A heat-resistant shrinkage diaphragm and its preparation method and application
By using heterogeneous interleaving distribution of core-shell structure fibers and polymer fibers in lithium-ion battery separators, combined with electrospinning and hot pressing technology, the problem of insufficient separator shrinkage of lithium-ion batteries at high temperatures is solved, and the battery is improved Thermal safety and electrochemical properties.
Patent Information
- Application Number
- CN202110489602.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-04-30
AI Technical Summary
Lithium-ion batteries are prone to short circuits when punctured by lithium dendrites under high temperature conditions, which poses a safety hazard. The existing polyolefin separator size shrinks at high temperatures to ensure battery safety.
The separator with heterogeneous interlaced distribution of core-shell structure fibers and polymer fibers was prepared by electrospinning technology. Fibre I is an inorganic nanoparticles and polymer polymer composite, and Fibre II is a polymer polymer C, through heat The pressure treatment forms a heat-resistant shrinkage diaphragm.
The low thermal shrinkage rate and excellent thermal closure performance of the separator at high temperatures are achieved, the thermal safety of lithium-ion batteries is improved, and the electrochemical performance is avoided from falling off inorganic particles.
Smart Images

Figure BDA0003050557170000121 
Figure BDA0003050557170000131 
Figure BDA0003050557170000132
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a heat-resistant shrinkage diaphragm and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries are prone to a large number of lithium dendrites under high current conditions, which can puncture the battery separator, causing internal short circuits in the battery and posing safety hazards. Since lithium-ion power batteries have higher operating temperatures and more complex driving environments, they may explode or burn in unconventional conditions, such as abnormal charging and discharging, abnormal heat, and abuse of mechanical conditions. Therefore, the thermal safety performance of lithium-ion power batteries is particularly important.
[0003] The safety of lithium-ion battery separators is one of the important conditions to ensure the thermal safety of lithium-ion power batteries. The safety performance of lithium-ion battery separators requires that the separators have good thermal dimensional stability, no obvious deformation under certain high temperature environments, a high thermal safety temperature, and good thermal closure performance.
[0004] At present, the common lithium battery separators on the market are mainly polyethylene (PE) and polypropylene (PP) separators. Compared with other materials, although polyolefin films have better mechanical properties and chemical stability, their performance is still not enough to guarantee the higher safety requirements of lithium-ion batteries, especially power lithium batteries.
[0005] For example, severe dimensional shrinkage of polyolefin separators at high temperatures can cause internal short circuits in the battery, which may eventually lead to fire or explosion accidents. In order to meet the higher requirements for separator performance in electric vehicles and lithium batteries for energy storage, it is necessary to develop new lithium-ion battery separators with good thermal safety performance. Therefore, it is urgent to develop new separators that can meet the market's thermal safety performance requirements.
[0006] Using new technologies and new materials to prepare new diaphragms is one of the ways to solve the above problems. Electrospinning is an effective technology. Electrospinning technology uses polymer solutions to spin at room temperature. The sources of spinnable materials are wide, the process is simple, and the morphology and structure of the obtained nanofibers can be adjusted, which can be used to prepare polymer nanofiber membranes. Fiber membranes prepared by electrospinning generally have a high porosity, so electrospinning diaphragms have good air permeability, which can greatly reduce the internal resistance of the battery and improve the charge and discharge performance.
[0007] At present, some studies have shown that the heat resistance of the separator can be improved by doping inorganic materials into the spinning solution for electrospinning. However, although the surface of the lithium battery separator prepared by the traditional electrospinning method is loaded with inorganic particles, it is impossible to avoid the shedding of inorganic particles during high-rate charge and discharge, thus affecting the electrochemical performance of the battery in the later stage.
[0008] Therefore, it is of great significance to provide a lithium-ion battery separator with good thermal and high safety performance. Summary of the invention
[0009] The purpose of the present invention is to overcome the above-mentioned defects in the prior art and provide a diaphragm with excellent heat shrinkage resistance and heat closure performance.
[0010] In order to achieve the above-mentioned object, the first aspect of the present invention provides a heat-resistant shrinkage diaphragm, which contains fiber I and fiber II, wherein the fiber I and the fiber II are randomly and staggeredly distributed; the fiber I is a core-shell structure fiber, the material of the core layer fiber of the core-shell structure fiber is a polymer A-inorganic nanoparticle composite formed by a composite of inorganic nanoparticles and a polymer A, and the material of the shell layer fiber of the core-shell structure fiber is a polymer B; the material of the fiber II is a polymer C;
[0011] Wherein, the polymer A is the same as the polymer C and is selected from at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer and polymethyl methacrylate; the polymer B is different from the polymer A, and the polymer B is selected from at least one of polyacrylonitrile, polyarylethersulfoneketone and polyethylene terephthalate;
[0012] In the separator, the content of the fiber I is higher than that of the fiber II, and the content of the core layer fiber of the fiber I is the same as that of the shell layer fiber.
[0013] A second aspect of the present invention provides a method for preparing a heat-resistant shrinkage diaphragm, the method comprising:
[0014] (1) mixing a dispersion liquid I containing inorganic nanoparticles and a dispersion liquid II containing a polymer A to obtain a dispersion liquid III containing the polymer A and inorganic nanoparticles;
[0015] (2) introducing the dispersion IV containing the high molecular polymer B and the dispersion III into a reservoir provided with an outer needle and a reservoir provided with an inner needle of a coaxial electrospinning device, respectively, introducing the dispersion V containing the polymer C into a reservoir provided with another needle, and simultaneously performing electrospinning to obtain a diaphragm precursor in which the fibers II and the fibers I are interlaced with each other in a random order, wherein the fibers I have a core-shell structure;
[0016] (3) hot pressing the membrane precursor to obtain a heat-resistant shrinkage membrane;
[0017] Wherein, the polymer A is the same as the polymer C and is selected from at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer and polymethyl methacrylate; the polymer B is different from the polymer A, and the polymer B is selected from at least one of polyacrylonitrile, polyarylethersulfoneketone and polyethylene terephthalate;
[0018] The flow rates of the dispersions III, IV, and V are controlled so that in the obtained heat-resistant shrinkage diaphragm, the content of the fiber I is higher than that of the fiber II, and the content of the core layer fiber of the fiber I is the same as that of the shell layer fiber.
[0019] The third aspect of the present invention provides a heat-resistant shrinkage diaphragm prepared by the method described in the second aspect.
[0020] The fourth aspect of the present invention provides use of the heat-resistant shrinkage diaphragm described in the first aspect or the third aspect in a lithium-ion battery.
[0021] The diaphragm provided by the present invention has a small heat shrinkage rate at high temperature, and also has excellent thermal pore-closing performance, good heat resistance and high thermal safety.
[0022] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0023] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0024] As mentioned above, the first aspect of the present invention provides a heat-resistant shrinkage diaphragm, which contains fiber I and fiber II, wherein the fiber I and the fiber II are randomly and staggeredly distributed; the fiber I is a core-shell structure fiber, the material of the core layer fiber of the core-shell structure fiber is a polymer A-inorganic nanoparticle composite formed by a composite of inorganic nanoparticles and a polymer A, and the material of the shell layer fiber of the core-shell structure fiber is a polymer B; the material of the fiber II is a polymer C;
[0025] Wherein, the polymer A is the same as the polymer C and is selected from at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer and polymethyl methacrylate; the polymer B is different from the polymer A, and the polymer B is selected from at least one of polyacrylonitrile, polyarylethersulfoneketone and polyethylene terephthalate;
[0026] In the separator, the content of the fiber I is higher than that of the fiber II, and the content of the core layer fiber of the fiber I is the same as that of the shell layer fiber.
[0027] The diaphragm provided by the present invention will not cause inorganic particles to fall off during high-rate charge and discharge, and at the same time has good heat resistance and high thermal safety.
[0028] According to the fiber diaphragm described in the first aspect of the present invention, several preferred specific embodiments are provided below. Specific implementation 1:
[0030] The polymer A and the polymer C are polyvinylidene fluoride, and the polymer B is polyacrylonitrile. Specific implementation 2:
[0032] The polymer A and the polymer C are polyvinylidene fluoride-hexafluoropropylene copolymers, and the polymer B is polyarylethersulfoneketone. Specific implementation 3:
[0034] The polymer A and the polymer C are a blend of polyvinylidene fluoride / polyvinylidene fluoride-hexafluoropropylene copolymer (the mass ratio of polyvinylidene fluoride to polyvinylidene fluoride-hexafluoropropylene copolymer is 3:7 to 7:3), and the polymer B is polyethylene terephthalate.
[0035] The inventors found that the diaphragms obtained in the above-mentioned specific embodiments 1-3 have better heat resistance and higher thermal safety.
[0036] Preferably, in the high molecular polymer A-inorganic nanoparticle composite, the content of the inorganic nanoparticles is 1-30% by weight, more preferably 1-20% by weight.
[0037] Preferably, the inorganic nanoparticles are selected from at least one of oxides of Group IIA metals, sulfates of Group IIA metals, hydroxides of Group IIA metals, oxides of Group IVB metals, oxides of Group IIIA metals, hydrated alumina and silicon dioxide.
[0038] More preferably, the inorganic nanoparticles are selected from at least one of aluminum oxide, magnesium oxide, silicon dioxide, zirconium dioxide, titanium dioxide, hydrated aluminum oxide, barium sulfate and magnesium hydroxide.
[0039] More preferably, the average particle size of the inorganic nanoparticles is 10-200 nm.
[0040] Preferably, the fiber separator has an average thickness of 20-50 μm.
[0041] Preferably, the average diameter of the fiber I is 0.5-2 μm, and the average diameter of the core layer fibers in the fiber I is 100-400 nm.
[0042] Preferably, the average diameter of the fibers II is 0.5-2 μm.
[0043] Preferably, the fiber I is a fiber prepared by coaxial electrospinning; and the fiber II is a fiber prepared by electrospinning.
[0044] As mentioned above, the second aspect of the present invention provides a method for preparing a heat-resistant shrinkage diaphragm, the method comprising:
[0045] (1) mixing a dispersion liquid I containing inorganic nanoparticles and a dispersion liquid II containing a polymer A to obtain a dispersion liquid III containing the polymer A and inorganic nanoparticles;
[0046] (2) introducing the dispersion IV containing the high molecular polymer B and the dispersion III into a reservoir provided with an outer needle and a reservoir provided with an inner needle of a coaxial electrospinning device, respectively, introducing the dispersion V containing the polymer C into a reservoir provided with another needle, and simultaneously performing electrospinning to obtain a diaphragm precursor in which the fibers II and the fibers I are interlaced with each other in a random order, wherein the fibers I have a core-shell structure;
[0047] (3) hot pressing the membrane precursor to obtain a heat-resistant shrinkage membrane;
[0048] Wherein, the polymer A is the same as the polymer C and is selected from at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer and polymethyl methacrylate; the polymer B is different from the polymer A, and the polymer B is selected from at least one of polyacrylonitrile, polyarylethersulfoneketone and polyethylene terephthalate;
[0049] The flow rates of the dispersions III, IV, and V are controlled so that in the obtained heat-resistant shrinkage diaphragm, the content of the fiber I is higher than that of the fiber II, and the content of the core layer fiber of the fiber I is the same as that of the shell layer fiber.
[0050] According to the method of the second aspect of the present invention, the memory provided with another needle can be a memory on another electrospinning device, or can be another memory in the same coaxial electrospinning device (except for the memory provided with an outer needle and the memory provided with an inner needle). According to a preferred specific embodiment of the present invention, electrospinning is performed simultaneously using two devices, a coaxial electrospinning device and a (normal) electrospinning device.
[0051] According to the method described in the second aspect of the present invention, a diaphragm precursor is obtained which is formed by fibers II and fibers I which are randomly and staggeredly distributed with each other, wherein the material of the fibers II is polymer C, the material of the core layer fibers of the fibers I is polymer A-inorganic nanoparticle composite, and the material of the shell layer fibers of the fibers I is polymer B.
[0052] Preferably, the electrospinning conditions include: spinning voltage of 15-30 kV, receiving distance of 10-30 cm, humidity of 20-50%, and temperature of 20-40°C.
[0053] Preferably, the hot pressing conditions include: temperature of 70-100° C., pressure of 3-7 MPa, and hot pressing time of 1-3 min.
[0054] Preferably, the aperture of the inner needle is 0.3-0.5 mm, and the aperture of the outer needle is 0.7-1.0 mm.
[0055] Preferably, the aperture of the other needle is 0.3-0.7 mm.
[0056] Preferably, the flow rates of the dispersion liquid III, the dispersion liquid IV, and the dispersion liquid V are each independently selected from 1-10 ml / h.
[0057] Preferably, in the dispersion III, the content of the inorganic nanoparticles is 1-30% by weight, more preferably 1-20% by weight, based on the total weight of the high molecular weight polymer A and the inorganic nanoparticles contained therein.
[0058] Preferably, the concentration of the inorganic nanoparticles in the dispersion I is 10-50% by weight, and the concentration of the high molecular polymer A in the dispersion II is 10-60% by weight.
[0059] Preferably, the dispersion I and the dispersion II are mixed so that the solid content of the dispersion III is 5-50 wt %.
[0060] Preferably, the concentration of the high molecular polymer B in the dispersion IV is 10-60 wt %.
[0061] Preferably, the concentration of the high molecular weight polymer C in the dispersion V is 10-60 wt %.
[0062] Preferably, the solvents in the dispersion I, the dispersion II, the dispersion IV, and the dispersion V are each independently selected from at least one of dimethylformamide, acetone, tetrahydrofuran, chloroform, dichloromethane, dimethyl sulfoxide, N-methylpyrrolidone, trifluoroethanol, trifluoroacetic acid, dimethylacetamide, ethanol, and hexafluoroisopropanol.
[0063] In the method described in the second aspect of the present invention, the types and characteristics of the inorganic nanoparticles correspond to the same as the types and characteristics of the inorganic nanoparticles described in the first aspect, and the present invention will not repeat them here.
[0064] According to a particularly preferred embodiment, the method described in the second aspect of the present invention comprises:
[0065] (a) dissolving the high molecular polymer B in an organic solvent to form a dispersion IV having a concentration of 10-60 wt %;
[0066] (b) dispersing inorganic nanoparticles in an organic solvent to form a dispersion I with a concentration of 10-50 wt %; dissolving a high molecular weight polymer A in an organic solvent to form a dispersion II with a concentration of 10-60 wt %; and mixing the dispersion I and the dispersion II to obtain a dispersion III;
[0067] (c) dissolving the high molecular weight polymer C in an organic solvent to form a dispersion V having a concentration of 10-60 wt %;
[0068] (d) introducing the dispersion IV and the dispersion III into the outer needle syringe and the inner needle syringe of the coaxial electrospinning device respectively, introducing the dispersion V into a storage device provided with another needle, and simultaneously performing electrospinning to obtain a membrane precursor, wherein the electrospinning conditions include: a spinning voltage of 15-30 kV, a receiving distance of 10-30 cm, a humidity of 20-50%, and a temperature of 20-40° C.;
[0069] (e) hot pressing the membrane precursor using a plate hot press at a temperature of 70-100° C., a pressure of 3-7 MPa, and a hot pressing time of 1-3 min to obtain the membrane.
[0070] As mentioned above, the third aspect of the present invention provides a heat-shrinkage-resistant separator prepared by the method described in the second aspect.
[0071] As mentioned above, the fourth aspect of the present invention provides the use of the heat-resistant shrinkage diaphragm described in the first aspect or the third aspect in a lithium-ion battery.
[0072] In the present invention, unless otherwise specified, pressure refers to gauge pressure.
[0073] The present invention will be described in detail below by way of examples.
[0074] In the following examples, unless otherwise specified, all raw materials used are commercially available products.
[0075] The electrospinning device (ie, another electrospinning device described below) and the coaxial spinning device used below were purchased from Beijing Xinyan Hechuang Technology Co., Ltd.
[0076] Unless otherwise specified, room temperature refers to 25±2°C.
[0077] Polyvinylidene fluoride (purchased from Arkema, France, trade name HSV900)
[0078] Polyacrylonitrile (purchased from J&K Company, Mw = 1.5 × 10 5 )
[0079] Poly(arylethersulfoneketone) (purchased from Dalian Baolimo Co., Ltd., Mw = 1 × 10 5 )
[0080] Polyvinylidene fluoride-hexafluoropropylene copolymer (purchased from Arkema, France, trade name SL-023)
[0081] Polyethylene terephthalate (purchased from Jinzhou Huifa Tianhe Chemical Co., Ltd., Mw = 2 × 10 4 )
[0082] Polycaprolactone (purchased from J&K Technology Co., Ltd., Mw = 14,000)
[0083] In the following examples, the average diameters of the fibers I and II in the separator were measured using NanoMeasure software in electron microscope images.
[0084] Example 1
[0085] (1) Weigh 15 g of polyacrylonitrile (polymer B), dissolve it in 85 g of DMF solvent, and stir at room temperature for 12 h until it becomes homogeneous and transparent to obtain a polymer solution (dispersion IV);
[0086] (2) Weigh 4 g of Al2O3 particles with an average particle size of 10 nm, add them to 10 g of DMF / acetone mixed solvent, the volume ratio of DMF to acetone is 7:3, and use a self-rotating and revolving stirrer to disperse at high speed for 30 min to obtain a uniform dispersion (dispersion liquid I); weigh 15 g of polyvinylidene fluoride (polymer A), dissolve it in 71 g of DMF solvent, stir at room temperature for 12 h until it is uniform and transparent, and obtain a uniform dispersion (dispersion liquid II), and add the dispersion liquid II to the dispersion liquid I to form an "Al2O3 particle-polymer composite" dispersion liquid III, and the solid content of the dispersion liquid III is 19 wt%;
[0087] (3) Weigh 20 g of polyvinylidene fluoride (polymer C), dissolve it in 80 g of a DMF / acetone mixed solvent, the volume ratio of DMF to acetone being 7:3, and stir at room temperature for 12 h until it becomes uniform and transparent, to obtain a polymer solution (dispersion solution V);
[0088] (4) placing the dispersion IV prepared in step (1) in the outer needle syringe ① of the coaxial electrospinning device, and placing the "Al2O3 particle-polymer composite" dispersion III prepared in step (2) in the inner needle syringe ② of the coaxial spinning device, the flow rates of syringes ① and ② are both 4 ml / h, the inner needle aperture is 0.3 mm, and the outer needle aperture is 0.7 mm; placing the dispersion V prepared in step (3) in the needle syringe ③ of another electrospinning device (i.e., the other needle) with a needle aperture of 0.3 mm and a flow rate of 2 ml / h, and simultaneously performing electrospinning to obtain a diaphragm precursor, the spinning voltage is 15 kV, the receiving distance is 10 cm, the humidity is 20%, and the temperature is 20°C;
[0089] (5) The diaphragm precursor obtained in step (4) is hot pressed using a plate hot press at a temperature of 70°C, a pressure of 3 MPa, and a hot pressing time of 1 min to obtain a diaphragm having an average thickness of 25 μm, an average diameter of fiber I of 1 μm, an average diameter of the core layer fibers in the fiber I of 200 nm, and an average diameter of the fiber II of 0.5 μm.
[0090] Example 2
[0091] (1) Weigh 20 g of poly(arylethersulfoneketone) (polymer B), dissolve it in 90 g of a tetrahydrofuran / N-methylpyrrolidone mixed solvent, the volume ratio of tetrahydrofuran to N-methylpyrrolidone being 5:5, and stir at room temperature for 12 h until the mixture becomes uniform and transparent, to obtain a polymer solution (dispersion liquid IV);
[0092] (2) Weigh 4 g of MgO particles with an average particle size of 50 nm, add them to 10 g of DMF / acetone mixed solvent, the volume ratio of DMF to acetone is 7:3, use a self-rotating and revolving mixer to disperse at high speed for 60 min to obtain a uniform dispersion (dispersion I). Weigh 16 g of polyvinylidene fluoride-hexafluoropropylene copolymer (polymer A), dissolve them in 70 g of DMF / acetone mixed solvent, the volume ratio of DMF to acetone is 7:3, stir at room temperature for 12 h until it becomes uniform and transparent, and obtain a uniform dispersion (dispersion II), and add the dispersion II to the dispersion I to form a "MgO particle-polymer composite" dispersion III, the solid content of which is 20% by weight.
[0093] (3) Weigh 15 g of polyvinylidene fluoride-hexafluoropropylene copolymer (polymer C), dissolve it in 80 g of DMF / acetone mixed solvent, the volume ratio of DMF to acetone is 7:3, stir at room temperature for 12 h until it becomes uniform and transparent, and obtain a polymer solution (dispersion liquid V);
[0094] (4) placing the dispersion IV prepared in step (1) in the outer needle syringe ① of the coaxial electrospinning device, and placing the "MgO particle-polymer complex" dispersion III prepared in step (2) in the inner needle syringe ② of the coaxial spinning device, the flow rates of syringes ① and ② are both 8 ml / h, the inner needle aperture is 0.3 mm, and the outer needle aperture is 0.9 mm; placing the dispersion V prepared in step (3) in the needle syringe ③ of another electrospinning device (i.e., the other needle) with a needle aperture of 0.5 mm and a flow rate of 2 ml / h, and simultaneously performing electrospinning to obtain a diaphragm precursor, the spinning voltage is 20 kV, the receiving distance is 15 cm, the humidity is 25%, and the temperature is 25°C;
[0095] (5) The membrane precursor obtained in step (4) is hot-pressed using a plate hot press at a temperature of 80°C, a pressure of 4 MPa, and a hot-pressing time of 1 min to obtain a fiber membrane, wherein the average thickness of the membrane is 30 μm, the average diameter of fiber I is 2 μm, the average diameter of the core layer fibers in fiber I is 400 nm, and the average diameter of fiber II is 0.5 μm.
[0096] Example 3
[0097] (1) Weigh 25 g of polyethylene terephthalate (polymer B), dissolve it in 75 g of hexafluoroisopropanol solvent, and stir at room temperature for 12 h until it becomes uniform and transparent to obtain a polymer solution (dispersion liquid IV);
[0098] (2) Weigh 6 g of SiO2 particles with an average particle size of 100 nm, add them to 12 g of DMF solvent, and use a self-rotating and revolving mixer to disperse them at high speed for 45 min to obtain a uniform dispersion (Dispersion I). Weigh 16 g of a blend of polyvinylidene fluoride / polyvinylidene fluoride-hexafluoropropylene copolymer (the mass ratio of polyvinylidene fluoride to polyvinylidene fluoride-hexafluoropropylene copolymer is 5:5, polymer A), dissolve them in 66 g of DMF / acetone mixed solvent, the volume ratio of DMF to acetone is 7:3, stir at room temperature for 12 h until it becomes uniform and transparent, and obtain a uniform dispersion (Dispersion II), and add the Dispersion II to the Dispersion I to form a "SiO2 particle-polymer composite" Dispersion III, the solid content of which is 22%.
[0099] (3) Weigh 22 g of a blend of polyvinylidene fluoride and polyvinylidene fluoride-hexafluoropropylene (polymer C, the mass ratio of polyvinylidene fluoride to polyvinylidene fluoride-hexafluoropropylene is 5:5), dissolve it in 78 g of a DMF / acetone mixed solvent, the volume ratio of DMF to acetone is 7:3, and stir at room temperature for 12 h until it becomes uniform and transparent, to obtain a polymer solution (dispersion liquid V);
[0100] (4) placing the dispersion IV prepared in step (1) in the outer needle syringe ① of the coaxial electrospinning device, and placing the "SiO2 particle-polymer composite" dispersion III prepared in step (2) in the inner needle syringe ② of the coaxial spinning device, the flow rates of syringes ① and ② are both 6 ml / h, the inner needle aperture is 0.5 mm, and the outer needle aperture is 0.9 mm; placing the dispersion V prepared in step (3) in the needle syringe ③ of another electrospinning device (i.e., the other needle) with a needle aperture of 0.7 mm and a flow rate of 4 ml / h, and simultaneously performing electrospinning to obtain a diaphragm, the spinning voltage is 25 kV, the receiving distance is 25 cm, the humidity is 30%, and the temperature is 30°C;
[0101] (5) The fiber diaphragm obtained in step (4) is hot pressed using a plate hot press at a temperature of 100° C., a pressure of 5 MPa, and a hot pressing time of 2 min to obtain a fiber diaphragm.
[0102] The average thickness of the fiber diaphragm is 35 μm, the average diameter of fiber I is 1.5 μm, the average diameter of the core layer fiber in the fiber I is 200 nm, and the average diameter of the fiber II is 1 μm.
[0103] Comparative Example 1
[0104] The diaphragm was prepared in a similar manner to Example 1, except that the same mass of polycaprolactone was used to replace the polyvinylidene fluoride in Example 1 (replacing both the polymer A and the polymer C).
[0105] The rest of the steps were the same as those in Example 1 to prepare a fiber diaphragm.
[0106] Test Case
[0107] 1. Thermal shrinkage: The thermal shrinkage of the diaphragm prepared in the above example was measured in an oven. The sample was heat treated at 150°C for 2 hours, and then the thermal shrinkage δ was calculated according to the formula. The specific results are shown in Table 1.
[0108]
[0109] Among them, S1 and S2 are the areas of the diaphragm before and after heat treatment;
[0110] Table 1
[0111] Examples Thermal shrinkage (%) Example 1 2 Example 2 1 Example 3 1 Comparative Example 1 18
[0112] 2. Thermal closed cell performance test
[0113] The diaphragms prepared in the above examples were heat treated at 100°C and 160°C for 2 hours respectively, and then the porosity of the diaphragms after heat treatment was tested. The specific results are shown in Table 2.
[0114] Table 2
[0115]
[0116] 3. The following properties of the diaphragm obtained in the above examples were tested. The specific test method is as follows and the test results are shown in Table 3.
[0117] (1) Porosity: Soak the diaphragm in n-butanol for 2 hours, and then calculate the porosity p1 according to the formula:
[0118]
[0119] Among them, ρ1 and ρ2 are the density of n-butanol and the dry density of the diaphragm, m1 and m2 are the mass of n-butanol absorbed by the diaphragm and the mass of the diaphragm itself;
[0120] (2) Liquid absorption rate: Soak the membrane in n-butanol for 12 hours, and then calculate the liquid absorption rate P2 according to the formula:
[0121]
[0122] Among them, W2 and W1 are the mass of n-butanol absorbed by the diaphragm and the mass of the diaphragm itself;
[0123] (3) Tensile strength: The tensile strength of the diaphragm was tested using the plastic tensile test method of GB1040-79;
[0124] (4) Conductivity: The ionic conductivity of the diaphragm was measured using an electrochemical workstation. The test frequency range was 0.001 Hz to 10 5 Hz, and then calculate the conductivity σ according to the formula:
[0125]
[0126] Where, σ is the ionic conductivity of the membrane (S / cm), d is the thickness of the membrane (cm), R b is the bulk resistance of the diaphragm (Ω), A is the effective contact area between the diaphragm and the electrode (cm 2 ).
[0127] (5) Thickness: Use a thickness gauge (accuracy 0.1 μm) to test the thickness, randomly select 5 points on the sample and take the average value;
[0128] Table 3
[0129] Examples Thickness / μm Porosity / % Liquid absorption rate / % Tensile strength / MPa Ionic conductivity / S / cm Example 1 25 55 367 15 <![CDATA[2.93×10 -3 ]]> Example 2 30 52 354 16 <![CDATA[2.75×10 -3 ]]> Example 3 35 53 331 17 <![CDATA[2.54×10 -3 ]]> Comparative Example 1 25 52 293 10 <![CDATA[1.93×10 -3 ]]>
[0130] In summary, the diaphragm provided by the present invention has a small thermal shrinkage rate and good heat resistance, and in particular, the diaphragm provided by the present invention has excellent thermal closure performance and higher thermal safety.
[0131] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A heat-resistant shrinkage diaphragm, characterized in that: The diaphragm contains fiber I and fiber II, wherein the fiber I and the fiber II are arranged in a random and staggered manner; the fiber I is a core-shell structure fiber, the material of the core layer fiber of the core-shell structure fiber is a polymer A-inorganic nanoparticle composite formed by a composite of inorganic nanoparticles and a polymer A, and the material of the shell layer fiber of the core-shell structure fiber is a polymer B; the material of the fiber II is a polymer C; Wherein, the polymer A is the same as the polymer C and is selected from at least one of polyvinylidene fluoride-hexafluoropropylene copolymer and polymethyl methacrylate; the polymer B is different from the polymer A, and the polymer B is selected from at least one of polyacrylonitrile and polyethylene terephthalate; In the diaphragm, the content of the fiber I is higher than that of the fiber II, and the content of the core layer fiber of the fiber I is the same as that of the shell layer fiber; In the high molecular polymer A-inorganic nanoparticle composite, the content of the inorganic nanoparticles is 1-30% by weight; and the average diameter of the fiber I is 0.5-2 μm, the average diameter of the core layer fiber in the fiber I is 100-400 nm; the average diameter of the fiber II is 0.5-2 μm.
2. The diaphragm according to claim 1, wherein The inorganic nanoparticles are selected from at least one of oxides of Group IIA metals, sulfates of Group IIA metals, hydroxides of Group IIA metals, oxides of Group IVB metals, oxides of Group IIIA metals, hydrated aluminum oxide and silicon dioxide; And / or, the average particle size of the inorganic nanoparticles is 10-200 nm.
3. The diaphragm according to claim 2, wherein: The inorganic nanoparticles are selected from at least one of aluminum oxide, magnesium oxide, silicon dioxide, zirconium dioxide, titanium dioxide, hydrated aluminum oxide, barium sulfate and magnesium hydroxide.
4. The diaphragm according to any one of claims 1 to 3, wherein: The average thickness of the separator is 20-50 μm.
5. A method for preparing a heat-resistant shrinkage diaphragm, characterized in that: The method includes: (1) mixing a dispersion liquid I containing inorganic nanoparticles and a dispersion liquid II containing a polymer A to obtain a dispersion liquid III containing the polymer A and inorganic nanoparticles; (2) introducing the dispersion IV containing the high molecular polymer B and the dispersion III into a reservoir provided with an outer needle and a reservoir provided with an inner needle of a coaxial electrospinning device respectively, introducing the dispersion V containing the polymer C into a reservoir provided with another needle, and simultaneously performing electrospinning to obtain a diaphragm precursor in which the fibers II and the fibers I are interlaced with each other in a disordered manner, wherein the fibers I have a core-shell structure; (3) hot pressing the diaphragm precursor to obtain a heat-resistant shrinkage diaphragm; Wherein, the polymer A is the same as the polymer C and is selected from at least one of polyvinylidene fluoride-hexafluoropropylene copolymer and polymethyl methacrylate; the polymer B is different from the polymer A, and the polymer B is selected from at least one of polyacrylonitrile and polyethylene terephthalate; The flow rates of the dispersions III, IV and V are controlled so that in the obtained heat-resistant shrinkage diaphragm, the content of the fiber I is higher than that of the fiber II, and the content of the core layer fiber of the fiber I is the same as that of the shell layer fiber.
6. The method according to claim 5, wherein: The electrospinning conditions include: spinning voltage of 15-30 kV, receiving distance of 10-30 cm, humidity of 20-50%, and temperature of 20-40° C.; And / or, the hot pressing conditions include: temperature of 70-100° C., pressure of 3-7 MPa, and hot pressing time of 1-3 min.
7. The method according to claim 5, wherein: The inner needle has a hole diameter of 0.3-0.5 mm, and the outer needle has a hole diameter of 0.7-1.0 mm; And / or, the aperture of the another needle is 0.3-0.7 mm.
8. The method according to any one of claims 5 to 7, wherein: The flow rates of the dispersion liquid III, the dispersion liquid IV, and the dispersion liquid V are each independently selected from 1-10 ml / h.
9. The method according to any one of claims 5 to 7, wherein: The inorganic nanoparticles are selected from at least one of oxides of Group IIA metals, sulfates of Group IIA metals, hydroxides of Group IIA metals, oxides of Group IVB metals, oxides of Group IIIA metals, hydrated aluminum oxide and silicon dioxide; And / or, the average particle size of the inorganic nanoparticles is 10-200 nm.
10. The method according to claim 9, wherein: The inorganic nanoparticles are selected from at least one of aluminum oxide, magnesium oxide, silicon dioxide, zirconium dioxide, titanium dioxide, hydrated aluminum oxide, barium sulfate and magnesium hydroxide.
11. The method according to any one of claims 5 to 7, wherein: In the dispersion III, the content of the inorganic nanoparticles is 1-30 wt % based on the total weight of the high molecular weight polymer A and the inorganic nanoparticles contained therein.
12. A heat-resistant shrinkage diaphragm prepared by the method according to any one of claims 5 to 11.
13. Use of the heat-resistant shrinkage diaphragm according to any one of claims 1 to 4 and 12 in lithium-ion batteries.