A dual-mode high-resolution interference lithography device and method
Through dual-mode interference lithography equipment, combined with immersion and surface plasmon lithography modules, multi-film layer design and strict coupled wave analysis methods are used to solve the problem of traditional interference lithography technology being difficult to achieve high resolution and mode compatibility. High-resolution and low-cost photolithography effects are achieved.
Patent Information
- Application Number
- CN202211050154.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-30
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-08-30
AI Technical Summary
Traditional interference lithography technology is difficult to achieve high-resolution imaging and is difficult to be compatible with multiple lithography modes. The cost and technical difficulty of existing technologies increase when improving resolution, and immersion lithography has strict requirements on photoresist materials and surface plasmons. The process feasibility of excimer lithography equipment is insufficient.
Design a dual-mode high-resolution interference lithography device, which combines the front-end optical path module and the back-end film module. The front-end optical path module is composed of a laser light source, an adjustment mirror group and a prism. Coherent light is formed through total reflection of the hypotenuse of the prism. Combined with immersion Type lithography module and surface plasmon lithography module use multi-layer design to achieve compatibility between the two modes, and optimize light intensity and contrast through strict coupled wave analysis methods.
It achieves the preparation of high-resolution graphics, expands the focal depth and working distance, simplifies mode switching, reduces costs, improves the uniformity of light intensity and contrast in the thickness direction of the photoresist, and achieves a resolution far lower than 1/4 wavelength. High resolution lithography.
Smart Images

Figure CN115309009B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of interference lithography, and in particular to a dual-mode high-resolution interference lithography device and method. Background Art
[0002] Interference lithography has the advantages of simple structure, low price, high efficiency, high resolution and large exposure area. Using interference lithography, fine periodic structures such as gratings and lattices can be prepared on a large area without the use of complex optical systems or photolithography masks. Therefore, it has great application prospects in the fields of sensing, solar cells and photonic crystals. However, based on the requirements for miniaturization and high integration of electronic and optoelectronic devices, modern information technology has increasingly higher requirements for micro-nano manufacturing processing accuracy, and the basic theory of traditional optics determines that the resolution will inevitably be limited by the optical diffraction limit. For example, the maximum resolution of laser interference lithography is generally 1 / 2 to 1 / 4 wavelength. Therefore, there is an urgent need to develop new interference lithography technologies that can effectively extend or even break through the diffraction limit.
[0003] To achieve the preparation of nanoscale graphics (below 100 nanometers), the wavelength of the light source can be continuously reduced by referring to the traditional projection lithography route, thereby improving its diffraction-limited resolution. However, this solution will significantly increase the technical difficulty and cost, weakening its advantages of simple structure and low price. In addition to reducing the wavelength, using immersion lithography technology to fill the space between the mask and the photoresist with a high refractive index immersion liquid can reduce the equivalent wavelength of exposure, which is also an effective way to further improve the limiting resolution. However, the existing immersion lithography technology can only increase the maximum resolution to about 1 / 4 wavelength. In addition, immersion lithography also puts forward more stringent requirements for the materials of photoresists, especially chemically amplified photoresists, and has certain limitations.
[0004] On the other hand, surface plasmon (SP) technology provides a new lithography solution that can break the diffraction limit. Surface plasmon is a surface electromagnetic wave that exists at the interface between metal and medium. Since its wavelength is much smaller than the wavelength of the illumination light, super-resolution lithography can be achieved. Interference lithography technology based on SP has great application prospects in the preparation of large-area nanostructures, but most of the related lithography devices reported so far are based on simulation design, and few have actual process feasibility. Summary of the invention
[0005] 1. Technical issues to be resolved
[0006] In view of the above problems, the present disclosure provides a dual-mode high-resolution interference lithography device and method, which are used to solve technical problems such as traditional interference lithography is difficult to achieve high-resolution imaging and difficult to be compatible with multiple lithography modes.
[0007] (II) Technical solution
[0008] On the one hand, the present disclosure provides a dual-mode high-resolution interference lithography device, including: a front-end optical path module, which includes a laser light source, an adjustment mirror group and a prism in sequence along the optical path, the light generated by the laser light source is adjusted by the adjustment mirror group to form at least two coherent light beams, the coherent light enters the prism vertically, and converges on the bottom surface of the prism after being totally reflected by the hypotenuse of the prism; a back-end film layer module, including an immersion lithography module or a surface plasmon lithography module; wherein the immersion lithography module includes a matching liquid layer, a substrate layer, and a photolithography film layer, the coherent light is emitted from the bottom surface of the prism, forms interference in the immersion lithography module and exposes the photolithography film layer; the surface plasmon lithography module includes a super lens film layer and a substrate layer, the super lens film layer includes a photoresist layer and a metal layer, the evanescent wave formed by the converged coherent light outside the bottom surface of the prism is coupled with the super lens film layer and exposes the photoresist layer.
[0009] Furthermore, the immersion lithography module includes a first matching liquid layer, a substrate layer, a photoresist film layer, and a second matching liquid layer in sequence along the optical path, and the first matching liquid layer fills the gap between the prism and the substrate layer; or the immersion lithography module includes a first matching liquid layer, a photoresist film layer, and a substrate layer in sequence along the optical path, and the first matching liquid layer fills the gap between the prism and the photoresist film layer.
[0010] Furthermore, the refractive indexes of the prism, the matching liquid layer, the substrate layer, and the photolithography film layer are similar or the same, so that the coherent light is transmitted in the immersion photolithography module and forms interference.
[0011] Furthermore, the structures and parameters of the matching liquid layer, substrate layer, and photolithography film layer are simulated and optimized using a rigorous coupled wave analysis method.
[0012] Furthermore, the surface plasmon lithography module includes a first metal layer, a photoresist layer, a second metal layer, and a substrate layer in sequence along the optical path; the first metal layer is close to or in contact with the bottom surface of the prism.
[0013] Furthermore, the structure and parameters of the photoresist layer, the metal layer, and the air gap between the prism and the back-end membrane module are simulated and optimized using a rigorous coupled wave analysis method.
[0014] Furthermore, when the rear-end film layer module is a surface plasmon lithography module, a focus detection module is also provided above the prism, and the focus detection module is used to detect the size and distribution of the gap between the bottom surface of the prism and the rear-end film layer module.
[0015] Furthermore, the prism is a prism with left-right axis symmetry; the prism is a material with a high refractive index, including one of optical glass, quartz glass, sapphire and metal halide crystal.
[0016] Furthermore, the wavelength of the laser light source is 157nm to 436nm; the adjustment mirror group includes a plurality of light spot expansion elements, polarization adjustment elements, spatial filtering elements, semi-reflective and semi-mirror elements, and reflector elements.
[0017] On the other hand, the present disclosure provides a method for dual-mode high-resolution interference lithography, comprising: S1, emitting laser light using a laser light source; using an adjustment mirror group to adjust the laser beam splitting to form at least two coherent light beams and make them enter a prism vertically; using a prism to totally reflect the coherent light at its hypotenuse and then converge it on the bottom surface of the prism; wherein the laser light source, the adjustment mirror group and the prism constitute a front-end optical path module; S2, using an immersion lithography module to make the coherent light form interference after being emitted through the bottom surface of the prism and expose the photolithography film layer; the immersion lithography module includes a matching liquid layer, a substrate layer and a photolithography film layer; or using a surface plasmon lithography module to make the evanescent wave formed by the converged coherent light outside the bottom surface of the prism couple with the super lens film layer and expose the photoresist layer; the surface plasmon lithography module includes a super lens film layer and a substrate layer, and the super lens film layer includes a photoresist layer and a metal layer.
[0018] (III) Beneficial effects
[0019] The disclosed dual-mode high-resolution interference lithography device and method use a coherent light beam and a prism to form a front-end optical path module, and by designing a variety of photolithography film layers in the rear-end film layer module, the compatibility of the two modes of immersion lithography and surface plasmon lithography is achieved. Since the front-end optical path module is relatively precise in structure, and the rear-end film layer module is small in size and easy to replace, the switching between the two modes is flexible and easy to operate. Further, by optimizing the design of multiple film layers in the two modes, the light intensity and contrast uniformity in the thickness direction of the photoresist are regulated, thereby achieving contrast optimization and the expansion of focal depth and working distance, and the preparation of high-resolution graphics can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The schematic diagram of the structure of the dual-mode high-resolution interference lithography device according to the embodiment of the present disclosure is shown;
[0021] Figure 2 A schematic diagram of the structure of an immersion lithography module in which the back-end film layer module is a module according to an embodiment of the present disclosure is shown;
[0022] Figure 3 The schematic diagram shows the structure of a back-end film layer module as a surface plasmon lithography module according to an embodiment of the present disclosure;
[0023] Figure 4 The schematic diagram of the structure of the laser light source and the adjustment mirror assembly according to the embodiment of the present disclosure is shown;
[0024] Figure 5The schematic diagram shows the structure of the front-end optical path module according to the first embodiment of the present disclosure;
[0025] Figure 6 The schematic diagram of the structure of the prism according to the first embodiment of the present disclosure is shown;
[0026] Figure 7 A schematic diagram of light intensity distribution obtained by simulation using a rigorous coupled wave analysis method according to the first embodiment of the present disclosure is shown;
[0027] Figure 8 Schematically shows a scanning electron microscope image measured in the first embodiment of the present disclosure;
[0028] Fig. 9 The schematic diagram of the structure of the prism according to the second embodiment of the present disclosure is shown;
[0029] Fig.10 A schematic diagram of light intensity distribution obtained by simulation using a rigorous coupled wave analysis method according to the second embodiment of the present disclosure is shown;
[0030] Fig.11 Schematically shows a scanning electron microscope image measured in Example 2 of the present disclosure;
[0031] Fig.12 The schematic diagram of contrast and light intensity distribution obtained by simulation using the rigorous coupled wave analysis method in the third embodiment of the present disclosure is shown schematically;
[0032] Fig.13 Schematically shows a scanning electron microscope image measured in Example 3 of the present disclosure;
[0033] Fig.14 A schematic diagram of light intensity distribution obtained by simulation using a rigorous coupled wave analysis method in Comparative Example 1 of the present disclosure is shown schematically;
[0034] Fig.15 The scanning electron microscope image measured in Comparative Example 1 of the present disclosure is schematically shown. DETAILED DESCRIPTION
[0035] In order to make the objectives, technical solutions and advantages of the present disclosure more clearly understood, the present disclosure is further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.
[0036] The terms used herein are only for describing specific embodiments and are not intended to limit the present disclosure. The terms "comprise", "include", etc. used herein indicate the existence of the features, steps, operations and / or components, but do not exclude the existence or addition of one or more other features, steps, operations or components.
[0037] It should be noted that if directional indication is involved in the embodiments of the present disclosure, the directional indication is only used to explain the relative position relationship, movement status, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.
[0038] The embodiment of the present disclosure provides a dual-mode high-resolution interference lithography device, see Figures 1 to 3 , including: a front-end optical path module, which includes a laser light source 1, an adjustment lens group 2 and a prism 3 in sequence along the optical path, the light generated by the laser light source 1 is adjusted by the beam splitting of the adjustment lens group 2 to form at least two coherent lights, the coherent lights vertically enter the prism 3, and converge on the bottom surface of the prism 3 after being totally reflected by the hypotenuse of the prism 3; a rear-end film layer module, including an immersion lithography module or a surface plasmon lithography module; wherein the immersion lithography module includes a matching liquid layer 11, a substrate layer 12, and a photolithography film layer 13, the coherent lights are emitted from the bottom surface of the prism 3, form interference in the immersion lithography module and expose the photolithography film layer 13; the surface plasmon lithography module includes a super lens film layer 21 and a substrate layer 22, the super lens film layer 21 includes a photoresist layer 211 and a metal layer 212, the evanescent wave formed by the converged coherent lights outside the bottom surface of the prism 3 is coupled with the super lens film layer 21 and exposes the photoresist layer 211.
[0039] The lithography device disclosed in the present invention uses a high refractive index prism 3 as a core optical device to make at least two fixed coherent light beams (such as Figure 1 The two beams (shown in Figure 1) are totally reflected by the hypotenuse of prism 3 and then converge through its bottom surface to enter the rear film module to form interference. The period of the interference fringes is determined by the angle of the hypotenuse of prism 3, the refractive index and the wavelength of the laser light source 1. On the exit surface (bottom surface) of prism 3, by adopting different photolithography film layer schemes, the exposure of two modes, immersion interference and surface plasmon (SP) interference, can be achieved simultaneously.
[0040] The back-end film layer module is a structure of multiple film layers. According to the needs of the two modes of immersion lithography and surface plasmon lithography, the immersion lithography may include a matching liquid layer 11, a substrate layer 12, and a photolithography film layer 13, and the surface plasmon lithography may include a photoresist layer 211, a metal layer 212, and a substrate layer 22. The present disclosure achieves compatibility between the two modes of immersion lithography and surface plasmon lithography by designing multiple photolithography film layers in the back-end film layer module. Since the front-end optical path module is relatively precise in structure, and the back-end film layer module is small in size and easy to replace, the switching between the two modes is flexible and easy to operate.
[0041] Based on the above embodiments, Figure 2As shown, the immersion lithography module includes a first matching liquid layer 111, a substrate layer 12, a photolithography film layer 13, and a second matching liquid layer 112 in sequence along the optical path. The first matching liquid layer 111 fills the gap between the prism 3 and the substrate layer 12 (the first photolithography layer structure, as shown in FIG. Figure 2 (a)); or the immersion lithography module includes a first matching liquid layer 111, a photolithography film layer 13, and a substrate layer 12 (a second photolithography layer structure, such as Figure 2 (b) shows that the first matching liquid layer 111 fills the gap between the prism 3 and the photoresist film layer 13 .
[0042] For the immersion lithography mode, a matching liquid needs to be coated on the exit surface of the prism 3. The refractive index of the first matching liquid layer 111 is required to be as similar as possible to the refractive index of the prism 3, so that the light beam enters the photolithography layer (the photolithography layer includes the substrate layer 12 and the photolithography film layer 13) without being totally reflected again at the bottom surface (exit surface) of the prism 3. The material of the substrate layer 12 is required to be transparent, and its refractive index value is within a specific range. For the first photolithography layer structure, a second matching liquid layer 112 is required to cover the photolithography film layer 13; for the second photolithography layer structure, the photolithography film layer 13 is placed on the substrate layer 12, and no additional matching liquid layer is required for covering. Of course, as needed, another matching liquid layer (second matching liquid layer 112) can be added under the photolithography layer, and its refractive index value is usually adjusted near the refractive index of the photolithography film layer 13.
[0043] On the basis of the above embodiment, the refractive indexes of the prism 3, the matching liquid layer 111, the substrate layer 12, and the photolithography film layer 13 are similar or the same, so that the interference light is transmitted in the immersion photolithography module and forms interference.
[0044] For the immersion lithography mode, the light beam is transmitted in the entire back-end film layer module. A matching liquid layer needs to be filled between the photolithography layer and the prism 3 so that the light beam enters the photolithography layer and exposes the photoresist in the photolithography film layer 13. The refractive index of the first matching liquid layer 111 is required to be as similar as possible to that of the prism 3; in the first photolithography layer structure, the substrate layer 12 is directly in contact with the first matching liquid layer 111. In order to achieve the transmission of the light beam in the photolithography layer, the refractive index of the substrate layer 12 is also required to be close to the first matching liquid layer 111 to avoid total reflection. The photolithography film layer 13 is a photoresist material that is sensitive to the wavelength of the light source. The second matching liquid layer 112 is directly infiltrated on the surface of the photolithography film layer 13 to further regulate and optimize the light field in the photolithography layer. The refractive index parameter design principle of each film layer (including the matching liquid) in the above-mentioned immersion lithography module is to make the light beam transmit in the photolithography layer, so the refractive index of each film layer should be similar or the same.
[0045] On the basis of the above-mentioned embodiments, the structures and parameters of the matching liquid layer 11, the substrate layer 12, and the photoresist film layer 13 are simulated and optimized using a rigorous coupled wave analysis method.
[0046] Furthermore, the refractive index can be adjusted to maximize the light field contrast in the photoresist film 13, and the consistency of the light field contrast and peak intensity in the depth direction of the photoresist is the best. To this end, the refractive index parameters of each film layer can be simulated and optimized using the Rigorous Coupled Wave Analysis (RCWA) method, and high-resolution interference lithography in the immersion lithography mode can be achieved according to different process requirements.
[0047] Based on the above embodiments, Figure 3 As shown, the surface plasmon lithography module includes a first metal layer 2121 , a photoresist layer 211 , a second metal layer 2122 , and a substrate layer 22 in sequence along the optical path; the first metal layer 2121 is close to or in contact with the bottom surface of the prism 3 .
[0048] For the surface plasmon lithography mode, there is a metal film layer (including a first metal layer 2121 and a second metal layer 2122) above and below the photoresist layer 211 in the rear-end film layer module. The entire rear-end film layer module is close to or in contact with the exit surface of the prism 3 (i.e., a certain air gap is allowed). The gap between the bottom surface (exit surface) of the prism 3 and the rear-end film layer module can be controlled by applying pressure to the bottom of the film layer. The interference light beam is totally reflected in the bottom surface of the prism 3 and an evanescent wave is generated outside the surface. The super lens film layer 21 formed by the metal-medium alternation of the rear-end film layer module is coupled with the evanescent wave, so that the photoresist layer 211 is photosensitized.
[0049] Based on the above embodiments, the structure and parameters of the photoresist layer 211 and the metal layer 212 and the air gap between the prism 3 and the back-end film layer module are simulated and optimized using a rigorous coupled wave analysis method.
[0050] For the surface plasmon lithography mode, the parameter design principle of each film layer in the back-end film layer module is: the real part of the dielectric constant of the first metal layer 2121 and the second metal layer 2122 is negative, and the material thickness and refractive index make the film layer structure meet the SP resonance condition, so that the light field contrast in the photoresist layer 211 is maximized, and at the same time, the light field contrast and peak intensity in the depth direction of the photoresist layer 211 are the best. For this reason, the RCWA method can also be used to simulate and optimize the refractive index parameters of each film layer, and high-resolution interference lithography in the surface plasmon lithography mode can be achieved according to different process requirements. Among them, the strict coupled wave analysis method is a common method in this field and will not be repeated here. In addition, since the grains, defects, surface oxidation and other phenomena that appear in the metal film layer during the preparation process cannot be fully reflected in the conventional RCWA simulation, the prediction of the actual light field also needs to take into account the stray light caused by the above phenomena. Only when the exposure signal reaches a certain intensity can it have a sufficiently high signal-to-noise ratio to achieve high-resolution exposure. The inventors have proved through experiments that when the signal peak light intensity is reduced to 0.1 or less of the sum of the two incident light intensities, nanometer-level high-resolution imaging cannot be achieved.
[0051] On the basis of the above embodiment, when the rear-end film layer module is a surface plasmon lithography module, a focus detection module 4 is further provided above the prism 3, and the focus detection module 4 is used to detect the gap size and gap distribution between the bottom surface of the prism 3 and the rear-end film layer module.
[0052] like Figure 1 As shown, for the surface plasmon lithography mode, since there is an air gap between the prism 3 and the rear-end film layer module, an in-situ focusing module 4 can be optionally installed to detect the gap size and gap distribution between the exit surface of the prism 3 and the rear-end film layer module. At this time, the distance between the incident surface of the prism 3 and the first metal layer 2121 should be limited to within 30 mm to avoid the focal depth of the focusing lens being unable to cover the exit surface due to the prism 3 being too high. At the same time, the incident surface of the prism 3 must reserve sufficient installation and moving space for the focusing lens; for the optional in-situ focusing module 4, a focusing method based on the principle of confocal frequency domain white light interference can be used to achieve precise detection of the absolute distance between the prism 3 and the rear-end film layer module. This method is based on multi-wavelength interference measurement technology, and the analysis of the air gap is achieved by collecting the reflective interference spectrum through the detection probe, which meets the absolute distance, high precision and large range of focusing requirements.
[0053] On the basis of the above embodiment, the prism 3 is a prism with left-right axis symmetry; the prism 3 is made of a material with a high refractive index, including one of optical glass, quartz glass, sapphire and metal halide crystal.
[0054] After the material of prism 3 is determined (refractive index is determined), the period of interference fringes is determined by the hypotenuse angle of the trapezoid, and the relationship is as follows:
[0055]
[0056] Among them, λ is the laser wavelength, θ is the incident angle of the interference light, and n is the refractive index of the incident layer; the incident angle θ and the hypotenuse angle of the trapezoidal prism (like Figure 1 The relationship shown) is:
[0057]
[0058] On the basis of the above embodiments, the adjustment mirror group 2 includes multiple types of spot expansion elements, polarization adjustment elements, spatial filtering elements, semi-reflective and semi-mirror elements, and reflector elements.
[0059] The front-end optical path module adopts the solution of splitting the same laser light source 1, and achieves the interference condition (such as Figure 4 As shown), the light source is a laser light source 1, and the wavelength can be selected according to the resolution requirements of the prepared pattern and the photoresist. The wavelength of the laser light source 1 can be 157nm~436nm, and the light spot energy distribution type (Gaussian or flat top) of the light source can be selected according to the illumination field size and light intensity uniformity requirements required by the photolithography process. According to the requirements of the quality, area, uniformity and other requirements of the interference pattern, an adjustment module 201 can be added to the front section of the beam splitting light path to process the properties of the light source, including but not limited to spot expansion, polarization state adjustment and light intensity uniformity improvement. The semi-reflective and semi-mirror element 202 of the corresponding wavelength is used for splitting light, and the reflectivity of the mirrors 203, 204, and 205 of the corresponding wavelength can reach 99%. The optical elements 206 and 207 are used to adjust the polarization state, light intensity and corresponding light path of the interference light beam formed by the same source.
[0060] The present disclosure expands the resolution limit of interference lithography for both immersion lithography and surface plasmon lithography. For immersion lithography, the minimum period of interference fringes is λ / 2n, which is determined by the refractive index of the prism, matching liquid, and lithography layer. For SP lithography, since the evanescent wave can retain the high-frequency part of the light field, there is almost no spatial frequency limit in theory, so its maximum resolution is mainly limited by the material and focal depth of the prism.
[0061] The traditional prism device simply contacts the substrate coated with photoresist with the prism or directly coats the photoresist on the prism. Although this method can use the excited evanescent field for interference exposure, there is a problem that the light field intensity and contrast in the photoresist film layer are unevenly distributed within the thickness range. As the interference fringe period decreases, this problem will cause the depth of focus to be greatly compressed, which will seriously affect the lithography effect.
[0062] The present disclosure optimizes this problem in both modes: for the immersion lithography mode, the contrast and uniformity within the photolithography film layer are optimized by combining multiple layers of transparent substrates with different refractive indices and matching liquids; for the SP lithography mode, the evanescent field formed by the prism is coupled within the photoresist layer through the design of the metal-dielectric film layer, thereby achieving an effective extension of the focal depth and working distance.
[0063] The present disclosure also provides a method for dual-mode high-resolution interference lithography, comprising: S1, using a laser light source 1 to emit laser light; using an adjustment lens group 2 to adjust the laser beam splitting to form at least two coherent light beams and make them enter the prism 3 vertically; using the prism 3 to make the coherent light totally reflected at its hypotenuse and then converged on the bottom surface of the prism 3; wherein the laser light source 1, the adjustment lens group 2 and the prism 3 form a front-end optical path module; S2, using an immersion lithography module to make the coherent light emerge from the bottom surface of the prism 3 Interference is formed and the photolithography film layer 13 is exposed; the immersion lithography module includes a matching liquid layer 11, a substrate layer 12 and a photolithography film layer 13; or a surface plasmon lithography module is used to couple the evanescent wave formed by the converged coherent light outside the bottom surface of the prism 3 with the super lens film layer 21 and expose the photoresist layer 211; the surface plasmon lithography module includes a super lens film layer 21 and a substrate layer 22, and the super lens film layer 21 includes a photoresist layer 211 and a metal layer 212.
[0064] The present disclosure provides a method for dual-mode high-resolution interference lithography that can switch between immersion lithography and SP lithography. The method uses at least two coherent laser beams and a prism 3 as the front-end optical path module, and then realizes the compatibility of the two modes through a variety of photolithography film layer designs in the back-end film layer module. For the immersion lithography mode, a double-layer immersion liquid + substrate matching method is adopted; for the SP lithography mode, a metal-medium (photoresist) multi-film layer solution is used to achieve it; because the front-end optical path module is relatively precise in structure, and the back-end film layer module is small in size and easy to replace, the switching between the two modes is flexible and easy to operate. The device and method can realize the preparation of high-resolution graphics far below 1 / 4 wavelength, and have been experimentally verified.
[0065] The present disclosure is further described below through specific implementations. The above dual-mode high-resolution interference lithography device and method are specifically described in the following embodiments. However, the following embodiments are only used to illustrate the present disclosure, and the scope of the present disclosure is not limited thereto.
[0066] like Figure 1As shown, the overall design of this embodiment is divided into two parts: a front-end optical path module and a back-end film layer module. The front-end optical path module mainly includes a laser light source 1 that generates two coherent light beams, an adjustment lens group 2 (not specifically shown in the figure), and a trapezoidal prism 3. The double light beams enter the prism 3 vertically, and after total reflection on the hypotenuse, they converge on the bottom surface of the prism 3. The back-end film layer module is a multi-film layer structure, which may include photoresist, substrate, and other photoresist film layers or matching liquid layers according to the needs of the two modes.
[0067] This embodiment proposes a relatively simple and low-cost method to achieve a high-resolution interference lithography device and method below 1 / 4 wavelength. This embodiment uses a relatively traditional design scheme in the front-end optical path module, and other prism interference lithography designs can also be used, such as four laser beams interfering to form a dot pattern in a regular square prism.
[0068] Immersion lithography has the advantages of simple film preparation, high light field uniformity, and good repeatability, but there are certain limitations in the selection of substrate and matching liquid (the substrate requires a transparent material, and the substrate and matching liquid must have a specific refractive index according to the resolution requirements). In addition, since the photolithography film layer and the matching liquid layer need to be in direct contact, the use of some photoresists that are sensitive to the surface environment is also limited.
[0069] The SP lithography mode has the advantages that the resolution is almost unaffected by the refractive index of the photolithography film, does not require the introduction of matching liquid, and has no special restrictions on the substrate. However, its photolithography film is relatively complex, requiring relatively precise thickness and roughness control, and the light intensity is greatly affected by the air gap. In the absence of a focus detection module, the dose fluctuates, affecting repeatability.
[0070] Therefore, this embodiment realizes the compatibility and easy switching of the two modes in a modular form, and the appropriate mode can be selected according to actual needs. In any mode, the exposure effect can be optimized through the film layer optimization design.
[0071] This embodiment uses the rigorous coupled wave analysis method (RCWA) to optimize the light field in the photoresist. The immersion lithography mode requires the design of the multilayer structure of the matching liquid and the transparent substrate material and the design of the parameters (mainly the refractive index); the SP lithography mode requires the design of the thickness, refractive index and air gap between the metal and photoresist layers and the prism. Through the design of multiple film layers, the light intensity and contrast in the two modes are controlled, thereby achieving contrast optimization and the expansion of focal depth and working distance.
[0072] According to the above scheme, 3 specific embodiments and 1 comparative example are provided below.
[0073] Example 1: 120nm period immersion interference lithography
[0074] According to the above requirements, a set of double-beam interference optical system is designed in the first embodiment. The laser light source 1 selects a single longitudinal mode ultraviolet continuous laser with a wavelength of 360nm, a maximum power of 50mW, and a Gaussian beam with a spot diameter of 1mm. It is equipped with an optical beam expansion module 51 (including beam expansion mirror group modules with double, five and ten times beam expansion magnifications), an ultraviolet beam splitter 52 (with a beam splitting ratio of 50:50), a light intensity fine-tuning module 53 (i.e., an adjustment mirror group 2) and a plurality of ultraviolet reflectors 54. The optical path difference is controlled within the coherence length of the light source through the optical path design, and the light is incident on the prism 3 (such as Figure 5 shown).
[0075] Prism 3 is a trapezoidal prism with an incident angle of 56.7°. It is made of sapphire and has a refractive index of 1.794 at the exposure wavelength. This angle and refractive index correspond to interference fringes with a period of 120 nm. The specific parameters of the prism are as follows: Figure 6 shown.
[0076] The rear film module behind the prism output surface, such as Figure 2 As shown in (a), the first matching liquid layer 111 uses a matching liquid with the same refractive index as sapphire, and the refractive index is 1.79; the substrate layer 12 is a sapphire substrate with a thickness of 0.5mm; the photoresist film layer 13 is an I-line photoresist with a thickness of 50nm, and the measured values of the photoresist dielectric constant are: n=1.58, k=0.018; the refractive index of the second matching liquid layer 112 is 1.69, and it is directly coated on the surface of the photoresist film layer 13. According to the numerical electromagnetic simulation algorithm program RCWA, the interference photoresist film layer structure is geometrically modeled, and then the refractive index of the structure is set. When two 360nm wavelength plane wave beams are incident at symmetrical angles, interference fringes can be obtained on the photoresist film layer 13. Figure 7 As shown, under the current parameters, completely uniform light intensity distribution can be achieved within the photoresist depth range (the peak light intensity deviation between 5 and 35 nm depth is only 0.07%), and the contrast can be as high as 0.82 or more, meeting the requirements of high-quality lithography imaging.
[0077] After exposing the photoresist for 3 seconds according to the parameters of the device, the sapphire substrate is removed from the prism 3 and the matching liquid is rinsed with deionized water for 30 seconds. The substrate is dried with nitrogen and placed on a 100-degree constant temperature hot plate for 60 seconds, and then conventionally developed and fixed to obtain a grating pattern with a period of 120 nm.
[0078] The measured SEM images are as follows Figure 8 As shown, it can be seen that the target photoresist pattern is well resolved and the line edges are clear, indicating that the light field contrast is high and the light intensity uniformity in the thickness direction of the photoresist has achieved the expected optimization effect.
[0079] Example 2: 104nm periodic immersion interference lithography
[0080] The prism 3 in the first embodiment is replaced by a trapezoidal prism with an incident angle of 72.06°, made of sapphire, and having a corresponding refractive index of 1.794 at the exposure wavelength. This angle and refractive index correspond to interference fringes with a period of 104 nm. The specific parameters of the prism are as follows: Fig. 9 shown.
[0081] The rear film module behind the prism output surface, such as Figure 2 As shown in (a), the first matching liquid layer 111 uses a matching liquid with the same refractive index as sapphire, and the refractive index is 1.79; the substrate layer 12 is a sapphire substrate with a thickness of 0.5 mm; the photoresist film layer 13 is an I-line photoresist with a thickness of 50 nm, and the measured dielectric constant of the photoresist is: n = 1.58, k = 0.018; the second matching liquid layer 112 is the same as the first matching liquid layer 111, and is directly coated on the surface of the photoresist film layer 13. Fig.10 As shown, according to RCWA simulation, under this parameter, uniform light intensity distribution can be achieved within the photoresist depth range (the peak light intensity deviation between 5 and 35 nm depth is less than 5%), and the contrast can be as high as 0.94 or above, meeting the requirements of high-quality lithography imaging.
[0082] After exposing the photoresist for 3 seconds according to the parameters of the device, the sapphire substrate was removed from the prism 3 and the matching liquid was rinsed with deionized water for 30 seconds. The substrate was dried with nitrogen and placed on a 100-degree constant temperature hot plate for 60 seconds, and then conventionally developed and fixed to obtain a grating pattern with a period of 104 nm.
[0083] The measured SEM images are as follows Fig.11 As shown, it can be seen that the target photoresist pattern is well resolved and the line edges are clear, indicating that the light field contrast is high and the light intensity uniformity in the thickness direction of the photoresist has achieved the expected optimization effect.
[0084] Example 3: 104nm periodic SP interference lithography
[0085] The light source and prism combination in Example 2 is used, and the rear-end film layer module below the prism exit surface is replaced by a surface plasmon lithography module, namely "first metal layer 2121-photoresist layer 211-second metal layer 2122-substrate layer 22". The first metal layer 2121 is a silver film with a thickness of 15nm, the photoresist layer 211 is an I-line photoresist with a thickness of 30nm, the second metal layer 2122 is a silver film with a thickness of 50nm, and the substrate layer 22 is a single-sided polished silicon substrate with a thickness of 0.5mm. After the substrate where the rear-end film layer is located contacts the prism 3, the size of the air gap between the two is adjusted by applying pressure to the bottom. In this Example 3, the average air gap measured by the installed in-situ focusing module 4 is 36nm. Fig.12As shown in the figure, according to the RCWA simulation, a uniform light intensity distribution can be achieved within the depth range of the photoresist under this parameter, with a contrast ratio of up to 0.9. At a 36nm air gap, the light intensity inside the photoresist exceeds 0.3 of the sum of the two incident light intensities. Within the air gap variation range, only the light intensity value changes, while the light field uniformity and contrast in the photoresist remain unchanged.
[0086] After exposing the photoresist for 5 seconds according to the parameters of the device, the substrate is removed, the top first metal layer 2121 (silver film layer) is torn off with tape, and it is placed on a 100-degree constant temperature hot plate and baked for 60 seconds, followed by conventional development and fixing to obtain a 104nm periodic grating pattern.
[0087] The measured SEM images are as follows Fig.13 As shown, it can be seen that the target photoresist pattern is well resolved and the line edges are clear, indicating that the light field contrast is high and the light intensity uniformity in the thickness direction of the photoresist has achieved the expected optimization effect.
[0088] Comparative Example 1: 104nm Periodic Immersion Interferometry
[0089] The light source and prism combination and the back-end film layer module in the second embodiment are used, and the second matching liquid layer 112 is replaced with a matching liquid with a refractive index of 1.46, and the other process parameters remain unchanged. Fig.14 As shown, according to the RCWA simulation, the photoresist center contrast will drop to about 0.5 under this parameter, which does not meet the optimized design and does not meet the requirements of high-quality lithography imaging.
[0090] The matching liquid was cleaned according to the process conditions in Example 2, and the photoresist was post-baked and developed to obtain a 104 nm periodic grating pattern.
[0091] The measured SEM images are as follows Fig.15 As shown, it can be seen that compared with the second embodiment, the quality of the grating pattern has been significantly degraded, and its edge roughness and pattern uniformity have also been significantly reduced, which is consistent with the simulation results.
[0092] Comparative Example 2: 104nm periodic SP interference lithography
[0093] The light source, prism, and rear film layer module combination in the third embodiment are used, and the air gap value is adjusted to 80nm. Fig.12 As shown in the figure, according to RCWA simulation, although the photoresist can still maintain uniform light intensity distribution and high contrast under this parameter in theory, its internal light intensity decays to less than 0.1 of the sum of the two incident light intensities. Considering the actual film flatness and stray light, it is expected that high-resolution graphic imaging will be difficult to achieve under this condition.
[0094] The light intensity under this parameter was compared with the light intensity in Example 3. The photoresist was exposed for 20, 40, and 60 seconds according to the light intensity ratio. No photolithographic pattern was observed under the scanning electron microscope.
[0095] In summary, the dual-mode high-resolution interference lithography device and method disclosed in the present invention can be compatible with high-resolution interference lithography in both immersion lithography and SP lithography modes according to different process requirements; and a relatively simple and low-cost method is used to achieve high-resolution interference lithography below 1 / 4 wavelength, solving the problems of small focal depth of traditional prism (evanescent field) interference lithography, and uneven distribution of light field intensity and contrast within the lithography film layer within the thickness range.
[0096] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present disclosure. It should be understood that the above description is only a specific embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure should be included in the protection scope of the present disclosure.
Claims
1. A dual-mode high-resolution interference lithography apparatus, characterized in that: include: A front-end optical path module comprises a laser light source (1), an adjustment lens group (2) and a prism (3) in sequence along the optical path; the light generated by the laser light source (1) is adjusted by the adjustment lens group (2) to form at least two coherent light beams; the coherent light beams vertically enter the prism (3), are totally reflected by the hypotenuse of the prism (3), and converge on the bottom surface of the prism (3); the prism (3) is a prism with left-right axis symmetry; Back-end film layer module, including immersion lithography module or surface plasmon lithography module; The immersion photolithography module comprises a matching liquid layer (11), a substrate layer (12), and a photolithography film layer (13); the coherent light is emitted from the bottom surface of the prism (3), forms interference in the immersion photolithography module, and exposes the photolithography film layer (13); The surface plasmon lithography module comprises a super lens film layer (21) and a substrate layer (22); the super lens film layer (21) comprises a photoresist layer (211) and a metal layer (212); an evanescent wave formed by the converged coherent light outside the bottom surface of the prism (3) couples with the super lens film layer (21) and exposes the photoresist layer (211).
2. The dual-mode high-resolution interference lithography apparatus according to claim 1, characterized in that: The immersion photolithography module comprises, in sequence along the optical path, a first matching liquid layer (111), a substrate layer (12), a photolithography film layer (13), and a second matching liquid layer (112), wherein the first matching liquid layer (111) is filled in a gap between the prism (3) and the substrate layer (12); or The immersion photolithography module comprises a first matching liquid layer (111), a photolithography film layer (13), and a substrate layer (12) in sequence along an optical path; the first matching liquid layer (111) fills a gap between the prism (3) and the photolithography film layer (13).
3. The dual-mode high-resolution interference lithography apparatus according to claim 1, characterized in that: The refractive indices of the prism (3), the matching liquid layer (11), the substrate layer (12), and the photolithography film layer (13) are similar or the same, so that the coherent light is transmitted in the immersion photolithography module and forms interference.
4. The dual-mode high-resolution interference lithography apparatus according to claim 1, characterized in that: The structures and parameters of the matching liquid layer (11), the substrate layer (12), and the photolithography film layer (13) are obtained by simulation and optimization using a rigorous coupled wave analysis method.
5. The dual-mode high-resolution interference lithography apparatus according to claim 1, characterized in that: The surface plasmon lithography module comprises, in sequence along an optical path, a first metal layer (2121), a photoresist layer (211), a second metal layer (2122), and a substrate layer (22); the first metal layer (2121) is close to or in contact with a bottom surface of the prism (3).
6. The dual-mode high-resolution interference lithography apparatus according to claim 1, characterized in that: The structure and parameters of the photoresist layer (211), the metal layer (212), and the air gap between the prism (3) and the back-end film layer module are obtained by simulation and optimization using a rigorous coupled wave analysis method.
7. The dual-mode high-resolution interference lithography apparatus according to claim 1, characterized in that: When the rear-end film layer module is a surface plasmon lithography module, a focus detection module (4) is also provided above the prism (3), and the focus detection module (4) is used to detect the size and distribution of the gap between the bottom surface of the prism (3) and the rear-end film layer module.
8. The dual-mode high-resolution interference lithography apparatus according to claim 1, characterized in that: The prism (3) is made of a material with a high refractive index, including one of optical glass, quartz glass, sapphire and metal halide crystal.
9. The dual-mode high-resolution interference lithography apparatus according to claim 1, characterized in that: The wavelength of the laser light source (1) is 157 nm to 436 nm; the adjustment mirror group (2) comprises a plurality of light spot expansion elements, polarization adjustment elements, spatial filtering elements, semi-reflective and semi-mirror elements, and reflector elements.
10. A method for dual-mode high-resolution interference lithography, characterized in that: include: S1, using a laser light source (1) to emit laser light; using an adjustment lens group (2) to adjust the laser beam splitting to form at least two coherent light beams and make them enter a prism (3) vertically; using the prism (3) to totally reflect the coherent light at its hypotenuse and then converge it on the bottom surface of the prism (3); wherein the laser light source (1), the adjustment lens group (2) and the prism (3) form a front-end optical path module; and the prism (3) is a prism with left-right axis symmetry; S2, using an immersion photolithography module to make the coherent light emit from the bottom surface of the prism (3) to form interference and expose the photolithography film layer (13); the immersion photolithography module comprises a matching liquid layer (11), a substrate layer (12) and the photolithography film layer (13); or A surface plasmon lithography module is used to couple the evanescent wave formed by the converged coherent light outside the bottom surface of the prism (3) with the super lens film layer (21) and expose the photoresist layer (211); the surface plasmon lithography module comprises the super lens film layer (21) and a substrate layer (22); and the super lens film layer (21) comprises the photoresist layer (211) and a metal layer (212).
Citation Information
Patent Citations
Method for laser interference lithography using diffraction grating
CN101828140A
Preparation device of sub-wavelength structure repeatedly intervened and exposed by surface plasma
CN106842823A