Aluminum honeycomb core etching method and clamping device
By using alkaline or acidic corrosive liquids and clamping devices, the problem of heat dissipation and energy absorption continuity in aluminum honeycomb core etching is solved, precise etching of aluminum honeycomb core wall thickness and improvement of energy absorption performance are achieved, which is suitable for high requirements. application.
Patent Information
- Application Number
- CN202210958520.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-09
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-08-09
AI Technical Summary
During the etching process of the aluminum honeycomb core, the heat is difficult to dissipate, resulting in local overburning, the reaction is difficult to control, and the energy absorption continuity is not ideal. The existing technology cannot meet the high energy absorption demand.
Alkaline or acidic corrosive liquid is used for etching, and the reaction rate and environment are controlled by sodium hydroxide, sodium carbonate, aluminum hydroxide and other ingredients, combined with a clamping device to support and stabilize the aluminum honeycomb core, and control the etching rate and environment.
It achieves precise etching of the wall thickness of the aluminum honeycomb core, improves the continuity and stability of the energy-absorbing performance, and is suitable for high-demand applications such as aerospace. It reduces energy-absorbing damage and ensures the controllability and safety of the reaction. .
Smart Images

Figure CN115287658B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of aluminum honeycomb core etching, and is an aluminum honeycomb core etching method and a clamping device. Background Art
[0002] The conventional aluminum honeycomb core structure is similar to the honeycomb structure. It is made of aluminum foil and adhesive according to a certain process. The pore size and wall thickness of the regular hexagonal structure can be changed according to different requirements. The countless I-beam structures make it have good flatness, high strength, good heat and sound insulation, light weight, stable energy absorption, etc. It is widely used in aerospace, rail transportation and other fields.
[0003] Conventional aluminum honeycomb core structure Figure 1 Aluminum foil, W is the lateral width perpendicular to the rubber strip, L is the longitudinal width parallel to the rubber strip, its wall thickness is 0.02mm-0.1mm, the size of the regular hexagonal core cell is between 1mm-30mm, and the thickness T can be controlled between 2mm-500mm according to actual use requirements; although the aluminum honeycomb core has good pressure bearing and energy absorption effects, and good energy absorption stability, the requirements for energy absorption performance have become increasingly higher in recent years. For different requirements, the energy absorption continuity of the aluminum honeycomb core is not ideal.
[0004] In addition, during the etching process of the aluminum honeycomb core, the entire chemical reaction is an exothermic reaction. Each core cell of the aluminum honeycomb core is very long and has only two exits. During the etching process, it is difficult for the heat to dissipate, which will cause local overburning. If the local reaction is too intense, the gas generated during the entire reaction process will overflow in large quantities, making the reaction process difficult to control, and even causing the reaction to boil, causing a frying pan. At present, it is very easy to corrode the aluminum foil wall or corrode it completely during the etching process. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides an etching method and a clamping device for an aluminum honeycomb core, which is not only suitable for lightweight and special-shaped honeycomb structures, but also suitable for structures with various energy absorption requirements and honeycomb structure requirements for special performance purposes.
[0006] The present invention is achieved through the following technical solutions:
[0007] An etching method for an aluminum honeycomb core comprises the following steps:
[0008] Step 1, first immerse the aluminum honeycomb core to be etched in an alkaline etching solution or an acidic etching solution, then take out the obtained aluminum honeycomb core and leave it in the air for several seconds, wherein the alkaline etching solution comprises, by mass percentage, 4%-6% sodium hydroxide, 25%-35% sodium carbonate, 40%-45% sodium bicarbonate, 1.5%-2% aluminum hydroxide, and the rest is deionized water, and the acidic etching solution comprises, by mass percentage, 5.85%-8.1% nitric acid, 42.5%-51% phosphoric acid, 9.9%-14.85% acetic acid, 2%-4% aluminum nitrate, and the rest is deionized water;
[0009] Step 2: Repeat the process described in step 1 several times to obtain an etched aluminum honeycomb core.
[0010] Preferably, the temperature of the alkaline or acidic corrosive solution in step 1 is 35-45°C.
[0011] Preferably, in step 1, the alkaline corrosive solution or the acidic corrosive solution is stored in a tank, and compressed air is introduced into the bottom of the tank.
[0012] Furthermore, the intake volume of the compressed air is 0.8-1m 3 / min.
[0013] Preferably, in step 1, the aluminum honeycomb core to be etched is immersed in the alkaline or acidic etching solution for 3-5 minutes and then taken out.
[0014] Preferably, in step 1, the obtained aluminum honeycomb core is taken out and allowed to remain in the air for 3-10 seconds.
[0015] Preferably, in step 1, the aluminum honeycomb core to be etched is clamped and installed on a traveling crane, and the aluminum honeycomb core is allowed to move freely up and down by the traveling crane.
[0016] A clamping device for an aluminum honeycomb core comprises a support frame and a pressing plate;
[0017] The support frame comprises an upper rectangular frame and a lower rectangular frame of the same shape, the width formed by the inner wall of the upper rectangular frame is greater than or equal to the width of the aluminum honeycomb core, the length formed by the inner wall of the upper rectangular frame is greater than or equal to the length of the aluminum honeycomb core, the four corners of the upper rectangular frame and the lower rectangular frame are fixedly connected by support columns, the width direction of the lower end of the lower rectangular frame is uniformly and spaced along the length direction of the lower rectangular frame, and the U-shaped frame is formed by bending a polytetrafluoroethylene plate;
[0018] The width of the pressing plate is equal to the width of the aluminum honeycomb core, and the length is equal to the length of the aluminum honeycomb core. The aluminum honeycomb core is placed on the upper surface of the U-shaped frame in the vertical direction, and the pressing plate is placed on the upper surface of the aluminum honeycomb core.
[0019] Furthermore, the upper rectangular frame, the lower rectangular frame, the support column and the pressing plate are all made of stainless steel.
[0020] Furthermore, a plurality of handrails are horizontally symmetrically fixed to the outer side of the upper rectangular frame in the width direction along the length direction of the upper rectangular frame. The handrails are distributed at both ends of the upper rectangular frame in the width direction, and the handrails in the length direction of the upper rectangular frame are symmetrically arranged.
[0021] Compared with the prior art, the present invention has the following beneficial technical effects:
[0022] The present invention provides an etching method for an aluminum honeycomb core, wherein the honeycomb core wall thickness is etched as required. Due to the special properties of aluminum, it can react with both acid and strong alkaline solution, so an alkaline etching solution or an acidic etching solution is used. The sodium hydroxide in the alkaline etching solution ensures a strong alkalinity, and the main function of sodium carbonate and sodium bicarbonate is to control the entire reaction rate, prevent the reaction from being too violent, and affect the effect of the aluminum honeycomb core, while continuously releasing OH - Ions ensure an alkaline environment for the entire process. Aluminum hydroxide is to ensure a smooth reaction and provide aluminum ions in the entire solution in advance. Nitric acid in the acidic corrosive solution ensures that the entire solution is strongly acidic. Phosphoric acid and acetic acid are mainly used to control the reaction rate while continuously releasing H + Ions ensure the acidic environment of the whole process. Aluminum nitrate provides aluminum ions in the whole solution in advance for the smooth reaction. The etching method can meet the honeycomb structure used in industries such as aerospace, rail transportation, automobile safety, and electronic information, which has high requirements for weight control and volume but low requirements for strength. The original single honeycomb and laminated honeycomb energy absorption can be used in the present invention to achieve smooth curve transition, reduce the damage caused by stage energy absorption, and can be used for personnel and precision instrument protection, energy absorption during collision, landing of spacecraft, etc.
[0023] The present invention provides a clamping device for an aluminum honeycomb core. The aluminum honeycomb core is installed in a support frame, and the aluminum honeycomb core can directly contact a U-shaped frame, which can prevent the stainless steel support frame from damaging the aluminum honeycomb core during operation. The aluminum honeycomb core is placed in a lower rectangular frame in a vertical direction, and the U-shaped frame supports the aluminum honeycomb core in the support frame. The pressure plate clamps the aluminum honeycomb core through the pressure generated by gravity, which can ensure that the aluminum honeycomb core does not shake during overall movement. The device has a certain structural stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Schematic diagram of the structure of aluminum honeycomb core.
[0025] Figure 2 This is a schematic diagram of the structure of the aluminum honeycomb core holding device of the present invention.
[0026] Figure 3This is a cross-sectional view of the aluminum honeycomb core after being supported by the aluminum honeycomb core supporting device described in the present invention.
[0027] Figure 4 This is the mechanical properties curve of normal honeycomb core.
[0028] Figure 5 This is a mechanical property curve diagram of the honeycomb core treated with alkaline corrosive solution according to Example 1 of the present invention.
[0029] In the figure: 1-support frame, 2-pressing plate, 3-aluminum honeycomb core. DETAILED DESCRIPTION
[0030] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.
[0031] The present invention discloses a high-precision etching method for changing the energy absorption performance of an aluminum honeycomb core, wherein the alkaline etching solution comprises, by mass percentage, sodium hydroxide (4%-6%), sodium carbonate (25%-35%), sodium bicarbonate (40%-45%), aluminum hydroxide (1.5%-2%), and the remainder is deionized water. The sodium hydroxide ensures a strong alkalinity, and the main functions of sodium carbonate and sodium bicarbonate are to control the entire reaction rate, prevent the reaction from being too violent, and affect the effect of the aluminum honeycomb core, while continuously releasing OH - Ions ensure the alkaline environment of the whole process, and aluminum hydroxide is to make the whole reaction smooth and provide aluminum ions in the whole solution in advance.
[0032] The acidic etching solution has the following components, by mass percentage: commercially available chemically pure nitric acid (13%-18%) with a purity of 45%, chemically pure phosphoric acid (50%-60%) with a purity of 85%, commercially available chemically pure acetic acid (9.9%-14.85%) with a purity of 99%, aluminum nitrate 2%-4%, and the remainder being deionized water.
[0033] Nitric acid ensures the strong acidity of the entire solution, while phosphoric acid and acetic acid are mainly used to control the reaction rate and continuously release H + Ions ensure the acidic environment of the entire process. In order for the entire reaction to proceed smoothly, aluminum nitrate provides aluminum ions in the entire solution in advance.
[0034] Since the alkaline corrosion reaction and the acid corrosion reaction process of the present invention are both exothermic reactions, the higher the temperature of the chemical reaction process, the faster the etching rate. The reaction temperature of the design is 35-45°C. The composition of the alkaline corrosion solution and the acid corrosion solution, as well as whether the etching process is stirred or not, will affect the etching rate. The stirring is pneumatic stirring, and the air intake is 0.8-1m 3 / min, the etching rate can be controlled to (1-3)×10 -2g / mm / min (aluminum consumption). Ensure that the entire process is controllable. The aluminum foil used to make aluminum honeycombs is relatively thin, generally less than 0.1mm thick. In order to avoid corroding the aluminum foil wall or corroding it completely, take the object out of the liquid surface every 3-5 minutes, and repeat after 3-10 seconds.
[0035] Since the current honeycomb sizes are relatively large, with a height of 300-500mm, a length and width of 250-700mm, and the shape is difficult to fix, the entire process is completed below the liquid surface, and the aluminum honeycomb core is easy to deform after being unfolded. In order to overcome the effects of buoyancy, strong acidity and the intensity of the reaction process in the liquid, it is necessary to use Figure 2 The device shown provides clamping and ensures shape stability.
[0036] The clamping device is mainly composed of a support frame 1 and a pressing plate 2. The support frame 1 includes an upper rectangular frame and a lower rectangular frame of the same shape. The width formed by the inner wall of the upper rectangular frame is greater than or equal to the width of the aluminum honeycomb core 3, and the length formed by the inner wall of the upper rectangular frame is greater than or equal to the length of the aluminum honeycomb core 3. The width of the pressing plate 2 is equal to the width of the aluminum honeycomb core 3, and the length is equal to the length of the aluminum honeycomb core 3. The upper rectangular frame and the lower rectangular frame are fixedly connected by four support columns with L-shaped cross sections. The upper rectangular frame, the lower rectangular frame, the support columns and the pressing plate 2 are all made of stainless steel. The width direction of the lower end of the lower rectangular frame is uniformly and spaced along the length direction of the lower rectangular frame. The U-shaped frame with the opening facing downward is arranged at intervals. The U-shaped frame is formed by bending a polytetrafluoroethylene plate. In this way, when the aluminum honeycomb core 3 is loaded into the support frame 1, the aluminum honeycomb core 3 directly contacts the U-shaped frame, which can prevent the stainless steel support frame 1 from damaging the aluminum honeycomb core 3 during operation. The device has certain structural stability and corrosion resistance requirements.
[0037] like Figure 3As shown, the aluminum honeycomb core 3 is placed in the lower rectangular frame in a vertical direction, and several U-shaped frames support the aluminum honeycomb core 3 in the support frame 1. The pressure plate 2 is placed on the upper surface of the aluminum honeycomb core 3. The pressure plate 2 clamps the aluminum honeycomb core 3 through the pressure generated by gravity, which can ensure that the aluminum honeycomb core 3 does not shake during the overall movement. Four cylindrical handrails are symmetrically welded horizontally outward on the outer side of the width direction of the upper rectangular frame. Each handrail is distributed at both ends of the width direction of the upper rectangular frame. The handrails in the length direction of the upper rectangular frame are symmetrically arranged, which is convenient for the staff to hold by hand to keep the support frame 1 balanced before moving. A U-shaped handle is fixed on the upper surface of the two sides in the width direction of the upper rectangular frame. The center of the U-shaped handle is located at the center of the corresponding straight side of the upper rectangular frame. A cylindrical connecting column is fixed at both ends of the inner side of each U-shaped handle, and the connecting column is located above the U-shaped handle. The support frame 1 can be connected to the overhead crane as a whole through the U-shaped handle and the connecting column. The aluminum honeycomb core 3 is generally 300-500mm in height, 250-700mm in length and width. It is manually loaded into the support frame 1, and then the pressing plate 2 clamps the aluminum honeycomb core 3 by pressure, which is convenient for loading and unloading. The aluminum honeycomb core 3 can move freely up and down by a crane.
[0038] During the whole process, compressed air needs to be pumped into the bottom of the tank to play a dual role of cooling and stirring, effectively controlling the degree of reaction.
[0039] When the present invention uses alkaline etching solution to perform high-precision etching on the aluminum honeycomb core, the main reaction equation is: 2Al+2H2O+2OH - =2AlO2 - +3H2↑, specifically includes the following steps:
[0040] 1. Turn on the existing environmental protection equipment, ensure the handling of hazardous substances during the whole process, and operators wear safety protection equipment to prevent possible unsafe incidents.
[0041] 2. Prepare 1000kg of alkaline corrosive liquid according to the previous composition ratio of the alkaline corrosive liquid, then pour it into the liquid storage tank, and use a crane to immerse the aluminum honeycomb core in the alkaline corrosive liquid. To ensure the stability of the corrosion rate of the corrosive liquid, measure the corrosion rate every 8 hours according to production needs.
[0042] 3. Every 3-5 minutes, lift the aluminum honeycomb core out of the liquid surface and keep it there for 3-10 seconds. This is mainly to make the concentration of the alkaline corrosive liquid and the temperature of the liquid in the storage tank uniform.
[0043] 4. According to the target energy absorption performance, the corresponding processing time is obtained. After that, the etching is repeated for a corresponding number of times according to the required energy absorption performance each time. The aluminum honeycomb core is removed and cleaned and dried as required.
[0044] 5. In order to further ensure the quality, the aluminum honeycomb core needs to be regularly inspected to ensure that its energy absorption performance meets the requirements.
[0045] When the present invention uses an acidic etching solution to perform high-precision etching on the aluminum honeycomb core, the main reaction equation is: 2Al+6H + =2Al 3+ +3H2↑, specifically includes the following steps:
[0046] 1. Turn on the existing environmental protection equipment to ensure the treatment of harmful substances during the whole process. Operators must wear safety protection equipment to prevent the volatile acid mist from entering the human body and the generated hydrogen from being discharged.
[0047] 2. Prepare 1000kg of acidic corrosive liquid according to the composition ratio of the previous acidic corrosive liquid, then pour it into the liquid storage tank, and use a crane to immerse the aluminum honeycomb core in the acidic corrosive liquid. To ensure the stability of the corrosion rate of the corrosive liquid, measure the corrosion rate every 8 hours according to production needs.
[0048] 3. Every 3-5 minutes, lift the aluminum honeycomb core out of the liquid surface and keep it there for 3-10 seconds. This is mainly to make the concentration of the acidic corrosive liquid and the temperature of the liquid in the storage tank uniform.
[0049] 4. According to the target energy absorption performance, the corresponding processing time is obtained. After that, the etching is repeated for a corresponding number of times according to the required energy absorption performance each time. The aluminum honeycomb core is removed and cleaned and dried as required.
[0050] 5. In order to further ensure the quality, samples need to be inspected regularly to ensure that their energy absorption performance meets the requirements.
[0051] During the entire reaction process, the acidic corrosive liquid will produce a pungent odor due to the intensity of the reaction, so attention should be paid to safety protection during the process.
[0052] After being treated with the above alkaline / acidic corrosive liquid, the wall thickness of the aluminum honeycomb will change greatly: the wall thickness of the honeycomb can be weakened, thereby changing the energy absorption performance of the aluminum honeycomb.
[0053] Example 1
[0054] The present invention etches an aluminum honeycomb core with a specific alkaline etching solution, wherein
[0055] Sodium hydroxide 5%, sodium carbonate 30%, sodium bicarbonate 40%, aluminum hydroxide 2%, and the rest is deionized water.
[0056] The reaction temperature is 40℃ and the air intake volume of the pneumatic stirring is 1m 3 / min, take out the aluminum honeycomb core every 4min, keep it in the air for 4s, repeat 5 times, and control the etching rate to 2×10 -2g / mm / min. Figure 5 The performance curve after treatment is shown in Figure 1. The performance curve of normal cellular is shown in Figure 2. Figure 4 As shown. Figure 4 As shown in the figure, due to the excellent pressure-bearing property of the honeycomb core material, when the external force reaches the maximum pressure-bearing strength of the honeycomb core, the honeycomb core will suddenly become unstable, and then become uniform in strength as the pressure and displacement change. The subsequent strength is also relatively stable, with a fluctuation within ±10%. Figure 5 As shown, the maximum pressure bearing strength of the honeycomb is eliminated, and any required value in the range from zero to the maximum value can be achieved through process adjustment. Therefore, the honeycomb core process can be controlled according to the requirements of the storage environment. The whole process can ensure that the performance fluctuation of the honeycomb core is within ±5%, thereby better ensuring the stability of the honeycomb core energy.
[0057] The above process can also be carried out by using an acidic etching solution with the following components instead of the alkaline etching solution: 6% nitric acid, 50% phosphoric acid, 15% acetic acid, 4% aluminum nitrate, and the remainder is deionized water. Figure 5 About the same.
Claims
1. An etching method for an aluminum honeycomb core, characterized in that: The aluminum honeycomb core has a height of 300-500 mm, a length and a width of 250-700 mm, a wall thickness of 0.02 mm-0.1 mm, and a regular hexagonal core cell size of 1 mm-30 mm, and comprises the following steps: Step 1: First, clamp the aluminum honeycomb core to be etched with a clamping device and install it on a crane. The aluminum honeycomb core is allowed to move freely up and down by the crane. Then, it is immersed in an alkaline or acidic corrosive solution at 35-45°C for 3-5 minutes. The alkaline or acidic corrosive solution is stored in a tank. Then, compressed air is introduced into the bottom of the tank for pneumatic stirring. The air intake is 0.8-1m 3 / min, then take out the obtained aluminum honeycomb core and leave it in the air for 3-10s, the alkaline etching solution comprises, by mass percentage, 4%-6% sodium hydroxide, 25%-35% sodium carbonate, 40%-45% sodium bicarbonate, 1.5%-2% aluminum hydroxide, and the rest is deionized water, the acidic etching solution comprises, by mass percentage, 5.85%-8.1% nitric acid, 42.5%-51% phosphoric acid, 9.9%-14.85% acetic acid, 2%-4% aluminum nitrate, and the rest is deionized water; Step 2: Repeat the process described in step 1 several times, controlling the etching rate to (1-3)×10 -2 g / mm / min, ensuring that the performance fluctuation of the honeycomb core is within ±5%, and obtaining the etched aluminum honeycomb core; The clamping device comprises a support frame (1) and a pressing plate (2); the support frame (1) comprises an upper rectangular frame and a lower rectangular frame of the same shape, the width formed by the inner wall of the upper rectangular frame is greater than or equal to the width of the aluminum honeycomb core (3), the length formed by the inner wall of the upper rectangular frame is greater than or equal to the length of the aluminum honeycomb core (3), the four corners of the upper rectangular frame and the lower rectangular frame are fixedly connected by support columns, the lower end of the lower rectangular frame is evenly and spacedly arranged with U-shaped frames with openings facing downwards in the width direction along the length direction of the lower rectangular frame, the U-shaped frames are formed by bending polytetrafluoroethylene plates, the upper rectangular frame, the lower rectangular frame, the supporting columns and the pressing plate (2) are all made of stainless steel, a plurality of handrails are horizontally symmetrically fixed to the outer side of the width direction of the upper rectangular frame along the length direction of the upper rectangular frame, the handrails are distributed at both ends of the width direction of the upper rectangular frame, and the positions of the handrails in the length direction of the upper rectangular frame are symmetrically arranged; The width of the pressing plate (2) is equal to the width of the aluminum honeycomb core (3), and the length is equal to the length of the aluminum honeycomb core (3). The aluminum honeycomb core (3) is placed on the upper surface of the U-shaped frame in the vertical direction, and the pressing plate (2) is placed on the upper surface of the aluminum honeycomb core (3).