A modified microcrystalline glassy sulfide solid solution and its preparation method and application
By doping P elements and other metals into the glassy sulfide solid electrolyte, the conductivity is increased and the rate performance is enhanced. The problems of low conductivity and safety hazards of conventional electrolytes are solved, and the high performance and safety of all-solid-state batteries are achieved.
Patent Information
- Application Number
- CN202211007122.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-22
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-08-22
AI Technical Summary
The conductivity of conventional glassy sulfide solid electrolytes is too low, which limits its application in all-solid-state batteries, and liquid electrolytes pose safety risks.
By doping P element and other metal elements, a modified glass-ceramic sulfide solid electrolyte is prepared to improve the conductivity and enhance the rate performance. The electrolyte is prepared using high-pressure tableting and vacuum heat treatment processes.
It significantly increases the conductivity rate and conductivity of Li+, improves the compatibility between the electrolyte and the lithium anode, and enhances the rate performance and safety of all-solid-state batteries.
Smart Images

Figure CN115312844B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of energy raw materials, and specifically relates to a modified microcrystalline glassy sulfide solid-state solution and a preparation method and application thereof. Background Art
[0002] At present, although lithium-ion batteries have been commercialized, liquid organic electrolytes have obvious safety risks, such as being flammable and corrosive. With the continuous development of lithium-ion battery technology, the demand for high-safety and high-energy density batteries has greatly increased. Solid-state batteries composed of solid electrolytes can solve the above problems well.
[0003] However, for all-solid-state electrolytes, solid electrolytes are non-flammable and non-volatile, which ensures the safety of the battery and can also avoid the problem of short battery life caused by the drying up of liquid electrolytes during battery cycles. However, the conductivity of conventional glassy sulfide solid electrolytes is too low, which limits their application in all-solid-state batteries. The present invention mainly improves the conductivity of the electrolyte and enhances its rate performance by replacing part of the P element with metal. Summary of the invention
[0004] In view of the defects in the prior art, the object of the present invention is to provide a modified microcrystalline glassy sulfide solid electrolyte, a preparation method and an application thereof.
[0005] The object of the present invention is achieved through the following solutions:
[0006] The first aspect of the present invention provides a modified microcrystalline glassy sulfide solid electrolyte, wherein the modified glassy sulfide solid electrolyte has a general formula of mLi 2 S-(1-mbn)(Q y S z )-nP 2 S 5 -bLiX, where 0<m<1, 0<n<1, 0<b<1, 0<1-mbn<0.7, Q is one or more of Sn, In, P, Si, Ge, As, Al, Zr, Se, Te, X is F, Cl, Br, I, (BH 4 ) - 、(TFSI) - 、(FSI) - ,(BF 4 ) - ,(PF 6 ) - , (ClO 4 ) - One or more of .
[0007] As an embodiment, m>n in the general formula of the solid electrolyte.
[0008] The present invention also relates to a method for preparing a modified microcrystalline glassy sulfide solid-state solution, the method comprising the following steps:
[0009] S1. In an argon atmosphere, the raw materials of the sulfide solid electrolyte are fully mixed to obtain a mixed solid powder and then seal the mixed solid powder;
[0010] S2, ball-milling the sealed mixed solid powder to obtain an initial solid electrolyte powder;
[0011] S3, pressing the solid electrolyte powder obtained in step S2 under high pressure to obtain an initial solid electrolyte sheet;
[0012] S4, vacuum sealing the initial solid electrolyte sheet obtained in step S3 and then heat treating it, and obtaining a modified glassy solid electrolyte after cooling.
[0013] As an embodiment, the sulfide solid electrolyte raw material in step S1 is Li 2 S.P. 2 S 5 , Q y S z , LiX.
[0014] As an implementation scheme, in step S2, the ball milling mixing speed is 400 to 550 rpm and the time is 15 to 24 hours.
[0015] As an implementation scheme, the high-pressure tableting pressure in step S3 is 200-370 MPa.
[0016] As an embodiment, the thickness of the initial solid electrolyte sheet obtained by pressing in step S3 is 500-700 μm.
[0017] As an embodiment, the vacuum treatment pressure in step S4 is 0 to 10 –4 Pa.
[0018] As an embodiment, the heat treatment temperature in step S4 is 300-500° C., and the heat treatment time is 3-10 hours.
[0019] The present invention also relates to the application of a modified microcrystalline glassy sulfide solid electrolyte in an all-solid-state battery.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] (1) The present invention generates vacancies through doping modification, so that Li + Conduct electricity smoothly and quickly, enhancing its conductivity;
[0022] (2) The present invention increases the conductivity through doping modification, so that it can be applied to all-solid-state batteries and its rate performance is improved;
[0023] (3) The present invention improves the compatibility of the electrolyte with the lithium negative electrode through doping modification, and a pure lithium negative electrode can be used as the negative electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:
[0025] Figure 1 The XRD pattern of the all-solid-state battery prepared in Example 1;
[0026] Figure 2 The impedance diagram of the all-solid-state battery obtained in Example 1;
[0027] Figure 3 The rate cycling performance of the full battery assembled in Example 1. DETAILED DESCRIPTION
[0028] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several changes and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0029] The data of the embodiments and comparative examples were fitted and calculated by AC impedance test.
[0030] Example 1
[0031] A modified glassy sulfide electrolyte 0.5Li 2 S-0.05GeS 2 -0.15P 2 S 5 -0.3Li(BH 4 ) is prepared as follows:
[0032] (1) In a glove box filled with argon, weigh Li according to the target molar ratio. 2 S.P. 2 S 5 ,GeS 2 , LiBH 4 , sealed in a ball mill to prevent it from contacting the air.
[0033] (2) Fix the sealed ball mill jar on a planetary ball mill and mill it at a speed of 550 rpm for 20 hours.
[0034] (3) The initial solid electrolyte powder obtained in step (2) was pressed into a sheet in a glove box with a thickness of 500 μm.
[0035] (4) The initial solid electrolyte sheet obtained in step (3) is placed in a quartz tube or a glass tube and vacuum-sealed.
[0036] (5) Place the sealed quartz tube or glass tube in step (4) in a muffle furnace and sinter for 10 hours at a temperature of 400°C, with a heating and cooling rate of 0.5°C / min -1 .
[0037] (6) the solid electrolyte material obtained in step (5), LiNi 0.8 Mn 0.1 Co 0.1 O 2 The conductive carbon black and the binder are mixed in a ratio of 20:75:1:4, and the mixture is ground evenly to obtain positive electrode powder. The positive electrode powder is dissolved in dimethyl ether, stirred evenly by magnetic force, and then coated on aluminum foil.
[0038] (7) The powder of the sulfide solid electrolyte material is placed in a tablet pressing mold and pressed into a solid electrolyte sheet. Then, the positive electrode sheet is placed on one side of the solid electrolyte and pressed under pressure. Finally, a lithium sheet is attached to the other side of the solid electrolyte and pressed into an all-solid-state battery. Figure 1 The XDR test image of the all-solid-state battery is shown below. Figure 2 The impedance diagram of the all-solid-state battery is shown as Figure 3 The figure shows the rate cycle diagram of the all-solid-state battery. The specific conductivity data of the solid-state battery is shown in Table 1.
[0039] Example 2
[0040] A modified glassy sulfide electrolyte 0.7Li 2 S-0.15In 2 S 3 -0.05P 2 S 5 The preparation steps of -0.1Li(TFSI) are as follows:
[0041] (1) In a glove box filled with argon, weigh Li according to the target molar ratio. 2 S.P. 2 S 5 、In 2 S 3 , LiTFSI, sealed in a ball mill to prevent it from contacting the air.
[0042] (2) Fix the sealed ball mill jar on a planetary ball mill and mill it at a speed of 400 rpm for 10 hours.
[0043] (3) The solid electrolyte powder obtained in step (2) is pressed into a sheet in a glove box with a thickness of 500 μm.
[0044] (4) The initial solid electrolyte sheet obtained in step (3) is placed in a quartz tube or a glass tube and vacuum-sealed.
[0045] (5) Place the sealed quartz tube or glass tube in step (4) in a muffle furnace and sinter for 8 hours at a temperature of 500°C, with a heating and cooling rate of 0.5°C / min -1 .
[0046] (6) The solid electrolyte material obtained in step (5), LiNi0.8Mn0.1Co0.1O2, conductive carbon black and binder are mixed in a ratio of 20:75:1:4, and the mixture is ground evenly to obtain positive electrode powder. The positive electrode powder is dissolved in dimethyl ether, magnetically stirred evenly and then coated on aluminum foil.
[0047] (7) The powder of the sulfide solid electrolyte material is placed in a tablet pressing mold and pressed into a solid electrolyte sheet. Then, the positive electrode sheet is placed on one side of the solid electrolyte and pressed under pressure. Finally, a lithium sheet is attached to the other side of the solid electrolyte and pressed into an all-solid-state battery. The specific conductivity data of the solid-state battery are shown in Table 1.
[0048] Example 3
[0049] A modified glassy sulfide electrolyte 0.3Li 2 S-0.24SiS 2 -0.06P 2 S 5 The preparation steps of -0.4LiI are as follows:
[0050] (1) In a glove box filled with argon, weigh Li according to the target molar ratio. 2 S.P. 2 S 5 、SiS 2 , LiI, sealed in a ball mill to prevent it from contacting the air.
[0051] (2) Fix the sealed ball mill jar on a planetary ball mill and mill it at a speed of 500 rpm for 16 hours.
[0052] (3) The solid electrolyte powder obtained in step (2) is pressed into a sheet in a glove box with a thickness of 500 μm.
[0053] (4) The initial solid electrolyte sheet obtained in step (3) is placed in a quartz tube or a glass tube and vacuum-sealed.
[0054] (5) Place the sealed quartz tube or glass tube in step (4) in a muffle furnace and sinter for 10 hours at a temperature of 400°C, with a heating and cooling rate of 0.5°C / min -1 .
[0055] (6) The solid electrolyte material obtained in step (5), LiNi0.8Mn0.1Co0.1O2, conductive carbon black and binder are mixed in a ratio of 20:75:1:4, and the mixture is ground evenly to obtain positive electrode powder. The positive electrode powder is dissolved in dimethyl ether, magnetically stirred evenly and then coated on aluminum foil.
[0056] (7) The powder of the sulfide solid electrolyte material is placed in a tablet pressing mold and pressed into a solid electrolyte sheet. Then, the positive electrode sheet is placed on one side of the solid electrolyte and pressed under pressure. Finally, a lithium sheet is attached to the other side of the solid electrolyte and pressed into an all-solid-state battery. The specific conductivity data of the solid-state battery are shown in Table 1.
[0057] Comparative Example 1
[0058] The raw material does not contain GeS2, and the rest is the same as in Example 1, with the general formula being 0.5Li 2 S-0.2P 2 S 5 -0.3Li(BH 4 (1) In a glove box filled with argon, weigh Li according to the target molar ratio. 2 S.P. 2 S 5 , LiBH 4 , sealed in a ball mill to prevent it from contacting the air.
[0059] (2) Fix the sealed ball mill jar on a planetary ball mill and mill it at a speed of 550 rpm for 20 hours.
[0060] (3) The solid electrolyte powder obtained in step (2) is pressed into a sheet in a glove box with a thickness of 500 μm.
[0061] (4) The initial solid electrolyte sheet obtained in step (3) is placed in a quartz tube or a glass tube and vacuum-sealed.
[0062] (5) Place the sealed quartz tube or glass tube in step (4) in a muffle furnace and sinter for 10 hours at a temperature of 400°C, with a heating and cooling rate of 0.5°C / min -1 .
[0063] (6) The solid electrolyte material obtained in step (5), LiNi0.8Mn0.1Co0.1O2, conductive carbon black and binder are mixed in a ratio of 20:75:1:4, and the mixture is ground evenly to obtain positive electrode powder. The positive electrode powder is dissolved in dimethyl ether, magnetically stirred evenly and then coated on aluminum foil.
[0064] (7) The powder of the sulfide solid electrolyte material is placed in a tablet pressing mold and pressed into a solid electrolyte sheet. Then, the positive electrode sheet is placed on one side of the solid electrolyte and pressed under pressure. Finally, a lithium sheet is attached to the other side of the solid electrolyte and pressed into an all-solid-state battery. The specific conductivity data of the solid-state battery are shown in Table 1.
[0065] Comparative Example 2
[0066] The raw materials do not contain In 2 S 3 , the rest is the same as in Example 2, the general structural formula is 0.7Li 2 S-0.2P 2 S 5 -0.1Li(TFSI).
[0067] The preparation steps of a modified glassy sulfide electrolyte are as follows:
[0068] (1) In a glove box filled with argon, weigh Li according to the target molar ratio. 2 S.P. 2 S 5 , LiTFSI, sealed in a ball mill to prevent them from contacting with air.
[0069] (2) Fix the sealed ball mill jar on a planetary ball mill and mill it at a speed of 400 rpm for 10 hours.
[0070] (3) The solid electrolyte powder obtained in step (2) is pressed into a sheet in a glove box with a thickness of 500 μm.
[0071] (4) The initial solid electrolyte sheet obtained in step (3) is placed in a quartz tube or a glass tube and vacuum-sealed.
[0072] (5) Place the sealed quartz tube or glass tube in step (4) in a muffle furnace and sinter for 8 hours at a temperature of 500°C, with a heating and cooling rate of 0.5°C / min -1 .
[0073] (6) The solid electrolyte material obtained in step (5), LiNi0.8Mn0.1Co0.1O2, conductive carbon black and binder are mixed in a ratio of 20:75:1:4, and the mixture is ground evenly to obtain positive electrode powder. The positive electrode powder is dissolved in dimethyl ether, magnetically stirred evenly and then coated on aluminum foil.
[0074] (7) The powder of the sulfide solid electrolyte material is placed in a tablet pressing mold and pressed into a solid electrolyte sheet. Then, the positive electrode sheet is placed on one side of the solid electrolyte and pressed under pressure. Finally, a lithium sheet is attached to the other side of the solid electrolyte and pressed into an all-solid-state battery. The specific conductivity data of the solid-state battery are shown in Table 1.
[0075] Comparative Example 3
[0076] The raw materials do not contain SiS 2 , the rest is the same as in Example 3, the general formula is 0.3Li 2 S-0.3P 2 S 5 -0.4LiI.
[0077] The preparation steps of a modified glassy sulfide electrolyte are as follows:
[0078] (1) In a glove box filled with argon, weigh Li according to the target molar ratio. 2 S.P. 2 S 5 , LiI, sealed in a ball mill to prevent it from contacting the air.
[0079] (2) Fix the sealed ball mill jar on a planetary ball mill and mill it at a speed of 500 rpm for 16 hours.
[0080] (3) The solid electrolyte powder obtained in step (2) is pressed into a sheet in a glove box with a thickness of 500 μm.
[0081] (4) The initial solid electrolyte sheet obtained in step (3) is placed in a quartz tube or a glass tube and vacuum-sealed.
[0082] (5) Place the sealed quartz tube or glass tube in step (4) in a muffle furnace and sinter for 10 hours at a temperature of 400°C, with a heating and cooling rate of 0.5°C / min -1 .
[0083] (6) the solid electrolyte material obtained in step (5), LiNi 0.8 Mn 0.1 Co 0.1 O 2 The conductive carbon black and the binder are mixed in a ratio of 20:75:1:4, and the mixture is ground evenly to obtain positive electrode powder. The positive electrode powder is dissolved in dimethyl ether, stirred evenly by magnetic force, and then coated on aluminum foil.
[0084] (7) The powder of the sulfide solid electrolyte material is placed in a tablet pressing mold and pressed into a solid electrolyte sheet. Then, the positive electrode sheet is placed on one side of the solid electrolyte and pressed under pressure. Finally, a lithium sheet is attached to the other side of the solid electrolyte and pressed into an all-solid-state battery. The specific conductivity data of the solid-state battery are shown in Table 1.
[0085] Table 1 Conductivity test data of embodiments and comparative examples
[0086] Electrolyte materials Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 <![CDATA[Conductivity (mS.cm -1 )]]> 3.9 2.67 2.53 0.9 0.95 0.99
[0087] By comparing the data of Examples 1-3 and Comparative Examples 1-3, it can be found that the conductivity of the all-solid-state battery prepared in Examples 1-3 is more excellent, and is significantly better than the test data of Comparative Examples 1-3. In summary, the modified microcrystalline glassy sulfide solid electrolyte of the present invention improves the electrolyte ion conductivity and broadens its application in all-solid-state batteries.
[0088] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various changes or modifications within the scope of the claims, which does not affect the essence of the present invention. In the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other arbitrarily.
Claims
1. A modified microcrystalline glassy sulfide solid electrolyte, It is characterized in that The modified glassy sulfide solid electrolyte has the general formula mLi 2 S-(1-mbn)(Q y S z )-nP 2 S 5 -bLiX, wherein 0<m<1, 0<n<1, 0<b<1, 0<1-mbn<0.7, Q is one or more of Sn, In, Si, Ge, As, Al, Zr, Se, Te, X is F, Cl, Br, I, (BH 4 ) - 、(TFSI) - 、(FSI) - ,(BF 4 ) - ,(PF 6 ) - , (ClO 4 ) - One or more of .
2. The modified microcrystalline glassy sulfide solid electrolyte according to claim 1, It is characterized in that In the general formula of the solid electrolyte, m>n.
3. A method for preparing the modified microcrystalline glassy sulfide solid electrolyte according to claim 1 or 2, It is characterized in that The method comprises the following steps: S1. In an argon atmosphere, the raw materials of the sulfide solid electrolyte are fully mixed to obtain a mixed solid powder and then seal the mixed solid powder; S2, ball-milling the sealed mixed solid powder to obtain an initial solid electrolyte powder; S3, pressing the solid electrolyte powder obtained in step S2 under high pressure to obtain an initial solid electrolyte sheet; S4, subjecting the initial solid electrolyte sheet obtained in step S3 to vacuum treatment and then heat treatment, and obtaining a modified glassy solid electrolyte after cooling.
4. The method for preparing the modified microcrystalline glassy sulfide solid electrolyte according to claim 3, It is characterized in that The raw material of the sulfide solid electrolyte in step S1 is Li 2 S.P. 2 S 5 , Q y S z , LiX.
5. The method for preparing the modified microcrystalline glassy sulfide solid electrolyte according to claim 3, It is characterized in that In step S2, the mixing ball milling speed is 400-550 rpm and the time is 15-24 hours.
6. The method for preparing the modified microcrystalline glassy sulfide solid electrolyte according to claim 3, It is characterized in that The high pressure in step S3 is 200-370 MPa.
7. The method for preparing the modified microcrystalline glassy sulfide solid electrolyte according to claim 3, It is characterized in that The thickness of the initial solid electrolyte sheet obtained by pressing in step S3 is 500-700 μm.
8. The method for preparing the modified microcrystalline glassy sulfide solid electrolyte according to claim 3, It is characterized in that The vacuum treatment pressure in step S4 is 0 to 10 –4 Pa.
9. The method for preparing the modified microcrystalline glassy sulfide solid electrolyte according to claim 3, It is characterized in that In step S4, the heat treatment temperature is 300-500° C., and the heat treatment time is 3-10 hours.
10. Use of the modified microcrystalline glassy sulfide solid electrolyte as claimed in claim 1 or 2 in an all-solid-state battery.
Citation Information
Patent Citations
SOLID STATE CATHOLYTE OR ELECTROLYTE FOR BATTERY USING LiAMPBSC (M=Si, Ge, AND / OR Sn)
CN105518906A
Preparation method of inorganic sulfide electrolyte
CN107195955A