Composite conductive diaphragm as well as preparation method and application thereof

By coating conductive materials on the lithium-ion battery separator, the thermal stability and rate performance of the separator are improved, and the problem of insufficient thermal shrinkage performance of the separator at high temperatures is solved, ensuring the safety and high-efficiency operation of the battery.

CN119009354APending Publication Date: 2024-11-22安徽得壹能源科技有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411130644.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing lithium-ion battery separators lack heat shrinkage performance under high temperature conditions, which may lead to internal short circuits and safety hazards, such as thermal runaway, fires and even explosions, which cannot meet the needs of high battery life and high rate performance.

Method used

By coating conductive paste on the surface of the diaphragm, conductive materials such as conductive carbon black, graphite, nanocarbon fiber and carbon nanotubes are selected, and conductive ceramics with excellent high temperature resistance are prepared. Coating and slurry reduce the heat shrinkage of the membrane and improve the wetting and rate performance of the electrolyte.

Benefits of technology

It significantly improves the thermal stability and rate performance of the diaphragm, reduces the thermal shrinkage rate of the battery, enhances the safety performance and electronic transmission efficiency of the battery, and is suitable for use in high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009354A_ABST
    Figure CN119009354A_ABST
Patent Text Reader

Abstract

The invention relates to a composite conductive diaphragm as well as a preparation method and application thereof. The composite conductive diaphragm comprises a diaphragm and conductive slurry coated on the surface of the diaphragm, the composite conductive diaphragm further comprises a diaphragm, a conductive ceramic coating and a conductive slurry coating, the surface of the diaphragm is coated with the conductive ceramic coating, and then the surface of the conductive ceramic coating is coated with a layer of conductive slurry with excellent conductivity. According to the composite conductive diaphragm and the preparation method provided by the invention, the thermal shrinkage rate of the diaphragm is effectively reduced, the safety performance of the battery is improved, and the transmission efficiency of electrons of positive and negative pole pieces in the battery and the rate capability of the battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a composite conductive diaphragm and a preparation method and application thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Lithium-ion batteries are the most widely used and most mature secondary battery system, mainly composed of positive electrode materials, negative electrode materials, separators, current collectors, and electrolytes. Among them, the separator is the medium that separates the positive and negative electrodes inside the battery. It can prevent short circuits inside the battery and facilitate the passage of lithium ions, playing an irreplaceable role.

[0004] With the continuous development of the new energy industry, the requirements for batteries are getting higher and higher. Therefore, the requirements for battery raw materials are also constantly increasing, resulting in more and more composite diaphragms beginning to occupy the main body of the market. For example, CN116598708A provides a composite diaphragm and its preparation method and application: coating an inorganic ceramic slurry on the surface of the base membrane to form an inorganic ceramic film; spraying PVDF slurry on the surface of the inorganic ceramic slurry to form a PVDF film; drying the base membrane coated with the inorganic ceramic slurry and PVDF slurry to obtain a composite ceramic diaphragm. This spraying method avoids the direct penetration of PVDF slurry into the micropores of the base membrane, causing the phenomenon of diaphragm pore blockage, but it only improves the safety performance;

[0005] In view of the current demand for lithium-ion batteries with long battery life and high rate, the above-reported diaphragms can no longer meet the demand. At the same time, the inventors discovered the importance of the thermal shrinkage performance of the diaphragm during their research: during the battery charging and discharging process, especially when overcharging or the temperature rises abnormally, a large amount of heat will be generated inside the battery. If the thermal shrinkage of the diaphragm is poor and it shrinks significantly under high temperature conditions, it may cause direct contact between the positive and negative electrodes (the so-called "internal short circuit"), causing serious safety hazards, such as thermal runaway of the battery, fire, or even explosion. Therefore, a diaphragm with good thermal stability and low thermal shrinkage can effectively avoid this situation and ensure the safe operation of the battery. Therefore, the development of diaphragms with improved thermal shrinkage performance, high wettability, and high rate performance is a problem that needs to be solved today. Summary of the invention

[0006] In order to solve the above problems, the present invention provides a composite conductive diaphragm and a preparation method and application thereof, which improves the wettability of the diaphragm to the electrolyte and the rate performance in the battery while improving the thermal shrinkage performance. The following technical solutions are specifically adopted:

[0007] The first aspect of the present invention provides a composite conductive diaphragm, which comprises: a diaphragm and a conductive slurry coating, wherein the conductive slurry coating is applied to the surface of the diaphragm and has a thickness of 1500 to 3000 nanometers; wherein the conductive slurry coating is a coating containing a conductive material, and the total mass content of the conductive material is 5%.

[0008] The second aspect of the present invention provides a composite conductive diaphragm, which includes: a diaphragm, a conductive ceramic coating and a conductive slurry coating, wherein the conductive ceramic coating is coated on the surface of the diaphragm, and the conductive slurry coating is coated on the surface of the conductive ceramic coating, and the thickness of the conductive ceramic coating and the conductive slurry coating are both 1500 to 3000 nanometers; wherein the conductive slurry coating is a coating containing a conductive material, and the total mass content of the conductive material is 5%.

[0009] Preferably, the conductive material is selected from one or more of conductive carbon black (SP), Ketjen black (KB), conductive graphite (KS 6), vapor deposited carbon nanofibers (VGCF), and carbon nanotubes (CNTs).

[0010] Preferably, the material of the diaphragm is selected from one or more of polypropylene (PP) diaphragm, polyethylene diaphragm (PE), cellulose diaphragm, ceramic diaphragm, non-woven fabric, and aramid.

[0011] The third aspect of the present invention provides a method for preparing the composite conductive diaphragm according to the first aspect, comprising the following steps:

[0012] S1: adding a binder to a dispersant to obtain a glue solvent;

[0013] S2: Grinding the conductive material into dry powder;

[0014] S3: adding the dry powder into the glue solvent and mixing evenly to obtain a conductive paste;

[0015] S4: coating the conductive slurry on the diaphragm to obtain a composite conductive diaphragm.

[0016] Preferably, in step S1, the binder is selected from one or more of polyvinylidene fluoride PVDF, polytetrafluoroethylene PTFE, polyacrylic acid PAA, acrylonitrile multipolymer LA132, sodium carboxymethyl cellulose CMC, and gelatin; the dispersant is one or more of N-methylpyrrolidone, water, methanol, ethanol, propanol, and isopropanol.

[0017] Preferably, in step S1, the amount of the binder added is 3% to 10% of the total mass of the glue solvent.

[0018] Further preferably, the added amount of the binder accounts for 5% of the total mass of the glue solvent.

[0019] Preferably, in step S4, the coating method is selected from one or more of gravure coating, coating, and spraying.

[0020] Preferably, in step S4, the conductive paste may be coated on a single surface or both surfaces of the diaphragm.

[0021] Preferably, in step S4, the membrane needs to be dried after coating, the drying temperature is 50 to 90° C., the drying form is vacuum drying, and the vacuum drying time is 2 to 24 hours.

[0022] A fourth aspect of the present invention provides a lithium battery, comprising the composite conductive diaphragm described in the first aspect, and further comprising: a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the composite conductive diaphragm is disposed between the positive electrode sheet and the negative electrode sheet.

[0023] The beneficial effects of the present invention are:

[0024] (1) The conductive material of the composite conductive diaphragm prepared by the present invention has excellent high temperature resistance and will not deform or melt when used at high temperatures. The addition of conductive material can help the diaphragm to dissipate heat to a certain extent, preventing the battery cell from overheating and causing performance degradation. That is, the present invention can reduce the thermal shrinkage rate of the diaphragm by coating the conductive slurry on the surface of the diaphragm, thereby improving the safety performance of the battery.

[0025] (2) The present invention coats a layer of conductive slurry with excellent conductivity on the surface of the base film. The diaphragm coated with the conductive coating can improve the wettability of the electrolyte on its surface, which can effectively improve the transmission efficiency of electrons in the positive and negative electrodes of the battery, and can also improve the rate performance of the battery.

[0026] (3) The preparation method of the composite conductive diaphragm provided in the embodiment of the present invention has a simple process and is conducive to large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0028] Figure 1 This is a schematic diagram of the structure of the composite conductive diaphragm of Example 1 / Example 2 of the present invention;

[0029] Figure 2 This is a schematic diagram of the structure of the composite conductive diaphragm of Example 3 / Example 4 of the present invention.

[0030] Among them, 1. PE film; 2. Ceramic slurry coating; 3. Conductive slurry coating. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical scheme and advantages of the present invention clearer, the embodiments of the present invention will be further described in detail below in conjunction with the accompanying drawings. It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those of ordinary skill in the art to which the present invention belongs.

[0032] In view of the current demand for lithium-ion batteries with long battery life and high rate, the above-reported diaphragms can no longer meet the demand. At the same time, the inventors discovered the importance of the thermal shrinkage performance of the diaphragm during their research: during the battery charging and discharging process, especially when overcharging or the temperature rises abnormally, a large amount of heat will be generated inside the battery. If the thermal shrinkage of the diaphragm is poor and it shrinks significantly under high temperature conditions, it may cause direct contact between the positive and negative electrodes (the so-called "internal short circuit"), causing serious safety hazards, such as thermal runaway of the battery, fire, or even explosion. Therefore, a diaphragm with good thermal stability and low thermal shrinkage can effectively avoid this situation and ensure the safe operation of the battery. Therefore, the development of diaphragms with improved thermal shrinkage performance, high wettability, and high rate performance is a problem that needs to be solved today.

[0033] Based on the above, the first aspect of the present invention provides a composite conductive diaphragm, which comprises: a diaphragm and a conductive slurry coating, wherein the conductive slurry coating is coated on the surface of the diaphragm and has a thickness of 1500 to 3000 nanometers; wherein the conductive slurry coating is a coating containing a conductive material, and the total mass content of the conductive material is 5%.

[0034] The second aspect of the present invention provides a composite conductive diaphragm, which includes: a diaphragm, a conductive ceramic coating and a conductive slurry coating, wherein the conductive ceramic coating is coated on the surface of the diaphragm, and the conductive slurry coating is coated on the surface of the conductive ceramic coating, and the thickness of the conductive ceramic coating and the conductive slurry coating are both 1500 to 3000 nanometers; wherein the conductive slurry coating is a coating containing a conductive material; the total mass content of the conductive material is 5%.

[0035] As a further technical solution, the conductive material is selected from one or more of conductive carbon black (SP), Ketjen black (KB), conductive graphite (KS 6), vapor deposited carbon nanofibers (VGCF), and carbon nanotubes (CNTs).

[0036] As a further technical solution, the material of the diaphragm is selected from one or more of polypropylene (PP) diaphragm, polyethylene diaphragm (PE), cellulose diaphragm, ceramic diaphragm, non-woven fabric, and aramid.

[0037] The third aspect of the present invention provides a method for preparing a composite conductive diaphragm, comprising the following steps:

[0038] S1: adding a binder to a dispersant to obtain a glue solvent;

[0039] S2: Grinding the conductive material into dry powder;

[0040] S3: adding the dry powder into the glue solvent and mixing evenly to obtain a conductive paste;

[0041] S4: coating the conductive slurry on the diaphragm to obtain a composite conductive diaphragm.

[0042] As a further technical solution, in step S1, the binder is selected from one or more of polyvinylidene fluoride PVDF, polytetrafluoroethylene PTFE, polyacrylic acid PAA, acrylonitrile multipolymer LA132, sodium carboxymethyl cellulose CMC, and gelatin; the dispersant is one or more of N-methylpyrrolidone, water, methanol, ethanol, propanol, and isopropanol.

[0043] As a further technical solution, in step S1, the amount of the binder added is 3% to 10% of the total mass of the glue solvent.

[0044] As a further technical solution, the added amount of the binder accounts for 5% of the total mass of the glue solvent.

[0045] As a further technical solution, in step S4, the coating method is selected from one or more of gravure coating, coating, and spraying.

[0046] As a further technical solution, in step S4, the conductive paste may be coated on a single surface or both surfaces of the diaphragm.

[0047] As a further technical solution, in step S4, the membrane needs to be dried after coating, the drying temperature is 50 to 90°C, the drying form is vacuum drying, and the vacuum drying time is 2 to 24 hours.

[0048] A fourth aspect of the present invention provides a lithium battery, comprising the composite conductive separator prepared as above, disposed between a positive electrode sheet and a negative electrode sheet.

[0049] The present invention can effectively reduce the thermal shrinkage rate of the diaphragm by coating a conductive slurry coating on the surface of the diaphragm, and improve the transmission efficiency of the electrons in the positive and negative pole pieces of the battery and the rate performance of the battery. The basic diaphragm material before being coated with the conductive slurry is usually a polymer material, which will soften or even melt at high temperatures, resulting in thermal expansion and subsequent cooling shrinkage. However, after being coated with the conductive slurry coating, the thermal stability of the diaphragm can be significantly improved and the thermal shrinkage phenomenon can be reduced. This is because the conductive material has a high melting point and thermal stability. When the battery temperature rises abnormally, the conductive coating can form a thermal barrier to delay or prevent heat from being transferred to the polymer substrate inside the diaphragm, thereby inhibiting the diaphragm from undergoing large deformation and shrinkage due to high temperature.

[0050] From the perspective of microstructure regulation: the conductive carbon black used in the conductive layer is nano-scale particles, distributed on the surface of the diaphragm and in some pores. This structure can not only provide mechanical support and reduce the deformation of the basic diaphragm at high temperatures, but also limit the overall thermal shrinkage of the diaphragm due to the interaction between carbon black particles and the space barrier effect.

[0051] The present invention will be further described in detail below in conjunction with specific embodiments. It should be noted that the specific embodiments are intended to explain the present invention rather than to limit it.

[0052] Embodiment 1

[0053] This embodiment provides a composite conductive diaphragm, comprising: a diaphragm and a conductive slurry coating (5% conductive carbon black) coated on the surface of the diaphragm; wherein the thickness of the conductive slurry coating is 1500 to 3000 nanometers.

[0054] The method for preparing the composite conductive diaphragm of this embodiment comprises the following steps:

[0055] 1. Add 5% conductive carbon black into a ball mill and grind into mixed dry powder by ball mill;

[0056] 2. Add the binder PVDF into NMP and mix evenly to obtain a 5% glue solvent;

[0057] 3. Add the mixed and ground dry powder in 1 to the 5% glue solution in 2 and mix evenly to obtain a conductive paste;

[0058] 4. The conductive paste obtained by the above mixing is conveyed to the coating machine through the feeding mechanism; the conductive paste is evenly coated on the surface of the 7μm PE diaphragm by gravure coating, and the coating speed of the coating machine is 15-20m / min;

[0059] 5. Transport the coated PE diaphragm to the oven for heating, drying and rolling;

[0060] 6. Coat the back of the rolled PE diaphragm and repeat steps 4 and 5. See the structural diagram for details. Figure 1 .

[0061] Then, cut the sample size: 100mm×100mm; draw a cross along the MD and TD directions, and mark the MD and TD directions; place the film between A4 papers (1 sheet each on the top and bottom), and heat at 105°C for 1 hour; after heating, measure the length and calculate the shrinkage rate (two-dimensional test) with a film ruler; shrinkage rate % = (L0-L1) / L0*100% (L0: initial sample length).

[0062] Embodiment 2

[0063] This embodiment provides a composite conductive diaphragm, including: a diaphragm and a conductive slurry coating (2% carbon nanotubes, 3% conductive carbon black) coated on the surface of the diaphragm; wherein the thickness of the conductive slurry coating is 1500 to 3000 nanometers.

[0064] The method for preparing the composite conductive diaphragm of this embodiment comprises the following steps:

[0065] 1. Add 2% carbon nanotubes and 3% conductive carbon black into a ball mill and grind them into mixed dry powder by ball mill;

[0066] 2. Add the binder PVDF into NMP and mix evenly to obtain a 5% glue solvent;

[0067] 3. Add the mixed and ground dry powder in 1 to the 5% glue solution in 2 and mix evenly to obtain a composite conductive paste;

[0068] 4. The composite conductive paste obtained by the above mixing is conveyed to the coating machine through the feeding mechanism; the conductive paste is evenly coated on the 7 μm PE film by gravure coating, and the coating speed of the coating machine is 15-20 m / min;

[0069] 5. Transport the coated PE diaphragm to the oven for heating, drying and rolling;

[0070] 6. Coat the back of the rolled PE diaphragm and repeat steps 4 and 5. See the structural diagram for details. Figure 1 ;

[0071] Then, cut the sample size: 100mm×100mm; draw a cross along the MD and TD directions, and mark the MD and TD directions; place the film between A4 papers (1 sheet each on the top and bottom), and heat at 105°C for 1 hour; after heating, measure the length and calculate the shrinkage rate (two-dimensional test) with a film ruler; shrinkage rate % = (L0-L1) / L0*100% (L0: initial sample length).

[0072] Embodiment 3

[0073] This embodiment provides a composite conductive diaphragm, including: a diaphragm, a conductive ceramic coating coated on the surface of the diaphragm, and a conductive slurry coating (5% conductive carbon black) coated on the surface of the conductive ceramic coating.

[0074] The method for preparing the composite conductive diaphragm of this embodiment comprises the following steps:

[0075] 1. Add 5% conductive carbon black into a ball mill and grind into mixed dry powder by ball mill;

[0076] 2. Add the binder PVDF into NMP and mix evenly to obtain a 5% glue solvent;

[0077] 3. Add the mixed and ground dry powder in 1 to the 5% glue solution in 2 and mix evenly to obtain a conductive paste;

[0078] 4. The conductive paste obtained by the above mixing is conveyed to the coating machine through the feeding mechanism; the conductive paste is evenly coated on the 12 μm ceramic diaphragm by coating, and the coating speed of the coating machine is 15-20 m / min;

[0079] 5. Transport the coated ceramic diaphragm to the oven for heating, drying and rolling;

[0080] 6. Then coat the back of the rolled ceramic diaphragm and repeat steps 4 and 5. See the structural diagram for details. Figure 2 ;

[0081] Then, cut the sample size: 100mm×100mm; draw a cross along the MD and TD directions, and mark the MD and TD directions; place the film between A4 papers (1 sheet each on the top and bottom), and heat it at 130°C for 1 hour; after heating, measure the length and calculate the shrinkage rate (two-dimensional test) with a film ruler; shrinkage rate % = (L0-L1) / L0*100% (L0: initial sample length).

[0082] Embodiment 4

[0083] This embodiment provides a composite conductive diaphragm, including: a diaphragm, a conductive ceramic coating coated on the surface of the diaphragm, and a conductive slurry coating (2% carbon nanotubes, 3% conductive carbon black) coated on the surface of the conductive ceramic coating.

[0084] The method for preparing the composite conductive diaphragm of this embodiment comprises the following steps:

[0085] 1. Add 2% carbon nanotubes and 3% conductive carbon black into a ball mill and grind them into mixed dry powder by ball mill;

[0086] 2. Add the binder PVDF into NMP and mix evenly to obtain a 5% glue solvent;

[0087] 3. Add the mixed and ground dry powder in 1 to the 5% glue solution in 2 and mix evenly to obtain a composite conductive paste;

[0088] 4. The composite conductive slurry obtained by mixing the above is conveyed to a coating machine through a feeding mechanism; the conductive slurry is evenly coated on the 12 μm ceramic diaphragm by coating, and the coating speed of the coating machine is 15 to 20 m / min;

[0089] 5. Transport the coated ceramic diaphragm to the oven for heating, drying and rolling;

[0090] 6. Then coat the back of the rolled ceramic diaphragm and repeat steps 4 and 5. See the structural diagram for details. Figure 2 ;

[0091] Then, cut the sample size: 100mm×100mm; draw a cross along the MD and TD directions, and mark the MD and TD directions; place the film between A4 papers (1 sheet each on the top and bottom), and heat it at 130°C for 1 hour; after heating, measure the length and calculate the shrinkage rate (two-dimensional test) with a film ruler; shrinkage rate % = (L0-L1) / L0*100% (L0: initial sample length).

[0092] Comparative Example 1

[0093] Comparative Example 1 is different from Examples 1 and 2 in that a 12 μm PE diaphragm is used to directly perform a heat shrinkage test: the sample size is cut to 100 mm × 100 mm; a cross is drawn along the MD and TD directions, and the MD and TD directions are marked; the film is placed between A4 papers (1 sheet each on the top and bottom), and heated at 105°C for 1 hour; after heating, the length is measured to calculate the shrinkage (two-dimensional test) using a film ruler; shrinkage % = (L0-L1) / L0*100% (L0: initial sample length).

[0094] Comparative Example 2

[0095] The difference between Comparative Example 2 and Examples 3 and 4 is that the 12μm ceramic diaphragm used is directly tested for thermal shrinkage: cut the sample size: 100mm×100mm; draw a cross along the MD and TD directions, and mark the MD and TD directions; place the membrane between A4 papers (1 sheet each on the top and bottom), and heat at 130°C for 1 hour; after heating, measure the length and calculate the shrinkage (two-dimensional test) with a film ruler; Shrinkage % = (L0-L1) / L0*100% (L0: initial sample length).

[0096] Comparative Example 3

[0097] This comparative example provides a modified diaphragm, including an electronic conductive coating (graphene and acetylene black mixed coating) and an inorganic hard coating (silicon carbide coating) on ​​both surfaces of a polyethylene / polypropylene diaphragm; the mass content of graphene in the electronic conductive coating is 33%; the thickness of the electronic conductive coating is 100 μm; the thickness of the inorganic hard coating is 100 μm.

[0098] A method for preparing a modified diaphragm in this comparative example comprises the following steps:

[0099] (1) Take a polyethylene / polypropylene diaphragm, clean it with ethanol, and dry it for later use;

[0100] (2) dispersing 0.8 mg of silicon carbide powder and 0.2 mg of polytetrafluoroethylene (PTFE) in water to prepare a uniform inorganic hard material slurry;

[0101] 0.3 mg of graphene, 0.5 mg of acetylene black and 0.1 mg of polyvinylidene fluoride (PVDF) were dispersed in N-methylpyrrolidone (NMP) to prepare a uniform electronic conductive slurry;

[0102] (3) The electronic conductive slurry prepared in step (2) is coated on one surface of the polyethylene / polypropylene diaphragm by a blade coating method, and vacuum dried at 50°C for 12 hours to form a 100 μm thick electronic conductive coating; then the diaphragm is turned over, and the inorganic hard material slurry prepared in step (2) is coated on the other surface of the diaphragm by a blade coating method, and vacuum dried at 50°C for 12 hours to form a 100 μm thick inorganic hard coating, thereby obtaining a modified diaphragm.

[0103] The modified diaphragm of this comparative example was tested for heat shrinkage: the sample size was cut to 100mm×100mm; a cross was drawn along the MD and TD directions, and the MD and TD directions were marked; the film was placed between A4 papers (1 sheet each on the top and bottom), and heated at 105°C for 1 hour; after heating, the length was measured and the shrinkage rate was calculated (two-dimensional test) using a film ruler; the shrinkage rate (%) = (L0-L1) / L0*100% (L0: initial sample length).

[0104] Comparative Example 4

[0105] The difference between this comparative example and comparative example 3 is that the temperature setting when the modified diaphragm is subjected to the heat shrinkage test is different.

[0106] The specific steps are: cut the sample size: 100mm×100mm; draw a cross along the MD and TD directions, and mark the MD and TD directions; place the film between A4 papers (1 sheet each on the top and bottom), and heat it at 130°C for 1 hour; after heating, measure the length and calculate the shrinkage rate (two-dimensional test) with a film ruler; shrinkage rate % = (L0-L1) / L0*100% (L0: initial sample length).

[0107] Embodiment 5

[0108] This embodiment uses the composite conductive diaphragm prepared in Example 1 of the present invention to prepare a lithium ion battery, and the steps are as follows:

[0109] Lithium iron phosphate, conductive agent and PVDF are dissolved in NMP and stirred to form a positive electrode slurry, wherein the appropriate ratio of lithium iron phosphate, conductive agent and PVDF is 96%:1.5%:2.5%, the prepared positive electrode slurry is coated on the positive electrode collector and dried to form a positive electrode sheet, and the positive electrode sheet is rolled, slit and die-cut; graphite, conductive carbon black, CMC and SBR are dissolved in water and stirred to form a negative electrode slurry, wherein the appropriate ratio of graphite, conductive carbon black, CMC and SBR is 96.5%:0.5%:1.2%:1.8%; the stirred negative electrode slurry is coated on the negative electrode collector, dried to form a negative electrode sheet, and the negative electrode sheet is rolled, slit and die-cut; the positive electrode sheet, the negative electrode sheet, the electrolyte and the composite conductive diaphragm prepared in the above embodiment 1 are assembled into a soft-pack battery.

[0110] Embodiment 6

[0111] This embodiment uses the composite conductive diaphragm prepared in Example 2 of the present invention to prepare a lithium ion battery, and the steps are as follows:

[0112] Lithium iron phosphate, conductive agent and PVDF are dissolved in NMP and stirred to form a positive electrode slurry, wherein the appropriate ratio of lithium iron phosphate, conductive agent and PVDF is 96%:1.5%:2.5%, the prepared positive electrode slurry is coated on the positive electrode collector and dried to form a positive electrode sheet, and the positive electrode sheet is rolled, slit and die-cut; graphite, conductive carbon black, CMC and SBR are dissolved in water and stirred to form a negative electrode slurry, wherein the appropriate ratio of graphite, conductive carbon black, CMC and SBR is 96.5%:0.5%:1.2%:1.8%; the stirred negative electrode slurry is coated on the negative electrode collector, dried to form a negative electrode sheet, and the negative electrode sheet is rolled, slit and die-cut; the positive electrode sheet, the negative electrode sheet, the electrolyte and the composite conductive diaphragm prepared in the above embodiment 2 are assembled into a soft-pack battery.

[0113] Embodiment 7

[0114] This embodiment uses the composite conductive diaphragm prepared in the third embodiment of the present invention to prepare a lithium ion battery, and the steps are as follows:

[0115] Lithium iron phosphate, conductive agent and PVDF are dissolved in NMP and stirred to form a positive electrode slurry, wherein the appropriate ratio of lithium iron phosphate, conductive agent and PVDF is 96%:1.5%:2.5%, and the prepared positive electrode slurry is coated on the positive electrode collector and dried to form a positive electrode sheet, and the positive electrode sheet is rolled, slit and die-cut; graphite, conductive carbon black, CMC and SBR are dissolved in water and stirred to form a negative electrode slurry, wherein the appropriate ratio of graphite, conductive carbon black, CMC and SBR is 96.5%:0.5%:1.2%:1.8%; the stirred negative electrode slurry is coated on the negative electrode collector, dried to form a negative electrode sheet, and the negative electrode sheet is rolled, slit and die-cut; the positive electrode sheet, the negative electrode sheet, the electrolyte and the composite conductive diaphragm prepared in the above embodiment three are assembled into a soft-pack battery.

[0116] Embodiment 8

[0117] This embodiment uses the composite conductive diaphragm prepared in Example 4 of the present invention to prepare a lithium ion battery, and the steps are as follows:

[0118] Lithium iron phosphate, conductive agent and PVDF are dissolved in NMP and stirred to form a positive electrode slurry, wherein the appropriate ratio of lithium iron phosphate, conductive agent and PVDF is 96%:1.5%:2.5%, the prepared positive electrode slurry is coated on the positive electrode collector and dried to form a positive electrode sheet, and the positive electrode sheet is rolled, slit and die-cut; graphite, conductive carbon black, CMC and SBR are dissolved in water and stirred to form a negative electrode slurry, wherein the appropriate ratio of graphite, conductive carbon black, CMC and SBR is 96.5%:0.5%:1.2%:1.8%; the stirred negative electrode slurry is coated on the negative electrode collector, dried to form a negative electrode sheet, and the negative electrode sheet is rolled, slit and die-cut; the positive electrode sheet, the negative electrode sheet, the electrolyte and the composite conductive diaphragm prepared in the above embodiment 4 are assembled into a soft-pack battery.

[0119] Comparative Example 5

[0120] This example uses the composite conductive diaphragm prepared in Comparative Example 1 of the present invention to prepare a lithium ion battery, and the steps are as follows:

[0121] Lithium iron phosphate, conductive agent and PVDF are dissolved in NMP and stirred to form a positive electrode slurry, wherein the appropriate ratio of lithium iron phosphate, conductive agent and PVDF is 96%:1.5%:2.5%, the prepared positive electrode slurry is coated on the positive electrode collector and dried to form a positive electrode sheet, and the positive electrode sheet is rolled, slit and die-cut; graphite, conductive carbon black, CMC and SBR are dissolved in water and stirred to form a negative electrode slurry, wherein the appropriate ratio of graphite, conductive carbon black, CMC and SBR is 96.5%:0.5%:1.2%:1.8%; the stirred negative electrode slurry is coated on the negative electrode collector, dried to form a negative electrode sheet, and the negative electrode sheet is rolled, slit and die-cut; the positive electrode sheet, the negative electrode sheet, the electrolyte and the composite conductive diaphragm prepared in the above comparative example 1 are assembled into a soft-pack battery.

[0122] Comparative Example 6

[0123] This example uses the composite conductive diaphragm prepared in Comparative Example 2 of the present invention to prepare a lithium ion battery, and the steps are as follows:

[0124] Lithium iron phosphate, conductive agent and PVDF are dissolved in NMP and stirred to form a positive electrode slurry, wherein the appropriate ratio of lithium iron phosphate, conductive agent and PVDF is 96%:1.5%:2.5%, and the prepared positive electrode slurry is coated on the positive electrode collector and dried to form a positive electrode sheet, and the positive electrode sheet is rolled, slit and die-cut; graphite, conductive carbon black, CMC and SBR are dissolved in water and stirred to form a negative electrode slurry, wherein the appropriate ratio of graphite, conductive carbon black, CMC and SBR is 96.5%:0.5%:1.2%:1.8%; the stirred negative electrode slurry is coated on the negative electrode collector, dried to form a negative electrode sheet, and the negative electrode sheet is rolled, slit and die-cut; the positive electrode sheet, the negative electrode sheet, the electrolyte and the composite conductive diaphragm prepared in the above comparative example 2 are assembled into a soft-pack battery.

[0125] Performance Testing

[0126] This example tests the performance of the composite conductive diaphragm and lithium ion battery prepared in the examples of the present invention and the comparative examples. The specific operating steps and operating parameters are as follows:

[0127] Thermal shrinkage test: The diaphragms in Examples 1 to 4 and Comparative Examples 1 to 4 were subjected to thermal shrinkage tests;

[0128] Discharge rate test: The lithium ion batteries prepared in Examples 5 to 8 and Comparative Examples 5 and 6 were charged to 3.65V at a current of 0.5C, constant current and constant voltage, and then charged at a constant voltage until the current dropped to 0.05C and then discharged to 2.0V at currents of 0.33C, 1.0C, and 2.0C, respectively. The discharge capacity at different discharge rates was recorded, and the discharge capacity at 0.33C was taken as 100%, and the corresponding battery capacity retention rate was calculated. Battery capacity retention rate at a certain discharge rate = (discharge capacity at the discharge rate / discharge capacity at 0.33C) × 100%.

[0129] Table 1 Test data of thermal shrinkage of composite conductive diaphragm

[0130] Shrinkage (105℃ / 1h) Shrinkage (130℃ / 1h) Embodiment 1 MD: 2.25%; TD: 1.09% Embodiment 3 MD: 0.97%; TD: 0.83% Embodiment 2 MD: 2.19%; TD: 1.02% Embodiment 4 MD: 0.94%; TD: 0.82% Comparative Example 1 MD: 3.82%; TD: 2.3% Comparative Example 2 MD: 1.2%; TD: 1.0% Comparative Example 3 MD: 2.33%; TD: 1.15% Comparative Example 4 MD: 1.04%; TD: 0.89%

[0131] Table 2 Capacity retention rate of composite conductive separator at different discharge rates

[0132]

[0133]

[0134] It can be seen from Table 1 that the thermal shrinkage test results of the composite diaphragms prepared in Examples 1 to 4 of the present invention and the diaphragms in Comparative Examples 1 to 4 are analyzed: in this embodiment, the thermal shrinkage of the diaphragm can be reduced by coating a layer of conductive slurry on the surface of the diaphragm.

[0135] It can be seen from Table 2 that by analyzing the test results of different rates on the battery cells prepared in Examples 5 to 8 of the present invention and the battery cells prepared in Comparative Examples 5 and 6, the preparation of the novel composite conductive diaphragm involved in the present invention can improve the rate performance of the battery.

[0136] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to perform equivalent replacements on parts thereof. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention. Although the above describes the specific implementation methods of the present invention, it is not intended to limit the protection scope of the present invention. Those skilled in the art should understand that, based on the technical solution of the present invention, various modifications or deformations that can be made by those skilled in the art without creative labor are still within the protection scope of the present invention.

Claims

1. A composite conductive diaphragm, characterized in that: The composite conductive diaphragm comprises: a diaphragm and a conductive slurry coating, wherein the conductive slurry coating is coated on the surface of the diaphragm and has a thickness of 1500 to 3000 nanometers; wherein the conductive slurry coating is a coating containing a conductive material, and the total mass content of the conductive material is 5%.

2. A composite conductive diaphragm, characterized in that: The composite conductive diaphragm includes: a diaphragm, a conductive ceramic coating and a conductive slurry coating, wherein the conductive ceramic coating is coated on the surface of the diaphragm, and the conductive slurry coating is coated on the surface of the conductive ceramic coating, and the thickness of the conductive ceramic coating and the conductive slurry coating are both 1500 to 3000 nanometers; wherein the conductive slurry coating is a coating containing a conductive material; and the total mass content of the conductive material is 5%.

3. The composite conductive diaphragm according to any one of claims 1 to 2, characterized in that: The conductive material is selected from one or more of conductive carbon black, Ketjen black, conductive graphite, vapor deposited carbon nanofibers, and carbon nanotubes; the material of the diaphragm is selected from one or more of polypropylene diaphragms, polyethylene diaphragms, cellulose diaphragms, ceramic diaphragms, non-woven fabrics, and aramid.

4. A method for preparing the composite conductive diaphragm according to claim 1, characterized in that: The following steps are involved: S1: adding a binder to a dispersant to obtain a glue solvent; S2: Grinding the conductive material into dry powder; S3: adding the dry powder into the glue solvent and mixing evenly to obtain a conductive paste; S4: coating the conductive slurry on the diaphragm to obtain a composite conductive diaphragm.

5. The preparation method according to claim 4, characterized in that: In step S1, the binder is selected from one or more of polyvinylidene fluoride, polytetrafluoroethylene, polyacrylic acid, acrylonitrile multipolymer, sodium carboxymethyl cellulose, and gelatin; the dispersant is one or more of N-methylpyrrolidone, water, methanol, ethanol, propanol, and isopropanol.

6. The preparation method according to claim 4, characterized in that: In step S1, the amount of the binder added is 3% to 10% of the total mass of the glue solvent; preferably, the amount of the binder added is 5% of the total mass of the glue solvent.

7. The preparation method according to claim 4, characterized in that: In step S4, the membrane needs to be dried after coating, the drying temperature is 50 to 90°C, the drying method is vacuum drying, and the vacuum drying time is 2 to 24 hours.

8. The preparation method according to claim 4, characterized in that: In step S4, the coating method is selected from one or more of gravure coating, coating, and spraying.

9. The preparation method according to claim 4, characterized in that: In step S4, the conductive paste is coated on a single surface or both surfaces of the diaphragm.

10. A lithium battery, characterized in that: The lithium battery comprises the composite conductive diaphragm according to any one of claims 1 to 3, and further comprises: a positive electrode sheet, a negative electrode sheet and an electrolyte, and the composite conductive diaphragm is arranged between the positive electrode sheet and the negative electrode sheet.

Citation Information

Patent Citations

  • Battery separator, preparation method thereof and lithium ion battery

    CN112117420A

  • Battery separator, preparation method thereof and lithium ion battery

    CN112117421A