Porous membranes containing adsorbent particles for improved urea capture

By embedding urea adsorbent particles in the membrane, the adsorption capacity and kinetics of urea are improved, the problem of low urea removal efficiency in the existing technology is solved, and efficient urea removal suitable for small artificial kidney devices is achieved.

CN115297953BActive Publication Date: 2024-10-15UMC UTRECHT HLDG GMBH +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080091823.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-11-22
Filing Date
2020-11-20
Publication Date
2024-10-15
Estimated Expiration
2040-11-20

AI Technical Summary

Technical Problem

It is difficult to effectively remove urea with existing technology, which limits the proportion of miniaturization to truly wearable devices, and has become one of the main obstacles to the realization of small artificial kidney devices.

Method used

Urea adsorbent particles embedded in a porous membrane matrix are used to improve the adsorption capacity and binding kinetics of urea, and the adsorption performance of the membrane is enhanced through the embedded particulate materials.

Benefits of technology

It achieves higher urea binding capacity and faster binding kinetics, which is suitable for use in dialysis devices, improving the efficiency of urea removal and the wearability of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003728062250000141
    Figure BDA0003728062250000141
  • Figure BDA0003728062250000151
    Figure BDA0003728062250000151
  • Figure BDA0003728062250000241
    Figure BDA0003728062250000241
Patent Text Reader

Abstract

The present invention relates to a method for preparing a membrane comprising adsorbent particles bound to urea. The invention also relates to the membrane itself comprising the adsorbent, and to methods of using the membrane. The membrane is used for subsequent reactions with small molecules such as urea, for example to remove urea from a solution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for preparing a membrane comprising adsorbent particles bound to urea. The invention also relates to the membrane itself comprising the adsorbent, and to methods of using the membrane. The membrane is used for subsequent reactions with small molecules such as urea, for example to remove urea from a solution. Background Art

[0002] Patients with end-stage renal disease (ESKD) or severe acute renal failure undergo dialysis (hemodialysis or HD or peritoneal dialysis or PD) to replace kidney function. Although life-saving, conventional dialysis has serious disadvantages. The treatment is time-consuming, and the removal of waste molecules and excess water is inadequate, significantly leading to low quality of life, serious health problems and high mortality (15-20% per year). The cost of treatment is very high.

[0003] In dialysis, patient fluid is typically dialyzed with a dialysis fluid, which is then discarded. It is desirable to regenerate the dialysate to allow for the use of smaller volumes. In an attempt at miniaturization, patient fluid is dialyzed with a relatively small amount of dialysis fluid, which is referred to as dialysate. During this process, waste solutes from the patient fluid move toward the dialysate by diffusion and / or convection, typically through a membrane such as a semipermeable membrane. If the waste solutes are later removed from the dialysate, they can be reused, which is referred to as regeneration of the dialysate. Efficient regeneration of the dialysate would reduce the need for large volumes of dialysate, making dialysis more practical to implement, less resource-dependent, and reducing waste streams.

[0004] A miniature artificial kidney device would be a major breakthrough in renal replacement therapy. The number of dialysis patients worldwide is estimated to be 3.4 million (see www.fresenius.com / media-library / Fresenius_Annual_Report_2018.pdf). Currently, approximately 89% of dialysis patients use HD technology, either in a center (>96%) or at home (<4%) (see ERA-EDTA Registration Annual Report 2017). In-center HD requires long-term and frequent visits to the hospital (approximately 3 times a week, 4 hours each time), while home HD provides more flexibility and autonomy. However, home HD still requires a bulky dialysis machine and a large supply of dialysate (at least 20L per treatment or a bulky fixed water purification system. A user-friendly, lightweight HD device independent of a fixed water source or a large supply of dialysate will increase the mobility of patients, allowing them to remain active in social life and travel freely.

[0005] The large fluctuations between water balance and uremic toxin levels during dialysis treatment with standard three times weekly HD can be attenuated with continuous or more frequent HD, which can improve the patient's condition (Nesrallah GE et al., J Am Soc Nephrol 2012; 23: 696-705; Susantitaphong P et al., Am J Kidney Dis 2012; 59: 689-99; Ting GO et al., Am J Kidney Dis 2003; 42: 1020-35). Allowing for more liberal diet. Significant cost reductions will be achieved by reducing the need for dialysis staff and related infrastructure, reducing medications and reducing hospitalizations due to reduced comorbidities.

[0006] Currently, approximately 11% of dialysis patients use PD (see Fresenius 2018 report). Although PD provides the opportunity for continuous dialysis compared to HD, the technology has some major disadvantages: low clearance of uremic toxins (Evenepoel P et al., Kidney Int 2006; 70: 794-9), time-consuming exchange procedures, and high technical failure rates (median technical survival is 3.7 years) due to high incidences of peritoneal infection (peritonitis) and membrane failure (Perl J et al., Clin J Am Soc Nephrol 2012; 7: 1145-54). The low dialysis efficacy is mainly due to the rapid dissipation of the concentration gradient between plasma and peritoneal dialysis fluid during the stay, thereby limiting solute transport (Gotch FA. Kinetic modeling of continuous flow peritoneal dialysis. Semin Dial 2001; 14: 378-83). A miniature PD device that continuously regenerates the dialysate and maintains the plasma-dialysate concentration gradient will greatly enhance the efficacy of PD. This will allow a reduction in the number of time-consuming exchanges while still improving waste solute removal. In addition, reducing the number of connections reduces the risk of contamination and reduces peritonitis rates (De Fijter CW, et al., Adv Perit Dial 1991; 7: 186-9; Piraino B, Sheth H Blood Purif 2010; 29: 145-9). Continuous glucose infusion by a micro PD device will reduce the functional degradation of the peritoneum by avoiding very high toxic glucose concentrations as used in conventional PD (Gotch 2001). By preventing the two main causes of technical failure in conventional PD (recurrent infection and loss of function of the peritoneum), the micro artificial kidney will significantly prolong technical survival.

[0007] Therefore, a user-friendly wearable or portable dialysis device that provides dialysis outside of the hospital would represent a quantum leap for dialysis patients and would significantly improve their quality of life. The device would allow for continuous or more frequent dialysis, which would improve the removal of waste solutes and excess fluids and, therefore, improve patient health. A miniaturized design that is independent of a fixed water supply provides freedom and autonomy to the patient.

[0008] In recent years, small prototype dialysis devices have been constructed that adequately remove some organic waste solutes and waste ions. However, to date, there is no adequate strategy for the removal of urea to allow miniaturization to truly wearable proportions, which is one of the major obstacles to the successful realization of a small artificial kidney device. Urea is the waste solute with the highest daily production (the major waste product of nitrogen metabolism) and produces toxic effects at high plasma concentrations. However, urea is difficult to bind and has low reactivity.

[0009] Adsorbents particularly suitable as urea adsorbents have long been known. DE2305186A1 / US3933753A discloses a macromolecular composition having a polystyrene-type scaffold characterized by a glyoxal moiety. The composition captures up to 1 mmol / g of urea. Further developed as described in US4012317, WO2004078797A1 discloses a similar ketoaldehyde material, achieving a urea binding capacity of 1.5 mmol / g.

[0010] EP121275A1 / US4897200A discloses a ninhydrin-based adsorbent. At clinically relevant urea concentrations, a urea binding capacity of 1.2 mmol / g dry adsorbent was shown within 8 hours. However, for effective miniaturization, a higher urea binding capacity is required. WO2019110557 discloses a ninhydrin-based adsorbent having a urea binding capacity of more than 2 mmol / g.

[0011] US4178241A discloses a polystyrene-based adsorbent with p-sulfur, p-nitro or p-amino moieties. For the sulfo moieties, urea binding was again shown to be about 1.5 mmol / g. Likewise, for each functional group, creatinine was shown to bind well over 90% of the normal adult daily production.

[0012] Membranes are known for filtration, and membranes for removing urea have also been proposed. WO2017116515A1 discloses the use of charged membranes to improve the separation of urea from dialysate, and suggests the use of electro-oxidative separation of urea. A disadvantage of this method is the generation of reactive oxygen species as a by-product.

[0013] It has also been found that membranes can be used to remove other waste solutes from fluids. Geremia et al. (DOI: 10.1016 / Jactbio.2019.04.009) describe membranes containing activated carbon particles. These membranes can bind uremic toxins, but activated carbon is a weak urea binder and does not actually show urea binding. Cheah et al. (Material Chemistry and Physics, 175 (2016), 151-157) confirmed this weak binding, and they described silica-based materials that non-covalently capture urea with amines or hydroxyls as an alternative.

[0014] WO2014007716 discloses a macroporous copper-chitosan polymer membrane for adsorbing urea from a dialysis solution. The membrane binds urea, but only at a low capacity. Furthermore, the removal is by a readily reversible binding, since the membrane is only able to have non-covalent interactions with urea via copper, which itself is also non-covalently bound.

[0015] WO2011102807A1 discloses epoxide-covered substrates. Epoxides can be used to recover solutes from solutions. They are also used to immobilize ureases that help process urea. The disadvantages of ureases are that they are sensitive to environmental factors, their production is expensive and laborious, and they react to produce toxic ammonium, which in turn requires the use of cation exchangers to remove, which add additional weight to the devices in which they are used, and cation exchangers contain materials such as zirconium phosphate that may not yet be wanted to bind calcium or potassium. WO2016126596 uses a different substrate, namely, reduced graphene oxide. While showing a high urea binding capacity, the representative captured urea is less than 15% of the initial urea content.

[0016] In order to enable the development of improved artificial kidney devices, there is a continuing need for materials that are easy to prepare, bind higher amounts of urea, without the risk of leaching components or trapped urea back into the dialysate and without producing harmful by-products, and that bind urea faster, with improved kinetics, and that combine the advantages of membranes with those of dedicated urea adsorbents, reducing the overall weight required for the device. Summary of the invention

[0017] The present invention is based on the surprising discovery that the performance of a urea adsorbent is improved when adsorbent particles are embedded in a porous membrane matrix. The binding capacity of the urea adsorbent is increased and the binding kinetics are also improved. Therefore, the present invention relates to a membrane comprising an embedded particulate material, wherein the membrane is a porous polymer membrane, wherein the particulate material comprises a urea adsorbent and the particle size of the particulate material is up to 250 μm along the maximum diameter. Preferably, the particulate material is present in the membrane in a content range of 5 wt % to 80 wt %, more preferably 25 wt % to 70 wt %, based on the total dry weight of the membrane and the particulate material. Preferably, the particle size of the particulate material is up to 150 μm along the maximum diameter, more preferably up to 85 μm. Preferably, the membrane is in the form of a hollow fiber, a full fiber or a flat sheet; more preferably, the membrane is in the form of a hollow fiber. Preferably, the membrane comprises at least one polymer selected from the group consisting of polysulfone, polyethersulfone, polyphenylsulfone, polyarylethersulfone, polyamide, polyetherimide, polyimide, polyethylene-co-vinyl alcohol, polyethylene-co-vinyl acetate, cellulose acetate, cellulose triacetate, polyvinylidene fluoride, polyvinyl chloride, polyacrylonitrile, polyurethane, polyetheretherketone and polyacrylic acid; more preferably, the membrane comprises polyethersulfone and / or polyvinylpyrrolidone. Preferably, the membrane has a molecular weight of at least 1 L / (m 2 ·h·Bar). Preferably, the urea adsorbent is an adsorbent that covalently captures urea. Preferably, the urea adsorbent is a macromolecular composition, which comprises a polymer backbone grafted with a side group that can covalently capture urea, wherein the side group that can covalently capture urea preferably comprises two or more adjacent carbonyl groups or hydrates thereof. Preferably, the urea adsorbent is selected from a ninhydrin type adsorbent, a benzoyl acetaldehyde type adsorbent and / or a trimethylol type adsorbent. In a preferred embodiment, the particulate material further comprises activated carbon particles, ion exchange particles such as ion exchange resin particles or ion exchange silica particles, silica particles such as unmodified silica particles or alkylated silica particles, zeolite particles, ceramic particles, polymer particles such as porous polymer particles or non-porous polymer particles, and / or molecularly imprinted particles; and / or the membrane further comprises additives such as hydrophilic additives, preferably polyvinyl pyrrolidone, chitosan, polyethylene glycol, dextran, glycerol, diethylene glycol, octanol, oxalic acid, maleic acid, tartaric acid, fumaric acid, lithium chloride and / or calcium chloride.

[0018] There is also provided the use of a membrane as defined above as a medicament for use in treatment of a disease or condition associated with urea accumulation.

[0019] There is also provided a method for preparing a membrane as defined above, comprising the steps of: i. providing urea adsorbent particles having a particle size of up to 250 μm along a maximum diameter; ii. mixing the urea adsorbent particles with a polymer material in a solvent for the polymer material to obtain a mixture; iii. extruding or casting the mixture to form a membrane; and iv. optionally, curing the membrane, preferably by phase inversion.

[0020] Also provided is a method for removing nucleophilic waste solutes from a fluid, comprising the steps of: i) providing a fluid containing nucleophilic waste solutes; iia) contacting the fluid with a membrane as described in any one of claims 1-10, or, iib) contacting the fluid and a dialysate through a membrane, wherein the dialysate is in contact with the membrane as described in any one of claims 1-10; iii) optionally, regenerating the fluid.

[0021] The present invention also provides a cartridge for use in a dialysis device, comprising a membrane as defined above. The present invention also provides a dialysis device, comprising a membrane as defined above or a cartridge as defined above. DETAILED DESCRIPTION

[0022] The present invention seeks to provide an improved adsorbent material having increased capacity and binding rate for nucleophilic waste solutes, an important example of which is urea. An adsorbent is a material that binds a target substance - in this case, an adsorbent binds a nucleophile, such as urea. The inventors have invented a membrane with a high urea binding capacity and fast binding kinetics, making the membrane suitable for use in dialysis. The membrane comprises adsorbent particles. The improved adsorbent membrane, which may be referred to as a mixed matrix membrane (MMM), because it comprises a particulate material embedded in a polymer matrix, allows miniaturization of the adsorbent cartridge and is therefore an important step towards a miniaturized artificial kidney device.

[0023] The present invention is based on the surprising discovery that the performance of a urea adsorbent is enhanced when the adsorbent particles are embedded in a porous membrane matrix. Not only is the binding capacity of the urea adsorbent increased, the binding kinetics are also improved. Thus, the present invention provides a membrane comprising an embedded particulate material,

[0024] wherein the membrane is a porous polymer membrane,

[0025] Wherein, the granular material comprises a urea adsorbent,

[0026] The particle size of the granular material is at most 250 μm along the maximum diameter.

[0027] Such membranes with embedded urea adsorbent particles are hereinafter referred to as membranes according to the invention. In general, the membranes of the invention achieve faster kinetics of removal of nucleophilic waste solutes, in particular urea, than other systems, such as free adsorbent particles. In addition, the membranes of the invention have a higher capacity to remove nucleophilic waste solutes, in particular urea, than other systems. Surprisingly, the amount of urea adsorbed by the membrane is higher than when the adsorbent particles are not embedded in the membrane but dispersed in an aqueous urea solution.

[0028] The membrane according to the present invention comprises embedded particulate material. The skilled person is familiar with membranes with embedded particulate material, for example membranes from WO2019175366 or WO2014007716 or Geremia et al. (DOI: 10.1016 / jactbio.2019.04.009). In general, embedded particulate material refers to particles captured by the polymer matrix constituting the membrane. The embedded particulate material may be completely surrounded by the membrane matrix, or may be partially exposed on the surface of the polymer.

[0029] membrane

[0030] The membrane can advantageously be used in (hemo)dialysis to remove urea, wherein the blood is led through the membrane, or through a semipermeable membrane, the blood is separated from a small amount of dialysate, which is then contacted with the membrane of the invention. The adsorbent particles in the membrane then bind nucleophilic waste solutes such as urea, so that the diffusion of these solutes across the (semipermeable) membrane continues and is not slowed down by saturation.

[0031] Membrane technology is well developed, and technicians can select the appropriate type of membrane in which the urea adsorbent is embedded, or in other words, a suitable polymer matrix in which the urea adsorbent is embedded can be selected to develop MMM (see "Basic Principles of Membrane Technology", M. Mulder's second edition, Kluwer Academic Publishers, ISBN0-7923-4247-x; and "Biomedical membranes and bioartificialorgans", D. Stamatialis, Ed., World Scientific / Oxford press, ISBN 978-981-3221-75-8 (2018)). Suitable membranes are made of polymers, so the membranes contain or consist of polymer matrices. The membranes are porous, and the pores can be macropores, micropores, or nanopores. Dense (non-porous) membranes are not suitable because the particulate material in such membranes will not be able to fully approach the fluid. Based on the application and relative importance of permeability therein, microfiltration membranes, ultrafiltration membranes, nanofiltration membranes, and reverse osmosis membranes can be defined, which have decreasing pore sizes. The required transmembrane pressure increases as the pore size decreases.

[0032] For applications where urea removal is the primary goal, microfiltration and / or ultrafiltration are preferred. In general, lower permeability can help improve the kinetics of urea binding because the residence time of the passing molecules is increased, thereby providing more time for the solute to bind to the embedded sorbent particles.

[0033] The membrane according to the present invention is particularly suitable for liquid filtration, so the preferred membrane is a filtration membrane, more preferably a liquid filtration membrane with a porous membrane. The filtration membrane can be a microfiltration membrane, an ultrafiltration membrane, a nanofiltration membrane and a reverse osmosis membrane. In a preferred embodiment, the membrane is a microfiltration membrane, an ultrafiltration membrane or a nanofiltration membrane. In a preferred embodiment, the membrane is a microfiltration membrane or an ultrafiltration membrane. In a preferred embodiment, the membrane is a nanofiltration membrane or a reverse osmosis membrane. In some preferred embodiments, for example, when used for water treatment, the membrane is a reverse osmosis membrane.

[0034] Microfiltration membranes are well known in the art. They typically have a flow rate of about 500-5000 L / (m 2 h Bar) permeability, and they are usually operated at a pressure of 0-1 bar. Examples of microfiltration membranes are organic membranes made using polymers including cellulose acetate (CA), polysulfone, polyvinylidene fluoride, polyethersulfone and / or polyamide. Inorganic membranes are less preferred because they are less easy to prepare using the method of the present invention.

[0035] Ultrafiltration membranes are also known and have pore sizes ranging from 0.1-0.01 μm. They are able to retain proteins, endotoxins, viruses and silica. Ultrafiltration membranes have a variety of applications extending from wastewater treatment to pharmaceutical applications and dialysis treatments. They typically have a pore size of about 50-800 L / (m 2 hBar) water permeability, and they are usually operated at a pressure of 0.2-10 bar. Examples of ultrafiltration membranes are organic membranes made using polymers including polysulfone, polyethersulfone, polypropylene, cellulose acetate and / or polylactic acid.

[0036] Nanofiltration membranes are also known and have pore sizes ranging from 0.001-0.01 μm. They can filter multivalent ions, synthetic dyes, sugars and certain salts. They typically have a pore size of about 1-15 L / (m 2 hBar) permeability to water, and they are usually operated at a pressure of 5-20 bar. Examples of nanofiltration membranes are organic membranes made using polymers including ethylene vinyl alcohol, polysulfone, polyethersulfone, polyvinylidene fluoride, polyamide and / or polyethylene terephthalate.

[0037] Reverse osmosis membranes are the finest separation membranes available, with pore sizes of 0.0001-0.001 μm. Reverse osmosis is able to retain almost all molecules except water and small hydrophilic molecules such as urea. Due to the size of the pores, the required osmotic pressure is significantly greater than that required for other filtration technologies. It usually has a pore size of about 1-5 L / (m 2 hBar) permeability, and they usually operate at a pressure of 8-100 bar. An example of a reverse osmosis membrane is an organic membrane made using cellulose triacetate (CTA).

[0038] In a preferred embodiment, a membrane according to the invention is provided, wherein the water permeability of the membrane is at least 1 L / (m 2 In other preferred embodiments, the water permeability of the membrane is at least 50 L / (m 2 hBar), more preferably 100 L / (m 2 hBar), even more preferably 150L / (m 2 hBar), and more preferably 200 L / (m 2 hBar), and more preferably 250 L / (m 2 hBar), the most preferred is 300L / (m 2 In other highly preferred embodiments, the water flux is at least 500 L / (m 2 hBar). Preferably, the water permeability is at most 5000 L / (m 2 hBar), more preferably at most 3500 L / (m 2hBar), still more preferably at most 2500 L / (m 2 hBar), even more preferably at most 1500 L / (m 2 hBar), still more preferably at most 800 L / (m 2 hBar), still more preferably at most 500 L / (m 2 hBar), still more preferably at most 400 L / (m 2 hBar), still more preferably at most 250 L / (m 2 hBar), still more preferably at most 150 L / (m 2 hBar), still more preferably at most 75 L / (m 2 hBar), yet more preferably at most 50, 25, 15, 10 or 5 L / (m 2 hBar). In the range of about 10 to about 1000 L / (m 2 The water permeability in the range of hBar) is very suitable, about 10 to about 500L / (m 2 hBar) is more suitable, 50 to 400L / (m 2 hBar) is more appropriate.

[0039] In a preferred embodiment, the membrane of the present invention comprises at least one polymer selected from the group consisting of polysulfone, polyethersulfone, polyphenylsulfone, polyarylethersulfone, polyamide, polyetherimide, polyimide, polyethylene-co-vinyl alcohol, polyethylene-co-vinyl acetate, cellulose derivatives such as cellulose acetate or cellulose triacetate, polyvinylidene fluoride, polyvinyl chloride, polyacrylonitrile, polyurethane, polyetheretherketone, polysaccharides such as chitosan, and polyacrylic acid. More preferably, the membrane comprises polyethersulfone and / or polyvinylpyrrolidone, more preferably comprises polyethersulfone and polyvinylpyrrolidone.

[0040] As known to the skilled person, mixtures of polymers can produce attractive films. In a preferred embodiment, the membrane according to the present invention comprises a total amount of 20 wt % to 95 wt %, preferably 30 wt % to 75 wt %, more preferably 40 wt % to 60 wt % of polymers, based on the dry weight of the membrane including the particles. Advantageously, the membrane comprises a first polymer such as polyethersulfone (PES, see Pavlenko et al., Nature Scientific Reports, 6 (2016) 34429), an EVAL polymer such as ethylene vinyl alcohol (see Tetala & Stamatialis, Sep. Pur. Tech., 104 (2013) 214-220) or a polyimide such as polyimide P84 (see et al., Sep. Pur. Tech., 80 (2011) 306-314), preferably PES, in an amount of 10-50 wt%, more preferably 20-40 wt%, most preferably about 30 wt%, based on the dry weight of the membrane containing the particles. Preferably, the membrane comprises a second polymer, such as polyvinyl pyrrolidone (PVP), polyethylene glycol (PEG) or polyethylene oxide (PEO), preferably PVP, in an amount of 1 wt% to 30 wt%, more preferably 10 wt% to 20 wt%, most preferably about 14 wt%, based on the dry weight of the membrane including the particles. The skilled person will appreciate that a variety of polymers may be used, particularly when a polymer solvent and a non-solvent are present to enable liquid-induced phase separation, preferably the particulate material is insoluble in the polymer solvent.

[0041] Membrane morphology can be controlled using methods known in the art. In a preferred embodiment, the membrane according to the present invention is provided, wherein the membrane is in the form of a hollow fiber, a full fiber or a flat sheet; preferably, the membrane is in the form of a hollow fiber.

[0042] The membrane of the present invention can be referred to as mixed matrix membrane (MMMs). MMMs can have one layer, two layers, three layers or more layers. The membrane of the present invention can be asymmetric or symmetric. In a preferred embodiment, MMM has two layers, and the particulate material is present in the layer closest to the dialysate of the double-layer mixed matrix membrane. In other preferred embodiments, the particulate material is present in all layers. In other preferred embodiments, the membrane has only a single layer, which is useful when the permeability and mechanical stability of the membrane exclude the need for multiple layers.

[0043] In a preferred embodiment, the film comprises a polymer having a molecular weight in the range of 1,000 to 1,000,000 grams per mole (g / mol), preferably in the range of 30,000 to 500,000 g / mol. Preferably, the polymer weight is a number average polymer weight. The film of the present invention preferably has a molecular weight cutoff (MWCO) in the range of 0.5 to 1000 kilodaltons (kDa), more preferably in the range of 5 to 50 kDa, or at most 40 kDa, more preferably at most 30 kDa, more preferably at most 25 kDa, most preferably at most 20 kDa. In a preferred embodiment, the molecular weight cutoff (MWCO) is from about 20 kDa to about 50 kDa. In other preferred embodiments, for example, a high flux membrane is required, and the molecular weight cutoff (MWCO) is about 20 kDa. In other preferred embodiments, for example, a membrane with a medium cutoff value is required, and the molecular weight cutoff (MWCO) is about 50 kDa.

[0044] In some embodiments, the membrane of the present invention has an average pore size of 1 to 2000 nm, more preferably 1 to 500 nm. The pore size is preferably at least 1 nm, more preferably at least 2 nm, and most preferably at least about 3 nm. Low pore size is preferably used for dialysis applications because it helps retain blood proteins such as albumin. Preferably, a combination of a pore size of about 3 nm and a molecular weight cutoff of about 10-50 kDa, such as about 20 kDa, is used. The pore size can be determined using known techniques, such as gas adsorption; the molecular weight cutoff is determined by filtering a mixture of molecules of various sizes, preferably MWCO determination.

[0045] The membrane of the present invention preferably has a surface area to volume ratio of at least 50 cm -1 , more preferably at least 100 cm -1 . The membrane of the present invention is preferably able to withstand the maximum flow rate of a mixture, preferably a dialysate or a filtrate such as a plasma filtrate, wherein the mixture contains a nucleophilic waste solute such as urea, in the range of 10-1000 milliliters per minute (mL / min), most preferably in the range of 300-800 mL / min. The maximum flow rate is preferably at least 10 mL / min, more preferably at least 50 mL / min, even more preferably at least 75 mL / min, even more preferably at least 100 mL / min, more preferably at least 250 mL / min, more preferably at least 300 mL / min. The maximum flow rate is preferably at most 1000 mL / min, more preferably at most 750 mL / min, even more preferably at most 600 mL / min, even more preferably at most 500 mL / min, more preferably at most 400 mL / min, more preferably at most 350 mL / min. For general dialysis applications, a flow rate of 100 mL / min is sufficient. For home dialysis, a flow rate of 300 mL / min is preferred.

[0046] The membrane of the present invention preferably has an ultrafiltration coefficient K uf In the range of 60 to 600 mL m -2 h -1 mmHg -1 range, more preferably 100 to 400 mL m -2 h -1 mmHg -1 range, most preferably 250 to 350 mL m -2 h -1 mmHg -1 . K is preferred uf At least 10 mL m -2 h -1 mmHg -1 , more preferably at least 50 mL m -2 h -1 mmHg -1 , more preferably at least 60 mL m-2 h -1 mmHg -1 , more preferably at least 75 mL m - 2 h -1 mmHg -1 , more preferably at least 100 mL m -2 h -1 mmHg -1 . K is preferred uf Up to 400 mL m -2 h -1 mmHg -1 , more preferably at most 350 mL m -2 h -1 mmHg -1 , more preferably at most 300 mL m -2 h -1 mmHg -1 , more preferably at most 250 mL m -2 h -1 mmHg -1 , more preferably at most 200 mL m -2 h -1 mmHg -1 , more preferably at most 150 mL m -2 h -1 mmHg -1 , more preferably at most 100 mL m -2 h -1 mmHg -1 .

[0047] The film of the present invention preferably has a swelling degree in the range of 1% to 15%, preferably 1% to 5%, most preferably about 2%. Preferably, the film does not swell substantially, more preferably at most 3%, even more preferably at most 1.5%, most preferably less than 1%, such as at most 0.5%.

[0048] The membrane according to the invention preferably has a urea binding capacity of at least 1.8 mmol / g, more preferably at least 2.0 mmol / g, even more preferably at least 2.5 mmol / g, more preferably at least 2.6 mmol / g, still more preferably at least 2.7 mmol / g, still more preferably at least 2.8 mmol / g, more preferably 2.9 mmol / g, still more preferably 3 mmol / g. The membrane according to the invention may preferably bind at least 0.75 mmol / g, more preferably 0.8 mmol / g of urea after 1 hour. The membrane according to the invention may preferably bind at least 1.8 mmol / g of urea, more preferably 2 mmol / g of urea after up to 16 hours. This urea binding is preferably as described elsewhere herein, more preferably at 70°C, most preferably as described in the examples.

[0049] Urea adsorbent

[0050] The membrane according to the present invention comprises a granular material. The granular material comprises at least a urea adsorbent. In a preferred embodiment, the granular material consists of a urea adsorbent.

[0051] An adsorbent is a material that binds a target substance - in this case, the adsorbent is a urea adsorbent, so it binds urea. As described in the background of the invention, urea adsorbents are well known in the art. The two main modes of binding urea are by covalent binding and by adsorption, particularly physical adsorption. Covalent binding is sometimes referred to as chemical adsorption. The urea adsorbents preferably used in the membranes of the present invention are urea adsorbents that covalently capture urea. In other preferred embodiments, multiple types of urea adsorbents are used, wherein at least one urea adsorbent covalently captures urea. Preferably, the binding includes covalent capture of urea, wherein at least 10% of the urea binding is covalent capture of urea. More preferably, the binding includes at least 50% covalent capture of urea, more preferably at least 70%, more preferably at least 80%, and even more preferably at least 90% covalent capture. In other preferred embodiments, substantially all urea capture is covalent urea capture. The urea adsorbent used in the present invention preferably has a urea binding capacity greater than 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 11.1, 1.2, 1.3, 1.4, 1 or 1.5 mmol urea / gram of adsorbent; more preferably, the adsorbent has a urea binding capacity greater than 0.1 mmol urea / gram of adsorbent; even more preferably, the adsorbent has a urea binding capacity greater than 0.5 mmol urea / gram of adsorbent; still more preferably, the adsorbent has a urea binding capacity greater than 1, still more preferably greater than 1.5, even more preferably greater than 2 mmol urea / gram of adsorbent, such as greater than 2.5 or greater than 2.6 mmol urea / gram of adsorbent. The covalency of urea capture can be assessed using spectroscopic techniques.

[0052] Examples of urea adsorbents include ninhydrin-type adsorbents (e.g., EP121275A1; US4897200A; WO2019110557); benzoyl acetaldehyde (PGA)-type adsorbents (e.g., DE2305186A1; US3933753A; US4012317; WO2004078797A1; EP19210947); aldehyde-based adsorbents, such as trimethylformic acid (TFM)-type adsorbents (capturing urea by TFM is described in Jong et al., ACS Omega 2019, 4, 11928-11937); copper composite adsorbents, such as copper-deacetylated chitosan type adsorbents (e.g. WO2014007716); para-functionalized polystyrene type adsorbents, characterized by, for example, para-thio, para-nitro or para-amino moieties (e.g. US4178241A); silica-based adsorbents with free hydroxyl or amino moieties (e.g. Cheah et al. (MaterialChemistry and Physics, 175 (2016), 151-157)); epoxide-covered adsorbents (e.g. WO2011102807A1); enzyme-based adsorbents, such as particles with immobilized urease (e.g. WO2011102807A1); and reduced graphene-based adsorbents (e.g. WO126596). Examples of urea adsorbents for covalently capturing urea in the embodiments include ninhydrin-type adsorbents, phenylacetaldehyde (PGA)-type adsorbents, trimethylformic acid (TFM)-type adsorbents, epoxide-covered adsorbents, and reduced graphene-based adsorbents.

[0053] The inventors have obtained good results using a urea adsorbent, wherein the urea adsorbent is a macromolecular composition comprising a polymer backbone grafted with a side group that can covalently capture urea, wherein the side group that can covalently capture urea preferably comprises two or more adjacent carbonyl groups or a hydrate thereof. In a preferred embodiment, a membrane comprising such an adsorbent is provided. More features and definitions will be provided later in this article. A portion having two or more adjacent carbonyl groups may also be a hydrate thereof, since these groups typically spontaneously hydrate and dehydrate under ambient conditions in an equilibrium state. It should be understood that adjacent carbonyl groups do not have to be directly adjacent, wherein a C(=O) portion is directly connected to an adjacent C(=O) portion; groups in which two or more carbonyl portions can participate in the same resonance stabilized isomer should also be considered, for example, wherein two or more carbonyl portions are separated only by unsaturated carbons or double bonds. Examples of suitable portions are shown in the following table, and reference names and reference numbers are shown in the following table.

[0054]

[0055]

[0056] In the above table, * indicates the position where the indicated moiety is attached to the polymer backbone. X represents a linker moiety comprising 1-10 backbone atoms selected from C, N, O and S, which are substituted to full valence by H. Examples of X may be -CH2-, -O-CH2CH2- and phenyl. X is preferably -CH2-. The moiety may be further substituted, for example by C 1-6 Hydrocarbon or C 1-6 Substitution with alkoxy or nitro, nitrile, amino, hydroxyl, carboxyl, phosphate moieties, etc. Variations in the structure of the adsorbent are possible and the invention encompasses the use of such adsorbents in membranes.

[0057] Examples 1, 2, 3 and 4 of the above table are moieties that, when attached to a polymer backbone, constitute a ninhydrin-type adsorbent. Examples 6, 7 and 8 of the above table are moieties that, when attached to a polymer backbone, constitute a PGA-type adsorbent. Example 10 of the above table is a moiety that, when attached to a polymer backbone, constitutes a TFM-type adsorbent. Examples 1 and 4 coexist in equilibrium under ambient conditions. Likewise for Examples 7 and 8.

[0058] In a particularly preferred embodiment, the urea adsorbent is selected from a ninhydrin-type adsorbent, a benzoyl acetaldehyde-type adsorbent and / or a trimethylol-type adsorbent. In other preferred embodiments, the urea adsorbent is selected from a ninhydrin-type adsorbent and / or a TFM-type adsorbent. In other preferred embodiments, the urea adsorbent is selected from a ninhydrin-type adsorbent and / or a PGA-type adsorbent. In other preferred embodiments, the urea adsorbent is selected from a TFM-type adsorbent and / or a PGA-type adsorbent. In a particularly preferred embodiment, the urea adsorbent is a ninhydrin-type adsorbent. In a particularly preferred embodiment, the urea adsorbent is a TFM-type adsorbent. In a particularly preferred embodiment, the urea adsorbent is a PGA-type adsorbent.

[0059] The particle size of the particulate material is at most 250 μm along the maximum diameter. Preferably, along the maximum diameter, it is at most 200 μm, more preferably at most 180 μm, more preferably at most 160 μm, more preferably at most 150 μm, more preferably at most 130 μm, more preferably at most 110 μm, more preferably at most 100 μm, still more preferably at most 90 μm, even more preferably at most 80 μm, still more preferably at most 70 μm. In a preferred embodiment, a film according to the invention is provided, wherein the particle size of the particulate material is at most 150 μm, preferably at most 85 μm, more preferably at most 70 μm along the maximum diameter.

[0060] In a preferred embodiment, the adsorbent particles have a regular shape, in particular a spherical shape, or an irregular shape. The adsorbent particles are preferably porous, more preferably having a surface area to weight ratio as described by Pavlenko et al. (Nature Scientific Reports, 6 (2016) 34429). The adsorbent particles can be applied in the form of fragments, fibers, powders or a combination thereof. Powders include, but are not limited to, metal powders, plastic powders, solid phase silica, fumed silica and activated carbon. As a result of grinding or milling the granular adsorbent, the particles are preferably substantially round or spherical. Smaller particles allow the formation of thinner films. Therefore, it is preferred that the maximum diameter of the particles has at most 65 μm or 63 μm, more preferably at most 60 μm, even more preferably at most 50 μm, and most preferably at most 40 μm. The maximum diameter is preferably at least 5 μm, more preferably at least 10 μm, even more preferably at least 15 μm, and most preferably at least 20 μm. For example, for urea adsorbent particles, a range of 20-40 μm is highly preferred.

[0061] In a preferred embodiment, the dimensions of the first two sections relate to the dimensions of the urea adsorbent and not to the dimensions of other particles contained in the granular material. Most preferably, the dimensions apply to all granular materials.

[0062] In a preferred embodiment, the adsorbent particles have a particle size of at most 100 μm in the smallest dimension, preferably at most 63 μm, more preferably at most 0.05-60 μm in the smallest dimension. It should be understood that the adsorbent particles may in particular be spheres or ellipsoids. Preferably, the adsorbent particles are substantially spherical. In this case, the smallest dimension is the diameter of the adsorbent particles. In the case where the adsorbent particles are ellipsoids, the largest dimension of the adsorbent particles is preferably at most 150 μm, more preferably at most 100 μm, still more preferably at most 80 μm, and most preferably at most 63 μm.

[0063] Preferably, the adsorbent particles have a particle size in the smallest dimension of 0.05-100 μm, more preferably 0.1-63 μm, even more preferably 0.5-60 μm, still more preferably 1-50 μm, most preferably 5-45 μm.

[0064] It will be appreciated that the particle size of the adsorbent particles can be determined and / or controlled using techniques such as grinding, milling, cutting and / or sieving, which are conventional techniques in the art. The particle size of the particles can be determined using, for example, light scattering or microscopy, such as electron microscopy, as demonstrated in the examples. In a preferred embodiment, the particle size of the particles is determined using electron microscopy. In a preferred embodiment, at least 80% of the particles are smaller than the particle size along the largest diameter, more preferably at least 90% are smaller than the particle size, even more preferably at least 95% are smaller than the particle size, still more preferably at least 99% are smaller than the particle size, and most preferably 100% are smaller than the particle size.

[0065] In a preferred embodiment, the particulate material is present in the membrane in the range of 5-80 wt%, preferably 25-70 wt%, based on the total dry weight of the membrane and particulate material.

[0066] Preferably, there are at least 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, 45 wt%, 50 wt%, 55 wt%, 60 wt%, 65 wt% or 70 wt% of the specific material. More preferably, at least 10 wt%, even more preferably at least 15 wt%, still more preferably at least 20 wt%, most preferably at least about 25 wt% of the specific material exists. Preferably, there are at most 75 wt%, 70 wt%, 65 wt%, 60 wt%, 55 wt%, 50 wt%, 45 wt%, 40 wt%, 35 wt%, 30 wt%, 25 wt%, 20 wt%, 15 wt% or 10 wt% of the specific material. More preferably, at most 60 wt%, even more preferably at most 50 wt%, still more preferably at most 40 wt%, most preferably at most about 30 wt% of the specific material exists.

[0067] In a preferred embodiment, the wt% of the first two paragraphs relate to the wt% of the urea adsorbent and not to the wt% of other particles contained in the particulate material. Most preferably, the wt% pertains to all particulate material.

[0068] In a preferred embodiment, the at least one adsorbent particle has a Brunauer-Emmet-Teller (BET) surface area of ​​at least 0.5 m 2 / g, more preferably at least 0.8m 2 / g, and more preferably at least 1m 2 / g, even more preferably at least 1.5 m 2 / g, most preferably at least 5m 2 The BET surface area of ​​the adsorbent particles is preferably 0.5-10,000 m 2 / g, more preferably 10-2,500m2 / g.

[0069] In a preferred embodiment, the average pore size of the at least one adsorbent particle is 0.1-250 nm, most preferably 25-150 nm. In a preferred embodiment, the average pore volume of the at least one adsorbent particle is 0.001-0.12 mL / g, more preferably 0.01-0.10 mL / g, most preferably 0.02-0.09 mL / g. In a preferred embodiment, the membrane of the present invention contains at least one additional adsorbent particle. The additional adsorbent particles may advantageously have the same size, shape, BET surface area and / or pore size as the adsorbent particles defined above. In a preferred embodiment, the content of the adsorbent particles embedded in the membrane is in the range of 5 wt% to 80 wt%, preferably in the range of 25 wt% to 70 wt%, more preferably in the range of 40 wt% to 60 wt%, based on the dry weight of the membrane containing the particles.

[0070] Further details of the adsorbent

[0071] In the context of the present invention, an adsorbent is a macromolecular composition which is a solid, suspended solid, colloidal suspension, aggregate, resin or polymer which can be dissolved or partially dissolved. It can bind nucleophilic waste solutes, and a urea adsorbent binds at least urea, after which the adsorbent can be recovered from the mixture. The binding can be covalent or non-covalent, for example by electrostatic interactions or by hydrophobic interactions.

[0072] PGA-type adsorbents are adsorbents comprising PGA-type moieties. PGA is phenylglyoxal or 1-phenylethane-1,2-dione or benzaldehyde. The PGA-type moiety is preferably a short aliphatic structure, preferably having only two carbon atoms, characterized by two adjacent carbonyl groups (or their hydrates), which are connected to an aromatic ring or aromatic rings, preferably to a phenyl moiety or a substituted phenyl moiety (e.g. substituted by a polymer backbone). Glyoxal and its hydrates are easily interconverted, and it should be understood that reference to PGA generally also requires reference to its hydrates. Typically, hydrates of glyoxal are formed in non-dry environments, and glyoxal can be dehydrated by heating; in aqueous environments, the two substances generally coexist in equilibrium. Preferred examples of PGA-type moieties are selected from n-oxalylphenyl, m-oxalylphenyl and p-oxalylphenyl, and their hydrates, wherein the benzene ring may optionally be further substituted. In some embodiments, the PGA-type moiety is selected from n-oxalylthiophenyl and m-oxalylthiophenyl. In other embodiments, the PGA-type moiety is selected from n-oxalylthiophenyl and p-oxalylthiophenyl. In some embodiments, the PGA-type moiety is selected from m-thiothiophene and p-thiothiophene.Most preferably, the PGA-type moiety is para-positioned.

[0073] The PGA-type adsorbents suitable for use in the present invention are suitable for binding nucleophilic waste solutes, and do so at a high capacity. These solutes react with the PGA-like moieties contained in the adsorbent. Preferably, the urea binding capacity of the PGA-type adsorbent is greater than 1.60, preferably greater than 1.80, and more preferably greater than 2.00 mmol urea / gram of adsorbent.

[0074] Ninhydrin-type adsorbents are adsorbents comprising a ninhydrin-type moiety. Ninhydrin is 2,2-dihydroxy-1H-indene-1,3(2H)-dione, also known as 2,2-dihydroxyindene-1,3-dione and 1,2,3-ninhydrin hydrate. The ninhydrin-type moiety is preferably a hydrate of a five-membered ring structure having three adjacent carbonyl groups fused to two adjacent positions of an aromatic ring or aromatic ring system, preferably to a phenyl moiety. Preferred examples of ninhydrin-type moieties are selected from 4-[2,2-dihydroxy-1H-indene-1,3(2H)]-dione, 5-[2,2-dihydroxy-1H-indene-1,3(2H)]-dione, 6-[2,2-dihydroxy-1H-indene-1,3(2H)]-dione and 7-[2,2-dihydroxy-1H-indene-1,3(2H)]-dione. More preferred ninhydrin-type moieties are selected from 5-[2,2-dihydroxy-1H-indene-1,3(2H)]-dione and 6-[2,2-dihydroxy-1H-indene-1,3(2H)]-dione. Ninhydrin has an axis of symmetry, so if no other substituents are present, 5-[2,2-dihydroxy-1H-indene-1,3(2H)]-dione and 6-[2,2-dihydroxy-1H-indene-1,3(2H)]-dione are identical.

[0075] The ninhydrin-type adsorbents suitable for use in the present invention are suitable for binding nucleophilic waste solutes. These solutes react with the ninhydrin-type moieties contained in the adsorbent. Preferably, the ninhydrin-type adsorbent has a urea binding capacity greater than 1.4, preferably greater than 2.1 mmol urea / gram of adsorbent.

[0076] Urea is a small, highly polar molecule that is highly soluble in water (>400 mg / mL) and protic organic solvents such as methanol, ethanol, and glycerol due to its polarity and ability to participate in hydrogen bond formation. Although urea is essential for its roles in biochemistry and it is an industrially important molecule, including as a nitrogen source for fertilizers and as a polymer precursor, it is often important to remove urea from fluid solutions.

[0077] The urea binding capacity of the PGA-based adsorbent used in the present invention is preferably greater than 1.51, 1.52, 1.53, 1.54, 1.55, 1.56, 1.57, 1.58, 1.59, 1.60, 1.61, 1.62, 1.63, 1.64, 1.65, 1.67, 1.68, 1.69, 1.70, 1.71, 1.72, 1.73, 1.74, 1.75, 1.76, 1.77, 1 .78, 1.79, 1.80, 1.85, 1.90, 1.95, 2.00, 2.05, 2.10, 2.15, 2.20, 2.25, 2.30, 2.35, 2.40, 2.45, 2.50, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.4, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, More preferably, the adsorbent has a urea binding capacity of greater than 1.60 mmol urea / gram of adsorbent; even more preferably, the adsorbent has a urea binding capacity of greater than 1.80 mmol urea / gram of adsorbent; still more preferably, the adsorbent has a urea binding capacity of greater than 2.00, still more preferably greater than 2.20, even more preferably A urea binding capacity of greater than 2.40, 2.45, 2.50, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8 or 4.9 mmol urea / gram of adsorbent, for example greater than 2.5 or greater than 2.6 mmol urea / gram of adsorbent.

[0078] The ninhydrin-type adsorbent preferably has a urea binding capacity greater than 1.5 mmol urea / gram of adsorbent. In a more preferred embodiment of this aspect, the adsorbent has a urea binding capacity greater than 1.6 mmol urea / gram of adsorbent. In a further preferred embodiment, the urea binding capacity of the ninhydrin-type adsorbent is greater than 1.63, 1.64, 1.65, 1.67, 1.68, 1.69, 1.70, 1.71, 1.72, 1.73, 1.74, 1.75, 1.76, 1.77, 1.78, 1.79, 1.80, 1.85, 1.90, 1.95, 2.00, 2.05, 2.10, 2.15, 2.20, 2.25, 2.30, 2.35, 2.40, 2.45, 2.50, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4 , 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9 mmol urea / gram adsorbent; more preferably, the adsorbent has a urea binding capacity greater than 2.10 mmol urea / gram adsorbent; even more preferably, the adsorbent has a urea binding capacity greater than 2.20 mmol urea / gram adsorbent; most preferably, the adsorbent has a urea binding capacity greater than 2.40 mmol urea / gram adsorbent, for example greater than 2.5 mmol urea / gram adsorbent or greater than 2.6 mmol urea / gram adsorbent.

[0079] In the present invention, the urea binding capacity of the adsorbent is preferably the maximum urea binding capacity, preferably the capacity measured after incubation of the adsorbent with excess urea in a solution (e.g., about 30 mM) at about 70° C. for about 24 hours. The amount of bound urea can be determined by directly analyzing the amount of urea bound to the adsorbent, or by analyzing the difference between the amount of urea present in the solution before and after exposure to the adsorbent, or by regenerating the adsorbent by dissociating the bound urea, and then determining the amount of released urea. The urea concentration can be determined by any method known in the art, for example, by elemental analysis as described in WO2004078797. Alternatively, the amount of ammonia released by urease can be used to indirectly quantify the urea concentration. Alternatively, a PAB reagent solution containing about 4% (w:v) 4-(dimethylamino)benzaldehyde and 4% (v:v) sulfuric acid in anhydrous ethanol can be used for UV-VIS analysis (422 nm) of urea reaction adducts using a pre-prepared calibration curve as described in WO2016126596. Various kits for determining urea concentration are commercially available and include instructions for use. The urea binding capacity of the adsorbent is preferably that of the free adsorbent, since the particles have not yet been embedded in the membrane of the present invention.

[0080] In a PGA-type adsorbent or a ninhydrin-type adsorbent, preferably at least 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95% or 100% of the polymerized monomers are PGA-type monomers or ninhydrin-type monomers. A preferred PGA-type adsorbent or a ninhydrin-type adsorbent is a PGA-type adsorbent or a ninhydrin-type adsorbent in which at least 30%, preferably at least 50%, more preferably at least 60%, even more preferably at least 70%, still more preferably at least 80%, most preferably at least 90% of the polymerized monomers are PGA-type monomers or ninhydrin-type monomers. In a further preferred PGA-type adsorbent or a ninhydrin-type adsorbent, at least 50% and at most 90% of the polymerized monomers are PGA-type monomers or ninhydrin-type monomers. In a more preferred embodiment, 55%-90% of the polymerized monomers are PGA-type monomers or ninhydrin-type monomers. In an even more preferred embodiment, 70%-90% of the polymerized monomers are PGA-type monomers or ninhydrin-type monomers. In a most preferred embodiment, 70%-80% of the polymerized monomers are PGA-type monomers or ninhydrin-type monomers. The amount of PGA-type monomers or ninhydrin-type monomers can be evaluated using conventional techniques known in the art such as solid-state NMR or IR spectroscopy. In a specific embodiment, 100% of the polymerized monomers are PGA-type monomers or ninhydrin-type monomers.

[0081] In a preferred embodiment, the PGA type adsorbent or ninhydrin type adsorbent according to the present invention is obtainable by polymerization, preferably suspension polymerization. In a preferred embodiment, the PGA type adsorbent or ninhydrin type adsorbent is obtainable by polymerization, wherein at most 50%, preferably at most 35%, more preferably at most 25%, even more preferably at most 20%, most preferably at most 10% of crosslinking monomers are used.

[0082] In the polymerization process for preparing the adsorbent, the comonomer may not be a PGA-type monomer or a ninhydrin-type monomer or a precursor thereof. Comonomers are other monomers that undergo polymerization and are covalently bound to the resulting polymer. Such resulting polymers are often referred to as copolymers, but for the sake of clarity, reference will be made herein only to the polymers, where the context will make it clear whether a copolymer may also be referred to. In the present invention, two types of comonomers are particularly relevant: hydrophilic comonomers and crosslinking comonomers.

[0083] In a preferred embodiment, the adsorbent comprises at least one comonomer, wherein the comonomer is preferably selected from the group consisting of styrene, isopropenylbenzene, divinylbenzene, vinylbenzenesulfonic acid, acrylic acid, methacrylic acid, methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, acrylonitrile, 2-hydroxyethyl-2-methyl-2-acrylic acid (HEMA), 2-hydroxypropyl-2-methyl-2-acrylic acid, 2-hydroxyethyl-2-acrylic acid, 2-hydroxypropyl-2-acrylic acid, N-(2-hydroxyethyl)methacrylamide, N-(2-hydroxypropyl) methacrylamide (HPMA), N-(2-hydroxyethyl) acrylamide, N-(2-hydroxypropyl) acrylamide, N,N'-alkylene bisacrylamide such as N,N'-methylene bisacrylamide (NMAA), N-isopropyl acrylamide (NIPAm), divinyl sulfone, butadiene, methacrylonitrile, vinyl sulfonamide, N-alkyl vinyl sulfonamide such as N-methyl vinyl sulfonamide and N,N-dialkyl vinyl sulfonamide such as N,N-dimethyl vinyl sulfonamide. In a more preferred embodiment, the comonomer is selected from the group consisting of divinylbenzene, vinylbenzenesulfonic acid, acrylic acid, (meth) acrylonitrile, vinyl sulfonamide, N-alkyl vinyl sulfonamide, N,N-dialkyl vinyl sulfonamide and 2-hydroxyethyl-2-methyl-2-enoate (HEMA). Even more preferably, the comonomer is selected from divinylbenzene and vinylbenzenesulfonic acid. Most preferably, both divinylbenzene and vinylbenzenesulfonic acid are present. In the context of this article, divinylbenzene can be 1,2-divinylbenzene, 1,3-divinylbenzene or 1,4-divinylbenzene, or a mixture thereof. 1,4-divinylbenzene or a mixture comprising 1,4-divinylbenzene is preferred because they provide more spacious crosslinking, which improves the solvent permeability of the resulting polymer. In the context of this article, vinylbenzenesulfonic acid can be 2-vinylbenzenesulfonic acid, 3-vinylbenzenesulfonic acid or 4-vinylbenzenesulfonic acid or a mixture thereof. 4-vinylbenzenesulfonic acid is preferred because it has ideal polymerization kinetics.

[0084] For crosslinked adsorbents, at least one crosslinking comonomer is preferably present. A crosslinking comonomer typically has more than one reactive moiety that can participate in a polymerization reaction. Preferably, such a crosslinking comonomer is selected from the group consisting of: divinylbenzene, N,N'-alkylenebisacrylamides such as N,N'-methylenebisacrylamide (NMAA), divinyl sulfone and butadiene, preferably providing divinylbenzene during polymerization to form the adsorbent. In the context of this article, the amount of crosslinking is defined as the amount of crosslinking comonomer present in the polymerization mixture during adsorbent formation. Greater amounts of crosslinking result in denser adsorbents; lesser amounts of crosslinking result in more porous or more macroporous adsorbents. Preferably, there is at most 10% crosslinking comonomer. More preferably, there is at most 5% crosslinking comonomer. Even more preferably, for the cross-linked adsorbent, there is 0.1% to 5% cross-linking comonomer, more preferably there is 0.2% to 4% cross-linking comonomer, even more preferably there is 0.4% to 4% cross-linking comonomer, and most preferably there is 0.8% to 3% cross-linking comonomer, for example about 1% to about 2%, or about 2%.

[0085] Adsorbents comprising hydrophilic comonomers are referred to herein as hydrophilic adsorbents. The hydrophilic comonomer enables aqueous solvents to more easily penetrate the adsorbent, allowing nucleophilic waste solutes to similarly more easily penetrate the adsorbent. This allows the interior of the adsorbent to also participate in the binding of nucleophilic waste solutes. There is a balance because hydrophilic comonomers are generally unable to bind nucleophilic waste solutes in the way that PGA-type moieties or ninhydrin-type moieties can. Therefore, an increase in the hydrophilic comonomer content makes the PGA-type moieties or ninhydrin-type moieties more effective, but reduces their number.

[0086] For hydrophilic adsorbents, at least one hydrophilic comonomer is preferably present. Preferably, such a hydrophilic comonomer is selected from the group consisting of vinylbenzenesulfonic acid, acrylic acid, methacrylic acid, methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, 2-hydroxyethyl-2-methyl-2-acrylic acid (HEMA), 2-hydroxypropyl-2-methyl-2-acrylic acid, 2-hydroxyethyl-2-acrylic acid, 2-hydroxypropyl-2-acrylic acid, N-(2-hydroxyethyl)methacrylamide, N-(2-hydroxypropyl)methacrylamide (HPMA), N-(2-hydroxyethyl)acrylamide, N-(2-hydroxypropyl)acrylamide and N-isopropylacrylamide (NIPAm), more preferably selected from the group consisting of vinylbenzenesulfonic acid, acrylic acid, methacrylic acid, 2-hydroxyethyl-2-methyl-2-acrylic acid (HEMA), 2-hydroxypropyl-2-methyl-2-acrylic acid, 2-hydroxyethyl-2-acrylic acid, 2-hydroxypropyl-2-acrylic acid, N-(2-hydroxyethyl)methacrylamide, N-(2-hydroxypropyl)methacrylamide (HPMA), N-(2-hydroxyethyl)acrylamide and N-(2-hydroxypropyl)acrylamide, preferably vinylbenzenesulfonic acid is present. The skilled person will understand that some comonomers such as methyl methacrylate can be easily modified to be hydrophilic by hydrolysis of their esters. Preferably, up to 60% of hydrophilic comonomers are present. More preferably, up to 50% of hydrophilic comonomers are present. Even more preferably, for hydrophilic adsorbents, there is 0-50% hydrophilic comonomer, more preferably there is 0-40% hydrophilic comonomer, even more preferably there is 5-40% hydrophilic comonomer, more preferably there is also 10-35% hydrophilic comonomer, even more preferably there is 15-35% hydrophilic comonomer, most preferably there is 20-30% hydrophilic comonomer, for example about 25%.

[0087] Illustrative examples of suitable adsorbents are shown below. Square brackets separate different monomer types contained in the adsorbent. The monomers are preferably present as random or random copolymers. Suitable amounts of different monomer types are described elsewhere herein.

[0088]

[0089]

[0090] Other properties of membrane

[0091] As is known in the art, other additives may be present in the membrane, for example in the polymer matrix. For example, in a preferred embodiment, a membrane according to the invention is provided, wherein the particulate material further comprises activated carbon particles, ion exchange particles such as ion exchange resin particles or ion exchange silica particles, silica particles such as unmodified silica particles or alkylated silica particles, zeolite particles, ceramic particles, polymer particles such as porous polymer particles or non-porous polymer particles, and / or molecularly imprinted particles, and / or

[0092] The membrane further comprises additives, such as hydrophilic additives, preferably polyvinyl pyrrolidone, chitosan, polyethylene glycol, dextran, glycerol, diethylene glycol, octanol, oxalic acid, maleic acid, tartaric acid, fumaric acid, lithium chloride and / or calcium chloride.

[0093] In a preferred embodiment, the membrane according to the present invention further comprises at least one hydrophilic additive. Adding a hydrophilic additive to the membrane can help adjust the membrane morphology, improve the water transport of the membrane, reduce membrane scaling, increase the blood compatibility of the membrane, or a combination thereof. Preferably, based on the dry weight of the membrane including the particles, the hydrophilic additive is present in an amount in the range of 0.01-50wt%, more preferably in an amount in the range of 0.5-10wt%. More preferably, the additive is present in at least 1wt%, preferably 2wt%, more preferably 5wt%, even more preferably 10wt%. More preferably, the additive is present in an amount of up to 15wt%, more preferably 8wt%, more preferably 3wt%.

[0094] Preferably, the hydrophilic additive is selected from the group consisting of polyvinyl pyrrolidone, polyethylene glycol, dextran, glycerol, diethylene glycol, octanol, oxalic acid, maleic acid, tartaric acid, fumaric acid, lithium chloride and calcium chloride. Most preferably, the hydrophilic additive is polyvinyl pyrrolidone. Polyvinyl pyrrolidone preferably has a molecular weight in the range of 2,500-2,500,000 g / mol, more preferably a molecular weight in the range of 2,500-500,000 g / mol.

[0095] The membrane usually has two main surfaces. In the case of sheets, these are opposite surfaces that roughly define the plane of the sheet. Both surfaces can be regarded as outer surfaces. In the case of hollow fibers, the outer surface and the inner surface are the two main surfaces. The inner surface defines the boundary between the membrane itself and its lumen. A full fiber has no holes, and therefore no inner surface in this sense, although it can have a porous structure that provides a surface area; this surface area does not separate the membrane from the lumen. The surface can be smooth or rough, and can be non-corrugated or corrugated, as known in the art. Corrugation refers to ribs protruding from the surface. Preferably, the corrugations are substantially or completely parallel. Preferably, the corrugations are along the longest dimension of the membrane. The corrugations preferably protrude at least 5% relative to the average membrane thickness, more preferably at least 10%, even more preferably 20%, still more preferably 30%, and most preferably at least 40%. The corrugations preferably protrude at most 150% relative to the average membrane thickness, more preferably at most 100%, even more preferably 75%, still more preferably 60%, and most preferably at most 50%. In a preferred embodiment, at least one surface is smooth. In a preferred embodiment, only one surface is smooth. In a preferred embodiment, both surfaces are smooth. In a preferred embodiment, at least one surface is corrugated. In a preferred embodiment, only one surface is corrugated. In a preferred embodiment, both surfaces are corrugated. When the surface is an exterior surface, it is smooth, most preferably smooth and non-corrugated. When the surface is an interior surface, it is corrugated, most preferably corrugated and smooth. As is known, corrugations increase surface area and are therefore preferred for any surface that requires increased surface area.

[0096] In a preferred embodiment, at least one additional type of adsorbent particles is included in the membrane of the present invention. The additional adsorbent particles may advantageously have the same particle size, shape, BET surface area and / or pore size as the urea adsorbent particles defined elsewhere herein. Preferably, the at least one additional adsorbent particle is selected from the group consisting of activated carbon particles, ion exchange resins, unmodified silica particles, C2 derived silica particles, C4 derived silica particles, C6 derived silica particles, C8 derived silica particles, C 16 The group consisting of derivatized silica particles, ion exchange silica particles, zeolites, zirconium oxides such as zirconium phosphate or zirconium oxide or zirconium oxyhydroxide or zirconium carbonate, ceramic particles, porous polymer particles, non-porous polymer particles and molecularly imprinted particles. Here, it should be understood that the ion exchange resin can be a weak or strong cation exchange resin or a weak or strong anion exchange resin.

[0097] In a preferred embodiment, the additional adsorbent particles are activated carbon particles. This is particularly advantageous because the activated carbon particles can remove waste solutes (particularly compounds other than urea) from the mixture.

[0098] The activated carbon particles preferably have an average pore size of 0.1-20 nm, most preferably 1-5 nm. On the other hand, the activated carbon particles preferably have a particle size in the range of 0.1-100 μm, preferably in the range of 0.1-30 μm, and most preferably the particle size of the activated carbon particles is less than 25 μm. In some embodiments, the activated carbon particles have a particle size of 100-10,000 m2 / g (m 2 / g), most preferably 2000m 2 / g of BET surface area, the activated carbon particles are optionally impregnated with at least one inorganic impregnant selected from the group consisting of iodine, silver, aluminum, manganese, zinc, iron, lithium and calcium. Preferably, aluminum, manganese, zinc, iron, lithium and calcium are in their cationic form. In a preferred embodiment, there is no such impregnation. The activated carbon particles are preferably selected from the group consisting of AC Norit A Supra particles and CMK3 particles.

[0099] Membrane preparation

[0100] The membrane according to the invention can be prepared using techniques known in the art. Particle-containing membranes are known in the art, for example from WO2006019293 or Geremia et al. (DOI: 10.1016 / actbio.2019.04.009). The method for preparing a membrane according to the invention differs in that it uses urea adsorbent particles having a particle size of up to 250 μm along the largest diameter. Therefore, the present invention provides, on the one hand, a method for preparing a membrane according to the invention, comprising the following steps:

[0101] i. Providing urea adsorbent particles having a particle size of up to 250 μm along the maximum diameter;

[0102] ii. mixing the urea adsorbent particles with a polymer material in a solvent for the polymer material to obtain a mixture;

[0103] iii. extruding or casting the mixture to form a film; and

[0104] iv. curing the film, preferably by phase inversion.

[0105] This method is referred to herein as the preparation method according to the invention.

[0106] In step i, urea adsorbent particles are provided. These particles have been defined previously herein. In a preferred embodiment, the particles have a particle size along the maximum diameter of at most 200 μm, preferably at most 150 μm, more preferably at most 100 μm, even more preferably at most 70 μm, and even more preferably at most 50 μm. The particles can be prepared as part of the method according to the present invention, or they can be obtained from commercial sources. In a preferred embodiment, as part of step i, the particles are classified, and the classification is to make the particles reach the desired particle size range. Classification can be performed by grinding, grinding, crushing or cutting, or any other material processing method known in the art. Classification may also include screening, which is a convenient way to ensure an upper particle size cutoff. Preferred urea adsorbent particles swell up to 20% along their longest axis when suspended in a liquid. More preferably, the particles swell up to 15%, even more preferably up to 10%, still more preferably up to 5%, and most preferably up to 2%. More preferably, the particles do not substantially swell when suspended in a liquid, which improves the mechanical stability of the resulting film after continuous wetting and dewetting or during storage.

[0107] In step ii, the urea adsorbent particles are mixed with a polymer material in a solvent for the polymer material. Therefore, this resulting suspension contains dissolved polymers, which then form a membrane in which adsorbent particles are suspended. Mixing can be carried out using any known method, such as described below or illustrated in the embodiments. Preferably, mixing is carried out for at least 1, 2, 3, 4, 5, 6, 12, 18, 24, 36, 48, 72 hours or longer. Preferably, mixing is carried out for up to 120 hours, more preferably up to 96 or 72 hours, such as 72 hours. Preferably, the urea adsorbent particles are suspended in the solvent alone without forming aggregates. Additional components of the membrane according to the present invention can be conveniently added here, such as other particles or, for example, additives for the membrane. These other components are part of the mixture obtained in step ii.

[0108] The mixture of step ii preferably has a viscosity of at least 1.5 Pa s, more preferably a viscosity of at least 10 Pa s, most preferably a viscosity of at least about 12.5 Pa s, such as a viscosity of about 15 Pa s. The mixture of step ii preferably has a viscosity of at most 150 Pa s, more preferably a viscosity of at most 100 Pa s, even more preferably a viscosity of at most 50 Pa s, most preferably a viscosity of at most 25 Pa s, for example a viscosity of at most 20 Pa s. The viscosity can be measured using any method known in the art. Preferably, the viscosity parameter is measured using a Stormer viscometer.

[0109] In step iii, the mixture of dissolved polymer and suspended urea adsorbent is extruded, for example co-extruded, or cast to form a film. Suitable details for this step are described below and illustrated in the examples.

[0110] In optional step iv, the film formed is cured. This can be done using any known method, for example as described below or as demonstrated in the examples. The preparation method of the invention preferably comprises step iv.

[0111] Further details of the method are preferably as follows: The method according to the present invention preferably comprises a coextrusion step using a spinning head having at least two concentrically arranged outlet openings, wherein a stream (A) containing a particulate material and a stream (B) of a polymer material in a solvent for a polymer material are fed separately and simultaneously through two adjacent outlet openings, after which the two streams are subjected to a phase inversion, preferably wherein the two streams are subjected to a two-step phase inversion process, to obtain the membrane according to the present invention as a fiber having a porous layer. Preferably, the stream (A) is a mixture comprising 0-50% by weight of the polymer matrix and 1-100% by weight of the particulate material. Preferably, the stream (B) comprises 3-50wt% of a polymer material. Preferably, the two-step phase inversion process comprises the use of a three-layer spinneret, wherein a stream (C) of a liquid, vapor or gas (preferably a liquid) is fed through the outermost third outlet to allow control of the pore size of the outer porous layer. It is further preferred that the stream (A) is fed through a spinning head on the inner side of the stream (B). In addition, preferably, a stream (D) of a polymer material in a solvent for the polymer material is coextruded, wherein the outlet opening for the feed of stream (A) is sandwiched between the outlet openings for the feed of streams (B) and (D), after which the three streams undergo a phase inversion to obtain the membrane according to the invention as a fiber having three porous layers. The phase inversion step is preferably followed by a heat treatment, a chemical treatment, a stretching or a further functionalization step to activate the particles, fix the porous structure of the fiber or reduce the particle size of the pores of the porous fiber.

[0112] Coextrusion is understood as the simultaneous extrusion of separate materials using a spinning head with multiple openings. Phase inversion is understood as phase separation, which can be induced by: temperature change of the homogeneous solution (thermal phase separation), evaporation of the solvent from a polymer solution containing a non-volatile non-solvent (evaporation-induced phase separation), penetration of non-solvent vapor (vapor-induced phase separation), or immersion of the homogeneous polymer solution in a non-solvent bath (immersion-induced phase separation). The latter is preferred in the preparation method of the present invention. Preferably, the two-step phase inversion method described in WO-A-2004 / 003268 specification, page 11, lines 2-20 is used. In short, before entering the coagulation bath, the outside of the nascent membrane, here the fiber shape, is in contact with the selected medium, resulting in a composition change of the outer layer. This is considered to be the first step of the phase separation process. When the membrane enters the coagulation bath, the nascent fibers will further phase separate and the structure will be blocked. This is considered to be the second step of the phase separation process. Use three-layer spinneret disclosed in WO-A-93 / 12868, in the first step, the logistics containing liquid, steam, gas or steam / gas mixture can be fed through the outermost 3rd outlet, to allow the pore size of the control outer porous layer. However, a method for preparing the film of hollow fiber form in which the pore size of an inwall is controlled is considered to be within the scope of the present invention. In this case, the logistics containing liquid, steam or gas is changed into the innermost outlet opening feed through spinning head.

[0113] Simple tube-in-hole spinnerets can also be used in the production method of the present invention, but provide less flexibility in changing the porosity of the fiber surface because no outlet openings are left in the first coagulation step to control the porosity of the outer layer. In addition to using a three-layer spinneret to control the porosity of the outer surface, the spun fibers can be spun through a "chimney" or closed box, where the atmosphere is controlled by a continuous flow of steam, gas or steam / gas mixture. When a hot coagulation bath is used, the steam evaporated from the coagulation bath can also be used to affect the outer layer pore structure.

[0114] In the coextrusion step, a stream (A) containing a particulate material and a stream (B) of a polymer material in a solvent for a polymer material are fed separately and simultaneously through two adjacent spinning head outlet openings. Stream (A) and stream (B) will eventually produce the first and second porous layers of the fiber, respectively. Preferably, based on the total weight of stream (A), stream (A) is a mixture of a polymer matrix containing 0-50wt%. The appropriate amount of particles depends on the type of polymer and the concentration of the polymer used. Typically, the amount of particles can vary between 1 and 95 weight %. Therefore, stream (A) contains 0-50 weight % of polymer material and 1-100 weight % of particulate material, and the rest is solvent, and the weight is based on the total weight of stream (A). More preferably, stream (A) contains 0.5-50 weight % of polymer material and 1-95 weight % of particulate material. Therefore, a fiber containing 100wt % of functionalized particulate material trapped in the second porous shell layer can be prepared in a single preparation step, and the film size is selected, preferably with an inner diameter of less than 0.5mm.

[0115] More preferably, stream (A) comprises 3-50 wt% and most preferably 5-20 wt% of polymeric material. Preferably, the polymer matrix content is less than 12 wt%, more preferably less than 10 wt%. The amount of particles in stream (A) is more preferably 1-97 wt% of stream (A), typically greater than 30 wt%, even more preferably greater than 40 wt%, most preferably 50-90 wt%, based on the dry weight of stream (A). The preferred amount depends on the specific polymer and particulate material used and the desired amount of particles in the first porous layer of the fiber to be obtained.

[0116] Stream (B) comprises 3-50 wt%, preferably 5-25 wt% of polymer material. In one embodiment, stream (B) is further supplied with 1 to 95 wt% of functionalized particulate material according to stream (A) to obtain a porous fiber having two adjacent layers of particulate material trapped in a polymer matrix, wherein the particulate material and / or the polymer matrix of the two layers may be different. For stream (A) and stream (B), the polymer material should be dissolved in a suitable solvent. Therefore, the type of solvent depends on the choice of polymer. Considering the phase inversion process, it is preferred to use a solvent that is well miscible with water. One or more solvents can even be used in combination with a non-solvent. Suitable solvents include, but are not limited to, N-methyl-pyrrolidone (NMP), dimethylacetamide (DMAc), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), formamide (FA), tetrahydrofuran (THF), [ε]-caprolactam, butyrolactone, especially 4-butyrolactone, cyclopentane, cyclohexanone and triethyl phosphate. Preferred solvents are NMP, DMAc, DMF, DMSO, THF, [ε]-caprolactam and 4-butyrolactone. Since the selection of polymers in stream (A) and stream (B) is independent of each other, the solvents can also be different. A mixture of solvents and non-solvents and additive components of any nature can be used in the coagulation bath to affect the structure of any layer of additives. Additives that can be applied to stream (A) and / or stream (B) for example affect viscosity, such as pore formers, such as viscosity enhancers, to reduce or prevent macropore formation and / or introduce hydrophilicity. Possible additives include, but are not limited to, polyvinylpyrrolidone (PVP), polyethylene glycol (PEG), polyethylene oxide (PEO), dextran, glycerol, diethylene glycol, (higher) alcohols such as octanol, carboxylic acids or organic acids such as oxalic acid, maleic acid, tartaric acid, fumaric acid, salts such as LiCl and CaCl2. Other additives have been described previously herein. It is within the capabilities of those skilled in the art to evaluate and apply suitable (mixtures) of (non)solvents, additives and process conditions to produce fibers with desired properties. Additives and / or non-solvents may partially replace the solvent and may vary between 0.01 and 50 wt%.

[0117] If a film in the shape of a fiber is to be obtained, in which the first porous layer entrained with particulate material forms an inner layer, then the stream (A) will be fed through the spinning head on the inner side of the stream (B), and vice versa for those embodiments in which the second porous layer is the outer layer of the fiber. For those embodiments in which a hollow core and / or a third layer or even more layers are to be obtained, it will be apparent to those skilled in the art that the spinning head can be adapted to include the desired number of outlet openings and to select the order in which the streams need to be submitted to these openings. In order to obtain a hollow core, it is known in the art, for example, to apply a drilling liquid stream (C) through the innermost opening, i.e. the needle. In the case where the fiber needs to retain a third polymer layer, this layer is formed by a stream (D), for which the same conditions and constraints as for stream (B) apply. For those cases in the coextrusion step, a stream (D) of polymer material in a polymer material solvent is coextruded with streams (A) and (B), wherein the outlet through which stream (A) is fed is sandwiched between the outlets through which streams (B) and (D) are fed, after which the three streams are phase-inverted.

[0118] As mentioned above, the phase inversion step preferably includes a coagulation medium. Water is a preferred coagulation medium. Other examples of possible coagulation media and non-solvents are methanol, ethanol, propanol, butanol, ethylene glycol, acetone, methyl ethyl ketone. In order to obtain the desired porosity in the fiber, a mixture of non-solvents and solvents is used in combination with changes in physical process parameters such as temperature, production rate, humidity, air gap length, stretching and winding speed.

[0119] In order to obtain the desired porosity in the membrane, a mixture of non-solvent and solvent is used, combined with changes in physical process parameters such as temperature, production rate, humidity, air gap length, stretching and winding speed. For fibers, the porosity of the membrane is mainly controlled by the flow of a liquid, vapor or gas stream, which passes through an outlet opening adjacent to the stream that eventually forms the fiber shell. The choice of the composition of the stream and the contact time before entering the coagulation bath determine whether the shell is dense or porous. When the stream that eventually forms the shell is in contact with air of moderate humidity, the surface of the outer layer becomes dense. In order to obtain the best accessibility of the entrapped adsorbent particles, it is preferred to allow a suitable medium to flow along the stream that eventually forms the shell during spinning. Preferably, the medium is a liquid mixture of a solvent and a non-solvent for the polymer. Preferably, the non-solvent is water.

[0120] Alternatively, a gas stream containing a non-solvent for polymer can be used. However, if steam is used, it is specified that the logistics that eventually forms the fiber shell layer contains a non-volatile solvent, so that the emission of the solvent into the steam path is smaller than that of the inward diffusion non-solvent steam. A vapor mixture of two non-solvents or a vapor mixture of a solvent and a non-solvent can also be used to influence fiber formation. In the case of a gas or steam stream, it is preferred that the non-solvent is water vapor. The technician can easily determine the amount of water vapor required for the first phase inversion effect in the gas stream. The porosity of the first porous layer can be controlled by changing the content of the polymer material, the amount and type of the additive, and the particle size, content and function of the particulate material, as explained in more detail in WQ-A-2004 / 003268, page 10, lines 4-26.

[0121] Therefore, the method effectively comprises the steps of contacting the adsorbent particles and the polymer as defined herein with a solvent to form a mixture, and extruding or casting the mixture, followed by solidification to form a membrane. The skilled person knows methods for preparing membranes, in particular mixed matrix membranes. An overview of membrane preparation techniques is given, for example, by Ladewig and Al-Shaeli (Fundamentals of Membrane Bioreactors - Chapter 2: Fundamentals of Membrane Methods, Springer 2017, pp. 13-37). A non-limiting example of a membrane preparation method is phase inversion. Phase inversion can be further specified in different techniques, such as precipitation by solvent evaporation, precipitation by controlled evaporation, thermal precipitation, precipitation from a gas phase, and impregnation precipitation. The latter is also referred to as non-solvent-induced phase inversion. In a preferred embodiment, solidification is a non-solvent-induced phase inversion, wherein the preferred non-solvent is water. It should be understood that in this case, after extrusion or casting, the mixture is substantially immediately contacted with water, for example by using a water bath. Preferably, extrusion of the mixture is performed using a spinneret. A particularly suitable method is described in EP1518011, which can be used to prepare the membrane of the present invention. In particular, the conditions described in

[0019] to

[0051] thereof are favorable.

[0122] Preferably, the polymer used to prepare the membrane of the present invention is at least one polymer selected from the group consisting of polysulfone, polyethersulfone, polyphenylsulfone, polyarylethersulfone, polyamide, polyetherimide, polyimide, polyethylene-co-vinyl alcohol, polyethylene-co-vinyl acetate, cellulose acetate, cellulose triacetate, polyvinylidene fluoride, polyvinyl chloride, polyacrylonitrile, polyurethane, polyetheretherketone and polyacrylic acid. Most preferably, the method comprises contacting the adsorbent particles as defined herein with polyethersulfone and polyvinylpyrrolidone.

[0123] In a preferred embodiment, the polymer content in the mixture for preparing the membrane is in the range of 3-50 wt%, preferably in the range of 5-35 wt%, most preferably in the range of 10-20 wt%, compared to the total weight of polymer and solvent (i.e., excluding the weight of adsorbent particles). Most preferably, the mixture comprises 5-15 wt% polyethersulfone and 1-5 wt% polyvinylpyrrolidone, compared to the total weight of polymer and solvent.

[0124] In a preferred embodiment, the solvent is selected from the group consisting of N-methylpyrrolidone (NMP), dimethylacetamide (DMAc), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), formamide (FA), tetrahydrofuran (THF), ε-caprolactam, butyrolactone, sulfolane, cyclohexanone and triethyl phosphate. NMP is the most preferred solvent. It is also preferred that the mixture consists essentially of the adsorbent particles, polymer and solvent as defined herein.

[0125] Device including membrane

[0126] The membrane of the present invention can be advantageously used in renal replacement therapy, such as peritoneal dialysis or hemodialysis. During this use, the membrane is usually present in a cartridge, which can be inserted replaceably into a (hemo) dialysis device. Therefore, the present invention provides a cartridge for a dialysis apparatus, which comprises a membrane according to the present invention. This dialysis device can be a hemodialysis device or a device for regenerating the peritoneal dialysis fluid in peritoneal dialysis. Therefore, the present invention provides a dialysis device, which comprises a membrane according to the present invention or a cartridge according to the present invention. This dialysis device can be a hemodialysis device or a device for regenerating the peritoneal dialysis fluid in peritoneal dialysis.

[0127] In addition to the membrane according to the present invention, such cartridges and dialysis devices are known in the art. In a particular embodiment, the cartridge is a disposable cartridge. In a particular embodiment, the cartridge is a regenerable cartridge (for example, when the adsorbent is a ninhydrin type adsorbent, it can be regenerated under acidic conditions, as described in WO2019110557). The cartridge may also be referred to as a box. The cartridge is preferably suitable for use with various different types of components and is arranged in various ways. The cartridge may include additional adsorbents or membranes. By removing nucleophilic waste solutes, the cartridge at least partially regenerates the dialysate and / or filtrate used during dialysis. The cartridge preferably includes a body with a fluid inlet and a fluid outlet. The interior of the cartridge is preferably constructed and arranged so that the fluid entering the interior from the inlet flows through the membrane and then through the outlet.

[0128] The membrane used in the dialysis device is preferably a semipermeable membrane. It can be in the form of a sheet and separates the two volumes by being a wall or being part of a wall. It can be in the form of a fiber bundle connecting the two volumes. A very suitable fiber bundle is described in WO2006019293, which describes a hollow or solid fiber bundle with a plurality of porous layers arranged concentrically.

[0129] The dialysis apparatus is a closed sterile system. It comprises one or two fluid circuits. It generally comprises two circuits: the so-called patient circuit, which is a fluid circuit arranged for a subject fluid such as blood or peritoneal dialysis fluid to flow through, and the so-called regeneration circuit, in which a dialysis fluid such as a dialysate and / or a filtrate circulates through a cartridge as described above. The two circuits are separated from each other by a (semi-permeable) membrane through which waste solutes can diffuse or transfer from the subject's fluid to the dialysate. Air, moisture, pathogens and fluids from the surrounding environment of the dialysis apparatus cannot enter the fluid circuit. The dialysis system only allows fluids (e.g., ultrafiltrate) and air to leave or enter these fluid circuits under a controlled environment.

[0130] The present invention also relates to a cartridge comprising a membrane according to the present invention. Preferably, the cartridge is suitable for use in a dialysis device. Preferably, the cartridge comprises a housing in which the membrane is placed. Preferably, the cartridge is constructed in such a way that during normal use, the membrane is in contact with a relevant fluid or mixture related to a treatment or non-treatment method for removing a compound containing amines or amides, respectively, as defined herein. Typically, the cartridge comprises at least one inlet and at least one outlet, respectively, for the inflow or outflow of a fluid.

[0131] The present invention also relates to a dialysis device comprising a membrane according to the present invention or a cartridge as described herein. Preferably, the dialysis device is a portable or wearable artificial kidney device. In a preferred embodiment, the dialysis device comprises at least one inlet and at least one outlet, respectively, for the inflow or outflow of fluid. It is also preferred that the dialysis device comprises a device allowing the temperature of the membrane of the present invention to be maintained at an elevated temperature, preferably in the range of 20°C to 90°C, more preferably in the range of 35°C to 80°C, most preferably in the range of 36°C to 75°C.

[0132] Medical Applications

[0133] In a fourth aspect, the invention provides medical applications of the membrane according to the invention. Thus, this aspect provides the use of the membrane according to the invention as a drug therapy, preferably in the treatment of a disease or condition associated with urea accumulation or improper urea removal. Such membranes are referred to herein as products used according to the invention. In this same application, cartridges as described above and dialysis devices as described above are provided, each of which comprises a membrane according to the invention (for use).

[0134] In the product used according to the invention, the product comprises an adsorbent, which is a substance or composition that achieves a medical effect and is a chemical entity or a composition of chemical entities. Here, the treatment comprises removing urea from the plasma of a patient suffering from a condition described herein. This effect is achieved by a specific binder for urea, which is an adsorbent, which is a chemical entity.

[0135] In a specific embodiment of this aspect, the present invention provides a membrane according to the present invention for use as a medicament for treating a disease or condition associated with the accumulation of ammonia or with inadequate removal of ammonia. In a further specific embodiment of this aspect, the present invention provides a membrane according to the present invention for use as a medicament, wherein the membrane is used to bind urea. In a further specific embodiment of this aspect, the present invention provides a membrane according to the present invention for use as a medicament, wherein the membrane is used to bind ammonia.

[0136] The treatment of a disease or condition can be the improvement, inhibition, prevention, delay, cure or prevention of the symptoms of the disease or condition, preferably the inhibition of the symptoms of the disease or condition. In the case of renal failure, urea can accumulate or can be insufficiently removed. Examples of diseases or conditions associated with urea accumulation or improper urea removal are end-stage renal disease (ESKD); severe acute renal failure; increased liver urea production due to gastrointestinal bleeding, for example; increased protein catabolism, for example due to extreme hunger due to trauma such as major surgery or muscle breakdown; increased renal reabsorption of urea, for example due to any cause of reduced renal perfusion, such as congestive heart failure, shock, severe diarrhea; iatrogenic conditions, due to the diuretic effect of urea infusion, due to drug therapy resulting in increased urea production, such as treatment with tetracyclines or corticosteroids; chronic renal failure; and urine outflow disorder.

[0137] The product for use according to the invention is suitable for use in a method of treatment. Such a method of treatment may be a method comprising the step of contacting a fluid from a subject, preferably a subject in need thereof, with a membrane according to the invention, preferably with an effective amount of the product for use according to the invention.

[0138] About dialysis treatment, the present invention can be used for various dialysis treatments to treat renal failure. As a term or similar term, dialysis treatment used in the full text is intended to include and cover any and all forms of treatment for removing waste, toxins and excess water from a subject suffering from a disease or illness. Hemotherapy, such as hemodialysis, hemofiltration and hemodiafiltration, includes intermittent therapy and continuous therapy for continuous renal replacement therapy (CRRT). Continuous treatment includes, for example, slow continuous ultrafiltration (SCUF), continuous venous hemofiltration (CVVH), continuous venous hemodialysis (CVVHD), continuous venous hemodiafiltration (CVVHDF), continuous arteriovenous hemofiltration (CAVH), continuous arteriovenous hemodiafiltration (CAVHD), continuous arteriovenous hemodiafiltration (CAVHDF), continuous ultrafiltration periodic intermittent hemodialysis, etc. The present invention can also be used for peritoneal dialysis, including, for example, continuous ambulatory peritoneal dialysis, automatic peritoneal dialysis, continuous flow peritoneal dialysis, etc. Furthermore, while in one embodiment, the present invention can be used in a method of providing dialysis treatment to a subject suffering from acute or chronic renal failure or nephropathy, it should be understood that the present invention can also be used for acute dialysis needs, for example, in an emergency room setting. However, it should be understood that the compositions of the present invention can also be effectively used in a variety of different applications, both physiological and non-physiological, in addition to dialysis.

[0139] In particular, the membrane according to the present invention is used to treat and / or prevent a disease selected from uremia and azotemia of a subject. In a preferred embodiment, the disease is uremia. Uremia is a disease with an undesirable high level of urea in the blood. The disease can be chronic or acute. It should be understood that during treatment and / or prevention, the membrane of the present invention can be in contact with one or more related fluids, such as the blood of the subject, or waste liquid produced by subjecting the subject to any one of hemodialysis, hemofiltration or hemodiafiltration or peritoneal dialysis. Hemodialysis, hemofiltration, hemodiafiltration and peritoneal dialysis are common methods for removing solutes from patient blood. In the setting of hemodialysis, blood flows on one side of the dialysis membrane, and the dialysate flows on the other side of the membrane. In hemodialysis, solutes flow to the dialysate through the membrane mainly due to the difference in concentration (i.e. diffusion). In hemofiltration, dialysate is not used. On the contrary, positive hydrostatic pressure drives water and solutes from the blood chamber through the filter membrane to the filtrate chamber, and is discharged from the filtrate chamber. Solute and water move across the membrane, and are removed from the blood due to the convection caused by the hydrostatic pressure difference. Replacement fluid is added to the blood (before and / or after blood contacts the dialysis membrane), to replace the supplement of the water transported on the membrane. Hemodiafiltration is a combination of hemodialysis and hemofiltration. Therefore, blood flows on one side of the dialysis membrane, and dialysate flows on the other side of the membrane, and replacement fluid is added to blood (before and / or after blood has contacted the dialysis membrane), and the transportation of solute from blood to the dialysis solution is based on diffusion and convection. In typical hemodialysis, hemofiltration or hemodiafiltration therapy, blood returns to the patient after contacting the dialysis membrane. Waste liquid contacted with the membrane of the present invention can be (again) used as, for example, dialysate or replacement fluid, because membrane removes amine-containing compounds, particularly urea, from the waste liquid. This is advantageous, especially in the microdialysis system of such as portable and wearable artificial kidney devices, especially because a small amount of fluid is required for treatment. Waste liquid can be directly recirculated during treatment, or alternatively stored for later use. In the case of hemodialysis, the waste liquid is waste dialysate. In the case of hemofiltration, the waste liquid is water containing solutes that has been in contact with the subject's blood and is pushed through the membrane due to convection. In the case of hemodiafiltration, the waste liquid is one or more waste dialysates, and water containing solutes that has been in contact with the subject's blood and is pushed through the membrane due to convection. In a preferred embodiment, the membrane is used to treat and / or prevent, preferably treat a disease selected from the group consisting of uremia and azotemia in a subject, wherein the subject undergoes hemodialysis, hemofiltration or hemodiafiltration or peritoneal dialysis, and wherein the membrane is in contact with the waste liquid as defined herein, and preferably the membrane is not in direct contact with the subject's blood.In a preferred embodiment, during the treatment, the membrane is maintained at an elevated temperature, preferably in the range of 20°C to 90°C, more preferably in the range of 35°C to 80°C, and most preferably in the range of 36°C to 75°C. In a preferred embodiment, the subject is a human. The subject can be of any gender, and similarly, the treatment is not limited to subjects of a particular age or any other characteristics. Preferably, the treatment is selected from the group consisting of hemodialysis, hemofiltration, hemodiafiltration and peritoneal dialysis. In any of these treatments, the duration of the treatment is preferably in the range of 1 to 36 hours, more preferably in the range of 1 to 24 hours. Most preferably, when the treatment is hemodialysis, the duration of the treatment is 4-8 hours. The present invention also relates to a method for treating and / or preventing a disease selected from the group consisting of uremia and azotemia, preferably uremia, in a subject as defined herein, the method comprising the step of contacting the blood of the subject and / or contacting the waste fluid produced by subjecting the subject to any one of hemodialysis, hemofiltration, hemodiafiltration or peritoneal dialysis; using a membrane according to the present invention. The treatment and / or prevention is preferably as disclosed above.

[0140] How to use

[0141] The membranes according to the invention are surprisingly effective in binding nucleophilic solutes, preferably nucleophilic waste solutes. In a fifth aspect, the invention provides a method for removing nucleophilic waste solutes from a fluid, comprising the steps of:

[0142] i) providing a fluid comprising a nucleophilic waste solute,

[0143] iia) bringing the fluid into contact with a membrane according to the invention or with a cartridge according to the invention, or alternatively

[0144] iib) contacting the liquid with a dialysate through a membrane, wherein the dialysate is in contact with a membrane according to the invention, or with a cartridge according to the invention, and

[0145] iii) optionally, regenerating the fluid.

[0146] This method is hereinafter referred to as the method for combining according to the present invention. The method may be a continuous process, wherein providing a fluid comprising a nucleophilic waste solute is by providing a fluid that flows continuously. In this case, preferably step iii) is not optional, and is also carried out continuously. The method for combining according to the present invention always comprises step i), step ii) (one of step iia) or step iib)), and optional step iii). The membrane in step iib) is preferably not a membrane according to the present invention, or a membrane according to the present invention, and the membrane further has a membrane according to the present invention described in step iib).

[0147] Nucleophilic waste solutes are dissolved nucleophilic substances that need to be removed. For example, in human blood, urea is a waste solute. In unpurified water used as drinking water, most organic nucleophiles are waste solutes. Examples of nucleophilic waste solutes are ammonia, urea, creatinine and small molecule organic amines, thiols or alcohols. Chemical binding properties make the membrane according to the present invention very suitable for various applications subjected to physiological and / or non-physiological conditions. In one embodiment, the membrane according to the present invention can be used to remove metabolic wastes, such as urea, creatinine, uric acid and / or other similar uremic toxins, biological substances, protein substances, etc. from blood, peritoneal dialysis fluid and / or solutions for dialysis and / or filtering blood, such as dialysate and / or filtrate. Due to its relevance described elsewhere in this article, it is highly preferred that nucleophilic waste solutes are urea and ammonia. In a preferred embodiment, the nucleophilic waste solute is ammonia. In other preferred embodiments, the nucleophilic waste solute is urea.

[0148] In step i), a fluid containing nucleophilic waste solutes is provided. This can be wastewater to be purified, can be a waste solvent to be purified, but can also be a (body) fluid from a subject, such as blood or peritoneal dialysis fluid. When the fluid of step i) is a fluid from a subject, it is preferably blood or peritoneal dialysis fluid, most preferably blood, and preferably a fluid previously obtained from a subject.

[0149] In step ii), there are two options. In a selection, step iia), the fluid itself directly contacts with the film according to the present invention, the composition according to the present invention or the film or cartridge according to the present invention. Step iia) is very suitable for the purification of solvents, or is suitable for fluids that are not intended for consumption or for medical purposes after removing waste solutes. Step iib) is separated by using dialysate and / or filtrate by the binding membrane of the present invention and the fluid provided in step i). Step iib) is particularly suitable for removing nucleophilic waste solutes from drug solutions or from fluids such as the body fluids of the subject derived from the subject. Contact preferably continues 24 hours, 12 hours, 6 hours, 4 hours, 3 hours, 2 hours, 60 minutes, 50 minutes, 40 minutes, 30 minutes, 20 minutes, 15 minutes, 10 minutes, 9 minutes, 8 minutes, 7 minutes, 6 minutes, 5 minutes, 4 minutes, 3 minutes, 2 minutes or 1 minute or shorter. Contact can also be continuous flow through adsorbent, in which case the total amount of the waste solute removed is more relevant.

[0150] Further, the membrane for separating fluid in step iib) is preferably a semipermeable membrane. These are known in the art, and can be, for example, a semipermeable membrane present in a conventional (hemo) dialysis device. The membrane according to the present invention as described above can also be used. Dialysate is known in the art, and can be in the range from ultrapure water to physiological buffer. The non-limiting example of dialysate is a medium comprising a known amount of Na, K, Ca, Mg, Cl, acetate, HCO3 and glucose, such as those obtained from MDN Neubrandenburg GmbH (Neubrandenburg, Germany) or from Baxter (Deerfield, Illinois, USA) or from Dirinco BV (Oss, the Netherlands).

[0151] In optional step iii), regenerate fluid. The membrane according to the present invention is porous or macroporous and is usually swellable in an aqueous medium so that a fluid can flow through it and permeate it. Regeneration of a fluid that has been in contact with an adsorbent is easily achieved by filtering, centrifuging or removing a cartridge containing an adsorbent. Regeneration of the fluid allows it to be further processed, or it is returned to the subject. In a preferred embodiment of this aspect, regenerate fluid.

[0152] Preferably, when the fluid is regenerated in step iii), the relevant physiological parameters are subsequently analyzed and adjusted where appropriate. Examples are ion concentration, osmotic concentration, pH, in particular Na concentration, Ca concentration and Mg concentration. Therefore, a preferred step iii) is a step of regenerating the fluid, after which at least one of the fluid pH, fluid sodium concentration, fluid magnesium concentration and fluid calcium concentration is determined and optionally adjusted to a reference value. A preferred reference value is a corresponding physiological value for the type of fluid. The adjustment can be performed in any suitable manner known in the art. Preferably, the adjustment is performed when a deviation from a reference value is detected.

[0153] In a preferred embodiment of the combined method, at least 1.40, 1.41, 1.42, 1.43, 1.44, 1.45, 1.46, 1.47, 1.48, 1.49, 1.50, 1.51, 1.52, 1.53, 1.54, 1.55, 1.56, 1.57, 1.58, 1.59, 1.60, 1.61, 1.62, 1.63, 1.64, 1.65, 1.67, 1.68, 1.69, 1.70, 1.71, 1.72, 1.73, 1.74, 1.75, 1.76, 1.77, 1.78, .78, 1.79, 1.80, 1.85, 1.90, 1.95, 2.00, 2.05, 2.10, 2.15, 2.20, 2.25, 2.30, 2.35, 2.40, 2.45, 2.50, 2.60, 2.70, 2.80, 2.90, 3.00 or 3.10 mmol of nucleophilic waste solutes are removed per gram of adsorbent; preferably, at least 1.55, 1.56, 1.57, 1.58, 1.59, 1.60, more preferably at least 2.20, even more preferably at least 2.50, and most preferably at least 2.55 mmol of nucleophilic waste solutes are removed per gram of adsorbent. Such removal preferably entails removing at least 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 85%, 90%, 91%, 92%, 93%, 94%, 95% or more of the initial concentration of the specific nucleophilic waste solute from the fluid provided in step i), and more preferably removing at least 50% or more.

[0154] The membrane of the present invention can also be used to remove amine- or amide-containing compounds from a mixture. Preferably, the compound is urea. It is also preferred that the mixture is as defined herein for a non-therapeutic method of removing amine- or amide-containing compounds. It should be understood that the use is preferably a non-therapeutic use.

[0155] The present invention also relates to a non-therapeutic method for removing amine- or amide-containing compounds from a mixture, wherein the method comprises contacting the mixture with a membrane according to the present invention. Preferably, the compound is urea. In a preferred embodiment, the mixture is an aqueous solution, such as a patient sample. Possible applications include removing amine-containing compounds from patient samples such as blood or urine or dialysates such as peritoneal dialysis fluids, for example to prepare the sample for further analysis. In other applications, the aqueous solution may, for example, contain a large amount of urea and biomolecules, such as proteins that denature under these conditions. In a preferred embodiment, in a non-therapeutic method, the membrane is maintained at an elevated temperature, preferably in the range of 20°C to 90°C, more preferably in the range of 37°C to 80°C, and most preferably in the range of 60°C to 75°C.

[0156] General Definition

[0157] In this document and its claims, the verb "comprise" and its variations are used in its non-restrictive sense, meaning to include the items after the word, but not excluding items not specifically mentioned. In addition, referring to an element by the indefinite article "a" or "an" does not exclude the possibility of having more than one element, unless the context clearly requires the presence and only one element. Therefore, the indefinite article "a" or "an" usually means "at least one". When used in conjunction with a numerical value (e.g., about 10), the word "about" or "approximately" preferably means that the value can be a given value of about 5% or less of the value. As used herein, "subject" refers to any animal, preferably a mammal, most preferably a human being. In a preferred embodiment, the subject is non-human.

[0158] In the context of the present invention, a decrease or increase in a parameter to be evaluated means a change of at least 5% in the value corresponding to the parameter. More preferably, a decrease or increase in a value means a change of at least 10%, even more preferably at least 20%, at least 30%, at least 40%, at least 50%, at least 70%, at least 90% or 100%. In the latter case, it may be the case that there is no longer a detectable value associated with the parameter.

[0159] The use of a substance as a drug as described herein may also be construed as the use of the substance in the production of a drug. Similarly, whenever a substance is used in therapy or as a drug, it may also be used in the preparation of a drug for therapy. The product used is suitable for use in a method of treatment.

[0160] In this application, when percentages are used to express the amount of monomers and comonomers in a mixture, these are mole percentages unless otherwise stated or clearly clear from the context.

[0161] In the present application, (hemo)dialysis refers to hemodialysis and dialysis. In general, a dialysis device may refer to any type of dialysis device as described herein.

[0162] The invention has been described above with reference to a number of exemplary embodiments. Modifications and alternative implementations of some parts or elements are possible and are included within the scope of protection as defined in the appended claims. All cited documents and patent documents are hereby incorporated by reference. BRIEF DESCRIPTION OF THE DRAWINGS

[0163] Figure 1 - Scanning electron microscopy image of a mixed matrix membrane prepared as described in Example 2. Figure 1 A) Cross-sectional image of the MMM corrugated lumen morphology of the membrane. Figure 1 B) Magnified image of the MMM wall showing the finger-like macroporous structure. The adsorbent particles are well dispersed without aggregation, and they are well surrounded by the polymer solution (white arrows). Figure 1C and 1D show the lumen (inner layer) and outer layer of the MMM, respectively, which presents a very thin dense layer on the lumen surface ( Figure 1 E) or outer surface ( Figure 1 F) has no visible pores. Compared with the inner dense layer (0.2 μm), the outer dense layer ( Figure 1 D) Slightly thicker (0.5 μm).

[0164] Figure 2 - Water permeability of MMMs prepared as described in Example 2 under varying pressures. Data are presented as mean ± SE (n=6). Linear approximation yields a value equal to 238 ± 9 L / (m 2 ·h·Bar) water permeability.

[0165] Figure 3 - Urea binding kinetics measured at 37°C, 50°C and 70°C using ninhydrin-type adsorbent particles in suspension (containing about 2.5 mmol ninhydrin per gram of adsorbent) with a mean diameter of 483±282 μm±SD (n=30).

[0166] Figure 4 - Urea binding results obtained over time on ninhydrin-type adsorbent particles (containing about 2.5 mmol / g ninhydrin) in suspension before (diameter of 483±282 μm±standard deviation) and after (diameter <63 μm) grinding and sieving (n=3).

[0167] Figure 5 - Urea binding results obtained over time on ninhydrin-type adsorbents (diameter < 63 μm) in suspension and on MMMs comprising particles of such adsorbents (mean ± standard deviation).

[0168] Figure 6 - Isotherms of urea binding on MMMs containing adsorbent prepared as described in Example 2 and on control hollow fibers (HF, PES / PVP) without adsorbent particles prepared as described in Example 2.2 (n=3).

[0169] Figure 7 - Dynamic urea binding results using MMMs containing adsorbent particles prepared as described in Example 2 In this experiment, urea solution was continuously recirculated through the membrane for 4 hours (n=5). The urea binding at 4 hours (indicated by asterisks) has been normalized by the amount of urea eluted from the MMMs.

[0170] Figure 8 - Urea binding kinetics using MMMs containing PGA-type adsorbent particles, prepared in the form of hollow fibers as described in Example 2. Here, the urea solution was continuously recirculated through the MMMs (n=2) or continuously stirred with ground adsorbent particles (n=3). The PGA-type adsorbent in the membranes showed a faster urea binding behavior than the free PGA-type adsorbent ground to obtain small particles.

[0171] Example

[0172] Example 1 - Preparation of adsorbent

[0173] 1.1 Preparation of ninhydrin-type adsorbent

[0174] Adsorbents of this type are known in the art and can be prepared, for example, as described in EP121275A1, US4897200A or WO2019110557.

[0175] 1.2 Preparation of PGA-type adsorbent

[0176] Adsorbents of this type are known in the art and can be prepared, for example, as described in US 3933753 A or WO 2004078797 A1. Alternatively, it can be produced as described below.

[0177] 1.2.1 Preparation of precursor monomers

[0178] In a three-necked round-bottom flask, p-(ethynylphenyl)ethanone (10.0 g, 69.4 mmol) was suspended in EtOH (350 mL) and Lindlar's catalyst (300 mg, 3 w%) was added. The air was replaced with H2 and the suspension was stirred at room temperature for 2-16 hours. In order to monitor the conversion (and thus prevent excessive reduction of VPE to alkanes), samples were frequently taken from the reaction mixture and, after evaporating EtOH under reduced pressure, were filtered by 1 The conversion rate was determined by H-NMR (CDCl3). After the conversion rate was > 90%, the balloon filled with H2 was removed and the reaction mixture was concentrated under reduced pressure. The crude product was redissolved in CH2Cl2 and purified by filtration through Hyflo. The filtrate was concentrated under reduced pressure to obtain crude pVPE (p-(vinylphenyl)ethanone) as a yellow liquid with a yield of 99% (10.1 g, 69.0 mmol). Melting point 29°C, melting enthalpy 90.6 J / g. 1H-NMR (CDCl3, 600MHz) δ7.92 (d, J=8.3Hz, 2H), 7.48 (d, J=8.2Hz, 2H), 6.75 (dd, J= 17.6Hz, 10.9Hz, 1H), 5.87 (d, J=17.6Hz, 1H), 5.39 (d, J=10.9Hz, 1H), 2.59 (s, 3H).

[0179] 1.2.2 Polymerization Precursor Monomers

[0180] Use two-phase suspension polymerization. Briefly, the aqueous phase is prepared by adding NaCl (11 mg), polymethacrylic acid sodium salt solution (452 ​​mg of 10% gel in water) and CaHPO4 (84 mg) to water (15 mL). The organic phase consists of VPE (2.1 g, 14.4 mmol, 2 mL), pore former (2.9 mL, heptane / toluene), 80% technical grade divinylbenzene (3-6 mol%) and a mixture of 50% benzoyl peroxide and dicyclohexyl phthalate (174 mg, 0.36 mmol, 2.5 mol%). After mixing and polymerization (heating at 73° C. in an oil bath under mechanical stirring for 16 hours), the resulting suspension is cooled to room temperature and poured onto a filter (cut-off 200 μm, Veco BV). The residue was washed with acetone and water and finally dried over P2O5 under vacuum to obtain pVPE (1.1-1.9 g, yield 52-90%).

[0181] 1.2.3 Preparation of PGA-type adsorbent based on poly-VPE

[0182] The obtained crude pVPE mixture is then further converted into a PGA type adsorbent. The acetyl aromatic groups in the pVPE beads are halogenated and subsequently converted into PGAH-groups in a one-pot process by Kornblum oxidation. In a glass reactor equipped with a polytetrafluoroethylene blade stirrer, pVPE beads (60.0 g) are swollen in DMSO (600 mL, 8.45 mol) for 30 minutes under continuous stirring, after which a 48% aqueous HBr solution (175 mL, 1.55 mol) is slowly added. One outlet of the reactor is covered with a septum containing a needle to allow the generated Me2S to escape. The suspension is stirred at 80°C for 8 hours, and then the reaction mixture is filtered (cutoff 200 μm, Veco BV). The residue is washed with water until the pH of the filtrate is >5, and the residue is dried over P2O5 under vacuum to obtain a PGA type adsorbent (55.2 g).

[0183] Example 2 - Preparation of membranes containing adsorbents

[0184] 2.1 General method for preparing membranes containing adsorbents

[0185] The required amount of polymer is weighed and thoroughly dissolved in ultrapure NMP. After three days of stirring, dry adsorbent particles with a maximum diameter of 120 μm are added and the suspension is stirred on a roller row for four hours. The resulting suspension is then cast on water to form a sheet film or extruded through a spinneret to form fibers.

[0186] 2.2 Preparation of PES / PVP membrane containing ninhydrin-type adsorbent

[0187] Prior to membrane preparation, particles of ninhydrin-type adsorbent or PGA-type adsorbent with an average diameter ± standard deviation of 483 ± 282 μm (e.g., about 2.5 mmol ninhydrin per gram of particles) were ground using a mortar and pestle. The ground adsorbent particles were then sieved through a 63 μm sieve. Hollow fiber (HF) mixed matrix membranes (MMMs) were prepared using adsorbent particles embedded in a PES / PVP polymer matrix. HF MMMs were prepared by dry-wet spinning techniques. A polymer coating solution was prepared by dissolving Ultrason E6020 PES (BASF, Ludwigshafen, Germany) and PVP K90 (molecular weight ≈ 360 kDa, Sigma-Aldrich Chemie GmbH, Munchen, Germany) in ultrapure N-methylpyrrolidone (NMP) (Acros Organics, Geel, Belgium). The particles were added to the coating solution so that the final weight of the particles was equal to 55% of the dry weight of the membrane. The PES / PVP / adsorbent polymer solution was stirred at 60°C for two days to ensure proper dispersion of the particles in the polymer solution. It was then transferred to a stainless steel syringe and left for 24 hours to degas. The concentrations of PES, PVP and adsorbent used for the study and the spinning parameters are detailed in Table 1. After degassing, the syringe was connected to a high-pressure injection pump and a spinneret to prepare HF (specifications in Table 1). Ultrapure water was used as a pore-forming solution. The air gap between the spinneret and the coagulation bath was adjusted to 5.5 cm. HF fell freely in the water coagulation bath. The prepared membrane was washed with demineralized water and stored in demineralized water for further use.

[0188]

[0189] Table 1 - Spinning parameters of mixed matrix membranes

[0190] Example 3 - Characterization of membranes containing adsorbents

[0191] 3.1 Scanning electron microscopy (SEM)

[0192] The morphology of HF MMMs (prepared as described in Example 2.2) was analyzed by SEM (JEOL JSM-IT 100, Tokyo, Japan). Samples of the membranes were dried in air and broken in liquid nitrogen to image the cross-sections. Prior to SEM imaging, the samples were gold sputtered (Cressington 108 automated sputtering (Cressington Scientific Instruments, Watford, UK).

[0193] Cross-sectional image of MMM ( Figure 1 A) shows the corrugated lumen morphology of the membrane. Although the corrugated morphology may indicate some instability of the membrane forming system, the grooves are well aligned with the flow direction axially. Such corrugations generally do not interfere with mass transfer, flow rate, and transmembrane pressure along the fiber. In addition, the presence of grooves in the lumen side of the fiber increases the active surface area, with advantages regarding the filtration and diffusion properties of the membrane. Moreover, the thick wall of the membrane allows more particles per unit length to be embedded in the polymer matrix, thereby enhancing the capture performance of the MMM.

[0194] From the enlargement of the MMM wall ( Figure 1 B) It can be seen that the typical finger-like macroporous structure of the SEM membrane can be seen in the inner cavity and outside of the membrane, while it disappears along the center of the wall cross section, where more particles are accommodated in the polymer matrix. The adsorbent particles are well dispersed without aggregation, and they are well surrounded by the polymer solution ( Figure 1 White arrow in B).

[0195] The inner and outer layers of the MMM (respectively Figure 1 C and 1D) have a very thin dense layer on the surface of the lumen ( Figure 1 E) or outer surface ( Figure 1 F) have no visible pores. However, compared with the inner dense layer (0.2 μm), the outer dense layer ( Figure 1 D) Slightly thicker (0.5 μm). For this reason, it is believed that the selective layer of the membrane that determines the molecular weight cut-off and filtration performance of the membrane is the outer dense layer.

[0196] 3.2 Water transmission experiment

[0197] The MMMs were also characterized for their water transport properties. 2Membrane components. 2-component epoxy glue (Griffon Combin Snel-Rapide, Bison International, Gos, the Netherlands) was used to prepare the components. Before the water transport experiment, the HF modules (n = 6) were pre-wetted with EtOH at a transmembrane pressure (TMP) of 0.2 Bar for 30 minutes and pre-compacted with ultrapure water at a TMP of 0.6 Bar for 30 minutes. Then, the amount of permeated water was measured over time at TMPs of 0.2, 0.4 and 0.6 Bar. The resulting water permeability was calculated as the water flux (L / (m 2 h)) is the slope of the linear fit of TMP (Bar). MMM is the water permeability equal to 238 ± 9 L / (m 2 ·h·bar) of ultrafiltration membrane ( Figure 2 ). Ultrafiltration coefficient of MMM (K uf ) is 309mL / (h·mmHg·m 2 ). The water flux through the membrane increased linearly with pressure, and there was no compression or rupture of the HF MMMs. In summary, these results indicate that the MMMs have excellent morphological characteristics and filtration properties for ultrafiltration.

[0198] Example 4 - Capture of urea using a membrane containing an adsorbent

[0199] 4.1 Steady-state capture of urea

[0200] 4.1.1 Effect of temperature on urea binding kinetics using ninhydrin-type adsorbents

[0201] Urea kinetic binding experiments were performed at 37°C, 50°C and 70°C to study the effect of temperature on the binding reaction of urea to ninhydrin groups in ninhydrin particles prepared from cross-linked polystyrene (PS-Nin) (about 2.5 mmol / g adsorbent). The free particles used for this experiment had an average diameter of 483±282 μm±standard deviation (N=30). Adsorbent beads (15 mg) were incubated with a urea solution (1.5 mL, 30 mM) in PBS. After 1, 2, 4, 8, 16 and 24 hours, the samples (n=3 for each time point) were placed in an oven on a rotating device and the urea concentration in the supernatant was analyzed at 37, 50 or 70°C using an AU 5800 conventional chemical analyzer (Beckman Coulter, Brear, CA) using a coupled enzyme reaction to obtain a colorimetric product (570 nm) proportional to the urea concentration. The amount of bound urea was calculated from the depletion of urea in solution by mass balance. Figure 3The results in are shown as mean ± standard deviation. Urea binding kinetics were faster at higher temperatures. In fact, at 70 °C, the particles bound 1.4 ± 0.0 mmol / g urea over a period of 24 h, which is much higher than in the case of binding at 50 °C and 37 °C. Even at 70 °C, saturation of the ninhydrin moiety with urea was not reached within 24 h. Here, the maximum achievable saturation was determined to be 1.6-1.7 mmol / g for the particles. Taking into account the faster binding kinetics at 70 °C, urea binding experiments were subsequently performed at 70 °C.

[0202] 4.1.2 Effect of particle size on urea binding kinetics

[0203] To investigate the effect of particle size on urea binding, urea kinetic binding experiments were performed at 70°C on PS-nin particles with an average diameter of 483 ± 282 μm (approximately 2.5 mmol / g ninhydrin) and on the same particles with a diameter less than 63 μm after grinding and sieving (Example 2.2). Larger adsorbent beads (15 mg) were incubated with urea solution (1.5 mL, 30 mM) in PBS (pH 7.4); the ground and sieved particles were incubated in urea solution (1.5 mL, 30 mM) in dialysate (pH 7.4). The samples were shaken at 70°C (n = 3 per time point) and the supernatant was collected by filtration after 1, 2, 4, 8, 16 and 24 hours. Urea concentration was determined by enzymatic assay Urea FS* (Diasys, Holzheim, Germany) or by AU 5800 conventional chemical analyzer (Beckman Coulter, Brea, CA). Both methods are based on a coupled enzymatic reaction that produces a colorimetric product proportional to the urea concentration. The amount of bound urea is calculated from the depletion of urea in solution by mass balance. Figure 4 The results in are shown as mean ± standard deviation. The urea binding kinetics on the smaller particles are much faster than on the larger particles. At 4 hours, the binding of urea on the smaller particles is more than twice that on the larger particles. The urea binding kinetics on the small particles are very fast in the first 4 hours and then slowly decrease. Over a period of 24 hours, the amount of urea bound is equal to 1.7 ± 0.1 mmol / g urea on the smaller particles and 1.4 ± 0.0 mmol / g urea on the larger particles. Despite the higher surface area, the maximum binding capacity (2.5 mmol / g) is not reached. Therefore, the particle size has a strong effect on the binding kinetics, but a much smaller effect on the binding capacity.

[0204] 4.1.3 Urea binding kinetics of MMM containing adsorbent particles

[0205] To investigate the effect of particle incorporation into the polymer matrix of MMMs, urea kinetic binding experiments were performed at 70°C on ground PS-Nin particles (approximately 2.5 mmol / g ninhydrin) with a diameter of less than 63 μm and on MMMs prepared as described in Example 2.2. Adsorbent beads (15 mg) and MMMs (27 mg, containing 15 mg embedded particles) were incubated with urea solution (1.5 mL, 30 mM) in dialysate (pH 7.4) and shaken at 70°C for 1, 2, 4, 8, 16 and 24 hours, the supernatant was collected (by filtering the particles) and the urea concentration in the supernatant was determined using an enzyme assay (Urea FS*, Diasys, Holzheim, Germany). The amount of bound urea was calculated by mass balance from the depletion of urea in the solution. Each time point is represented by three different samples (n=3) ( Figure 5 ). Figure 5 The results in are shown as mean ± standard deviation. Over an 8 h period, the urea binding kinetics are very similar for the suspended particles and the particles in MMMs. Interestingly, at 8 h, urea binding in suspension reaches a plateau, while the particles embedded in MMMs remain bound. At 24 h, urea binding to the particles in suspension is equal to 1.7 ± 0.1 mmol / g, while it is 2.1 ± 0.1 mmol / g for the particles embedded in MMMs. After a longer period of time, urea binding to the particles in MMMs can reach saturation (maximum binding capacity of about 2.5 mmol / g). This illustrates how the polymer matrix does not limit the ability of urea to reach the particles; significant binding is even enhanced compared to free adsorbent particles.

[0206] Further improved urea binding was demonstrated using a PGA-type adsorbent in a hollow fiber MMM. In a comparative experiment, MMMs containing 88 mg of PGA-type adsorbent were contacted with a PBS buffer containing 30 mM urea at a temperature of 70°C using a recirculation device with a flow rate of 5 mL / min (total volume 25 mL). Urea binding was determined at different time points, as shown in FIG. Figure 8 As shown (n=2; for t=6-8h, n=1). For comparison, static batch experiments were performed using 5 mg of the same PGA-type adsorbent in a total volume of 1 mL of the same urea solution under continuous stirring at 70°C and urea binding was determined at different time points (n=3). Figure 8 The results in show that the binding kinetics of PGA-type adsorbents in MMMs are faster than those of the ground adsorbents under stirred conditions.

[0207] 4.1.4 Urea isotherms of combined MMM and control membranes

[0208] Urea binding at different concentrations was measured with MMM (prepared as described in Example 2.2) and PES / PVP control HF. The PES / PVP control HF was prepared using dry-wet spinning technology, as described in Acta Biomaterialia 90 ((2019))100. Briefly, the polymer coating solution was prepared by dissolving Ultrason E6020 PES (15 wt%) (BASF, Ludwigshafen, Germany) and PVP K90 (7 wt%) (molecular weight ≈ 360 kDa, Sigma-Aldrich Chemie GmbH, Munchen, Germany) in ultrapure NMP (78 wt%) (Acros Organics, Geel, Belgium). The polymer solution was mixed on a roller table for 3 days, after which it was transferred to a stainless steel syringe and left to degas for 24 hours. The syringe was then connected to a high-pressure syringe pump and a designed spinneret. The dopant solution pumping rate was set to 0.4 mL / min. Ultrapure water was used as the pore solution, and the pumping speed of the pore solution was set to 1.2 mL / min. The air gap between the spinneret and the coagulation bath was adjusted to 10 cm. A collecting wheel (speed 8.3 m / min) was used to collect the generated HF. The prepared membrane was washed with demineralized water and stored for further use.

[0209] 27 mg MMM (15 mg granules in MMM) and 27 mg control HF were incubated with 1.5 mL urea solution in the dialysate (pH 7.4) at different concentrations. After 24 hours, the samples were placed in a horizontal shaking water bath at 70°C, the supernatant was collected, and the urea concentration in the supernatant was determined using an enzyme assay (Urea FS*, Diasys, Holzheim, Germany). The amount of bound urea was calculated from the depletion of urea in the solution by mass balance. Figure 6 The results in are shown as mean ± standard deviation (N=3). The figure shows the relationship between binding capacity (mmol / g) and equilibrium urea concentration (mM). The PES / PVP control HF did not bind urea, indicating that only the adsorbent particles inside the MMMs were responsible for urea binding.

[0210] Interestingly, at an equilibrium concentration of 90.1 mmol / g, the amount of urea bound to MMM was equal to 3.4 ± 0.1 mmol / g, exceeding the expected value for a 1 to 1 binding to ninhydrin. This higher binding of urea can be explained via multilayer binding of urea, where urea molecules adsorb via hydrogen bonds (physisorption) to urea covalently bound (chemisorption) to the ninhydrin moiety of the particle.

[0211] 4.1.5 Urea dynamic binding

[0212] The total surface area of ​​the 3HF (prepared as described in Example 2) was 23.3 cm 2 The membrane assembly with a total amount of particles embedded in the PES / PVP matrix equal to 77 mg was used to study urea binding under dynamic conditions. 2-component epoxy glue (GriffonCombin Snel-Rapide, Bison International, Gos, the Netherlands) was used to prepare the assembly. Before the dynamic urea binding experiment, the HF module (n = 5) was kept in half water. A dedicated device (Convergence, Enschede, the Netherlands) was used to perform a urea dynamic experiment in filtration mode (TMP = 0.15 Bar), in which a urea solution 30mM in the dialysate was continuously recirculated through the fiber at a flow rate of 20mL / min. The binding experiment (n = 5) was performed at 70°C for 4 hours. In order to maintain the temperature of the urea solution at 70°C in the recirculating system, the feed solution was heated to 70°C, the pipes were insulated, and the HF module was immersed in a water bath heated to 90°C, and samples of the urea solution were collected every hour for quantification. At the end of the binding experiment, the HF module was removed from the 90°C water bath and emptied. 24.5 mL of MilliQ water was recirculated through the module at a flow rate of 20 mL / min for 1 hour at room temperature to collect urea that could elute from the MMM. Urea concentration was quantified using an enzymatic assay (Urea FS*, Diasys, Holzheim, Germany).

[0213] The combined results are shown in Figure 7 , after a period of 4 hours, the membrane was able to bind 3.4±0.3mmol / g and did not seem to reach saturation. When the binding experiments were performed in dynamic mode, the binding kinetics were much faster than static conditions. Not only were the kinetics faster, but the total amount of urea bound to the adsorbent particles was also higher compared to static conditions. The amount of urea bound per gram of particles in the MMM was higher than the total amount of ninhydrin moieties in the particles (about 2.5mmol / g). The reasons are 1) all ninhydrin moieties in the particles are saturated, and 2) urea molecules adsorb on urea covalently bonded (chemisorption) to the ninhydrin moieties of the particles through hydrogen bonds (physical adsorption), thus having multilayer bonding, which can be achieved by saturating the formed surface with covalently bonded urea.

[0214] When the MMM modules were rinsed with MilliQ water at the end of the experiment (n=2), 0.05 mmol was detected after 1 hour. The 4-hour urea binding was normalized by the amount of urea eluted from the MMM. Figure 7Indicated by an asterisk in the figure, it is expected that for longer rinse times, all the urea physically adsorbed in the system will be eluted. This experiment confirms that under dynamic conditions, the binding of urea to the MMM is a combination of chemisorption and physical adsorption. Because urea does not bind to the control membrane without adsorbent particles, the binding is an effect of the membrane according to the present invention.

[0215] In summary, recycling and filtration of the urea solution through the membrane improves the binding kinetics and overall binding. In addition, when the maximum chemisorption capacity is reached, the adsorption of urea can continue, which may be due to hydrogen bonding of urea molecules to the newly formed covalently bound urea surface.

[0216] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A membrane suitable for dialysis comprising embedded particulate material, in, The membrane is a porous polymer membrane comprising at least one polymer selected from the group consisting of polysulfone, polyethersulfone, polyphenylsulfone, polyarylethersulfone, polyamide, polyetherimide, polyimide, polyethylene-co-vinyl alcohol, polyethylene-co-vinyl acetate, cellulose acetate, cellulose triacetate, polyvinylidene fluoride, polyvinyl chloride, polyacrylonitrile, polyurethane, polyetheretherketone and / or polyacrylic acid, wherein the particulate material comprises a urea adsorbent, the urea adsorbent being an adsorbent that covalently captures urea, wherein at least 10% of the urea binding is covalent capture of urea; and wherein the particle size of the granular material is at most 250 μm along the maximum diameter; The urea adsorbent is a macromolecular composition comprising a polymer backbone grafted with side groups that can covalently capture urea.

2. The film according to claim 1, in, The particulate material is present in the film in an amount ranging from 5 wt % to 80 wt % based on the total dry weight of the film and the particulate material.

3. The film according to claim 1, in, The particle size of the particulate material is at most 150 μm along the largest diameter.

4. The film according to claim 1, in, The membranes are in the form of hollow fibers, full fibers or flat sheets.

5. The film according to claim 1, in, The membrane comprises polyethersulfone and / or polyvinylpyrrolidone.

6. The film according to claim 1, in, The water permeability of the membrane is at least 1 L / (m 2 ·h·Bar).

7. The film according to claim 1, in, The urea adsorbent is selected from ninhydrin type adsorbent, benzoyl acetaldehyde type adsorbent and / or trimethylolformic acid type adsorbent.

8. The film according to claim 1, in, The particulate material also includes activated carbon particles, ion exchange particles, silica particles, zeolite particles, ceramic particles, polymer particles and / or molecular imprinted particles, and / or Wherein, the film further comprises additives.

9. The film according to claim 1, in, The particulate material is present in the film in an amount ranging from 25 wt% to 70 wt%, based on the total dry weight of the film and the particulate material.

10. The film according to claim 1, in, The particle size of the particulate material is at most 85 μm along the largest diameter.

11. The film according to claim 1, in, The particle size of the particulate material is at most 70 μm along the largest diameter.

12. The film according to claim 1, in, The membranes are hollow fibers.

13. The film according to claim 1, in, The side group capable of covalently capturing urea comprises two or more adjacent carbonyl groups or hydrates thereof.

14. The film according to claim 8, in, The ion exchange particles are ion exchange resin particles or ion exchange silica particles.

15. The film according to claim 8, in, The silicon dioxide particles are unmodified silicon dioxide particles or alkylated silicon dioxide particles.

16. The film according to claim 8, in, The polymer particles are porous polymer particles or non-porous polymer particles.

17. The film according to claim 8, in, The additive is a hydrophilic additive.

18. The film according to claim 17, in, The hydrophilic additive is polyvinyl pyrrolidone, chitosan, polyethylene glycol, dextran, glycerol, diethylene glycol, octanol, oxalic acid, maleic acid, tartaric acid, fumaric acid, lithium chloride and / or calcium chloride.

19. Use of the membrane according to any one of claims 1 to 18 in the preparation of a dialysis device.

20. The use according to claim 19, in, The dialysis device is used to treat diseases or conditions associated with urea accumulation.

21. A method for preparing a membrane as claimed in any one of claims 1 to 18, The following steps are involved: i. Providing urea adsorbent particles having a particle size of up to 250 μm along the maximum diameter; ii. mixing the urea adsorbent particles with a polymer material in a solvent for the polymer material to obtain a mixture; iii. extruding or casting the mixture to form a film; and iv. Optionally, curing the film.

22. The method according to claim 21, in, In step iv, the film is cured by phase inversion.

23. A method for removing nucleophilic waste solutes from a fluid for non-therapeutic purposes, The following steps are involved: i) providing a fluid comprising a nucleophilic waste solute; iia) contacting the fluid with the membrane of any one of claims 1 to 18; or, iib) contacting the fluid and a dialysate through a membrane, wherein the dialysate is in contact with the membrane of any one of claims 1 to 18; iii) optionally, regenerating the fluid.

24. A cartridge for use in a dialysis device comprising a membrane as claimed in any one of claims 1 to 18.

25. A dialysis device comprising a membrane as claimed in any one of claims 1 to 18 or a cartridge as claimed in claim 24.