Use of cellulose derivatives and method for surface sizing
By using a water-based surface sizing composition of cellulose ether on paperboard, the problem of compressive strength degradation of paperboard in humid environment is solved, its moisture resistance and compressive strength are improved, and it meets the requirements for use under high humidity and high temperature conditions. Demand has promoted its application as a sustainable packaging material.
Patent Information
- Application Number
- CN202180018905.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-03-04
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-03-04
AI Technical Summary
The compressive strength of cardboard deteriorates in humid environments, and its waterproof and moisture-proof properties are poor, making it difficult to meet the needs of use in humid conditions.
An aqueous surface sizing composition containing cellulose ether is used for surface sizing of fiber webs such as paper and cardboard to provide compressive strength and moisture resistance, especially in high-humidity and high-temperature environments.
Significantly improves the compressive strength and moisture resistance of cardboard, extending its service life in humid environments and enabling lighter structures, enhancing its competitiveness as a sustainable packaging material.
Smart Images

Figure GDA0004580310640000101 
Figure HDA0003830061240000011 
Figure HDA0003830061240000012
Abstract
Description
[0001] The present invention relates to the use of at least one cellulose derivative and to a method for surface sizing of fibrous webs such as paper, board and the like.
[0002] The advent of e-commerce has revolutionized consumer habits and the packaging market in the 21st century. As a result, the demand for packaging materials has increased dramatically. At the same time, concerns about climate change, dwindling fossil oil reserves and the accumulation of plastics in nature have forced suppliers around the world to constantly seek more sustainable packaging to protect and transport their products.
[0003] Paperboard, especially corrugated paperboard, is one of the most used packaging materials in the world due to its low price, lightweight structure and recyclability. For example, in e-commerce, corrugated paperboard accounts for up to 80% of the entire packaging material demand. Traditionally, the use of cellulose-based packaging materials such as paperboard has been considered as a sustainable alternative due to its renewable source, recyclability and established recycling systems. In addition, recycled fiber materials, such as old corrugated containers (OCC) and deinked paper (DIP), are often used as raw materials for paperboard. In addition to recyclability and renewable sources, the fluted three-layer structure of corrugated paperboard leads to extremely high stiffness and a relatively low basis weight. The low weight in turn means low energy demand during transportation.
[0004] Despite its obvious advantages, paperboard also has its limitations. One of the main disadvantages of paperboard is its poor resistance to water and moisture. The main components of paperboard are fibers based on amphiphilic cellulose, whose hydrophilic hydroxyl groups give the fibers mechanical strength but at the same time make them susceptible to moisture. In disposable cups, food packaging and beverage packaging, for example, the problem is usually solved by covering the surface of the paperboard with a protective polyethylene film. In the case of packaging paperboard, such as corrugated board, however, strict requirements for cost efficiency, lightness and recyclability limit the use of protective films and coatings. Usually, the only surface treatment that linerboard, i.e. the surface layer of corrugated board, undergoes during the manufacturing process is starch-based surface sizing. The application of starch is mainly used to increase the mechanical strength of the paperboard.
[0005] For paperboard used as packaging material, such as boxes and containers, the compressive strength of the paperboard is one of the most important properties, which determines the strength of the packaging. When packages are stored and / or transported, they are mainly subjected to compressive forces, for example, caused by other packages when packages are stacked on top of each other. The reason for compressive strength failure is the collapse of the structure of the paperboard under the compressive forces. The mechanisms of compression failure are not fully understood; however, they are different from the mechanisms of tensile strength failure, in which the fibers are torn from the structure by tension. Therefore, the compressive strength of paperboard cannot be predicted from its tensile strength properties.
[0006] Furthermore, under wet conditions, the compressive strength of paperboard may deteriorate rapidly. The hydroxyl groups of starch used in surface sizing are sensitive to water molecules, resulting in a decrease in strength properties under wet conditions. Nowadays, many commodities are produced in countries with wet environmental conditions, such as Southeast Asia, from where they are shipped all over the world. This increases the demand for paperboard with improved compressive strength even in wet conditions.
[0007] In view of the above, there is a need to improve the moisture resistance of fibrous packaging materials such as paperboard, and to enhance their compressive strength properties in a humid environment.
[0008] The object of the present invention is to minimize or even eliminate the disadvantages existing in the prior art.
[0009] The object of the present invention is to increase the strength properties of fiber webs such as paper, board or the like, such as compressive strength, tear strength and / or bursting strength, in particular the compressive strength, even in a wet environment.
[0010] Another object of the present invention is to improve the moisture resistance of fiber webs such as paper, board and the like, in particular board, such as linerboard.
[0011] Another object of the present invention is to provide a fiber web such as paper, board etc. having a high compressive strength, especially under high humidity conditions.
[0012] All described embodiments and advantages apply to the use and method according to the invention, where applicable, even if this is not always explicitly stated.
[0013] These objectives are achieved by the features of the present invention. The present invention also provides some preferred embodiments.
[0014] A typical use of the surface size composition according to the invention comprising at least one cellulose derivative selected from cellulose ethers (excluding carboxyalkyl cellulose) is to provide compressive strength to fibrous webs such as paper, board, etc., which preferably comprise recycled cellulose fibers.
[0015] In a typical method for surface sizing of a fiber web such as paper, paperboard, etc. according to the present invention, the method comprises
[0016] - obtaining a fiber web, preferably comprising recycled cellulose fibers, such as paper, cardboard, etc.,
[0017] - applying an aqueous surface sizing composition on the surface of the fiber web in a surface sizing station or in a coating station, wherein the surface sizing composition comprises at least one cellulose derivative selected from cellulose ethers (excluding carboxyalkyl cellulose) and provides compressive strength to the fiber web.
[0018] It has now surprisingly been found that the use of at least one cellulose derivative selected from cellulose ethers in a surface sizing composition provides compressive strength properties to fibrous webs such as paper, paperboard, etc., not only under standard ambient conditions (temperature +23°C, relative humidity 50%), but also in particular under high humidity and high temperature ambient conditions (temperature +38°C, relative humidity 90%). The present invention provides a moisture-resistant and bio-based alternative for food production that does not compete with conventionally used starches. The improved compressive strength properties and moisture resistance obtained by using cellulose ethers provide a broad field of possible end-use applications and reduce moisture-related damage to paper, paperboard, etc. in geographical areas with high humidity levels and high temperatures. Furthermore, the improvement in compressive strength properties may enable even lighter structures, making fibrous webs such as paperboard a more sustainable packaging option.
[0019] In the present context, the term "humidity resistance" is defined as the ability of paper, paperboard, etc. to maintain its compressive strength in high humidity. According to the present invention, the use of a cellulose derivative selected from cellulose ethers in the surface sizing composition provides, i.e. maintains and / or increases, the compressive strength, tear strength and / or bursting strength of a fiber web such as paper, paperboard, etc. under standard conditions and in particular when the fiber web is exposed to ambient conditions, wherein the relative humidity is ≥80%, preferably ≥85%, more preferably ≥90% and the temperature is ≥30° C., preferably ≥35° C., more preferably ≥38° C. In particular, the compressive strength, expressed as SCT strength for paper, paperboard, etc. and measured according to ISO 9895 standard (2008), can be increased, both when exposed to standard ambient conditions (+23° C., relative humidity 50%) and in particular when exposed to ambient conditions, wherein the relative humidity is ≥80%, preferably ≥85%, more preferably ≥90% and the temperature is ≥30° C., preferably ≥35° C., more preferably ≥38° C.
[0020] The cellulose ethers suitable for the present invention are water-soluble, at least in cold water (+15° C.). The cellulose ethers may be selected from alkyl celluloses, hydroxyalkyl celluloses, hydroxyalkyl alkyl celluloses and any mixtures thereof. The cellulose ethers may contain one or more alkyl and / or hydroxyalkyl groups, which may be the same or different from each other. Suitable alkyl groups are, for example, methyl, ethyl and propyl groups. Suitable hydroxyalkyl groups are, for example, hydroxymethyl, hydroxyethyl and hydroxypropyl groups. The cellulose ethers may have a degree of substitution DS of alkyl and hydroxyalkyl groups in the range of 0.1-3, preferably 0.5-2.7, more preferably 0.7-2.5, even more preferably 1.0-2.1 or from 1.0 to less than 2.0. According to a preferred embodiment, the cellulose ethers are selected from the group consisting of methyl cellulose, ethyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, (hydroxyethyl) methyl cellulose and (hydroxypropyl) methyl cellulose.
[0021] The cellulose ether may even contain other functional groups in addition to alkyl, hydroxyalkyl and hydroxyl groups. Other functional groups may be selected from, for example, carboxylate, carboxyalkyl, sulfonate, phosphonate, amine, amide and alkyl ester groups. If the cellulose ether contains one or more other groups in addition to alkyl and / or hydroxyalkyl groups, the degree of substitution of the alkyl and / or hydroxyalkyl groups is higher than the degree of substitution of the other groups.
[0022] Carboxyalkylcelluloses, such as carboxymethylcellulose, are excluded from the scope of the present invention. The surface sizing composition used according to the invention therefore does not contain carboxyalkylcelluloses, such as carboxymethylcellulose. According to one embodiment, even the cellulose ethers do not contain carboxylate and carboxyalkyl groups as functional groups.
[0023] The cellulose backbone of the cellulose ether may be derived from plant-based cellulose or microbial cellulose. Preferably, the cellulose backbone of the cellulose ether is derived from plant-based cellulose, more preferably wood-based cellulose.
[0024] The cellulose ether suitable for use in the present invention may have a weight average molecular weight of ≤300000 g / mol, preferably ≤100000 g / mol, more preferably ≤45000 g / mol, even more preferably ≤20000 g / mol. The weight average molecular weight of the cellulose derivative may be in the range of 1000-300000 g / mol, preferably 2000-100000 g / mol, more preferably 3000-45000 g / mol or even more preferably 5000-20000 g / mol. According to a preferred embodiment, the weight average molecular weight of the cellulose derivative may be in the range of 5000-18000 g / mol. Sometimes the weight average molecular weight of the cellulose derivative may be in the range of 5000-15000 g / mol. The low molecular weight of the cellulose ether may provide a surface sizing composition with a low viscosity, which means that the solid content of the surface sizing composition may be increased while still being able to apply the sizing composition in a surface sizing station or in a coating station using conventional application methods. On the other hand, the use of cellulose derivatives with high molecular weight can provide higher surface sizing efficiency due to the improved ability to enhance interfiber bonding, thus even further improving compressive strength properties.
[0025] The surface sizing composition preferably does not contain any solvent other than water, and in particular the surface sizing composition does not contain any organic solvent, such as alcohol.
[0026] According to a preferred embodiment, the viscosity of the aqueous surface sizing composition may be less than 2000 mPas, preferably less than 500 mPas, more preferably less than 100 mPas, and even more preferably less than 50 mPas. The viscosity of the aqueous surface sizing composition ensures that the composition can be effectively applied to the surface of the fiber web. In some embodiments, the aqueous surface sizing composition comprising cellulose ether can be applied to the fiber web in a coating station using any conventional coating method, such as knife coating, rod coating, roller coating, curtain coating or spraying. Generally, the aqueous surface sizing composition comprising a cellulose derivative selected from cellulose ethers can be preferably applied to the surface of the fiber web in a surface sizing station comprising any conventional surface sizing equipment such as a pool sizing press, a film sizing press or a gate roller sizing press.
[0027] According to one embodiment, the surface sizing composition may comprise at least one cellulose derivative selected from the above-mentioned cellulose ethers and starch. In this embodiment, the viscosity of the cellulose derivative has a small effect on the final viscosity of the surface sizing composition, which enables the use of a cellulose derivative with a higher solid content and / or a high molecular weight.
[0028] The aqueous surface sizing composition may comprise at least 1 wt. %, preferably at least 2 wt. %, more preferably at least 4 wt. % of a cellulose derivative selected from cellulose ethers. According to an embodiment, the surface sizing composition may comprise 1-25 wt. %, preferably 1.5-18 wt. %, more preferably 2-14 wt. %, even more preferably 4-12 wt. % of a cellulose derivative. The percentages are calculated from the total weight of the surface sizing composition.
[0029] In addition to the cellulose ether, the surface sizing composition may contain additives conventionally used for surface sizing of paper, paperboard, etc. Such additives may be selected from hydrophobic agents, colorants, inorganic pigments, surfactants, plasticizers, defoamers, fluorescent brighteners, rheology modifiers, strength additives and aluminum compounds, which may enhance the sizing properties of the surface sizing composition and / or improve its runnability in a coating station or surface sizing station such as a size press, and / or otherwise adjust the surface properties of the final paper, paperboard, etc.
[0030] The surface sizing composition may have a solids content of 1-30 wt%, preferably 1-20 wt%, more preferably 4-16 wt%, even more preferably 7-16 wt%, calculated from the total weight of the surface sizing composition. Preferably the surface sizing composition is free of inorganic pigments and mineral particles.
[0031] According to one embodiment, the surface sizing composition may be applied to the surface of the fiber web in an amount of at least 0.25 g / m 2 , preferably at least 0.5g / m 2 , more preferably at least 1 g / m 2 Such an amount is applied to the surface of the fiber web. For example, the surface sizing composition can be applied in such an amount that the cellulose ether is 0.25-9 g / m 2 , preferably 0.5-7g / m 2 , more preferably 0.65-5g / m 2 or 1-3g / m 2 , sometimes even more preferably from more than 1g / m 2 Up to 3g / m 2 The amount of surface sizing applied to the surface of the fiber web can be increased to increase the strength of the final paper, paperboard, etc., especially the compressive strength.
[0032] According to a preferred embodiment, the method comprises applying the aqueous surface sizing composition at least two or three times or more successively on the surface of the fiber web. The use of multiple consecutive applications of the surface sizing composition can allow an increase in the pick-up of the composition and thus a further improvement in the strength properties can be achieved. In addition, multiple applications increase the degrees of freedom associated with the viscosity and / or solids content of the surface sizing composition.
[0033] After applying the surface sizing composition on the surface of the fiber web, the web is dried in the drying section of a paper or board machine. In case the surface sizing composition is applied two, three or more times consecutively, the fiber web may be dried between consecutive applications of the surface sizing composition.
[0034] The present invention is particularly applicable to a method for producing a fiber web such as paper or paperboard containing recycled cellulose fibers. According to one embodiment, the fiber web such as paper, paperboard, etc., to which the surface sizing composition is applied, contains recycled cellulose fibers derived from old corrugated cardboard (OCC) and / or other recycled fiber materials. OCC may include used recycled unbleached or bleached kraft pulp fibers, hardwood semi-chemical pulp fibers, straw pulp fibers, or any mixture thereof. In addition to recycled fibers, the fiber web may contain cellulose fibers obtained by kraft pulping and / or chemical-thermomechanical pulping. According to one embodiment of the present invention, the fiber web contains at least 20% by weight, preferably at least 50% by weight of recycled cellulose fibers, for example derived from OCC and / or other recycled fiber materials. In some embodiments, the fiber web may contain even> 70% by weight, sometimes even> 80% by weight of recycled fibers, for example derived from OCC and / or other recycled fiber materials. The amount of recycled fibers in the fiber web may be 20-100 wt.-%, preferably 55-100 wt.-%, more preferably 75-95 wt.-%, calculated on a dry basis from the total weight of all fibers in the fiber web.
[0035] The pH of the fiber raw material used to form the fiber web, preferably comprising recycled fibers, may be ≥ 6, such as 6-8.
[0036] The fiber web may also contain inorganic mineral pigment fillers and various other additives.
[0037] According to one embodiment of the fiber web, the fiber web may have a basis weight of at least 20 g / m2 on a dry basis. 2 , preferably at least 60g / m 2 , more preferably at least 80g / m 2 , even more preferably at least 100 g / m 2 The basis weight of the fiber web, calculated on a dry basis, may be in the range of 20-500 g / m 2 , preferably 50-400g / m2 , preferably 60-350g / m 2 Or sometimes even 100-200g / m 2 within the range.
[0038] According to a preferred embodiment, the present invention is used to manufacture a fiber web, such as paperboard, preferably a multi-layer paperboard, wherein the fiber web is a layer in a multi-layer paperboard selected from a testliner, a kraft board or a corrugated medium. The present invention is particularly suitable for surface sizing of linerboard, such as a testliner containing recycled fibers or a kraft board mainly containing mechanical pulp. The testliner can contain a layered structure of two to four layers and / or have a weight of 80-350 g / m 2 The invention is also applicable to the surface sizing of corrugated paper, especially when recycled fibers are used as raw materials. The corrugated paper can have a single-layer structure. The basis weight can be between 110-180 g / m 2 within the range.
[0039] The use of a surface sizing composition comprising a cellulose derivative selected from cellulose ethers improves the strength properties of the final paper or paperboard, such as SCT strength, tear strength and / or burst strength, especially the compressive strength expressed as SCT strength and / or RCT strength. These are important strength properties for paper and paperboard, especially for grades used for packaging. Short-span Compression Test (SCT) strength can be used to predict the compression resistance of the final product, such as a paperboard box. Boxes made of boxboard are exposed to high loads when stacked during storage and transportation, which makes compressive strength, i.e. SCT strength, perhaps the most important strength property. Tear strength is another important mechanical property for linerboard. High tear strength prevents linerboard from cracking during folding, bending and cutting. Bursting strength represents the rupture resistance of paper / paperboard, which is defined as the hydrostatic pressure required to rupture the sample when pressure is uniformly applied to the sides of the sample. Ring compression test (RCT) strength can also be used to predict the compression resistance of the final product, i.e. the resistance of paper / paperboard to combined buckling and compression failure.
[0040] One use of at least one cellulose derivative selected from the group consisting of cellulose ethers (excluding carboxyalkyl cellulose) according to the present invention is in a surface sizing composition for increasing the strength properties and / or moisture resistance of paper, paperboard or the like.
[0041] In a method for surface sizing of fiber webs such as paper, board, etc. according to the present invention, an aqueous surface sizing composition is applied on the surface of the fiber web, wherein the surface sizing composition comprises at least one cellulose derivative selected from cellulose ethers (excluding carboxyalkyl cellulose).
[0042] One embodiment relates to the use of at least one cellulose derivative selected from cellulose ethers (excluding carboxyalkyl cellulose) in a surface sizing composition for improving the strength properties and / or moisture resistance of paper, paperboard, and the like. Example
[0043] Some embodiments of the invention are described in the following non-limiting examples.
[0044] Two cellulose derivatives were tested in the surface sizing of paperboard and their effect on compressive strength was studied in standard (RH 50%, 23°C) and high humidity (RH 90%, 38°C) conditions.
[0045] Base Board Sheet
[0046] The non-surface-sizing grooved sheet was used as the substrate sheet in the test. The properties of the substrate sheet are given in Table 1.
[0047] Table 1 Properties of substrate sheets
[0048]
[0049]
[0050] Cellulose derivatives
[0051] Two water-soluble cellulose derivatives were tested, methylcellulose MC (Sigma Aldrich) and (hydroxypropyl)methylcellulose HPMC (Sigma Aldrich). HPMC was tested with two different weight average molecular weights of 10000 and 22000 g / mol. The tested MC had a weight average molecular weight of 14000 g / mol.
[0052] The cellulose derivatives tested for sample preparation are soluble in cold water but insoluble in hot water. First, a masterbatch with the highest feasible concentration is prepared for each cellulose derivative, and the actual surface sizing sample is prepared by diluting the masterbatch. The cellulose derivative is provided in the form of a dry powder. First, one-third of the required amount of water is heated to a gelatinization temperature significantly higher than the cellulose derivative. The cellulose derivative powder is then added to hot water (MC:>80°C, HPMC:>90°C) and the dispersion is mixed until the powder is uniformly dispersed. Thereafter, the dispersion is placed in an ice bath and the remaining water is added as cold tap water. The powder dissolves rapidly during the cooling process. The solutions are mixed for half an hour, and then they are placed in a cold room (+5°C) overnight to precipitate.
[0053] Reference starch
[0054] Reference starch (Raisamyl 01121, Chemigate) is cooked before being used for surface sizing. Weigh the starch in powder form, add it to cold tap water and mix until fully dispersed. Thereafter, heating is started. The starch begins to dissolve in a temperature range of 60 to 70°C and forms a light yellow liquid. When the temperature reaches 95°C, the starch is cooked for at least 30 to 40 minutes, then cooled to a suitable sizing temperature in a heating cabin and then poured into a 100ml sample bottle. Starch with a solid content of 12wt-% is used as a reference starch to represent the compressive strength that can be obtained by a common surface sizing procedure. In addition, a 5wt-% starch sample was prepared to provide more comparable data for cellulose derivatives with a low solid content. In addition, the effect of the solid content of starch on the acceptance and compressive strength of the paperboard was determined.
[0055] Execution of surface sizing experiments
[0056] A laboratory-scale tank sizing press (Labor Sizepresse SP5607) with a sizing roller (diameter 110 mm) was used. The sizing parameters, such as the pressure and rotation speed of the rollers, were kept constant to ensure comparability of the results. The exception was the sizing temperature, which was varied according to the gelatinization temperature of the tested cellulose derivatives and the retrogradation temperature of the starch. The sizing temperature was 40°C for HPMC and 30°C for MC. The starch was surface sized at a temperature of about 65°C to avoid partial retrogradation of the amylose.
[0057] The volume of sizing in the tank and the drying time in the drum dryer were kept constant in all tests. After each surface sizing treatment, the samples were dried using a drum dryer. The speed of the drying felt was adjusted so that the sized sheet traveled in the dryer for about 90 seconds. Table 2 lists all sizing parameters and the values of each parameter.
[0058] Table 2 Surface sizing parameters tested for each material
[0059] Surface sizing parameters Numeric Rubber volume (ml) 100 Drying time in drum dryer (s) 90 Pressure (bar) 2 Speed (m / s) 2
[0060] The acceptance of the surface sizing on the paperboard was evaluated under standard conditions (RH=50%, T=23°C) by weighing the sheet before and after surface sizing. The weight difference was then calculated and divided by the surface area of the sheet. Since the surface sizing adheres to both sides of the paperboard, the acceptance was divided by two to obtain the acceptance for each side.
[0061] In some tests, the sheets were passed through the size press two or three times. In this procedure, the sheets were dried in a drum dryer between each pass.
[0062] The surface sizing test of the substrate with pure water was performed multiple times as a reference to observe the effect of multiple exposure to water on the compressive strength of the paperboard.
[0063] Compressive strength measurement
[0064] Only the cross direction (CD) compressive strength was measured. The length of each sample piece was the width of the A5 sample sheet (148 mm) and the sample width was 15 mm. The compressive strength was measured by the short span compression test (SCT) method using an L&W compression strength tester (STFI). The measurements were performed according to the ISO 9895 standard (2008). For all cellulose derivative samples, two parallel measurements were performed on all 8 sample pieces, with a total of 16 measurements per sample. 8 parallel measurements were performed for the base paper reference sample.
[0065] All SCT measurements were performed at RH=50% and T=23°C. High humidity (RH 90%) samples were also measured under standard conditions after spending an overnight in a conditioning chamber at RH=90% and T=38°C. In other words, the samples were conditioned to provide a high moisture content to the cardboard test pieces. After conditioning, the samples were brought to the SCT equipment in plastic bags to maintain high humidity conditions until the actual measurements were taken. It was assumed that moisture could not penetrate the plastic bags, so the sample pieces were assumed to lose their moisture only when they were outside the bag. Therefore, the time outside the bag was minimized and kept as constant as possible for each sample. A maximum of 8 samples were placed in the conditioning chamber at a time. All sample groups were placed in separate plastic bags, 4 pieces per group.
[0066] In addition to measuring the SCT value, the surface sizing properties of each cellulose derivative were evaluated by comparing the SCT increase obtained in direct proportion to the amount of sizing received. This so-called "sizing efficiency" determines how much compressive strength the material can provide to the paperboard when one gram is applied per square meter per side.
[0067] result
[0068] The appearance of the surface sized samples was similar to the starch sized samples. The only noticeable difference was the curl and slightly darker hue of the sized substrate sheet.
[0069] Receiving amount
[0070] The pick-up of the surface sizing depends strongly on the solid content of the size. All cellulose derivative solutions with 5 wt-% solid content have pick-up values close to that of 5 wt-% starch solutions. This indicates a similar tendency to adhere to the board surface and penetrate into the board structure. When the sheet passes through the size press two or three times, the pick-up per pass remains almost unchanged.
[0071] The effect of molecular weight on the obtained uptake was investigated using two HPMC samples with the same concentration but with different molecular weights of the cellulose derivative. The sample with the lower molecular weight resulted in higher uptake values in all four test points. Figure 1 The effect of molecular weight on the uptake of surface sizing is shown. It can be assumed that lower molecular weights may allow the cellulose derivative to penetrate into smaller pores and deeper into the structure of the paper sheet.
[0072] SCT intensity at RH 50%, 23℃
[0073] It was found that all tested cellulose derivative solutions could improve the compressive strength of the substrate at RH 50% and 23°C. Figure 2 In fact, the SCT values achieved for the paperboard sheet surfaces sized with the 8 wt-% HPMC solution were comparable to those obtained with the 12 wt-% reference starch solution, despite lower solids content and pickup. Even higher SCT values were obtained when the sheet surfaces were sized twice and three times with the 8 wt-% HPMC solution. Moreover, the 5 wt-% MC solution significantly increased the SCT value of the base paper in 50% relative humidity.
[0074] Figure 3 A comparison between the 5 wt-% solutions is shown. It can be seen that HPMC outperforms the reference starch in all three test points. The paperboard samples surface sized twice with MC solution exhibited better compressive strength than the corresponding paperboard samples surface sized twice with starch or HPMC solution. One possible explanation for this is the higher content of hydrophobic functional groups in the methylcellulose molecules. The hydrophobicity may protect the cellulose fibers of the substrate from swelling during the second exposure to water, therefore mitigating the down-regulation effect in the second round of sizing. The comparison between low and high molecular weight HPMC samples shows that high molecular weight can improve compressive strength despite lower uptake and assumed lower penetration into the smallest pores of the paperboard structure.
[0075] Furthermore, it was observed that 2 wt-% high molecular weight HPMC solution provided better sizing efficiency (SCT increase / acceptance) than the other tested combinations.
[0076] SCT intensity at RH 90%, 38°C
[0077] The SCT results of cellulose derivatives in 90% relative humidity and 38°C temperature were even more promising than those in RH 50%. The use of cellulose derivatives in surface sizing also improved the high wet compressive strength of the substrate sheet, as shown in Figure 2. Figure 4 The best one-pass result was achieved by the 5 wt-% MC solution, which outperformed the 8 wt-% HPMC solution and the 12 wt-% reference starch solution. The comparison of the 5 wt-% solution showed that the substrate sheets surface-sized twice with the MC solution (two passes) also had higher compressive strength than the corresponding samples sized with starch or HPMC. The high SCT values obtained with the MC solution in high humidity support the proposed theory on the protective effect of the hydrophobic functional groups in the MC molecules.
[0078] Comparison between low and high molecular weight HPMC samples showed that high molecular weight HPMC could also improve compressive strength in RH 90%.
[0079] It was concluded that the surface sizing using the aqueous surface sizing composition comprising water-soluble MC and HPMC was performed without any major difficulties and that the two cellulose derivatives provided improved compressive strength to paperboard. Particularly under high humidity conditions, the cellulose derivative samples showed better SCT strength results than the samples surface sized using conventional starch.
[0080] Even though the present invention has been described with reference to what are currently considered to be the most practical and preferred embodiments, it should be understood that the present invention should not be limited to the above-described embodiments, but the present invention is also intended to cover different modifications and equivalent technical solutions.
Claims
1. Use of a surface sizing composition for providing compressive strength to a fiber web, the fiber web comprising recycled cellulose fibers, wherein the surface sizing composition comprises at least one cellulose derivative, the cellulose derivative being a cellulose ether selected from the group consisting of alkyl cellulose, hydroxyalkyl cellulose, hydroxyalkyl alkyl cellulose and any mixture thereof, excluding carboxyalkyl cellulose, wherein: The surface sizing composition has a solid content of 4-30 wt % and comprises 4-25 wt % of cellulose ether, the percentage being calculated from the total weight of the surface sizing composition, and wherein the cellulose ether is present in an amount of 0.5-9 g / m 2 Amount within the range of .
2. The use according to claim 1, characterized in that The cellulose ether is selected from the group consisting of methyl cellulose, ethyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, (hydroxyethyl) methyl cellulose and (hydroxypropyl) methyl cellulose.
3. The use according to claim 1 or 2, characterized in that The cellulose ether has a weight average molecular weight of ≤ 300,000 g / mol.
4. The use according to claim 1 or 2, characterized in that: The surface sizing composition is applied on the surface of the fiber web in a surface sizing station or in a coating station.
5. The use according to claim 1, characterized in that: The surface sizing composition is applied on the surface of the fiber web in at least two consecutive applications.
6. The use according to claim 1 or 2, characterized in that: The aqueous surface sizing composition also comprises starch.
7. The use according to claim 1 or 2, characterized in that: The compressive strength is a short span compressive test strength measured at a temperature ≥ 30°C and a relative humidity ≥ 80%.
8. The use according to claim 1 or 2, characterized in that: The fiber web is a layer in a multi-layer paperboard selected from linerboard.
9. The use according to claim 8, characterized in that The fiber web is kraft paperboard.
10. The use according to claim 1, characterized in that The fibrous web is corrugated paper.
11. The use according to claim 1, characterized in that The viscosity of the surface sizing composition is less than 2000 mPa·s.
12. The use according to claim 1, characterized in that The fiber web has a thickness of at least 20 g / m 2 The basis weight.
Citation Information
Patent Citations
Corrugated paper box production method
CN108263024A