A method for preparing small peptide chelated copper using waste printed circuit boards

By using waste printed circuit boards to prepare small peptide chelated copper through ultrasonic cleaning, crushing and hydrogen peroxide catalysis, combined with absolute ethanol replacement crystallization technology, the problems of complex production processes and low raw material utilization in the existing technology are solved. The preparation of high-purity small peptide chelated copper is achieved, which reduces environmental pollution and equipment costs and is suitable for industrial applications.

CN115215920BActive Publication Date: 2024-10-01CHONGQING TECH & BUSINESS UNIV
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
CN202210906491.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-29
Publication Date
2024-10-01
Estimated Expiration
2042-07-29

AI Technical Summary

Technical Problem

The existing method for preparing small peptide chelated copper has a complicated production process, low raw material utilization, low product purity and quality, and has environmental pollution problems.

Method used

Using waste printed circuit boards as raw materials, small peptide chelated copper is formed through ultrasonic cleaning, crushing, hydrogen peroxide catalysis and ultrasonic mechanical stirring. It is combined with absolute ethanol displacement crystallization technology to achieve the preparation of high-purity products.

Benefits of technology

It has achieved simplification of the process flow, increased product purity and copper content, reduced equipment costs and environmental pollution, is suitable for industrial production, and provides a high value-added resource reuse solution.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The purpose of the present invention is to provide a method for preparing small peptide chelated copper using waste printed circuit boards in view of the shortcomings of the existing preparation of small peptide chelated copper, and the method has the characteristics of simple process flow, safe operation, no waste liquid generation, easy industrial amplification, high raw material utilization rate, etc. The present invention uses commercially available waste printed circuit boards as raw materials, and realizes the preparation of small peptide chelated copper using waste printed circuit boards through the steps of preparing waste printed circuit board powder, preparing small peptide chelated copper crude liquid, and preparing small peptide chelated copper products. The method provided by the present invention not only effectively realizes the reuse of metal copper resources, but also the by-products can be used for the production of new materials, which has practical guiding significance for the innovative comprehensive utilization of waste printed circuit boards. The products prepared by the method of the present invention can be widely used in agriculture, forestry, animal husbandry and other industries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biochemical engineering, and particularly relates to a method for preparing small peptide chelated copper by utilizing waste printed circuit boards. Background Art

[0002] With the development of the digital age, electronic products are becoming more and more popular, and their updates and iterations are getting faster and faster. But at the same time, it has also led to serious electronic waste pollution. In 2019, the total amount of electronic waste generated worldwide reached a record 53.6 million metric tons. As one of the most important components of electronic equipment, the number of printed circuit boards has also increased with the increase in the amount of electronic waste. Waste printed circuit boards contain a large amount of metal resources, of which copper accounts for more than 90% of metal materials. If waste printed circuit boards are effectively treated and utilized as resources, it will not only reduce environmental pollution, but also generate higher economic value.

[0003] Trace element copper is one of the essential nutrients in the growth of animals and plants. In animals, it is a component or activator of enzymes, participates in the metabolic process of various substances in the body, and affects the body's immune and antioxidant properties; in plants, it is a component of multiple enzymes, can stabilize pigments, promote photosynthesis, participate in the lignification of cell walls, and affect the formation of pollen and crop carbon and nitrogen metabolism. Trace element copper was originally supplied to animals and plants as an additive in the form of inorganic salts. With the development of the industry, animal and plant copper additives are mainly in the form of chelates at this stage. Among them, small peptide chelated copper, as a new generation of efficient green trace element nutrients, is widely used in water-soluble fertilizers, foliar fertilizers, plant nutrition regulators, chelated compound fertilizers, feeds and fungicides. Small peptide chelated copper has the characteristics of stability, high efficiency, and low toxicity. It is easy to digest and absorb in the intestine, which is beneficial to animal growth, can prevent and treat trace element deficiency, improve animal immunity, and is beneficial to the full utilization of nutritional components in feed. It also acts as an amino acid enhancer. In addition, small peptide chelated copper can slowly release metal ion copper and polypeptide organic active substances in crops, which not only improves the absorption and utilization rate, but also can quickly kill bacteria while supplementing nutrition.

[0004] There are existing methods for preparing small peptide chelated copper, such as the invention patent with the announcement number CN106035983B "A method for preparing nanopeptide chelated copper as a feed additive" authorized on August 20, 2019. The method disclosed in the patent is: using soybean meal powder and copper sulfate as raw materials, through the preparation of buffer solution, preparation of dry peptide powder, preparation of small peptide solution, preparation of copper solution, preparation of nanopeptide chelated copper solution and other steps, and then separation and drying to obtain nanopeptide chelated copper. The disadvantages of this method are: ① The production process is complicated, the technical requirements are high, the production capacity is limited, and it is not convenient for industrial production; ② The comprehensive utilization rate of raw materials is low, resulting in the waste of some raw materials such as soybean meal powder and anhydrous copper sulfate; ③ The obtained product is a mixture of multiple small peptide chelated copper, the product purity and quality are low, and the economic value is low; ④ Strong alkali is used in the production process, which has high requirements for equipment and certain environmental pollution. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing small peptide chelated copper using waste printed circuit boards in view of the shortcomings of the existing preparation of small peptide chelated copper. The method has the characteristics of simple process flow, safe operation, no waste liquid generation, easy industrial scale-up, high raw material utilization rate, etc. The small peptide chelated copper prepared by the method has the characteristics of high product purity, high copper content, low dosage, easy absorption, broad market prospects, etc.

[0006] The mechanism of the present invention is: small peptide is a small molecule active peptide composed of 2 to 3 amino acids and with a molecular weight of less than 1000Da. The free carboxyl, thiol and amino groups in its structure can enhance the affinity of small peptides for copper ions and improve the firmness of small peptides and copper ions. Therefore, small peptides can form stable chelates with copper ions in a certain proportion. Among the metal materials of waste printed circuit boards, copper accounts for more than 90%. Under the action of hydrogen peroxide, the copper element in the waste printed circuit board powder can be oxidized into copper ions, and under the enhanced mass transfer effect of ultrasonic coupled mechanical stirring, it can quickly form small peptide chelated copper with small peptides. In addition, the separation and purification of small peptide chelated copper can be further achieved through anhydrous ethanol replacement crystallization technology to obtain a high-purity product.

[0007] The object of the present invention is achieved by: a method for preparing small peptide chelated copper using waste printed circuit boards, using commercially available waste printed circuit boards as raw materials, preparing waste printed circuit board powder, preparing small peptide chelated copper crude liquid, preparing small peptide chelated copper products, etc. to achieve the preparation of small peptide chelated copper using waste printed circuit boards. The specific method steps are as follows:

[0008] (1) Preparation of waste printed circuit board powder

[0009] Using commercially available waste printed circuit boards as raw materials, the waste printed circuit boards are placed in an ultrasonic cleaning machine at a ratio of 1:50 to 200 of the mass (g) of the waste printed circuit boards to the volume (mL) of distilled water, and cleaned for 30 to 60 minutes at room temperature and an ultrasonic output power of 60 to 90 W. After the ultrasonic cleaning is completed, the cleaned waste printed circuit boards are dried at a temperature of 60°C for 20 to 50 minutes, and then disassembled into small pieces of 3 to 6 cm, and then placed in a high-speed pulverizer for crushing, and the powder obtained by screening with a 40-mesh filter sieve is collected, which is the waste printed circuit board powder for the next step of treatment.

[0010] (2) Preparation of crude peptide chelated copper solution

[0011] After step (1) is completed, the waste printed circuit board powder is placed in a hydrogen peroxide solution according to a ratio of 1:25-125 of the mass (g) of the waste printed circuit board powder prepared in step (1) to the volume (mL) of a hydrogen peroxide solution with a volume fraction of 2.5-10%, to obtain a waste printed circuit board powder reaction liquid. Then, according to a ratio of 1:25-125 of the mass (g) of the waste printed circuit board powder to the volume (mL) of a small peptide solution with a concentration of 0.1-0.5M, the small peptide solution is added to the waste printed circuit board powder reaction liquid, and then the mixed solution is placed in an ultrasonic reactor equipped with a mechanical stirrer, and a chelating reaction is carried out for 0.5-3 hours under the conditions of a temperature of 30-60°C, an ultrasonic output power of 60-120W, and a stirring speed of 100-300r / min. After the reaction is completed, the reaction mixture is centrifuged for 5 to 10 minutes at a speed of 10,000 to 15,000 r / min and a temperature of 20 to 30°C, and the centrifugal clear liquid and centrifugal sediment are collected respectively. The collected centrifugal sediment mainly contains resin, glass fiber, etc., which can be used as filling materials, unburned cement bricks and colored brick materials, automotive brake pad additives, etc.; the collected centrifugal clear liquid is a small peptide chelated copper crude liquid, and the copper leaching rate is 91.5 to 95.5%, which is used for the next step of treatment. Among them, the small peptide is glutathione, glycylglycine, glycyl-L-glutamine, and is not limited to the listed small peptides.

[0012] (3) Preparation of small peptide chelated copper products

[0013] After step (2) is completed, the crude peptide chelated copper solution prepared in step (2) is placed in a vacuum distillation device, and vacuum concentrated under the conditions of a vacuum degree of 0.09-0.095 MPa and a temperature of 60-80°C, and concentrated to 0.1-0.3 times the original volume, thereby obtaining a peptide chelated copper concentrate. Then, according to the volume ratio of the peptide chelated copper concentrate to anhydrous ethanol of 1:1, anhydrous ethanol is added to the peptide chelated copper concentrate, and stirred at a temperature of 50-70°C for 20-40 minutes, and then the peptide chelated copper concentrate containing anhydrous ethanol is allowed to stand at a low temperature of 4-8°C for 12-24 hours, and finally the mixed solution after standing at a low temperature is centrifuged at a speed of 10000-15000 r / min and a temperature of 10-20°C for 5-10 minutes, and the upper light liquid and the lower crystal are collected respectively. The collected upper light liquid is subjected to vacuum distillation treatment, and the ethanol can be further used in step (3). The liquid after ethanol recovery can be used for the preparation of the small peptide solution in step (2). The collected lower crystals are dried at a temperature of 50 to 70°C for 12 to 24 hours to obtain a small peptide chelated copper product with a purity of 91.2 to 94.5%.

[0014] After the present invention adopts the above technical solution, it mainly has the following effects:

[0015] 1. The method of the present invention has the characteristics of simple process flow, safe operation, no waste liquid generation, easy industrial scale-up, high raw material utilization rate, and low equipment and operation costs.

[0016] 2. The present invention mainly uses small peptides, hydrogen peroxide, etc. in the production process, the reaction conditions are mild, the process is safe and controllable, and can be further promoted and applied to the production of other chelates.

[0017] 3. The present invention adopts ultrasonic mechanical stirring coupling technology in the production process, which can effectively control the reaction conditions, enhance mass transfer, thereby improving production efficiency and further reducing production operation costs.

[0018] 4. The small peptide chelated copper product produced by the method of the present invention has high purity and a copper content (>30%) higher than that of EDTA copper. The usage amount can be reduced by 56% compared with EDTA copper. It also has a low molecular weight and is easy to absorb, making it an ideal substitute for EDTA copper.

[0019] 5. The method of the present invention uses waste printed circuit boards as raw materials to produce high value-added products such as peptide chelated copper, which not only effectively realizes the recycling of metal copper resources, but also the by-products can be used for the production of new materials, which has practical guiding significance for the innovative and comprehensive utilization of waste printed circuit boards.

[0020] The products prepared by the method of the present invention can be widely used in agriculture, forestry, animal husbandry and other industries. DETAILED DESCRIPTION

[0021] The present invention is further described below in conjunction with specific implementation modes.

[0022] Example 1

[0023] A method for preparing small peptide chelated copper using waste printed circuit boards, the specific method steps are as follows:

[0024] (1) Preparation of waste printed circuit board powder

[0025] Using commercially available waste printed circuit boards as raw materials, the waste printed circuit boards were placed in an ultrasonic cleaning machine at a ratio of 1:50, with the mass (g) of the waste printed circuit boards and the volume (mL) of distilled water, and cleaned for 60 minutes at room temperature and an ultrasonic output power of 60 W. After the ultrasonic cleaning was completed, the cleaned waste printed circuit boards were dried at a temperature of 60°C for 20 minutes, then disassembled into 3 cm small pieces, and then placed in a high-speed pulverizer for crushing, and the powder obtained by screening with a 40-mesh filter sieve was collected, which was the waste printed circuit board powder for the next step of treatment.

[0026] (2) Preparation of crude peptide chelated copper solution

[0027] After the completion of step (1), the waste printed circuit board powder is placed in a hydrogen peroxide solution at a ratio of 1:25 of the mass (g) of the waste printed circuit board powder prepared in step (1) to the volume (mL) of a hydrogen peroxide solution with a volume fraction of 2.5%, to obtain a waste printed circuit board powder reaction solution. Then, the small peptide solution is added to the waste printed circuit board powder reaction solution at a ratio of 1:25 of the mass (g) of the waste printed circuit board powder to the volume (mL) of a small peptide solution with a concentration of 0.5M, and then the mixed solution is placed in an ultrasonic reactor equipped with a mechanical stirrer, and the chelation reaction is carried out for 0.5h at a temperature of 30°C, an ultrasonic output power of 60W, and a stirring speed of 100r / min. After the reaction is completed, the mixed solution after the reaction is centrifuged at a speed of 10000r / min and a temperature of 20°C for 5min, and the centrifugal clear liquid and centrifugal sediment are collected respectively. The collected centrifugal sediment mainly contains resin, glass fiber, etc., which can be used as filling materials, unburned cement bricks and colored brick materials, automobile brake pad additives, etc. The collected centrifugal clear liquid is the small peptide chelated copper crude liquid, and the copper leaching rate is 91.5%, which is used for the next step of treatment. Among them, the small peptide is glycyl-L-glutamine.

[0028] (3) Preparation of small peptide chelated copper products

[0029] After step (2) is completed, the crude peptide chelated copper solution prepared in step (2) is placed in a vacuum distillation device, and vacuum concentrated under the conditions of a vacuum degree of 0.09 MPa and a temperature of 60°C, and concentrated to 0.1 times the original volume, thereby obtaining a peptide chelated copper concentrate. Then, according to the volume ratio of the peptide chelated copper concentrate to anhydrous ethanol of 1:1, anhydrous ethanol is added to the peptide chelated copper concentrate, and stirred at a temperature of 50°C for 20 minutes, and then the peptide chelated copper concentrate containing anhydrous ethanol is allowed to stand at a low temperature of 4°C for 12 hours, and finally the mixed solution after standing at a low temperature is centrifuged at a speed of 10000 r / min and a temperature of 10°C for 5 minutes, and the upper light liquid and the lower crystal are collected respectively. The collected upper light liquid was subjected to vacuum distillation treatment, and the ethanol can be further used in step (3). The liquid after ethanol recovery can be used for the preparation of the small peptide solution in step (2). The collected lower crystals were dried at 50°C for 12h to obtain a small peptide chelated copper product with a purity of 91.2%.

[0030] Example 2

[0031] A method for preparing small peptide chelated copper using waste printed circuit boards, the specific method steps are as follows:

[0032] (1) Preparation of waste printed circuit board powder

[0033] Using commercially available waste printed circuit boards as raw materials, the waste printed circuit boards were placed in an ultrasonic cleaning machine at a ratio of 1:100, and cleaned for 45 minutes at room temperature and an ultrasonic output power of 75 W. After ultrasonic cleaning, the cleaned waste printed circuit boards were dried at 60°C for 35 minutes, then disassembled into 4 cm small pieces, and then placed in a high-speed pulverizer for crushing, and the powder obtained by screening with a 40-mesh filter sieve was collected, which was the waste printed circuit board powder for the next step of treatment.

[0034] (2) Preparation of crude peptide chelated copper solution

[0035] After the completion of step (1), the waste printed circuit board powder is placed in a hydrogen peroxide solution at a ratio of 1:75, wherein the mass (g) of the waste printed circuit board powder prepared in step (1) is 1:75 to the volume (mL) of a hydrogen peroxide solution with a volume fraction of 5%, to obtain a waste printed circuit board powder reaction solution. Then, the small peptide solution is added to the waste printed circuit board powder reaction solution at a ratio of 1:75, wherein the mass (g) of the waste printed circuit board powder is 1:75 to the volume (mL) of a small peptide solution with a concentration of 0.3M, and then the mixed solution is placed in an ultrasonic reactor equipped with a mechanical stirrer, and the chelation reaction is carried out for 2 hours at a temperature of 40°C, an ultrasonic output power of 90W, and a stirring speed of 200r / min. After the reaction is completed, the mixed solution after the reaction is centrifuged at a speed of 12000r / min and a temperature of 25°C for 7 minutes, and the centrifugal clear liquid and centrifugal sediment are collected respectively. The collected centrifugal sediment mainly contains resin, glass fiber, etc., which can be used as filling materials, unburned cement bricks and colored brick materials, automobile brake pad additives, etc. The collected centrifugal clear liquid is the small peptide chelated copper crude liquid, and the copper leaching rate is 92.6%, which is used for the next step of treatment. Among them, the small peptide is glycylglycine.

[0036] (3) Preparation of small peptide chelated copper products

[0037] After step (2) is completed, the crude peptide chelated copper solution prepared in step (2) is placed in a vacuum distillation device, and vacuum concentrated under the conditions of a vacuum degree of 0.092 MPa and a temperature of 70°C, and concentrated to 0.2 times the original volume, thereby obtaining a peptide chelated copper concentrate. Then, according to the volume ratio of the peptide chelated copper concentrate to anhydrous ethanol of 1:1, anhydrous ethanol is added to the peptide chelated copper concentrate, and stirred at a temperature of 60°C for 30 minutes, and then the peptide chelated copper concentrate containing anhydrous ethanol is allowed to stand at a low temperature of 6°C for 18 hours, and finally the mixed solution after standing at a low temperature is centrifuged at a speed of 12000 r / min and a temperature of 15°C for 7 minutes, and the upper light liquid and the lower crystal are collected respectively. The collected upper light liquid was subjected to vacuum distillation treatment, and the ethanol can be further used in step (3). The liquid after ethanol recovery can be used for the preparation of the small peptide solution in step (2). The collected lower crystals were dried at 60°C for 18 hours to obtain a small peptide chelated copper product with a purity of 92.7%.

[0038] Example 3

[0039] A method for preparing small peptide chelated copper using waste printed circuit boards, the specific method steps are as follows:

[0040] (1) Preparation of waste printed circuit board powder

[0041] Using commercially available waste printed circuit boards as raw materials, the waste printed circuit boards were placed in an ultrasonic cleaning machine at a ratio of 1:200 of the mass (g) of the waste printed circuit boards to the volume (mL) of distilled water, and cleaned for 30 minutes at room temperature and an ultrasonic output power of 90 W. After the ultrasonic cleaning was completed, the cleaned waste printed circuit boards were dried at a temperature of 60°C for 50 minutes, then disassembled into 6 cm small pieces, and then placed in a high-speed pulverizer for crushing, and the powder obtained by screening with a 40-mesh filter sieve was collected, which was the waste printed circuit board powder for the next step of treatment.

[0042] (2) Preparation of crude peptide chelated copper solution

[0043] After step (1) is completed, the waste printed circuit board powder is placed in a hydrogen peroxide solution according to a ratio of 1:125 of the mass (g) of the waste printed circuit board powder prepared in step (1) to the volume (mL) of a hydrogen peroxide solution with a volume fraction of 10%, to obtain a waste printed circuit board powder reaction solution. Then, the small peptide solution is added to the waste printed circuit board powder reaction solution according to a ratio of 1:125 of the mass (g) of the waste printed circuit board powder to the volume (mL) of a small peptide solution with a concentration of 0.1M, and then the mixed solution is placed in an ultrasonic reactor equipped with a mechanical stirrer, and the chelation reaction is carried out for 3 hours at a temperature of 60°C, an ultrasonic output power of 120W, and a stirring speed of 300r / min. After the reaction is completed, the mixed solution after the reaction is centrifuged at a speed of 15000r / min and a temperature of 30°C for 10 minutes, and the centrifugal clear liquid and centrifugal sediment are collected respectively. The collected centrifugal sediment mainly contains resin, glass fiber, etc., which can be used as filling materials, unburned cement bricks and colored brick materials, automobile brake pad additives, etc. The collected centrifugal clear liquid is the small peptide chelated copper crude liquid, and the copper leaching rate is 95.5%, which is used for the next step of treatment. Among them, the small peptide is glutathione.

[0044] (3) Preparation of small peptide chelated copper products

[0045] After step (2) is completed, the crude peptide chelated copper solution prepared in step (2) is placed in a vacuum distillation device, and vacuum concentrated under the conditions of a vacuum degree of 0.095 MPa and a temperature of 80°C, and concentrated to 0.3 times the original volume, thereby obtaining a peptide chelated copper concentrate. Then, according to the volume ratio of the peptide chelated copper concentrate to anhydrous ethanol of 1:1, anhydrous ethanol is added to the peptide chelated copper concentrate, and stirred at a temperature of 70°C for 40 minutes, and then the peptide chelated copper concentrate containing anhydrous ethanol is allowed to stand at a low temperature of 8°C for 24 hours, and finally the mixed solution after standing at a low temperature is centrifuged at a speed of 15000 r / min and a temperature of 20°C for 10 minutes, and the upper light liquid and the lower crystal are collected respectively. The collected upper light liquid was subjected to vacuum distillation treatment, and the ethanol can be further used in step (3). The liquid after ethanol recovery can be used for the preparation of the small peptide solution in step (2). The collected lower crystals were dried at 70°C for 24 hours to obtain a small peptide chelated copper product with a purity of 94.5%.

Claims

1. A method for preparing small peptide chelated copper using waste printed circuit boards, the specific steps of the method are as follows: (1) Preparation of waste printed circuit board powder Using commercially available waste printed circuit boards as raw materials, the waste printed circuit boards are placed in an ultrasonic cleaning machine according to the ratio of the mass of the waste printed circuit boards to the volume of distilled water of 1 g to 50 to 200 mL, and cleaned for 30 to 60 minutes at room temperature and an ultrasonic output power of 60 to 90 W; after the ultrasonic cleaning is completed, the cleaned waste printed circuit boards are dried at a temperature of 60° C. for 20 to 50 minutes, and then disassembled into small pieces of 3 to 6 cm, and then placed in a high-speed pulverizer for crushing, and the powder obtained by screening with a 40-mesh filter sieve is collected for the next step of processing; (2) Preparation of crude peptide chelated copper solution After step (1) is completed, the waste printed circuit board powder is placed in a hydrogen peroxide solution according to the ratio of the mass of the waste printed circuit board powder prepared in step (1) to the volume ratio of the hydrogen peroxide solution with a volume fraction of 2.5 to 10% of 1 g: 25 to 125 mL to obtain a waste printed circuit board powder reaction liquid; then, according to the ratio of the mass of the waste printed circuit board powder to the volume ratio of the small peptide solution with a concentration of 0.1 to 0.5 M of 1 g: 25 to 125 mL, the small peptide solution is added to the waste printed circuit board powder reaction liquid, and the mixed liquid is placed in a machine equipped with In a stirred ultrasonic reactor, the chelation reaction is carried out for 0.5 to 3 hours at a temperature of 30 to 60° C., an ultrasonic output power of 60 to 120 W, and a stirring speed of 100 to 300 r / min. After the reaction is completed, the mixed solution after the reaction is centrifuged for 5 to 10 minutes at a speed of 10,000 to 15,000 r / min and a temperature of 20 to 30° C., and the centrifugal clear liquid and centrifugal sediment are collected respectively. The collected centrifugal clear liquid is a crude solution of small peptide chelated copper, and the copper leaching rate is 91.5 to 95.5%, which is used for the next step of treatment, wherein, Small peptides are glutathione, glycylglycine, and glycyl-L-glutamine; (3) Preparation of small peptide chelated copper products After step (2) is completed, the crude peptide chelated copper solution prepared in step (2) is placed in a vacuum distillation device, and vacuum concentrated under the conditions of a vacuum degree of 0.09 to 0.095 MPa and a temperature of 60 to 80° C. to 0.1 to 0.3 times the original volume; then, anhydrous ethanol is added to the peptide chelated copper concentrate in a volume ratio of 1:1, and the mixture is stirred at a temperature of 50 to 70° C. for 20 to 40 minutes, and then The small peptide chelated copper concentrate containing anhydrous ethanol is then allowed to stand at a low temperature of 4 to 8°C for 12 to 24 hours. Finally, the mixed solution after standing at a low temperature is centrifuged for 5 to 10 minutes at a speed of 10,000 to 15,000 r / min and a temperature of 10 to 20°C, and the upper light liquid and the lower crystals are collected respectively. The collected lower crystals are dried at a temperature of 50 to 70°C for 12 to 24 hours to obtain a small peptide chelated copper product with a purity of 91.2 to 94.5%.

Citation Information

Patent Citations

  • A method for preparing copper-chelated nanopeptides as a feed additive

    CN106035983B

  • Method for preparing casein peptide chelated copper

    CN101756041A

  • Preparation method of composite peptide-copper chelate by utilizing meat processing byproduct

    CN102754739A

  • Preparation method and application of small peptide chelated copper compound

    CN102827910A

  • Preparation method of feed additive nano small peptide chelated copper

    CN106035983A