A method for eliminating short shavings in stamping and blanking
By molding the scrap cutting edge on the top of the blade on the scrap disengagement side during the punching process, the problem of short strips in the punching is solved, and the production of no indentation on the surface of the stamping part is achieved, which improves the Production efficiency and batch pass rate.
Patent Information
- Application Number
- CN202210660461.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-06-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-06-13
AI Technical Summary
In stamping production, short strips of hair produced during the stamping process cause accumulation of A-side of the mold, causing indentation defects on the surface of the stamping part and production shutdown. The prior art cannot fundamentally suppress the mechanism of hair generation and affecting production efficiency.
By molding the scrap cutting edge top surface on the scrap side, increasing the strong deformation shape of the plate, adjusting the shape and angle of the edge to avoid short strips of hairs due to secondary shearing, ensuring that no secondary shearing occurs during the punching process short strips of slag.
It effectively eliminates the short strips of hair produced by secondary shear during the cutting waste, avoids the accumulation of short strips of hair and indentation defects, ensures the pass rate and production continuity of stamping parts, and improves the opening rate of the whole line.
Smart Images

Figure CN115213285B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of vehicle engineering, in particular to a method for eliminating short strips of hair in stamping and blanking. Background Art
[0002] With the continuous development of the automobile industry, the degree of production automation of domestic automobile enterprises is getting higher and higher, and the degree of automation of stamping production is changing with each passing day. At present, a high-speed automated stamping equipment group of 16 times / min has been used for stamping production. The high efficiency of automated production is reflected in the effective stroke, and the effective stroke is guaranteed by the opening rate of the whole line. In stamping production, blanking is a process that stamping parts must go through. In this process, due to the influence of the mold structure accuracy or the accuracy of the stamping equipment during high-speed production, various blanking shavings often appear. These shavings appear at irregular times, shapes, and sizes during the production process, and accumulate or transfer to the A surface of the mold with the high-speed production mold edge, and finally form irregular indentation defects in irregular positions on the blanking parts. In order to ensure the qualified rate of stamping parts in batches, when stamping parts with indentation defects are found, the whole line must be stopped and the mold must be cleaned before continuing to produce stamping parts without indentation defects. If the indentation defects of stamping parts occur frequently, it is bound to cause too many shutdowns of batch production, affecting the opening rate of the whole line of production batches.
[0003] The existing technology to solve the problem of stamping and blanking shavings is limited to the sharpness trimming of the blanking edge, blanking gap adjustment, edge contour adjustment, edge penetration depth adjustment, etc. These process directions are based on the blanking edge, and have high requirements on the equipment accuracy of the blanking die and the material of the blanking edge. Although most of the shavings can be optimized, the generation of shavings cannot be completely suppressed from the mechanism of shaving generation. Therefore, there has been no effective solution to the problem of stamping and blanking shavings, especially the short shavings that appear in the secondary shearing during the cutting of blanking waste.
[0004] CN112317595A discloses a stamping trimming process for preventing waste chips from being generated, comprising: after the process before the trimming process is completed, a process notch is punched out on the workpiece, and the process notch is set at the contact point position of the trimming blade and the waste knife during the trimming process; trimming and waste shearing are performed. The radius of the process notch is R, R=0.5mm. The present invention solves the problem of waste chips generated by secondary shearing caused by sheet tearing caused by the waste knife during the trimming process by setting a process notch on the workpiece after the process before the trimming process is completed, and the process notch is located at the contact position of the trimming blade and the waste knife during the trimming process, thereby reducing the generation of waste chips. Summary of the invention
[0005] In order to solve the above-mentioned problems existing in the prior art, the present invention provides a method for eliminating short strips of hair in stamping and blanking, which effectively eliminates the phenomenon of short strips of hair caused by secondary shearing during the cutting of waste materials in stamping and blanking, thereby eliminating the problem of surface indentation of stamping parts caused by the accumulation and transfer of short strips of hair to the A surface of the mold, and ultimately eliminates production shutdowns caused by surface indentations of stamping parts caused by short strips of hair, thereby ensuring the effective stroke of stamping production.
[0006] The objective of the present invention is achieved through the following technical solutions:
[0007] A method for eliminating short shavings in stamping and blanking, characterized in that it comprises the following steps:
[0008] Step 1: Stabilize the punching state and determine the state of the shavings: After the punching is completed, the shavings generated during the cutting process of the punching waste are short shavings generated by the secondary shearing. Under the premise that the process part shape and the working state of the punching edge are reasonable, if the number of short shavings reaches the preset value and the accumulation is transferred to the A surface of the mold, proceed to step 2;
[0009] Step 2: Select a reasonable position within the top surface of the waste cutting edge of the upper die on the waste separation side to increase the strong deformation shape of the plate;
[0010] Step 3: Perform batch production verification on the high-speed automated production line to determine the status of short lint elimination.
[0011] Furthermore, the step 1 comprises:
[0012] S1. Determine the state of the dandruff:
[0013] S11. Determine whether the conformity between the process part and the blanking die surface before blanking is reasonable;
[0014] S12. Determine whether the working state of the punching edge is reasonable and stable;
[0015] S13. Determine whether the state of the punching shavings belongs to the type of short shavings produced by secondary shearing;
[0016] S2. If the dandruff state satisfies the above three conditions at the same time, the number of short dandruff generated is confirmed according to the area where the short dandruff is generated.
[0017] Furthermore, the step S2 comprises:
[0018] S21. If the number of short shavings is 5-10, optimize the working state of the cutting edge;
[0019] S22. If the number of short shavings is more than 10 and the shavings are accumulated and transferred to the mold surface A, proceed to step 2.
[0020] Furthermore, the step 2 comprises:
[0021] S3. Determine the top surface angle of the waste cutting edge of the upper die on the waste separation side;
[0022] S4. Determine the width of the top surface of the waste cutting edge of the upper die on the waste separation side;
[0023] S5. Determine the waste cutting edge of the upper die on the side where the waste is separated from the sheet material with strong deformation shape;
[0024] S6. Determine the width of the strong deformation modeling distance of the plate from the edge contour of the part;
[0025] S7. Determine the width of the edge profile of the waste cutting edge to increase the distance between the plate and the strong deformation model;
[0026] S8. Determine to increase the length of the strong deformation modeling of the plate;
[0027] S9. Determine to increase the width of the strong deformation modeling of the plate;
[0028] S10. Determine to increase the height of the strong deformation modeling of the plate;
[0029] S11. Determine the radius of the ball corners at both ends of the plate's strong deformation shape.
[0030] Preferably, in the step 2:
[0031] S8. Determine that the length of the plate strong deformation molding is increased to 80-100mm;
[0032] S9. Determine that the width of the plate strong deformation molding is increased to 5-7mm;
[0033] S10. Determine to increase the height of the plate strong deformation modeling by 3-5mm;
[0034] S11. Determine that the radius R of the ball corners at both ends of the plate strong deformation shape is increased to 5mm.
[0035] Furthermore, the step 2 further includes:
[0036] S12. After the waste is separated from the upper die, the top surface of the waste cutting edge is increased to form a strong deformation shape of the plate, and the interference test is carried out using the pre-punching process parts:
[0037] If the shape and waste do not interfere when the convex and concave edges come into contact, increase the height of the strong deformation shape of the plate;
[0038] If the interference between the shape and the scrap surface reaches 1-2mm when the convex and concave edges come into contact, proceed to step three.
[0039] Furthermore, the step three comprises:
[0040] S13. The highest production frequency of the whole line is used to verify the elimination of short-cut hair;
[0041] S14. The highest production frequency of the whole line is verified, and no other types of punching shavings appear;
[0042] S15. The highest production frequency of the entire line verifies that the blanking section of the blanked parts is reasonable and free of burrs.
[0043] Furthermore, in step S15, the highest production frequency of the entire line is used to verify that the blanking section of the blanking part is reasonable and burr-free:
[0044] S151. If there is no burr, the work is completed;
[0045] S152. If other types of shavings appear, the height of the strong deformation of the plate is corrected;
[0046] S153. If burrs appear on the punching section, correct the width of the sheet material's strong deformation molding.
[0047] Preferably, in step S152:
[0048] If irregular blocky shavings appear, reduce the height of the strong deformation modeling of the plate;
[0049] If flaky chips appear, increase the width of the strong deformation molding of the plate.
[0050] Preferably, in step S153:
[0051] If hard burrs appear, reduce the width of the strong deformation molding of the plate;
[0052] If soft burrs appear, increase the width of the strong deformation molding of the plate.
[0053] The present invention has the following beneficial effects:
[0054] In order to solve the problem of short strips of hair generated in the process of cutting off stamping and blanking waste, the present invention provides a method for eliminating short strips of hair in stamping and blanking, fundamentally eliminating the secondary shearing process in the waste cutting process, thereby eliminating the short strips of hair phenomenon caused by secondary shearing in the cutting of stamping and blanking waste, and effectively eliminating the problem of surface indentation of stamping parts caused by the accumulation and transfer of short strips of hair to the A surface of the mold, and finally eliminating the production shutdown caused by surface indentation of stamping parts caused by short strips of hair, thereby ensuring the effective stroke of stamping production.
[0055] When solving the problem of punching and blanking shavings, the present invention fully considers the mechanism of punching and blanking shavings generation, especially the short strips of shavings generated by secondary shearing during the cutting of the waste material, and starts from the idea of eliminating secondary shearing, completely eliminates the secondary shearing process of punching, and ensures that no short strips of shavings generated by secondary shearing are generated during the primary punching process, which is a process method for completely suppressing the secondary shearing of punching. Compared with the existing method of solving the problem of punching and blanking shavings by starting from the size and shape of the punching edge, the present invention solves the problem of punching and blanking shavings more directly and thoroughly, and fundamentally eliminates the short strips of shavings generated by secondary shearing during the cutting of the waste material. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show typical embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0057] Figure 1 Schematic diagram of the secondary shear formation mechanism of the blanking waste cut off;
[0058] Figure 2 This is a schematic diagram of the short strips of shavings that appear when the waste is cut off by punching;
[0059] Figure 3 A schematic diagram of adding strong deformation of the plate to the top surface of the waste cutting edge of the upper die on the waste separation side in an embodiment of the present invention;
[0060] Figure 4 A schematic diagram of the working principle of adding strong deformation molding of the plate to the top surface of the waste cutting edge of the upper die on the waste separation side of the present invention;
[0061] In the figure:
[0062] 1-Strong deformation of the plate;
[0063] A-Waste detachment side puncture drift point;
[0064] C-waste support side puncture drift point;
[0065] D- A symbol-shaped deformed convex point after the scrap support side is punctured;
[0066] E-waste is separated from the sharp corner of the side cutting edge;
[0067] F- sharp angle of the cutting edge on the waste support side;
[0068] G-short hair;
[0069] L1-short hair length;
[0070] B3-short strip width;
[0071] K- waste cutting edge of upper die on the waste separation side;
[0072] B-strong deformation width of the plate;
[0073] L-the length of the strong deformation shape of the plate;
[0074] H-plate has high deformation and high shape;
[0075] B1-the width of the strong deformation shape of the plate from the edge contour of the part;
[0076] B2-the width of the strong deformation shape of the plate from the waste cutting edge contour;
[0077] R-the radius of the ball corners at both ends of the strong deformation shape of the plate;
[0078] A1- The waste separation side upper die waste cutting edge top surface profile increases the waste separation side puncture drift point after the plate is strongly deformed;
[0079] C1- The waste separation side upper die waste cutting edge top surface profile increases the waste support side puncture drift point after the plate is strongly deformed;
[0080] D1- The top surface of the punching die edge increases the deformation convex point after the waste material is pierced and extends after the strong deformation of the plate. DETAILED DESCRIPTION
[0081] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention.
[0082] Example
[0083] A method for eliminating short shavings in stamping and blanking, the specific steps are as follows:
[0084] Step 1: Stabilize the punching state and determine the state of the shavings: After the punching is completed, the shavings generated in the process of cutting the punching waste are short shavings generated by secondary shearing. Under the premise that the process part shape and the working state of the punching edge are reasonable, the number of short shavings generated is confirmed according to the area where the short shavings are generated. If the number of short shavings reaches the preset value and is accumulated and transferred to the A surface of the mold, proceed to step 2;
[0085] S1. Determine the state of the dandruff:
[0086] S11. Determine whether the conformity between the process part and the blanking die surface before blanking is reasonable;
[0087] S12. Determine whether the working state of the punching edge is reasonable and stable;
[0088] S13. Determine whether the state of the punching shavings belongs to the type of short shavings produced by secondary shearing;
[0089] S2. If the dandruff state meets the above three conditions at the same time, the number of short dandruff generated is confirmed according to the area where the short dandruff is generated:
[0090] S21. If the number of short shavings is 5-10, the working state of the cutting edge needs to be optimized;
[0091] S22. If the number of short shavings is more than 10 and the accumulation is transferred to the mold surface A, proceed to step 2;
[0092] Step 2: Select a reasonable position on the top surface of the waste cutting edge of the upper die to increase the strong deformation of the plate:
[0093] S3. Determine the top surface angle of the waste cutting edge of the upper die on the waste separation side;
[0094] S4. Determine the width of the top surface of the waste cutting edge of the upper die on the waste separation side;
[0095] S5. Determine the waste cutting edge of the upper die on the side where the waste is separated from the sheet material with strong deformation shape;
[0096] S6. Determine the width of the strong deformation modeling distance of the plate from the edge contour of the part;
[0097] S7. Determine the width of the edge profile of the waste cutting edge to increase the distance between the plate and the strong deformation model;
[0098] S8. Determine that the length of the plate strong deformation molding is increased to 80-100mm;
[0099] S9. Determine that the width of the plate strong deformation molding is increased to 5-7mm;
[0100] S10. Determine to increase the height of the plate strong deformation modeling by 3-5mm;
[0101] S11. Determine to increase the radius of the ball corners at both ends of the plate strong deformation shape R5mm;
[0102] S12. After the waste is separated from the upper die, the top surface of the waste cutting edge is increased to form a strong deformation of the plate, and the interference test is carried out using the pre-punching process parts:
[0103] If the shape does not interfere with the waste material when the convex and concave edges come into contact, the height of the strong deformation shape of the plate needs to be appropriately increased;
[0104] If the interference between the shape and the scrap surface reaches 1-2mm when the convex and concave edges come into contact, proceed to step 3;
[0105] Step 3: The high-speed automated production line conducts batch production verification to determine the elimination status of short slivers and ensure the production line opening rate:
[0106] S13. The highest production frequency of the whole line is used to verify the elimination of short-cut hair;
[0107] S14. The highest production frequency of the whole line is verified, and no other types of punching shavings appear;
[0108] S15. The highest production frequency of the whole line verifies that the blanking section of the blanking parts is reasonable and burr-free;
[0109] S151.Yes, the work is completed;
[0110] S152. No, if other types of shavings appear, correct the height of the plate's strong deformation modeling; if irregular block shavings appear, reduce the height of the plate's strong deformation modeling; if thin shavings appear, increase the width of the plate's strong deformation modeling;
[0111] S153. No, if burrs appear on the punching section, correct the width of the strong deformation of the plate; if hard burrs appear, reduce the width of the strong deformation of the plate; if soft burrs appear, increase the width of the strong deformation of the plate.
[0112] The following is a comparison between the working principles of the prior art and the embodiments of the present invention:
[0113] like Figure 1 , Figure 2As shown, the top surface profile of the waste cutting edge K of the upper die on the waste detachment side of the prior art does not increase the strong deformation shape 1 of the plate. In stamping and blanking, during the waste cutting process, due to the design of the waste cutting edge, the upper die waste cutting edge has a cutting edge on the waste detachment side and a cutting edge on the waste support side. The sharp corner area of the upper die cutting edge on the waste detachment side belongs to suspended blanking when working. During blanking, the sharp corner of the sharp corner E of the cutting edge on the waste detachment side is punctured first. When the sharp corner blanking edge contacts the waste surface, due to the lack of support from the lower support edge, the hydrostatic pressure during blanking will increase, and the waste surface contacted by the sharp corner will undergo a process of elongation and deformation. Then the hydrostatic pressure reaches enough to tear the surface of the waste material, and a tear-off cut appears on the surface of the waste material. As the sharp corner of the punching blade continues to penetrate, the tear-off cut on the surface of the waste material continues to grow. In the process of the tear-off cut growing, the waste material on the waste detachment side is pulled by the punching blade on the waste detachment side, and the waste section on the waste detachment side drifts to the waste detachment side, forming the waste detachment side puncture drift point A. As the part contour is punched, the sharp corner F of the waste support side blade works. After the part contour is punched, the waste support side puncture point drifts, forming the waste support side puncture drift point C. The waste material on the waste support side resists the tearing of the waste due to the support of the lower die waste cutting blade, causing the waste section on the waste support side to drift to the waste detachment side, forming the shape deformation convex point D after the waste support side is punctured. After the waste puncture and tearing process is completed, the waste section that drifted from the waste support side to the waste separation side before the waste cutting edge starts normal punching has passed the waste cutting edge of the lower die. During the punching, the waste section on the waste support side that passed the waste cutting edge of the lower die was punched on one side, and secondary shearing occurred on the waste section on the waste support side. After punching to the bottom, the burrs of the single-sided punching remain in the lower part of the waste section and exist in the punching gap surface, which forms a short strip of shavings G that has been sheared twice, with a short strip of shavings length L1 and a short strip of shavings width B3. As the punching edge detaches, due to the influence of the length increase of the waste material after being cut off, the friction force is relatively large when the gap surface of the upper die waste cutting edge detaches from the waste section, and the burr of single-sided punching, that is, the short strips of hair chips of secondary shearing, adheres to the punching gap surface of the upper die waste cutting edge. Finally, as the upper die waste cutting edge detaches from the lower die edge, as the number of punching times increases, the burr of single-sided punching, that is, the short strips of hair chips of secondary shearing, continues to accumulate into a ball. When it reaches a certain weight, it will fall off from the punching gap surface of the upper die waste cutting edge due to gravity. The falling point is facing the contour area of the lower die punching punch. When it falls, it is very likely to fall on the A surface of the lower die punching convex model, and finally form irregular indentation defects in uncertain positions on the punched parts, which cannot guarantee the qualified rate of stamping parts batches. In addition, stamping parts indentation defects occur frequently, resulting in too many shutdowns of batch production, affecting the opening rate of the entire line of production batches.
[0114] like Figure 3 , Figure 4As shown, the embodiment of the present invention prevents the surface of the waste from being damaged by adding a strong deformation shape 1 of the plate, a width B of the strong deformation shape, a length L of the strong deformation shape, a height H of the strong deformation shape, a width B1 of the strong deformation shape of the plate from the contour of the part edge, a width B2 of the strong deformation shape of the plate from the contour of the waste cutting edge, and a spherical corner radius R at both ends of the strong deformation shape of the plate to the top surface of the waste cutting edge K of the upper die on the waste detachment side. During stamping and blanking, before the sharp corner of the waste cutting edge of the upper die on the waste detachment side pierces, the strong deformation shape of the plate added to the top surface of the waste cutting edge of the upper die on the waste detachment side first contacts the surface of the waste and performs necessary deformation on the waste. This deformation greatly reduces the original suspended blanking distance, and the hydrostatic pressure when the sharp corner blanking edge contacts the waste surface will not be too large, and the waste surface contacted by the sharp corner will not be excessively elongated and deformed. When the hydrostatic pressure reaches enough to tear the scrap surface, the scrap detachment side upper die scrap cutting edge top profile increases the scrap detachment side puncture drift point A1 after the sheet is strongly deformed, and the puncture process ends. As the part contour is blanked, the scrap detachment side upper die scrap cutting edge top profile increases the scrap support side puncture drift point C1 after the sheet is strongly deformed. At the beginning of normal blanking, the scrap surface just appears torn off, and immediately enters the normal blanking stage. The waste material is cut off to form the top surface of the punching die cutting edge. After the sheet is strongly deformed and shaped, the waste material is punctured and the deformation convex point D1 is extended. There is no phenomenon that the waste section on the waste support side drifts to the waste detachment side. The waste section on the waste support side no longer crosses the waste cutting edge of the lower die. There is no single-sided punching during punching. There is no secondary shearing on the waste section on the waste support side. After punching to the bottom, there is no single-sided punching burr remaining in the lower part of the waste section and existing in the punching gap surface. This fundamentally eliminates the short strips of hair scraps from secondary shearing. At the same time, there is no short strip of hair scraps falling off from the punching gap surface of the upper die waste cutting edge during production, and no short strip of hair scraps falling on the A surface of the lower die punching convex model. There are no irregular and irregular indentation defects on the punched parts, which completely guarantees the qualified rate of stamping parts batches, completely eliminates the problem of excessive downtime in batch production, and effectively guarantees the opening rate of the entire production batch.
[0115] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for eliminating short shavings in stamping and blanking. It is characterized in that The following steps are involved: Step 1: Stabilize the punching state and determine the state of the shavings: After the punching is completed, the shavings generated during the cutting process of the punching waste are short shavings generated by the secondary shearing. Under the premise that the process part shape and the working state of the punching edge are reasonable, if the number of short shavings reaches the preset value and the accumulation is transferred to the A surface of the mold, proceed to step 2; Step 2: Select a reasonable position within the top surface of the waste cutting edge of the upper die on the waste separation side to increase the strong deformation shape of the plate; the step 2 includes: S3. Determine the top surface angle of the waste cutting edge of the upper die on the waste separation side; S4. Determine the width of the top surface of the waste cutting edge of the upper die on the waste separation side; S5. Determine the waste cutting edge of the upper die on the side where the waste is separated from the sheet material with strong deformation shape; S6. Determine the width of the strong deformation modeling distance of the plate from the edge contour of the part; S7. Determine the width of the edge profile of the waste cutting edge to increase the distance between the plate and the strong deformation model; S8. Determine to increase the length of the strong deformation modeling of the plate; S9. Determine to increase the width of the strong deformation modeling of the plate; S10. Determine to increase the height of the strong deformation modeling of the plate; S11. Determine the radius of the ball corners at both ends of the plate strong deformation modeling; S12. After the waste is separated from the upper die, the top surface of the waste cutting edge is increased to form a strong deformation shape of the plate, and the interference test is carried out using the pre-punching process parts: If the shape and waste do not interfere when the convex and concave edges come into contact, increase the height of the strong deformation shape of the plate; If the interference between the shape and the scrap surface reaches 1-2mm when the convex and concave edges come into contact, proceed to step 3; Step 3: Perform batch production verification on the high-speed automated production line to determine the status of short lint elimination.
2. A method for eliminating short shavings in stamping and blanking as claimed in claim 1, It is characterized in that The step one comprises: S1. Determine the status of the dandruff: S11. Determine whether the conformity between the process part and the blanking die surface before blanking is reasonable; S12. Determine whether the working state of the punching edge is reasonable and stable; S13. Determine whether the state of the punching shavings belongs to the type of short shavings produced by secondary shearing; S2. If the dandruff state satisfies the above three conditions at the same time, the number of short dandruff generated is confirmed according to the area where the short dandruff is generated.
3. A method for eliminating short hair scraps in stamping and blanking as claimed in claim 2, It is characterized in that The step S2 comprises: S21. If the number of short shavings is 5-10, optimize the working state of the cutting edge; S22. If the number of short shavings is more than 10 and the shavings are accumulated and transferred to the mold surface A, proceed to step 2.
4. A method for eliminating short hair scraps in stamping and blanking as claimed in claim 1, It is characterized in that In the step 2: S8. Determine that the length of the plate strong deformation molding is increased to 80-100mm; S9. Determine that the width of the plate strong deformation molding is increased to 5-7mm; S10. Determine to increase the height of the plate strong deformation modeling by 3-5mm; S11. Determine that the radius R of the ball corners at both ends of the plate strong deformation shape is increased to 5mm.
5. A method for eliminating short shavings in stamping and blanking as claimed in claim 1, It is characterized in that The step three comprises: S13. The highest production frequency of the whole line is used to verify the elimination of short-cut hair; S14. The highest production frequency of the whole line is verified, and no other types of punching shavings appear; S15. The highest production frequency of the entire line verifies that the blanking section of the blanked parts is reasonable and free of burrs.
6. A method for eliminating short shavings in stamping and blanking as claimed in claim 5, It is characterized in that In step S15, the highest production frequency of the entire line verifies that the blanking section of the blanking part is reasonable and burr-free: S151. If there is no burr, the work is completed; S152. If other types of shavings appear, the height of the strong deformation of the plate is corrected; S153. If burrs appear on the punching section, correct the width of the sheet material's strong deformation molding.
7. A method for eliminating short hair chips in stamping and blanking as claimed in claim 6, It is characterized in that In step S152: If irregular blocky shavings appear, reduce the height of the strong deformation modeling of the plate; If flaky chips appear, increase the width of the strong deformation molding of the plate.
8. A method for eliminating short hair chips in stamping and blanking as claimed in claim 6, It is characterized in that In step S153: If hard burrs appear, reduce the width of the strong deformation molding of the plate; If soft burrs appear, increase the width of the strong deformation molding of the plate.