16 carbon atoms, and also from aminocarboxylic acids / corresponding lactams having 7 to 12 carbon atoms. Examples of suitable monomers of this type may include suberic acid, azelaic acid and sebacic acid as representatives of aliphatic dicarboxylic acids, 1,4-butanediamine, 1,5-pentanediamine, piperazine, 4,4′-diaminodicyclohexylmethane, 2,2-(4,4′-diaminodicyclohexyl)propane and 3,3′-dimethyl-4,4′-diaminodicyclohexylmethane or m-xylenediamine as representatives of lactams / aminocarboxylic acids, and caprolactam, enantholactam, 3-aminoundecanoic acid and laurolactam as representatives of diamines and caprolactams.
[0070] Suitable copolyamides of this type are described more particularly in DE-A-102009011668.
[0071] Component B is used in an amount of 0.1 to 10% by weight, preferably 0.5 to 7.5% by weight, in particular 1 to 5% by weight.
[0072] Component B is at least one having more than 6 hydroxyl groups and a number average molecular weight M n Polyols greater than 2000 g / mol.
[0073] Component B preferably has more than 8, more preferably more than 10 hydroxyl groups.
[0074] Component B preferably has a number average molecular weight M greater than 3000 g / mol, more preferably greater than 5000 g / mol, in particular greater than 10000 g / mol. n The maximum number average molecular weight is preferably 35000 g / mol, more preferably 25000 g / mol. Particularly preferred number average molecular weights of component B are 10000 to 30000 g / mol, more preferably 12500 to 22500 g / mol, most preferably 15000 to 20000 g / mol.
[0075] Weight average M w It is preferably 10,000 to 250,000 g / mol, more preferably 25,000 to 120,000 g / mol, and particularly 30,000 to 80,000 g / mol.
[0076] Component B can be selected from all suitable polyols. As long as they have more than 6 hydroxyl groups and a number average molecular weight M n Greater than 2000g / mol.
[0077] An example of a suitable polyol is ethylene vinyl alcohol copolymer, available from Mitsubishi Chemical under the trade name Soarnol TM Or by Kuraray under the trade name EVAL TM Commercially available. Other high molecular weight polyols are also suitable.
[0078] Preferably, component B is an ethylene-vinyl alcohol copolymer. Preferably, in the ethylene-vinyl alcohol copolymer, the content of ethylene units is 10 to 60 mol%, more preferably 20 to 50 mol%, especially 25 to 50 mol%.
[0079] In addition to ethylene and vinyl alcohol, residual amounts of vinyl acetate may be present in the copolymer, preferably 20 mol% or less, more preferably 10 mol% or less, in particular 5 mol% or less. Most preferably, no residual amounts of vinyl acetate are present. Ethylene-vinyl alcohol copolymers can be obtained by partial or complete hydrolysis of ethylene-vinyl acetate copolymers.
[0080] The number average molecular weight M of particularly suitable ethylene-vinyl alcohol copolymers is n The number average molecular weight M is preferably 10,000 to 30,000 g / mol, more preferably 12,500 to 22,500 g / mol, and most preferably 15,000 to 20,000 g / mol. n The molecular weight is 18000 g / mol and the weight average molecular weight is 50000 g / mol.
[0081] Polyols can also contain other functional groups that are not hydroxyl groups. However, it is preferred that polyols contain only hydroxyl groups as functional groups. Polyols can be linear, branched or hyperbranched. Specifically, highly branched or hyperbranched structures that are partly composed of hydroxyl functional groups as described in, for example, EP 2 227 507 B1 and DE 10 2002 051 241 A1 are also suitable for achieving the desired effect. For example, highly branched or hyperbranched polyetheramines with a hydroxyl number of 50 to 1000 mg KOH / g, preferably 100 to 900 mg KOH / g, more preferably 150 to 800 mg KOH / g can be used.
[0082] As component C, 0.05 to 3% by weight, preferably 0.1 to 2% by weight, in particular 0.1 to 1% by weight, of at least one sterically hindered phenolic antioxidant is used.
[0083] Component C preferably has a molecular weight of greater than 500 g / mol, more preferably greater than 1000 g / mol.
[0084] Therefore, in one embodiment, the present invention relates to a thermoplastic molding composition comprising
[0085] a) 30 to 99.85% by weight of at least one thermoplastic polyamide as component A;
[0086] b) 0.1 to 10% by weight of at least one organic compound having more than 6 hydroxyl groups and a number average molecular weight M greater than 2000 g / mol n The polyol is used as component B;
[0087] c) as component C, 0.05 to 3% by weight of at least one sterically hindered phenolic antioxidant having a molecular weight of more than 1000 g / mol;
[0088] d) 0 to 3% by weight of at least one organic compound having more than 3 carboxylic acid groups and / or carboxylate groups and having a number average molecular weight M greater than 300 g / mol n A polycarboxylic acid compound as component D;
[0089] e) 0 to 50% by weight of at least one fibrous and / or particulate filler as component E;
[0090] f) 0 to 25% by weight of other additives as component F;
[0091] The total weight % of components A to F is 100 weight %.
[0092] Preferred components A, B, C, D, E and F are described in the present application.
[0093] In addition, component C should preferably exhibit a high thermal stability, for example a maximum weight loss of 5%, more preferably a maximum weight loss of 2%, measured in a TGA (thermogravimetric analysis) experiment at 300°C under nitrogen (from 40°C to 120°C at 10°C / min, holding the temperature for 15 minutes after isothermal, then from 120°C to 600°C at 20°C / min).
[0094] Component C preferably has at least one, more preferably at least two, branched chains C 3-12 The alkyl-substituted phenol group acts as a steric hindering group and is covalently linked to the structure of component C.
[0095] Suitable sterically hindered phenols C are in principle all compounds which have a phenolic structure and which have at least one bulky group on the phenolic ring. 3-12 -alkyl, preferably branched C 3-6 -alkyl, more preferably isopropyl or tert-butyl.
[0096] Preferably, a compound of the formula
[0097]
[0098] in
[0099] R 1 and R 2 is an alkyl, substituted alkyl or substituted triazole group, and wherein the group R 1 and R 2 can be the same or different, and R 3 is an alkyl group, a substituted alkyl group, an alkoxy group or a substituted amino group. The alkyl and alkoxy residues preferably have 1 to 12 carbon atoms, more preferably 1 to 6 carbon atoms. The substituents are preferably C 1-12 -alkyl, more preferably C 1-6 -alkyl, most preferably C 1-4 -alkyl. 1 To R 3 At least one of is preferably a bulky group as defined above.
[0100] Antioxidants of the aforementioned type are described, for example, in DE-A 27 02 661 (USA 4 360 617).
[0101] Other preferred sterically hindered phenols are those derived from substituted phenylcarboxylic acids, in particular those derived from substituted phenylpropionic acids, which preferably have at least one bulky group on the phenyl group. They contain at least one, preferably two, covalently linked substituted phenylcarboxylic acid units in the structure, which preferably have at least one bulky group on the phenyl group.
[0102] The preferred phenyl carboxylic acid is phenyl-C1-12 -carboxylic acid, more preferably phenyl-C 2-6 As mentioned above, the phenyl group is preferably a phenol group having at least one bulky group on the phenol ring. Therefore, the above sterically hindered phenol is preferably combined with C 1-12 -alkane carboxylic acid is covalently linked, more preferably a straight chain C 2-6 -Alkanecarboxylic acid.
[0103] Particularly preferred compounds of this type are compounds of the formula
[0104]
[0105] Where R 4 , R 5 , R 7 and R 8 are independently C1-C8 alkyl, which itself may have substitutions (at least one of which is a bulky group), and R 6 R is a divalent aliphatic group having 1 to 10 carbon atoms, and its main chain may also have a CO bond. 4 To R 8 At least one of is a bulky group as defined above.
[0106] Preferred compounds corresponding to these formulae are
[0107]
[0108] (From BASF SE 245)
[0109]
[0110] (From BASF SE 259)
[0111] All of the following should be mentioned as examples of sterically hindered phenols:
[0112] 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 1,6-hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (from BASF SE 1010), distearyl 3,5-di-tert-butyl-4-hydroxybenzylphosphonate, 2,6,7-trioxa-1-phosphabicyclo[2.2.2]oct-4-ylmethyl 3,5-di-tert-butyl-4-hydroxyhydrocinnamate, 3,5-di-tert-butyl-4-hydroxyphenyl-3,5-distearylthiotriazepine, 2-(2'hydroxy-3'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, 2,6-di-tert-butyl-4-hydroxymethylphenol, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 4,4'-methylenebis(2,6-di-tert-butylphenol), 3,5-di-tert-butyl-4-hydroxybenzyldimethylamine.
[0113] Compounds which have proven to be particularly effective and which are therefore preferably used are 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 1,6-hexanediol bis(3,5-di-tert-butyl-4-hydroxyphenyl) propionate ( 259), pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and N,N'-hexamethylenebis-3,5-di-tert-butyl-4-hydroxyhydrocinnamamide ( 1098), and the above products from BASF SE 245 and 1010, which has particularly good applicability.
[0114] In some cases, sterically hindered phenols having not more than one sterically hindering group in the ortho position to the phenolic hydroxyl group have proven to be particularly advantageous; in particular when assessing color fastness to storage under diffuse light over a long period of time.
[0115] As component D, at least one polyol having more than 3 carboxylic acid and / or carboxylate groups and having a number average molecular weight M greater than 300 g / mol may be used. n The amount of component D is 0 to 3% by weight, preferably 0 to 2% by weight, more preferably 0 to 0.8% by weight.
[0116] If present, component D is present in an amount of 0.01 to 3 wt%, preferably 0.1 to 2 wt%, more preferably 0.2 to 0.8 wt%.
[0117] If component D is present, the maximum amount of component A is reduced by the minimum amount of component D. It is thus reduced by 0.01% by weight, preferably by 0.1% by weight, more preferably by 0.2% by weight.
[0118] The polyamide molding composition of the present invention does not need to contain component D. Therefore, according to a first embodiment, component D is not contained in the thermoplastic molding composition. However, by additionally using component D, the heat aging resistance of the thermoplastic molding composition can be further improved. Therefore, according to a second embodiment of the present invention, the thermoplastic molding composition contains 0.01 to 3% by weight, preferably 0.1 to 2% by weight, more preferably 0.2 to 0.8% by weight of component D. Molding compositions containing these amounts of component D are particularly preferred according to the present invention.
[0119] The number average molecular weight (M n ) is preferably greater than 500 g / mol, more preferably greater than 1000 g / mol, particularly greater than 2000 g / mol, more particularly greater than 3000 g / mol, most particularly greater than 2500 g / mol. Most preferably, the weight average molecular weight M w In the range of 4000 to 80000 g / mol, more preferably 15000 to 45000 g / mol.
[0120] An essential feature of component D is the presence of more than 3 carboxylic acid groups and / or carboxylate groups in the polycarboxylic acid compound. The acid functional groups may be present as free acid groups or free acid salts. Importantly, the acid or acid salt functional groups are present in the polycarboxylic acid compound.
[0121] Component D preferably has more than 5 carboxylic acid and / or carboxylate groups, more preferably more than 8 carboxylic acid and / or carboxylate groups, most preferably more than 12 carboxylic acid and / or carboxylate groups.
[0122] The carboxylic acid group is preferably a carboxylate group. Therefore, the carboxylic acid group may be partially or completely neutralized or partially or completely in salt form. Ammonium, alkali metal, alkaline earth metal, iron, copper salts or mixtures thereof are preferred. Most preferred are alkali metal salts of the carboxylic acid group. The polycarboxylic acid compound preferably has partially or completely neutralized carboxylic acid groups, more preferably neutralized with alkali metal cations.
[0123] Component D can be selected from a variety of polycarboxylic acid compounds, as long as the minimum number and minimum number-average molecular weight requirements of carboxylic acid and / or carboxylate groups are met. Possible polycarboxylic acid compounds of component D are polyacrylic acid or polyacrylates, polymethacrylic acid and polymethacrylate, copolymers containing maleic acid groups, for example polyolefins containing maleic acid groups in the main chain or as grafts, for example neutralized ethylene-maleic anhydride copolymers, or polymers substituted by sufficient number of acid or acid salt groups.
[0124] The polymers containing carboxylic acid and / or carboxylate groups may be linear, branched or highly branched. It is also possible to use polymers having a sufficient number of carboxylic acid and / or carboxylate end groups. For example, mention may be made of branched or highly branched or hyperbranched polyesters having the desired number of carboxylic acid and / or carboxylate end groups.
[0125] In the following, polyacrylic acids and polyamines in which the N atoms are partially or polysubstituted by CH2CHOOH groups are discussed in more detail.
[0126] Suitable polycarboxylic acid compounds are disclosed in the above-mentioned documents, for example US 2010 / 0028580, WO 2012 / 106319A2. Examples are polyacrylic acid (CAS: 9004-01-04), including copolymers based on polyacrylic acid of suitable molecular weight and structure. Suitable products are BASF SE's NR2500.
[0127] Highly branched or hyperbranched structures are also suitable. Complexing agents based on amino acid structures containing at least two or more amino groups and at least four or more carboxyl groups are particularly suitable. In all cases, it is desirable to apply component D as an acid salt to obtain higher thermal stability.
[0128] Component D may also be a polymer selected from polyamines, the N atoms of which are partially or completely substituted by CH2COOH groups which are partially or completely neutralized by alkali metal cations.
[0129] In the context of component D, the term "polyamine" refers to polymers and copolymers containing at least one amino group per repeating unit. The amino group can be selected from NH2 groups, NH groups, preferably tertiary amino groups. In polymers, tertiary amino groups are preferred because the alkaline polyamines have been converted into carboxymethyl derivatives and the N atoms are completely substituted or preferably partially (e.g. 50 to 95 mol%, preferably 70 to 90 mol%) replaced by CH2COOH groups, which are partially or completely neutralized by alkali metal cations. In the context of the present invention, such polymers in which more than 95 mol% to 100 mol% of the N atoms are replaced by CH2COOH groups will be considered to be completely substituted by CH2COOH groups. NH2 groups from, for example, polyethyleneamines or polyalkyleneimines can be substituted by one or two CH2COOH groups per N atom, preferably with two CH2COOH groups per N atom.
[0130] The number of CH2COOH groups in the polymer divided by the potential total number of CH2COOH groups (assuming one CH2COOH group per NH group and two CH2COOH groups per NH2 group) will also be referred to in the context of the present invention as the "degree of substitution".
[0131] The degree of substitution can be determined, for example, preferably in accordance with ASTM D 2084-07, by determining the amine number (amine value) of the polymer and its respective polyamine prior to conversion into the CH 2 COOH-substituted polymer.
[0132] Examples of polyamines are polyvinylamines, polyalkylenepolyamines and in particular polyalkyleneimines, such as polypropyleneimine and polyethyleneimine.
[0133] In the context of the present invention, polyalkylenepolyamines are preferably understood to mean polyalkylenepolyamines containing at least 6 nitrogen atoms and at least 5 C2-C 10- Polyalkylene units, preferably those polymers of C2-C3-alkylene units, such as pentaethylenehexamine, and in particular polyethyleneimines having 6 to 30 ethylene units per molecule. In the context of the present invention, polyalkylenepolyamines are understood to mean those polymer materials obtained by homopolymerization or copolymerization of one or more cyclic imines or by grafting (co)polymers with at least one cyclic imine. Examples are polyethyleneamines grafted with ethyleneimine and polyimideamines grafted with ethyleneimine.
[0134] Preferred polymers are polyalkyleneimines, such as polyethyleneimine and polypropyleneimine, preferably polyethyleneimine.Polyalkyleneimines, such as polyethyleneimine and polypropyleneimine, may be linear, substantially linear or branched.
[0135] In one embodiment of the present invention, the polyethyleneimine is selected from highly branched polyethyleneimines. Highly branched polyethyleneimines are characterized by their high degree of branching (DB). The degree of branching can be determined, for example, by 13 C-NMR spectroscopy is preferably determined in D2O and is defined as follows:
[0136] DB=D+T / D+T+L
[0137] where D (branched) corresponds to the fraction of tertiary amino groups, L (linear) corresponds to the fraction of secondary amino groups, and T (terminal) corresponds to the fraction of primary amino groups.
[0138] In the context of the present invention, highly branched polyethyleneimines are polyethyleneimines having a DB in the range from 0.25 to 0.90.
[0139] In one embodiment of the present invention, the polyethyleneimine is selected from highly branched polyethyleneimine (homopolymer) having an average molecular weight M w In the range of 600 to 75000 g / mol, preferably in the range of 800 to 25000 g / mol.
[0140] In another embodiment of the invention, the polyethyleneimine is selected from copolymers of ethyleneimine, for example copolymers of ethyleneimine with at least one diamine which has two NH2 groups per molecule in addition to ethyleneimine, for example propyleneimine, or copolymers with at least one compound having three NH2 groups per molecule, for example melamine.
[0141] In one embodiment of the present invention, the polymer is selected from branched polyethyleneimines, which are partially or completely substituted with CH2COOH groups, wherein the CH2COOH groups are replaced by Na + Partial or complete neutralization.
[0142] In the context of the present invention, the polymer is used in covalently modified form and in particular in such a way that up to a total of up to 100 mol %, preferably a total of 50 mol % to 98 mol % of the nitrogen atoms of the primary and secondary amino groups of the polymer have been reacted - the percentages being based on the total N atoms of the primary and secondary amino groups in the polymer - with at least one carboxylic acid, for example C1-CH2COOH or at least one equivalent of hydrocyanic acid (or its salt) and one equivalent of formaldehyde. In the context of the present application, the reaction (modification) can therefore be, for example, an alkylation. Most preferably, up to a total of up to 100 mol %, preferably a total of 50 mol % to 99 mol % of the nitrogen atoms of the primary and secondary amino groups of the polymer have been reacted with formaldehyde and hydrocyanic acid (or its salt), for example by a Strecker synthesis reaction. The tertiary nitrogen atoms of the polyalkyleneimines which can form the basis of the polymer generally do not contain CH2COOH groups.
[0143] The polymer may, for example, have a number average molecular weight (M) of at least 500 g / mol. n ); preferably, the number average molecular weight of the polymer is in the range of 500 to 1,000,000 g / mol, particularly preferably 800 to 50,000 g / mol, determined by determining the amine number (amine value) of the corresponding polymer before and after alkylation, for example according to ASTM D 2084-07, and calculating the corresponding value of the CH2COOH group. The molecular weight refers to the corresponding sodium salt.
[0144] Preferably, the CH2COOH groups of the polymer are partially or completely neutralized by alkali metal cations. Unneutralized COOH groups can be free acids, for example. Preferably, 90 to 100 mol % of the CH2COOH groups of the polymer are in neutralized form.
[0145] The CH2COOH groups of the polymer may be partially or fully neutralized with any type of alkali metal cation, preferably with K + , and particularly preferably with Na + .
[0146] Most preferably, component D is based on polyethyleneimines N-substituted with acetic acid or acetate groups and their respective carboxylates, preferably alkali metal salts. The polyethyleneimines thus have an amount of branching units in the polymer backbone of 20 to 50%, more preferably 25 to 35%. Suitable products are BASF SE's P.
[0147] Thus, in one embodiment, the present invention relates to a thermoplastic molding composition comprising
[0148] a) 30 to 99.85% by weight of at least one thermoplastic polyamide as component A;
[0149] b) 0.1 to 10% by weight of at least one organic compound having more than 6 hydroxyl groups and a number average molecular weight M greater than 2000 g / mol n The polyol is used as component B;
[0150] c) as component C, 0.05 to 3% by weight of at least one sterically hindered phenolic antioxidant;
[0151] d) 0.01 to 3% by weight, preferably 0.1 to 2% by weight, more preferably 0.2 to 0.8% by weight, of at least one organic compound having more than 3 carboxylic acid groups and / or carboxylate groups and having a number average molecular weight M greater than 300 g / mol n As component D, the polycarboxylic acid compound having more than 3 carboxylic acid groups and / or carboxylate groups is a polyethyleneimine N-substituted with acetic acid or acetate groups;
[0152] e) 0 to 50% by weight of at least one fibrous and / or particulate filler as component E;
[0153] f) 0 to 25% by weight of other additives as component F;
[0154] The total weight % of components A to F is 100 weight %.
[0155] Preferred components A, B, C, D, E and F are described in the present application.
[0156] As component E, the thermoplastic molding composition comprises 0 to 50% by weight, preferably 0 to 45% by weight, more preferably 0 to 40% by weight, of at least one fibrous and / or particulate filler.
[0157] Preferably, Component E comprises glass fibers and is present in an amount of about 10 to 50 wt%, more preferably 15 to 45 wt%, most preferably 20 to 40 wt%.
[0158] If component E is present, the maximum amount of component A is reduced by the minimum amount of component E so that the total amount of components A to F is still 100% by weight.
[0159] Fibrous or particulate fillers E which may be mentioned are carbon fibers, glass fibers, glass beads, amorphous silica, calcium silicate, calcium metasilicate, magnesium carbonate, kaolin, chalk, powdered quartz, mica, barium sulfate and feldspar.
[0160] Preferred fibrous fillers which may be mentioned are carbon fibers, aramid fibers and potassium titanate fibers, particular preference being given to glass fibers in the form of E glass. These can be used in the form of rovings or in the form of commercially available chopped glass.
[0161] The fibrous fillers may have been surface pretreated with silane compounds to improve compatibility with thermoplastics.
[0162] Suitable silane compounds have the following general formula:
[0163] (X-(CH2) n ) k -Si-(OC m H 2m+1 ) 4-k
[0164] The substituents are defined as follows:
[0165]
[0166] n is an integer of 2-10, preferably 3-4.
[0167] m is 1-5, preferably 1-2, and
[0168] k is 1-3, preferably 1.
[0169] Preferred silane compounds are aminopropyltrimethoxysilane, aminobutyltrimethoxysilane, aminopropyltriethoxysilane and aminobutyltriethoxysilane, and the corresponding silanes which contain a glycidyl group as substituent X.
[0170] The amount of silane compounds generally used for surface coating is from 0.01 to 2% by weight, preferably from 0.025 to 1.0% by weight and in particular from 0.05 to 0.5% by weight (based on component E).
[0171] Acicular mineral fillers are also suitable.
[0172] For the purposes of the present invention, needle-shaped mineral fillers are mineral fillers with strongly developed needle-shaped properties. An example is needle-shaped wollastonite. The mineral preferably has an L / D (length to diameter) ratio of 8:1 to 35:1, preferably 8:1 to 11:1. The mineral filler can optionally be pretreated with the above-mentioned silane compounds, but pretreatment is not necessary.
[0173] Other fillers that can be mentioned are kaolin, calcined kaolin, wollastonite, talc and chalk, and lamellar or needle-shaped nanofillers, the amount of which is preferably 0.1 to 10%. Preferred materials for this purpose are boehmite, bentonite, montmorillonite, vermiculite, hectorite and laponite. The lamellar nanofiller is organically modified by prior art methods so that it has good compatibility with organic binders. Adding lamellar or needle-shaped nanofillers to the nanocomposite material of the present invention further improves mechanical strength.
[0174] As component F, the molding compositions of the invention may contain 0 to 25% by weight, preferably 0 to 20% by weight, more preferably 0 to 15% by weight, of further additives.
[0175] If other additives are used, the minimum amount is preferably 0.1 wt%, more preferably 0.25 wt%, most preferably 0.5 wt%.
[0176] The thermoplastic molding compositions of the invention may contain as component F customary processing aids, other stabilizers, oxidation retarders, agents for combating thermal and UV decomposition, lubricants and mold release agents, colorants (eg dyes and pigments), nucleating agents, plasticizers, and the like.
[0177] As component F1, the molding compositions of the invention may comprise from 0.05 to 3% by weight, preferably from 0.1 to 1.5% by weight and in particular from 0.1 to 1% by weight of lubricants.
[0178] Preference is given to salts of Al, alkali metals or alkaline earth metals, or esters or amides of fatty acids having 10 to 44 carbon atoms, preferably 12 to 44 carbon atoms.
[0179] The metal ion is preferably an alkaline earth metal and Al, particularly preferably Ca or Mg.
[0180] Preferred metal salts are Ca stearate and Ca montanate, and Al stearate.
[0181] It is also possible to use mixtures of the various salts in any desired mixing ratio.
[0182] The carboxylic acids may be monobasic or dibasic. Examples which may be mentioned are pelargonic acid, palmitic acid, lauric acid, margaric acid, dodecanedioic acid, behenic acid, and particular preference is given to stearic acid, capric acid and montanic acid (a mixture of fatty acids having 30 to 40 carbon atoms).
[0183] The aliphatic alcohol may be monohydric to tetrahydric. Examples of alcohols are n-butanol, n-octanol, stearyl alcohol, ethylene glycol, propylene glycol, neopentyl glycol, pentaerythritol, preferably glycerol and pentaerythritol.
[0184] The aliphatic amines may be monobasic to tribasic. Examples are stearylamine, ethylenediamine, propylenediamine, hexamethylenediamine, di(6-aminohexyl)amine, particularly preferably ethylenediamine and hexamethylenediamine. Preferred esters or amides are, respectively, glyceryl distearate, glyceryl tristearate, ethylenediamine distearate, glyceryl monopalmitate, glyceryl trilaurate, glyceryl monobehenate and pentaerythritol tetrastearate.
[0185] It is also possible to use mixtures of various esters or amides, or mixtures of esters in combination with amides, in any desired mixing ratio.
[0186] As component F2, the molding composition of the invention can comprise 0.05 to 3% by weight, preferably 0.1 to 1.5% by weight and in particular 0.1 to 1% by weight of a copper stabilizer, preferably a Cu(I) halide, in particular in the form of a mixture with an alkali metal halide, preferably KI, in a ratio of in particular 1:4, sterically hindered phenols, or mixtures thereof.
[0187] Preferred monovalent copper salts used are cuprous acetate, cuprous chloride, cuprous bromide and cuprous iodide. The materials include these in an amount of 5 to 500 ppm, preferably 10 to 250 ppm, based on the polyamide.
[0188] Advantageous properties are particularly obtained if the copper is present in the polyamide in molecular distribution. This can be achieved if a concentrate in the form of a homogeneous solid solution comprising polyamide and comprising a salt of monovalent copper and comprising an alkali metal halide is added to the molding composition. For example, a typical concentrate consists of 79 to 95% by weight of polyamide and 21 to 5% by weight of a mixture of copper iodide or copper bromide and potassium iodide. The copper concentration in the homogeneous solid solution is preferably 0.3 to 3% by weight, in particular 0.5 to 2% by weight, based on the total weight of the solution, and the molar ratio of cuprous iodide to potassium iodide is 1 to 11.5, preferably 1 to 5.
[0189] Suitable polyamides for use in the concentrates are homopolyamides and copolyamides, in particular nylon-6.
[0190] According to a preferred embodiment of the invention, the molding composition is free of copper, in particular copper stabilizers, such as Cu / (I) halides, and combinations of Cu(I) halides with alkali metal halides.
[0191] More preferably, the thermoplastic molding composition of the present invention is free of metal halides.Metal halide-free systems, so-called electro-friendly systems, are of great interest because electric vehicles, electrification and connectivity are growing trends in almost all industries.
[0192] The thermoplastic molding composition is therefore preferably free of metal halides, in particular Cu halides and alkali metal halides.
[0193] The molding compositions of the invention may contain from 0.001 to 10% by weight, preferably from 0.05 to 5% by weight, in particular from 0.1 to 2.5% by weight, of particles having a particle size of up to 10 μm (d 50 The iron powder may be obtained by thermal decomposition of pentacarbonyl iron.
[0194] Iron occurs in many allotropes:
[0195] 1. α-Fe (ferrite) forms a body-centered cubic lattice, is magnetizable, dissolves small amounts of carbon, and occurs in pure iron up to 928°C. At 770°C (Curie temperature), it loses its ferromagnetic properties and becomes paramagnetic; iron in the temperature range of 770 to 928°C is also called β-Fe. At normal temperature and a pressure of at least 13000 MPa, α-Fe becomes so-called ε-Fe, whose volume decreases by about 0.20 cm 3 / mol, so the density increases from 7.85 to 9.1 (at 20000MPa);
[0196] 2. γ-Fe (austenite) forms a face-centered cubic lattice, is non-magnetic, dissolves a large amount of carbon, and is only observed in the temperature range of 928 to 1398°C;
[0197] 3.δ-Fe, body-centered, exists from 1398℃ to the melting point of 1539℃.
[0198] Metallic iron is usually silvery white, with a density of 7.874 (heavy metal), a melting point of 1539°C, a boiling point of 2880°C, and a specific heat (from 18°C to 100°C) of about 0.5g. -1 K -1 , tensile strength 220N / mm 2 Up to 280N / mm 2 These values apply to chemically pure iron.
[0199] The industrial production of iron uses the melting of iron ore, iron slag, calcined pyrite or blast furnace dust, and the remelting of scrap and alloys.
[0200] The iron powder of the invention is prepared via thermal decomposition of iron pentacarbonyl, preferably at temperatures of 150 to 350° C. The particles thus obtainable have a preferably spherical shape, thus being spherical or almost spherical (the name otherwise used is spherolitic).
[0201] Preferred iron powders have the following particle size distribution; the particle size distribution here is determined by laser scattering in a very dilute aqueous suspension (eg using Beckmann LS13320). The particle sizes (and distributions) described below can optionally be obtained by grinding and / or sieving.
[0202] dxx here means that XX% of the total volume of the particles is less than the stated value.
[0203] d 50 Values: up to 10 μm, preferably 1.6 to 8 μm, particularly 2.9 to 7.5 μm, in particular 3.4 to 5.2 μm.
[0204] d 10 Value: preferably 1 to 5 μm, particularly 1 to 3 μm, in particular 1.4 to 2.7 μm.
[0205] d 90 Values: preferably 3 to 35 μm, in particular 3 to 12 μm and very particularly 6.4 to 9.2 μm.
[0206] The iron powder preferably has an iron content of 97 to 99.8 g / 100 g, preferably 97.5 to 99.6 g / 100 g. The content of other metals is preferably less than 1000 ppm, in particular less than 100 ppm and very particularly less than 10 ppm.
[0207] The Fe content is usually determined by infrared spectroscopy.
[0208] The C content is preferably 0.01 to 1.2 g / 100 g, preferably 0.05 to 1.1 g / 100 g, and in particular 0.4-1.1 g / 100 g. This C content in the preferred iron powder corresponds to the content in the powder which has not been reduced with hydrogen after the thermal decomposition process.
[0209] The carbon content is usually determined by a method based on ASTM E1019 by burning the sample in an oxygen stream and then detecting the resulting CO 2 gas using IR (by means of Leco CS230 or CS-mat 6250 from Juwe).
[0210] The nitrogen content is preferably at most 1.5 g / 100 g, preferably 0.01 to 1.2 g / 100 g.
[0211] The oxygen content is preferably at most 1.3 g / 100 g, preferably 0.3 to 0.65 g / 100 g.
[0212] N and O are determined by heating the sample to about 2100°C in a graphite furnace. Here the oxygen obtained by the sample is converted into CO and measured by an IR detector. The N released from the nitrogen-containing compound under the reaction conditions is discharged with the carrier gas and detected and recorded by a TCD (thermal conductivity detector) (both methods are based on ASTM E1019).
[0213] The tap density is preferably 2.5 to 5 g / cm 3 , especially 2.7 to 4.4 g / cm 3 This generally means the density of the powder when it is, for example, filled into a container and compacted by vibration. The iron powder can further preferably be surface-coated with iron phosphate, with iron phosphite or with SiO2.
[0214] The BET surface area according to DIN ISO 9277 is preferably in the range of 0.1 to 10 m 2 / g, especially 0.1-5m 2 / g, preferably 0.2-1m 2 / g, and especially 0.4-1m 2 / g.
[0215] In order to achieve a particularly good dispersion of the iron particles, a masterbatch involving a polymer can be used. Suitable polymers for this purpose are polyolefins, polyesters or polyamides, and preferably the masterbatch polymer is identical to component A. The mass fraction of iron in the polymer is generally 15 to 80% by weight, preferably 20 to 40% by weight.
[0216] If component D is used in the molding composition according to the invention, the elastomeric polymer is different from component D. Thus, in the case where the composition comprises component D, the polymer of component F, in particular the elastomeric polymer, is different from the polymer of component D.
[0217] Likewise, the polymer of component F is different from the polymer of component B.
[0218] Examples of further customary additives F are elastomeric polymers (also often referred to as impact modifiers, elastomers or rubbers) in amounts of up to 25% by weight, preferably up to 20% by weight.
[0219] These are very common copolymers, preferably composed of at least two of the following monomers: ethylene, propylene, butadiene, isobutylene, isoprene, chloroprene, vinyl acetate, styrene, acrylonitrile and acrylic and / or methacrylic esters having 1 to 18 carbon atoms in the alcohol component.
[0220] Polymers of this type are described, for example, in Houben-Weyl, Methoden der organischen Chemie, Vol. 14 / 1 (Georg-Thieme-Verlag, Stuttgart, Germany, 1961), pages 392 to 406, and in the monograph Toughened Plastics by CB Bucknall (Applied Science Publishers, London, UK, 1977).
[0221] Some preferred types of such elastomers are described below.
[0222] Preferred types of such elastomers are those known as ethylene-propylene (EPM) and ethylene-propylene-diene (EPDM) rubbers.
[0223] EPM rubbers typically have few residual double bonds, whereas EPDM rubbers may have from 1 to 20 double bonds per 100 carbon atoms.
[0224] As examples of diene monomers for EPDM rubbers, there may be mentioned conjugated dienes such as isoprene and butadiene; non-conjugated dienes having 5 to 25 carbon atoms such as 1,4-pentadiene, 1,4-hexadiene, 1,5-hexadiene, 2,5-dimethyl-1,5-hexadiene and 1,4-octadiene; cyclodienes such as cyclopentadiene, cyclohexadiene, cyclooctadiene and dicyclopentadiene; and alkenyl norbornenes such as 5-ethylidene-2-norbornene, 5-butylidene-2-norbornene, 2-methylallyl-5-norbornene and 2-isopropenyl-5-norbornene; and tricyclic dienes such as 3-methyltricyclo[5.2.1.0 2,6 ]-3,8-decadiene, and mixtures thereof. Preference is given to 1,5-hexadiene, 5-ethylidene norbornene and dicyclopentadiene. The diene content of the EPDM rubber is preferably from 0.5 to 50% by weight, in particular from 1 to 8% by weight, based on the total weight of the rubber.
[0225] EPM rubbers and EPDM rubbers can also be grafted preferably with reactive carboxylic acids or derivatives of these. Examples of these are acrylic acid, methacrylic acid and derivatives thereof, such as glycidyl (meth)acrylate, and maleic anhydride.
[0226] Another group of preferred rubbers are copolymers of ethylene with acrylic acid and / or methacrylic acid and / or with esters of these acids. The rubber may also contain dicarboxylic acids, such as maleic acid and fumaric acid; or derivatives of these acids, such as esters and anhydrides; and / or monomers containing epoxy groups. These dicarboxylic acid derivatives or monomers containing epoxy groups are preferably introduced into the rubber by adding monomers containing dicarboxylic acid groups and / or epoxy groups and having the general formula I or II or III or IV to the monomer mixture.
[0227] R 1 C(COOR 2 )=C(COOR 3 )R 4 (I)
[0228]
[0229] Where R 1 To R 9 is hydrogen or an alkyl group having 1 to 6 carbon atoms, m is an integer from 0 to 20, g is an integer from 0 to 10, and p is an integer from 0 to 5.
[0230] Group R 1 To R 9 Preferred is hydrogen, where m is 0 or 1 and g is 1. Corresponding compounds are maleic acid, fumaric acid, maleic anhydride, allyl glycidyl ether and vinyl glycidyl ether.
[0231] Preferred compounds of formula I, II and IV are maleic acid, maleic anhydride and (meth)acrylates containing epoxy groups, such as glycidyl acrylate and glycidyl methacrylate; and esters with tertiary alcohols, such as tert-butyl acrylate. Although the latter do not have free carboxyl groups, their behavior is similar to that of free acids, so they are called monomers with latent carboxyl groups.
[0232] The copolymer is advantageously composed of 50 to 98% by weight of ethylene, 0.1 to 20% by weight of monomers comprising epoxy groups and / or methacrylic acid and / or monomers comprising anhydride groups, the remainder being (meth)acrylate.
[0233] Particularly preferred are copolymers consisting of:
[0234] - 50 to 98% by weight, in particular 55 to 95% by weight, of ethylene,
[0235] 0.1 to 40% by weight, in particular 0.3 to 20% by weight, of glycidyl acrylate and / or glycidyl methacrylate, (meth)acrylic acid and / or maleic anhydride, and
[0236] 1 to 45% by weight, in particular 5 to 40% by weight, of n-butyl acrylate and / or 2-ethylhexyl acrylate.
[0237] Other preferred (meth)acrylates are the methyl, ethyl, propyl, isobutyl and tert-butyl esters.
[0238] Comonomers that can be used with these are vinyl esters and vinyl ethers.
[0239] The above-mentioned ethylene copolymers can be prepared by methods known per se, preferably by random copolymerization at high pressure and high temperature. Suitable methods are well known.
[0240] Other preferred elastomers are emulsion polymers, the preparation of which is described, for example, by Blackley in the monograph “Emulsion Polymerization”. The emulsifiers and catalysts which can be used are known per se.
[0241] In principle, it is possible to use elastomers of homogeneous structure or elastomers with a shell structure. The shell structure is determined by the order in which the individual monomers are added. The morphology of the polymer is also influenced by this addition sequence.
[0242] Monomers for preparing the rubber part of the elastomers which may be mentioned here merely as examples are acrylates, for example n-butyl acrylate, 2-ethylhexyl acrylate, the corresponding methacrylates, butadiene and isoprene, and mixtures thereof. These monomers may be copolymerized with other monomers, for example styrene, acrylonitrile, vinyl ethers, and with other acrylates or methacrylates, for example methyl methacrylate, methyl acrylate, ethyl acrylate or propyl acrylate.
[0243] The soft or rubber phase of the elastomer (glass transition temperature below 0°C) can be the core, outer cladding or intermediate shell (in the case of elastomers, the structure has more than two shells). Elastomers with more than one shell can also have more than one shell consisting of a rubber phase.
[0244] If one or more hard components (glass transition temperature above 20° C.) are involved, in addition to the rubber phase, in the structure of the elastomer, these are usually prepared by polymerizing styrene, acrylonitrile, methacrylonitrile, α-methylstyrene, p-methylstyrene or acrylates or methacrylates (e.g. methyl acrylate, ethyl acrylate or methyl methacrylate) as main monomers. In addition to these, relatively small proportions of other comonomers can also be used.
[0245] It has proven to be advantageous in some cases to use emulsion polymers having reactive groups on their surface. Examples of groups of this type are epoxy, carboxyl, latent carboxyl, amino and amide groups, as well as functional groups that can be introduced by concomitant use of monomers of the following general formula.
[0246]
[0247] The substituents can be defined as follows:
[0248] R 10 is hydrogen or C1-C4 alkyl;
[0249] R 11 is hydrogen, C1-C8 alkyl or aryl, especially phenyl;
[0250] R 12 is hydrogen, C1-C 10 -alkyl, C6-C 12 -aryl, or -OR 13 .
[0251] R 13 is C1-C8-alkyl or C6-C 12 - an aryl group, which may be optionally substituted by an O-containing group or an N-containing group.
[0252] X is a chemical bond, C1-C 10 -alkylene or C6-C 12 -arylene, or
[0253]
[0254] Y is OZ or NH-Z, and
[0255] Z is C1-C 10 -alkylene or C6-C 12 -Arylene.
[0256] The grafting monomers described in EP-A 208 187 are also suitable for introducing reactive groups on the surface.
[0257] Other examples which may be mentioned are acrylamide, methacrylamide and substituted acrylates or methacrylates, for example (N-tert-butylamino)ethyl methacrylate, (N,N-dimethylamino)ethyl acrylate, (N,N-dimethylamino)methyl acrylate and (N,N-di-ethylamino)ethyl acrylate.
[0258] The particles of the rubber phase may also have been crosslinked. Examples of crosslinking monomers are 1,3-butadiene, divinylbenzene, diallyl phthalate and dicyclopentadienyl acrylate, and also the compounds described in EP-A 50 265.
[0259] It is also possible to use monomers called graft-linked monomers, i.e. monomers with two or more polymerizable double bonds that react at different rates during polymerization. Preferably, this type of compound is used, wherein at least one reactive group is polymerized at a rate roughly the same as other monomers, and another reactive group (or multiple reactive groups) is, for example, polymerized significantly slower. Different polymerization rates produce a certain proportion of unsaturated double bonds in rubber. If another phase is grafted onto this type of rubber afterwards, at least some double bonds present in the rubber react with the grafted monomer to form a chemical bond, i.e. the grafted phase at least has a certain degree of bonding to the chemical bonding on the grafting basis.
[0260] Examples of this type of graft-linked monomers are monomers containing allyl groups, in particular allyl esters of ethylenically unsaturated carboxylic acids, such as allyl acrylate, allyl methacrylate, diallyl maleate, diallyl fumarate and diallyl itaconate, and the corresponding monoallyl compounds of these dicarboxylic acids. In addition, there are a variety of other suitable graft-linked monomers. For further details, reference may be made, for example, to U.S. Patent No. 4,148,846.
[0261] The proportion of these crosslinking monomers in the impact-modifying polymer is generally up to 5% by weight, preferably not more than 3% by weight, based on the impact-modifying polymer.
[0262] Some preferred emulsion polymers are listed below. Here we can first mention graft polymers having a core and having at least one shell and having the following structure:
[0263]
[0264] Instead of graft polymers whose structure has more than one shell, homogeneous, i.e. single-shell elastomers composed of 1,3-butadiene, isoprene and n-butyl acrylate or of copolymers thereof can also be used. These products can also be prepared by the concomitant use of crosslinking monomers or monomers having reactive groups.
[0265] Examples of preferred emulsion polymers are n-butyl acrylate-(meth)acrylic acid copolymers, n-butyl acrylate / glycidyl acrylate or n-butyl acrylate / glycidyl methacrylate copolymers, graft polymers having an inner core composed of n-butyl acrylate or based on butadiene and an outer cladding composed of the above copolymers, and copolymers of ethylene with comonomers providing reactive groups.
[0266] The elastomers described can also be prepared by other conventional methods, for example by suspension polymerization.
[0267] Silicone rubbers are described, for example, in DE-A 37 25 576, EP-A 235 690, DE-A 38 00 603 and EP-A 319 290.
[0268] Of course, mixtures of the rubber types listed above may also be used.
[0269] UV stabilizers which may be mentioned, usually in amounts of up to 2% by weight, based on the molding composition, are various substituted resorcinols, salicylates, benzotriazoles and benzophenones.
[0270] Materials that may be added as colorants are inorganic pigments such as titanium dioxide, ultramarine blue, iron oxide and carbon black, and organic pigments such as phthalocyanine, quinacridone, perylene, and dyes such as anthraquinone.
[0271] Materials that can be used as nucleating agents are sodium phenylphosphinate, alumina, silica, and preferably talc.
[0272] The thermoplastic molding compositions may also comprise, as component F, flame retardants.
[0273] As component F, the thermoplastic molding material can comprise 1.0 to 10.0% by weight, preferably 2.0 to 6.0% by weight, in particular 3.0 to 5.0% by weight, of at least one phosphazene of the general formula (IX) or (X) as flame retardant.
[0274] The minimum amount of component F is at least 1.0% by weight, preferably 2.0% by weight and in particular 3.0% by weight.
[0275] The maximum amount of component F is 10.0% by weight, preferably 6.0% by weight, particularly preferably 5.0% by weight.
[0276] "Phosphazene" is understood to mean a cyclic phosphazene of the general formula (IX)
[0277]
[0278] Wherein m is an integer from 3 to 25, R 4 and R 4’ are the same or different and represent C1-C 20 -alkyl-, C6-C 30 -Aryl-, C6-C 30 -Arylalkyl- or C6-C 30 Alkyl substituted aryl or linear phosphazenes
[0279]
[0280] wherein n represents 3 to 1000, and X represents N=P(OPh)3 or N=P(O)OPh and Y represents P(OPh)4 or -P(O)(OPh)2.
[0281] The production of such phosphazenes is described in EP-A 0 945 478 .
[0282] Particularly preferred is the formula (XI) P3N3C 36 Cyclic phenoxyphosphazene
[0283]
[0284] or a linear phenoxyphosphazene according to formula (XII)
[0285]
[0286] The phenyl group may be optionally substituted. Phosphazenes in the context of the present application are described in Mark, JE, Allcock, HR, West, R., Inorganic Polymers, Prentice Hall, 1992, pages 61 to 141.
[0287] Preferably, a cyclic phenoxyphosphazene having at least three phenoxyphosphazene units is used as component F. The corresponding phenoxyphosphazenes are described, for example, in paragraphs
[0051] to
[0053] of US 2010 / 0261818. In particular, reference may be made to formula (I) therein. In addition, the corresponding cyclic phenoxyphosphazenes are described in EP-A-2100919, in particular in paragraphs
[0034] to
[0038] thereof. The preparation can be carried out according to the description of paragraph
[0041] of EP-A-2100919. In one embodiment of the invention, the phenyl group in the cyclic phenoxyphosphazene may be replaced by C 1-4 - Alkyl substitution. This is preferred when pure phenyl groups are involved.
[0288] For further reference to cyclophosphazene, see Chemie Lexikon, 9th edition, keyword “phosphazenes”. The preparation is effected, for example, via cyclophosphazenes obtainable from PCl5 and NH4Cl, in which the chlorine group in the cyclophosphazene has been replaced by a phenoxy group by reaction with phenol.
[0289] Cyclophenoxyphosphazene compounds can be prepared, for example, as described in Allcock, HR, Phosphorus-Nitrogen Compounds (Academic Press, 1972) and Mark, JE, Allcock, HR, West, R., Inorganic Polymers (Prentice Hall, 1992).
[0290] Component F is preferably a mixture of cyclic phenoxyphosphazenes having three and four phenoxyphosphazene units. The weight ratio of rings comprising three phenoxyphosphazene units to rings comprising four phenoxyphosphazene units is preferably about 80:20. Rings of larger phenoxyphosphazene units may likewise be present, but in smaller amounts. Suitable cyclic phenoxyphosphazenes are available from Fushimi Pharmaceutical under the trade name FP-100 was obtained. This was an off-white / yellowish solid having a melting point of 110° C., a phosphorus content of 13.4% and a nitrogen content of 6.0%. The proportion of rings containing three phenoxyphosphazene units was at least 80.0% by weight.
[0291] The thermoplastic molding material preferably comprises 1.0 to 6.0% by weight, preferably 2.5 to 5.5% by weight and in particular 3.0 to 5.0% by weight, of at least one aliphatic or aromatic ester of phosphoric acid or polyphosphoric acid as flame retardant.
[0292] For this purpose, non-migrating phosphates with a melting point between 70° C. and 150° C. are preferred in particular. This makes the product easy to meter and exhibits significantly less migration in the molding material. Particularly preferred examples are the commercially available phosphate esters PX-200 from Daihachi (CAS: 139189-30-3) or Sol-DP from ICL-IP. Other phosphates with appropriately substituted phenyl groups are also conceivable, if they allow the preferred melting range to be achieved. Depending on the substitution pattern in the ortho or para position of the aromatic ring, the general structural formula is as follows:
[0293]
[0294]
[0295] in
[0296] R 1 =H, methyl, ethyl or isopropyl, but preferably H.
[0297] N = between 0 and 7, but preferably 0.
[0298] R 2-6 =H, methyl, ethyl or isopropyl, but preferably methyl. 6Preferred with R 4 and R 5 same.
[0299] m=can but need not be the same, and is between 1, 2, 3, 4 and 5, but preferably 2.
[0300] R= can be H, methyl, ethyl or cyclopropyl, but methyl and H are preferred.
[0301] PX-200 is a specific example:
[0302]
[0303] It is particularly preferred when at least one aromatic ester of polyphosphoric acid is used. Such aromatic polyphosphates are available, for example, from Daihachi Chemical under the trade name PX-200.
[0304] As component F, the thermoplastic molding materials of the invention can comprise 5.0 to 30.0% by weight, preferably 10.0 to 25.0% by weight, in particular 12.0 to 20.0% by weight, for example about 16.0% by weight, of at least one metal phosphinate or the phosphinates specified below as flame retardant.
[0305] The minimum amount of component D is 5.0% by weight, preferably 10.0% by weight and in particular 12.0% by weight.
[0306] The maximum amount of component F is 30.0% by weight, preferably 25.0% by weight, particularly preferably 20.0% by weight.
[0307] Examples of preferred flame retardants of component F are metal phosphonates derived from hypophosphorous acid. For example, metal salts of hypophosphorous acid with Mg, Ca, Al or Zn as metal can be used. Aluminum hypophosphite is particularly preferred.
[0308] Also suitable are phosphinates of the formula (I) and / or phosphinates of the formula (II) or polymers thereof
[0309] in
[0310] R 1 , R 2 are identical or different and represent hydrogen, linear or branched C1-C6-alkyl, and / or aryl;
[0311] R 3 Indicates a straight or branched chain C1-C 10 -alkylene, C6-C 10 -Arylene, C6-C 10 -alkylene aryl or C6-C 10 - arylenealkyl;
[0312] M represents Mg, Ca, Al, Sb, Sn, Ge, Ti, Zn, Fe, Zr, Ce, Bi, Sr, Mn, Li, Na, K and / or a protonated nitrogen base;
[0313] m=1 to 4; n=1 to 4; x=1 to 4, preferably m=3, x=3.
[0314] Preferably, R 1 , R 2 are identical or different and represent hydrogen, methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-pentyl and / or phenyl.
[0315] Preferably, R 3 represents a methylene group, an ethylene group, an n-propylene group, an isopropylene group, an n-butylene group, a tert-butylene group, an n-pentylene group, an n-octylene group or an n-dodecylene group, a phenylene group or a naphthylene group; a methylene phenyl group, an ethylene phenyl group, a tert-butyl phenyl group, a methylene naphthyl group, an ethylene naphthyl group or a tert-butyl naphthyl group; a phenylene methyl group, a phenylene ethyl group, a phenylene propyl group or a phenylene butyl group.
[0316] Particularly preferably, R 1 , R 2 is hydrogen, methyl, ethyl, and M is Al, and Al hypophosphite is particularly preferred.
[0317] The production of the phosphinates is preferably carried out by precipitation of the corresponding metal salts from aqueous solution. However, the phosphinates can also be precipitated in the presence of suitable inorganic metal oxides or sulfides as support materials (white pigments, such as TiO2, SnO2, ZnO, ZnS, SiO2). This accordingly provides surface-modified pigments which can be used as laser-markable flame retardants for thermoplastic polyesters.
[0318] The use of metal salts of substituted phosphinic acids is preferred, wherein one or two hydrogen atoms have been replaced by phenyl, methyl, ethyl, propyl, isobutyl, isooctyl or the group R'-CH-OH, by R'-hydrogen, phenyl, tolyl, compared to hypophosphorous acid. The metal is preferably Mg, Ca, Al, Zn, Ti, Fe. Diethylaluminum phosphinate (DEPAL) is particularly preferred.
[0319] With regard to the description of phosphinates or diphosphinates, reference is made to DE-A 199 60 671 as well as DE-A 44 30 932 and DE-A 199 33 901.
[0320] Other flame retardants are, for example, halogen-containing flame retardants.
[0321] Suitable halogen-containing flame retardants are preferably brominated compounds, such as brominated diphenyl ether, brominated trimethylphenylindane (FR 1808 from DSB), tetrabromobisphenol A and hexabromocyclododecane.
[0322] Suitable flame retardants are preferably brominated compounds, such as brominated oligocarbonates (BC 52 or BC 58 from Great Lakes), having the structural formula:
[0323]
[0324] Particularly suitable are polybenzyl methacrylates where n>4 (eg FR1025 from ICL-IP having the formula
[0325]
[0326] Preferred brominated compounds also include oligomeric reaction products (n>3) of tetrabromobisphenol A with epoxides (eg, FR2300 and 2400 from DSB) having the formula:
[0327]
[0328] The brominated oligostyrenes preferably used as flame retardants have an average degree of polymerization (number average) of 3 to 90, preferably 5 to 60, measured in toluene by vapor pressure osmometry. Cyclic oligomers are also suitable. In a preferred embodiment of the invention, the brominated oligostyrenes have the formula I shown below, in which R represents hydrogen or an aliphatic group, in particular an alkyl group, such as CH2 or C2H5, and n represents the number of repeated chain structural units. R 1 This may be H or bromine, or a fragment of a conventional free radical former.
[0329]
[0330] The numerical value n can be from 1 to 88, preferably from 3 to 58. The brominated oligostyrene contains 40.0 to 80.0% by weight, preferably 55.0 to 70.0% by weight of bromine. Preference is given to products consisting mainly of polydibromostyrene. The substance can be melted without decomposition, for example soluble in tetrahydrofuran. The substance is either generated by ring bromination of optionally aliphatic hydrogenated styrene oligomers (obtained, for example, by thermal polymerization of styrene) (according to DT-OS 25 37 385), or by free radical oligomerization of suitable brominated styrenes. The formation of flame retardants can also be achieved by ionic oligomerization of styrene and subsequent bromination. The amount of brominated oligomers necessary to give the polyamide flame retardant properties depends on the bromine content. The bromine content in the molding material of the present invention is from 2.0 to 30.0% by weight, preferably from 5.0 to 12.0% by weight.
[0331] The brominated polystyrenes according to the invention are generally obtained by the process described in EP-A 047 549.
[0332]
[0333] The brominated polystyrene obtainable and commercially available by this process is predominantly a ring-substituted tribrominated product. n' (see III) typically has values of 125 to 1500, which corresponds to a molecular weight of 42500 to 235000, preferably 130000 to 135000.
[0334] The bromine content (based on the content of ring-substituted bromine) is generally at least 50.0% by weight, preferably at least 60.0% by weight and in particular 65.0% by weight.
[0335] Commercially available powdered products generally have a glass transition temperature of 160° C. to 200° C. and are available, for example, from Albemarle under the trade name HP-7010 and from Ferro Corporation under the trade name PB 68 obtained.
[0336] Mixtures of brominated oligostyrenes and brominated polystyrenes can also be used in the molding materials of the present invention, the mixing ratio being freely selectable.
[0337] Also suitable are chlorine-containing flame retardants such as Decoran from OxyChem. is preferred.
[0338] Suitable halogen-containing flame retardants are preferably ring-brominated polystyrene, brominated polybenzyl acrylate, brominated bisphenol A epoxide oligomer or brominated bisphenol A polycarbonate.
[0339] In one embodiment of the present invention, no halogen-containing flame retardants are used in the thermoplastic molding materials according to the invention.
[0340] In the context of the present invention, flame-retardant melamine compounds suitable as component F are melamine compounds which, when added to glass-fiber-filled polyamide molding materials, reduce the flammability and influence the behavior of fire in a flame-retardant manner, resulting in improved performance in the UL94 test and in the glow-wire test.
[0341] The melamine compound is, for example, selected from melamine borate, melamine phosphate, melamine sulfate, melamine pyrophosphate, melam, melem, melon or melamine cyanurate or mixtures thereof.
[0342] The melamine cyanurate of the present invention is preferably a reaction product of melamine (Formula I) and cyanuric acid / isocyanuric acid (Formulas Ia and Ib) in equimolar amounts.
[0343]
[0344] It is obtained, for example, by reacting an aqueous solution of the starting compound at 90° C. to 100° C. The commercially available product is a white powder with an average particle size of d 50 1.5 to 7 μm, d 99 The value is less than 50μm.
[0345] Other suitable compounds (often also described as salts or adducts) are melamine sulfate, melamine, melamine borate, oxalates, primary phosphates (phosphate prim.), secondary phosphates (phosphate sec.) and primary pyrophosphates (phosphate sec.), melamine neopentyl glycol borate. According to the invention, the molding material preferably does not contain polymeric melamine phosphates (CAS no. 56386-64-2 or 218768-84-4).
[0346] This will be understood to mean melamine polyphosphates of 1,3,5-triazine compounds having an average degree of condensation number n of 20 to 200 and a 1,3,5-triazine content of 1.1 to 2.0 mol per mole of phosphorus atom selected from the following 1,3,5-triazine compounds: melamine, melam, melem, melonamine, cyanuric acid diamide, cyanuric acid amide, 2-ureido melamine, acetoguanamine, benzoguanamine and diaminophenyl triazine. Preferably, the n value of these salts is generally 40 to 150, and the proportion of 1,5-triazine compounds per mole of phosphorus atom is preferably 1.2 to 1.8. In addition, the pH of a 10% by weight aqueous slurry of the salt produced according to EP-B 1095030 is generally greater than 4.5 and preferably at least 5.0. The pH is usually determined by adding 25 g of salt and 225 g of clean water to a 300 ml beaker at 25°C, stirring the resulting aqueous slurry for 30 minutes, and then measuring the pH. The above n value, i.e., the number average degree of condensation, can be determined by 31P solid-state NMR. JR van Wazer, CF Callis, J. Shoolery and R. Jones, J. Am. Chem. Soc., 78, 5715, 1956 disclosed that the number of adjacent phosphate groups gives a unique chemical shift, thereby clearly distinguishing orthophosphates, pyrophosphates and polyphosphates.
[0347] Suitable guanidine salts are
[0348]
[0349] In the context of the present invention, "compound" is understood to mean not only benzoguanamine itself and its adducts / salts, but also nitrogen-substituted derivatives and their adducts / salts.
[0350] Also suitable is ammonium polyphosphate (NH4PO3) n , wherein n is about 200 to 1000, preferably 600 to 800, and tris(hydroxyethyl)isocyanurate (THEIC) of formula IV
[0351]
[0352] or with aromatic carboxylic acid Ar(COOH) m The reaction product of the aromatic carboxylic acid Ar(COOH) m wherein Ar represents a monocyclic, bicyclic or tricyclic aromatic six-membered ring system and m is 2, 3 or 4 and may optionally be present in a mixture with one another.
[0353] Examples of suitable carboxylic acids include phthalic acid, isophthalic acid, terephthalic acid, 1,3,5-benzenetricarboxylic acid, 1,2,4-benzenetricarboxylic acid, pyromellitic acid, benzilic acid, prehniticacid, 1-naphthoic acid, 2-naphthoic acid, naphthalene dicarboxylic acid, and anthracenecarboxylic acid.
[0354] According to the process of EP-A 584 567, the preparation is effected by reaction of tris(hydroxyethyl)isocyanurate with acids, their alkyl esters or their halides.
[0355] Such reaction products are mixtures of monomers and oligoesters, which may also be crosslinked. The degree of oligomerization is generally from 2 to about 100, preferably from 2 to 20. It is preferred to use THEIC and / or its reaction products with phosphorus-nitrogen compounds, especially (NH4PO3) n or mixtures of melamine pyrophosphate or polymerized melamine phosphate. (NH4PO3) n The mixing ratio with THEIC is preferably 90.0 to 50.0:10.0 to 50.0, in particular 80.0 to 50.0:50.0 to 20.0% by weight, based on the mixture of these compounds.
[0356] Likewise suitable flame retardants are phenylguanidine compounds of the formula V
[0357]
[0358] Therein, R, R′ denotes a straight-chain or branched alkyl radical having 1 to 10 carbon atoms, preferably hydrogen, and in particular adducts thereof with phosphoric acid, boric acid and / or pyrophosphoric acid.
[0359] Also preferred are allantoin compounds of formula VI,
[0360]
[0361] wherein R, R' are as defined in formula V, and salts thereof with phosphoric acid, boric acid and / or pyrophosphoric acid, and glycoluril of formula VII or salts thereof with the above acids
[0362]
[0363] wherein R is as defined in Formula V.
[0364] Suitable products are commercially available or can be obtained according to DE-A 196 14 424.
[0365] The cyanoguanidine (Formula VIII) used in the present invention can be obtained, for example, by reacting calcium cyanamide with carbonic acid, the resulting cyanamide dimerizing at pH 9 to pH 10 to provide cyanoguanidine.
[0366]
[0367] The commercially available product is a white powder with a melting point of 209°C to 211°C.
[0368] Particular preference is given to using melamine cyanurate (e.g. melamine cyanurate from BASF SE). MC25).
[0369] It is also possible to use individual metal oxides, such as antimony trioxide, antimony pentoxide, sodium antimonate and similar metal oxides. However, such metal oxides are preferably avoided since they are already present in component F. For the description of pentabromobenzyl acrylate and antimony trioxide or antimony pentoxide, reference is made to EP-A 0 624 626.
[0370] Phosphorus, such as red phosphorus, can also be used as a flame retardant. For example, red phosphorus can be used in the form of a masterbatch.
[0371] The following dicarboxylic acids can also be used
[0372]
[0373] in
[0374] R 1 To R 4 independently of one another represent halogen or hydrogen, provided that at least one radical R 1 To R 4 represents halogen,
[0375] X=1 to 3, preferably 1, 2
[0376] m=1-9, preferably 1-3, 6, 9, especially 1-3
[0377] n=2 to 3
[0378] M = alkaline earth metal, Ni, Ce, Fe, In, Ga, Al, Pb, Y, Zn, Hg.
[0379] Preferred dicarboxylates as group R 1 To R 4 , containing independently Cl or bromine or hydrogen, particularly preferably all radicals R 1 To R 4 It is Cl and / or Br.
[0380] Be, Mg, Ca, Sr, Ba, Al, Zn, Fe are preferred as metal M.
[0381] Such dicarboxylates are commercially available or can be prepared according to the methods described in US Pat. No. 3,354,191.
[0382] Also useful as component F are functional polymers. These polymers may be, for example, flame retardant polymers. Such polymers are described, for example, in US 8,314,202 and contain 1,2-bis[4-(2-hydroxyethoxy)phenyl]ethanone repeating units. Another suitable functional polymer for increasing the amount of carbon residues is poly(2,6-dimethyl-1,4-phenylene oxide) (PPPO).
[0383] The thermoplastic molding composition of the invention can be prepared by known methods by mixing the starting components in conventional mixing equipment, such as screw-type extruders, Brabender mixers or Banbury mixers, and then extruding them. After extrusion, the extrudate can be cooled and granulated. It is also possible to premix the individual components and then add the remaining starting materials individually and / or likewise in the form of a mixture. The mixing temperature is generally 230 to 320° C.
[0384] These materials are suitable for producing any type of fibers, foils and moldings. Some examples are: cylinder heads, motorcycle covers, intake manifolds, charge air cooler covers, plug connectors, gears, cooling fan wheels and cooling water tanks.
[0385] In the electrical and electronic fields, the flow-improved polyamides can be used to manufacture plugs, plug components, plug connectors, membrane switches, printed circuit board modules, microelectronic components, coils, I / O plug connectors, plugs for printed circuit boards (PCBs), plugs for flexible printed circuits (FPCs), plugs for flexible integrated circuits (FFCs), high-speed plug connections, terminal strips, connector plugs, device connectors, cable harness assemblies, circuit mounts, circuit mount assemblies, three-dimensional injection molded circuit mounts, electrical connection elements, and electromechanical assemblies.
[0386] Possible uses inside the car are instrument panels, steering column switches, seat assemblies, headrests, center consoles, gearbox assemblies and door modules, and possible uses outside the car are for door handles, exterior mirror assemblies, windshield wiper assemblies, windshield wiper protection housings, grilles, roof rails, sunroof frames, engine hoods, cylinder head covers, air intake ducts (especially intake manifolds), windshield wipers, and exterior body work assemblies.
[0387] The combination of components B, C and D produces an effective system to stabilize polyamide at temperatures of 180°C and above while maintaining a completely metal halide-free system.
[0388] In a preferred embodiment, the thermoplastic molding compositions are completely free of halogen, so that they also contain no halogen-containing flame retardants.
[0389] In particular, the combination of high molecular weight EVOH with specific high molecular weight phenolic radical scavengers and optionally high molecular weight polyacids has proven to be an effective system for stabilizing polyamides. Even under moisture absorption or under electrical tension, the additives do not float to the surface. Thus, contamination and corrosion of electrical components can be avoided. Example
[0390] The following components were used:
[0391] PA1: polyamide 6, viscosity number 150 ml / g, measured at 25° C. as a 0.5% strength by weight solution in 96% strength by weight sulfuric acid to ISO 307, melting point: 220° C. (from BASF SE B27).
[0392] PA2: polyamide-66, viscosity number 150 ml / g, measured at 25° C. as a 0.5% strength by weight solution in 96% strength by weight sulfuric acid to ISO 307, melting point: 260° C. (from BASF SE A27).
[0393] PA3: polyamide 66 / 6, viscosity number 150 ml / g, measured at 25° C. as a 0.5% strength by weight solution in 96% strength by weight sulfuric acid to ISO 307, melting point: 195° C. (from BASF SE C27).
[0394] GF: Standard E glass fiber, NEG-T249H
[0395] Lubricant: Ethylene bisstearamide (EBS), from Lonza Cologne GmbH
[0396] Stabilizer 1a: Cuprous iodide (CAS: 7681-65 to 4)
[0397] Stabilizer 1b: Potassium iodide (CAS: 7681-11-0)
[0398] Stabilizer 2: EVOH (ethylene-vinyl alcohol copolymer; CAS: 25067-34-9) with an ethylene content of 20%-50%
[0399] Stabilizer 3: 1010, from BASF SE
[0400] Stabilizer 4: P from BASF SE
[0401] Stabilizer 5: DPE (dipentaerythritol, CAS: 126-58-9)
[0402] Stabilizer 6: Iron powder (CAS: 7439-89-6)
[0403] Colorant: Solvent Black 7 (CAS: 8005 to 02-5)
[0404] Preparation of particles
[0405] The naturally colored polyamide granules were dried in an oven at 100° C. for 4 hours to a humidity of less than 0.1%. Then, a molding composition was prepared by melt compounding. The components were mixed in a twin-screw extruder with a diameter of 25 mm and an L / D ratio of 36. The processing conditions were set at 16 kg / h and 260 to 330° C., with a flat temperature profile depending on the base resin. The extrudate obtained was cooled and pelletized.
[0406] The obtained pellets are used for injection molding tensile rods or plates according to ISO 527-2 and for Charpy sticks according to ISO 179-1. The molding temperature is between 280° C. and 330° C. melt temperature of the base resin and 80° C. to 120° C. mold temperature. The compositions and mechanical data for the inventive (INV) and comparative (COMP) examples are listed in the following Tables 1 and 2.
[0407] The tensile modulus of elasticity, tensile stress at break and tensile strain at break are determined according to ISO 527. The Charpy (notched) impact strength is determined according to ISO 179-2 / 1eU and ISO 179-2 / 1eAf, respectively. The melting point and crystallization temperature are determined according to ISO 11357. All specifications are subject to the version valid in 2020.
[0408] Heat aging experiments were conducted in a standard laboratory oven at elevated temperature and air as shown in the table below. The retention of tensile strength and elongation at break after heat aging was compared to the values of the original specimens, with the non-heat aged control specimens considered to be 100%.
[0409] Table 1
[0410]
[0411] Table 2
[0412]
[0413] The above examples show that by using stabilizer 2 (polyol according to component B) and stabilizer 3 (sterically hindered phenol antioxidant according to component C), polyamide molding compositions can be obtained, which show high retention of tensile strength and elongation at break after prolonged heat treatment. By additionally using stabilizer 4 (which is a polycarboxylic acid compound of component D), the heat aging resistance of the polyamide molding composition can be further increased, see Examples INV2, INV4 and INV5.
Claims
1. A thermoplastic molding composition comprising a) 30 to 99.85% by weight of at least one thermoplastic polyamide As component A; b) 0.1 to 10% by weight of at least one hydroxyl group having more than 6 hydroxyl groups and a number average molecular weight M n Polyols greater than 2000 g / mol As component B; c) 0.05 to 3% by weight of at least one sterically hindered phenolic antioxidant As component C; d) 0.01 to 3% by weight of at least one polyethylenimine having more than 3 carboxylic acid groups and / or carboxylate groups, based on N-substituted polyethyleneimine with acetic acid or acetate groups, and having a number average molecular weight M n Polycarboxylic acid compounds greater than 300 g / mol As component D; e) 0 to 50% by weight of at least one fibrous and / or particulate filler As component E; f) 0 to 25% by weight of other additives As component F; The total weight % of components A to F is 100 weight %.
2. The thermoplastic molding composition according to claim 1, wherein component B has more than 8 hydroxyl groups.
3. The thermoplastic molding composition according to claim 2, wherein component B has more than 10 hydroxyl groups.
4. Thermoplastic molding composition according to claim 1 or 2, wherein component B has a number average molecular weight M n Greater than 3000g / mol.
5. Thermoplastic molding composition according to claim 4, wherein component B has a number average molecular weight M n Greater than 5000g / mol.
6. Thermoplastic molding composition according to claim 5, wherein component B has a number average molecular weight M n Greater than 10000 g / mol.
7. The thermoplastic molding composition according to claim 1 or 2, wherein component B is an ethylene-vinyl alcohol copolymer having an ethylene unit content of 10 to 60 mol%.
8. The thermoplastic molding composition according to claim 1 or 2, wherein component C has a molecular weight of more than 500 g / mol.
9. The thermoplastic molding composition according to claim 8, wherein component C has a molecular weight of greater than 1000 g / mol.
10. Thermoplastic molding composition according to claim 1 or 2, wherein component D has a number average molecular weight M n Greater than 500g / mol.
11. Thermoplastic molding composition according to claim 10, wherein component D has a number average molecular weight M n Greater than 1000g / mol.
12. Thermoplastic molding composition according to claim 11, wherein component D has a number average molecular weight M n Greater than 5000g / mol.
13. Thermoplastic molding composition according to claim 1 or 2, wherein component C has at least one branched C 3-12 - Alkyl substituted phenol group.
14. Thermoplastic molding composition according to claim 13, wherein component C has at least two C 3-12 - Alkyl substituted phenol group.
15. The thermoplastic molding composition according to claim 1 or 2, wherein component D is present in an amount of 0.1 to 2% by weight.
16. The thermoplastic molding composition according to claim 15, wherein component D is present in an amount of 0.2 to 0.8% by weight.
17. The thermoplastic molding composition according to claim 1 or 2, wherein component E comprises glass fibers and is present in an amount of 10% to 50% by weight.
18. The thermoplastic molding composition according to claim 17, wherein component E is present in an amount of 15% to 45% by weight.
19. The thermoplastic molding composition according to claim 18, wherein component E is present in an amount of 20% to 40% by weight.
20. Process for producing a thermoplastic molding composition according to claim 1, by mixing components A to F.
21. Use of the thermoplastic molding composition according to claim 1 for producing fibers, foils and moldings of any type.
22. Fibers, foils or moldings produced from the thermoplastic molding composition according to claim 1.
23. Use of a mixture comprising or consisting of: b) 0.1 to 10 parts by weight of at least one hydroxyl group having more than 6 hydroxyl groups and a number average molecular weight M n Polyols greater than 2000 g / mol As component B; c) 0.05 to 3 parts by weight of at least one sterically hindered phenolic antioxidant As component C; d) 0.01 to 3 parts by weight of at least one polyethyleneimine having more than 3 carboxylic acid groups and / or carboxylate groups, based on N-substituted acetic acid or acetate groups, and having a number average molecular weight M n Polycarboxylic acid compounds greater than 300 g / mol As component D.
24. The use according to claim 23, wherein the amount of component D is 0.1 to 2 parts by weight.
25. The use according to claim 24, wherein the amount of component D is 0.2 to 0.8 parts by weight.
Citation Information
Patent Citations
flowable polyamides with hyperbranched polyesters / polycarbonates
DE102004051241A1
Thermoplastic molded mass, useful for the preparation of fibers, molded bodies or foil, comprises a thermoplastic polyamide, a high- or hyper- branched polyester in an acid or alcohol component containing aromatic core, and an additive
DE102009011668A1
process for the production of polyamides
DE10313681A1
synergistic flame retardant combination for polymers
DE19614424A1
Flame retardant combination
DE19933901A1