A new processing method for precision hybrid integrated circuit

Through fiber laser drilling and cutting, electroplated copper electrodes and magnetron sputtering technology, the problems of low accuracy and unstable performance of hybrid integrated circuits are solved, high-precision lines and stable signal transmission are achieved, product life is extended, and product life is achieved Precision metallization design for micropores and large slots.

CN115334751BActive Publication Date: 2024-11-22SHANDONG ZHONGWEI ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210930366.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-03
Publication Date
2024-11-22
Estimated Expiration
2042-08-03

AI Technical Summary

Technical Problem

The existing thick film hybrid integrated circuit process has problems such as low printing accuracy, high electrical mobility of silver paste, resulting in unstable electrical performance, and the inability to achieve micropore precision filling and large-slot metallization design.

Method used

Use 150W fiber laser for drilling and cutting, use electroplated copper to replace silver paste as electrode, combine magnetron sputtering and electroplating technology to carry out precision circuit processing, and use CCD scanning positioning and laser resistance adjustment to improve line accuracy and uniform metal layer sex.

Benefits of technology

The circuit accuracy is improved to within 35μm, the electrical signal transmission stability and product life are extended, and the micro-hole filling and large-slot metallization design is perfectly realized, and the metal layer is more uniform and complete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115334751B_ABST
    Figure CN115334751B_ABST
Patent Text Reader

Abstract

A novel processing method for precision hybrid integrated circuits relates to the technical field of precision hybrid integrated circuits and solves the problems of low processing precision, unstable performance and limited design space structure of hybrid integrated circuits, including laser drilling, printing slurry, slurry sintering, magnetron sputtering, full-plate electroplating, circuit processing, AOI inspection, solder mask ink processing, surface treatment processing, laser cutting processing and vacuum packaging process; solves the problem of line accuracy and can make the circuit line width and spacing within 35μm; uses electroplated copper instead of silver paste as electrodes to control the electromigration problem, ensure the stability of electrical signal transmission and extend the service life of the product; micropores with a diameter of 0.08mm can achieve precise hole filling, large slot hole metallization can perfectly achieve coating, and the metal layer is more uniform and complete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of precision hybrid integrated circuits, and in particular to a novel processing method of precision hybrid integrated circuits. Background Art

[0002] The existing thick film hybrid integrated circuit process is to print metal paste and then sinter at high temperature to complete the processing of various ceramic surface circuits. The sintering of the resistor paste uses silver paste or silver palladium paste as electrodes to connect, and then laser adjusts. This is the only hybrid circuit processing technology currently. There are three technical defects. First, the printing process limits the printing accuracy of the circuit, and the line width and spacing can only be 150μm; second, the electromigration of silver paste is large, and the electrical performance indicators are unstable. During the packaging and potting process, it is easy to be contaminated by sulfur in the sealant, resulting in sulfur changes, which not only makes the electrical signal output unstable but also seriously affects the product life. Third, it is impossible to achieve micro-hole precision filling and large slot hole metallization design, which limits the product space design needs. These three problems need to be solved urgently. Summary of the invention

[0003] In view of the problems of low processing precision, unstable performance and limited design space structure of hybrid integrated circuits in the prior art, the present invention provides a novel processing method for precision hybrid integrated circuits, which has the following advantages: solving the problem of line precision, and making the circuit line width and spacing within 35μm; using electroplated copper instead of silver paste as electrodes, controlling the electromigration problem, ensuring the stability of electrical signal transmission, and extending the service life of the product; the micropore diameter of 0.08mm can achieve precise hole filling, the large slot hole metallization can achieve perfect coating, and the metal layer is more uniform and complete.

[0004] The present invention provides a novel method for processing a precision hybrid integrated circuit, comprising the following steps:

[0005] Step (1): laser drilling, using a 150W fiber laser for drilling and cutting, the hole diameter is 0.08mm-0.1mm, holes and grooves larger than 0.1mm are processed by laser cutting, the cutting speed is 3mm / s, the roughness of the hole wall and groove wall is not more than 2.5μm, after cutting, the scraper is used for scraping, then ultrasonic cleaning, and then drying at 150°C;

[0006] Step (2): slurry printing and sintering. On the basis of conventional ruthenium oxide resistor slurry, deoxygenation treatment and viscosity adjustment are performed. The slurry is deoxygenated and stirred with an ultrasonic oscillator, and then allowed to stand for 60 minutes. A 300# stainless steel screen is used to perform slurry printing by CCD scanning positioning. After confirmation of qualification, pre-baking is performed at 150°C for 30 minutes. The slurry is allowed to stand for more than 15 minutes. Then, a 280# screen is used to print ceramic glaze. After printing, the slurry is allowed to stand for 30 minutes, and then the slurry is directly placed in an air tunnel sintering furnace for sintering.

[0007] Step (3): magnetron sputtering and electroplating, the ruthenium oxide resistor slurry is treated with plasma for surface cleaning, argon and oxygen are used for cleaning, the treatment time is 30 minutes, and then magnetron sputtering is performed, the vacuum degree is 1*10 -4 MPa, chamber temperature 350℃, titanium plating 100nm, copper plating 800nm, after magnetron sputtering, use 2% H2SO4 to clean for 10s at room temperature, and then electroplating copper on the whole plate;

[0008] Step (4): Precision circuit processing, use a sandblasting brush machine to clean and dry the copper surface, then perform film lamination on the board surface, place the film-laminating substrate in a CCD scanning and positioning exposure machine for exposure, let the exposed substrate stand for 15 minutes and then place it in a DES line for dry film development, circuit etching, dry film removal, and then wash with water and dry.

[0009] Step (5): Circuit inspection: Use the AOI optical inspection system to optically scan the entire layout, compare the circuit data on the computer with the scanned data, and pass if it does not exceed the tolerance range;

[0010] Step (6): solder resist ink processing, use a common printing machine to print solder resist ink on the plate, let the printed substrate stand for 15 minutes, then put it into an oven for pre-curing, the curing time is 15 minutes, put the cured substrate into a CCD scanning and positioning exposure machine for exposure, let the exposed substrate stand for 15 minutes and then put it into a solder resist developer for development, and put the substrate after solder resist development into an oven for high-temperature curing, the curing time is 45 minutes;

[0011] Step (7): Surface treatment: the substrate is gold plated, and the gold thickness ranges from 0.025 μm to 1.0 μm;

[0012] Step (8): Laser resistance adjustment. According to different products, corresponding jigs are made, and then the cross-sectional area of ​​the resistance slurry is adjusted online by laser. The control accuracy of the resistance can reach within ±2%;

[0013] Step (9): laser processing, using a 150W fiber laser to cut the shape and non-metallized holes, with a cutting speed of 2mm / s and nitrogen cooling;

[0014] Step (10): Packaging: Check the processed products and pack them in anti-static vacuum bags.

[0015] Furthermore, before drilling and cutting in step (1), the ceramic surface is manually marked with red, thereby increasing the continuity and integrity of the laser cutting and ensuring uniform cutting.

[0016] Furthermore, the slurry printing thickness in step (2) is greater than 18 μm.

[0017] Furthermore, the thickness of the glaze layer of the ceramic glaze printed in step (2) is greater than 20 μm.

[0018] Furthermore, in step (2), the sintering temperature is 850° C. and the sintering time is 35 min-45 min.

[0019] Furthermore, the vacuum degree during cleaning in step (3) is set to 2*10 -2 MPa.

[0020] Furthermore, the thickness of the electroplated copper in step (3) is 10 μm-127 μm.

[0021] Furthermore, in step (4), development is performed using 1.1% anhydrous sodium carbonate at room temperature, etching is performed using acidic cupric chloride solution with a Baume degree controlled at about 2.5, and film stripping is performed using 3-5% sodium hydroxide at 45°C.

[0022] Furthermore, in step (4), the film laminating temperature is 110° C., the exposure wavelength in the exposure machine is 365 nm, and the exposure time is 15 s.

[0023] Furthermore, in step (6), the exposure wavelength in the exposure machine is 410 nm and the exposure time is 25 s.

[0024] The beneficial effects of the present invention are: solving the problem of line accuracy, and the circuit line width and spacing can be within 35μm; using electroplated copper instead of silver paste as electrodes to control the electromigration problem, ensure the stability of electrical signal transmission, and extend the service life of the product; the micropore diameter of 0.08mm can achieve precise hole filling, the large slot hole metallization can achieve perfect coating, and the metal layer is more uniform and complete.

[0025] The overall circuit material is electroplated copper. The cost of copper is much lower than that of silver, especially for large-surface metal circuits, which greatly reduces the material cost. Copper is not as active as silver in the metal element table, so the electromigration of the entire copper circuit is much smaller than that of the silver circuit, which effectively guarantees the stability of the electrical performance of the entire copper circuit, especially the signal transmission of some signal lines is more stable and consistent. Copper has much better corrosion resistance than silver. Silver will be contaminated and corroded by the sulfur contained in the sealant. Therefore, during the service life of the silver circuit, copper is not affected by sulfur, thereby extending the service life of the product. The basic positioning accuracy is guaranteed by positioning hole design and CCD scanning positioning. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0027] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0028] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0029] like Figure 1 As shown, a novel method for processing a precision hybrid integrated circuit comprises the following steps:

[0030] Step (1): laser drilling. Before drilling and cutting, the ceramic surface is painted red by manual marking to increase the continuity and integrity of laser cutting and ensure the uniformity of cutting. A 150W fiber laser is used for drilling and cutting. The hole diameter is 0.08mm-0.1mm. Holes and grooves larger than 0.1mm are processed by laser cutting. The cutting speed is 3mm / s. The roughness of the hole wall and groove wall is not more than 2.5μm. After cutting, the scraper is used for scraping, and then the water-soluble red coating material is cleaned by ultrasonic wave, and then the ceramic surface is dried at 150°C.

[0031] Step (2): slurry printing and sintering. On the basis of conventional ruthenium oxide resistor slurry, deoxygenation treatment and viscosity adjustment are performed. The slurry is deoxygenated and stirred with an ultrasonic oscillator, and then allowed to stand for 60 minutes. A 300# stainless steel screen is used for slurry printing by CCD scanning positioning. The printing thickness is greater than 18 μm. After confirmation of qualification, pre-baking is performed at 150°C for 30 minutes. The slurry is allowed to stand for cooling for more than 15 minutes. Then, a 280# screen is used for printing ceramic glaze. The glaze layer thickness is greater than 20 μm. After printing, the slurry is allowed to stand for 30 minutes. Then, the slurry is directly placed in an air tunnel sintering furnace for sintering. The sintering temperature is 850°C and the sintering time is 35 minutes to 45 minutes.

[0032] Step (3): Magnetron sputtering and electroplating, the ruthenium oxide resistor slurry is cleaned by plasma, argon and oxygen are used for cleaning, and the vacuum degree is set to 2*10 -2 MPa, treatment time 30min, followed by magnetron sputtering, vacuum degree 1*10 - 4 MPa, chamber temperature 350℃, titanium plating 100nm, copper plating 800nm, after magnetron sputtering, use 2% H2SO4 to clean for 10s at room temperature, and electroplating copper on the whole board, the thickness of electroplated copper is 10μm-127μm;

[0033] Step (4): Precision circuit processing, use a sandblasting brush machine to clean and dry the copper surface, then perform film processing on the board surface, the film laminating temperature is 110°C, the film-laminating substrate is placed in a CCD scanning and positioning exposure machine for exposure, the exposure wavelength is 365nm, the exposure time is 15s, the exposed substrate is placed in a DES line for dry film development, circuit etching, and dry film removal, the development is carried out using 1.1% anhydrous sodium carbonate at room temperature, the etching is carried out using acidic cupric chloride solution, the Baume degree is controlled at about 2.5, the film is removed using 3-5% sodium hydroxide at 45°C, and then washed with water and dried;

[0034] Step (5): Circuit inspection: Use the AOI optical inspection system to optically scan the entire layout, compare the circuit data on the computer with the scanned data, and pass if it does not exceed the tolerance range;

[0035] Step (6): solder resist ink processing, use an ordinary printing machine to print solder resist ink on the plate, the color of the ink is selected by the customer, the screen is 200#, the thickness is more than 20μm, the printed substrate is allowed to stand for 15 minutes, and then placed in an 85℃ oven for pre-curing, the curing time is 15 minutes, the cured substrate is placed in a CCD scanning and positioning exposure machine for exposure, the exposure wavelength is 410nm, the exposure time is 25s, the exposed substrate is allowed to stand for 15 minutes and then placed in a solder resist developer for development, the development uses anhydrous sodium carbonate with a concentration of 1.5%, the temperature is 35℃, the substrate after solder resist development is placed in a 150℃ oven for high temperature curing, the curing time is 45 minutes;

[0036] Step (7): Surface treatment. The conventional surface treatment process for ceramic substrates is gold plating. The thickness of gold is selected according to the packaging process requirements of the later customers. Generally, there are electroplated gold and chemical nickel gold. Chemical nickel gold and chemical nickel bar gold are commonly used. The gold thickness range is 0.025μm-1.0μm. The substrate containing slurry cannot be treated with alkaline solution in the gold plating pre-treatment process, and can only be treated with 1-2% weak acid;

[0037] Step (8): Laser resistance adjustment. According to different products, corresponding jigs are made, and then the cross-sectional area of ​​the resistance slurry is adjusted online by laser. The control accuracy of the resistance can reach within ±2%;

[0038] Step (9): Laser processing, using a 150W fiber laser to cut the shape and non-metallized holes, with a cutting speed of 2mm / s and nitrogen cooling, so that the cutting flash can be controlled not to be too long, the cutting edge has no edge collapse, and the finish will be much better, not exceeding 2.5μm;

[0039] Step (10): Packaging. Check the processed products and use anti-static vacuum absorption bags for packaging. The packaging layer cannot exceed 10 layers and the vacuuming time is controlled within 45 seconds. A calcium oxide moisture absorption bag should be placed in the packaging bag. The packaging should not leak and the product should not be misplaced.

[0040] The beneficial effects of the present invention are: solving the problem of line accuracy, and the circuit line width and spacing can be within 35μm; using electroplated copper instead of silver paste as electrodes to control the electromigration problem, ensure the stability of electrical signal transmission, and extend the service life of the product; the micropore diameter of 0.08mm can achieve precise hole filling, the large slot hole metallization can achieve perfect coating, and the metal layer is more uniform and complete.

[0041] The overall circuit material is electroplated copper. The cost of copper is much lower than that of silver, especially for large-surface metal circuits, which greatly reduces the material cost. Copper is not as active as silver in the metal element table, so the electromigration of the entire copper circuit is much smaller than that of the silver circuit, which effectively guarantees the stability of the electrical performance of the entire copper circuit, especially the signal transmission of some signal lines is more stable and consistent. Copper has much better corrosion resistance than silver. Silver will be contaminated and corroded by the sulfur contained in the sealant. Therefore, during the service life of the silver circuit, copper is not affected by sulfur, thereby extending the service life of the product. The basic positioning accuracy is guaranteed by positioning hole design and CCD scanning positioning.

[0042] Although the present invention has been described in detail by referring to the accompanying drawings and in combination with the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person skilled in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person skilled in the art who is familiar with the present technical field can easily think of changes or substitutions within the technical scope disclosed by the present invention, and they shall be within the scope of protection of the present invention.

Claims

1. A method for processing a precision hybrid integrated circuit, characterized in that: The following steps are involved: Step (1): laser drilling, using a 150W fiber laser for drilling and cutting, the hole diameter is 0.08mm-0.1mm, holes and grooves larger than 0.1mm are processed by laser cutting, the cutting speed is 3mm / s, the roughness of the hole wall and groove wall is not more than 2.5μm, after cutting, scrape with a scraper, then clean with ultrasonic wave, and then dry at 150℃; Step (2): slurry printing and sintering. On the basis of conventional ruthenium oxide resistor slurry, deoxygenation treatment and viscosity adjustment are performed. The slurry is deoxygenated and stirred with an ultrasonic oscillator, and then allowed to stand for 60 minutes. A 300# stainless steel screen is used to perform slurry printing using CCD scanning positioning. After confirmation of qualification, pre-baking is performed at 150°C for 30 minutes. The slurry is allowed to stand for more than 15 minutes, and then a 280# screen is used to print ceramic glaze. After printing, the slurry is allowed to stand for 30 minutes, and then the slurry is directly placed in an air tunnel sintering furnace for sintering. Step (3): Magnetron sputtering and electroplating. The ruthenium oxide resistor slurry is cleaned by plasma. Argon and oxygen are used for cleaning. The treatment time is 30 minutes. Then magnetron sputtering is performed. The vacuum degree is 1*10 -4 MPa, chamber temperature 350℃, titanium plating 100nm, copper plating 800nm, after magnetron sputtering, use 2% H2SO4 to clean for 10s at room temperature, and then electroplating copper on the whole plate; Step (4): Precision circuit processing: Use a sandblasting brush to clean and dry the copper surface, then apply film to the board surface. After applying the film, place the substrate in a CCD scanning and positioning exposure machine for exposure. After the exposure, place the substrate in a DES line for 15 minutes to develop the dry film, etch the circuit, remove the dry film, and then wash with water and dry it. Step (5): Circuit inspection: Use the AOI optical inspection system to optically scan the entire layout, compare the circuit data on the computer with the scanned data, and pass if it does not exceed the tolerance range; Step (6): solder resist ink processing: use a common printing machine to print solder resist ink on the plate, let the printed substrate stand for 15 minutes, then put it into an oven for pre-curing, the curing time is 15 minutes, put the cured substrate into a CCD scanning and positioning exposure machine for exposure, let the exposed substrate stand for 15 minutes, then put it into a solder resist developer for development, and put the substrate after solder resist development into an oven for high temperature curing, the curing time is 45 minutes; Step (7): Surface treatment: the substrate is plated with gold, and the thickness of the gold is in the range of 0.025 μm to 1.0 μm; Step (8): Laser resistance adjustment. According to different products, corresponding jigs are made, and then the cross-sectional area of ​​the resistance slurry is adjusted online by laser. The control accuracy of the resistance can reach within ±2%; Step (9): Laser processing, using a 150W fiber laser to cut the shape and non-metallized holes, with a cutting speed of 2mm / s and nitrogen cooling; Step (10): Packaging: Check the processed products and use anti-static vacuum bags for packaging.

2. The method for processing a precision hybrid integrated circuit according to claim 1, characterized in that: Step (1) Before drilling and cutting, the ceramic surface is manually marked with red, thereby increasing the continuity and integrity of the laser cutting and ensuring uniform cutting.

3. The method for processing a precision hybrid integrated circuit according to claim 1, characterized in that: In step (2), the slurry printing thickness is greater than 18 μm.

4. The method for processing a precision hybrid integrated circuit according to claim 1, characterized in that: The thickness of the glaze layer of the printed ceramic glaze in step (2) is greater than 20 μm.

5. The method for processing a precision hybrid integrated circuit according to claim 1, characterized in that: The sintering temperature of step (2) is 850°C and the sintering time is 35 min-45 min.

6. The method for processing a precision hybrid integrated circuit according to claim 1, characterized in that: Step (3) The vacuum degree during cleaning is set to 2*10 -2 MPa.

7. The method for processing a precision hybrid integrated circuit according to claim 1, characterized in that: The thickness of the electroplated copper in step (3) is 10 μm-127 μm.

8. The method for processing a precision hybrid integrated circuit according to claim 1, characterized in that: In step (4), development is performed using 1.1% anhydrous sodium carbonate at room temperature, etching is performed using acidic copper chloride solution with a Baume degree controlled at about 2.5, and film stripping is performed using 3-5% sodium hydroxide at 45°C.

9. The method for processing a precision hybrid integrated circuit according to claim 1, characterized in that: Step (4) The film lamination temperature is 110°C, the exposure wavelength in the exposure machine is 365nm, and the exposure time is 15s.

10. The method for processing a precision hybrid integrated circuit according to claim 1, characterized in that: Step (6) The exposure wavelength in the exposure machine is 410 nm and the exposure time is 25 s.