Polyoxyalkylene polymer mixture and curable composition
By synthesizing a polyoxyalkylene polymer mixture with a specific terminal structure ratio, the problem of low resilience of hydrolyzable silyl polymers in the prior art is solved, and a cured product with low modulus and high resilience is achieved. A sealing material that is not easy to seep.
Patent Information
- Application Number
- CN202180023913.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-31
- Filing Date
- 2021-03-22
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-03-22
AI Technical Summary
In the prior art, although the polyoxyalkylene-based polymer cured substance containing hydrolyzable silyl groups can inhibit ooze exudation when using a reactive diluent, the resilience is low, and the modulus is increased to improve the resilience will lead to The softness is reduced, making it difficult to maintain low modulus and high resilience.
By synthesizing a polymer with an average of 1.5 or more of the terminal structure per 1 molecule, combining a polyoxyalkylene-based polymer mixture with hydrolyzable silyl, terminal olefin and internal olefin groups, the proportion of the terminal structure is adjusted to form a low The specific method includes introducing hydrolyzable silyl groups, terminal olefin groups and internal olefin groups into the polyoxyalkylene polymer to ensure that the moles of the hydrolyzable silyl group accounts for the total moles of the total moles. The ratio is between 40 and 75%, to improve resilience.
It realizes the improvement of the resilience of the cured substance while maintaining low modulus, and is suitable for sealing materials that are not prone to leakage, taking into account both softness and mechanical properties.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to a mixture of polyoxyalkylene polymers having a hydrolyzable silyl group, and a curable composition containing the mixture. Background Art
[0002] Polymers having a hydrolyzable silyl group are known as wet-process reactive polymers, and are included in many industrial products such as adhesives, sealants, coating agents, paints, and pressure-sensitive adhesives, and are used in a wide range of fields.
[0003] As the main chain skeleton of such polymers, polyoxyalkylene polymers, saturated hydrocarbon polymers, (meth)acrylate polymers, etc. are known. In particular, polyoxyalkylene polymers having a hydrolyzable silyl group are easy to handle at room temperature with a relatively low viscosity, and the cured product obtained after the reaction also shows good elasticity, and have a wide range of applications.
[0004] Patent document 1 discloses a room temperature curable composition containing a polyoxyalkylene polymer having a hydrolyzable silyl group at at least one end. As a method for producing the polymer, the following method is described: after converting the terminal hydroxyl group of the polyoxyalkylene polymer into an alkoxide group, an organic halide such as allyl chloride is reacted to introduce a carbon-carbon double bond into the terminal, and further a hydrosilane is subjected to an addition reaction to convert the terminal into a hydrolyzable silyl group.
[0005] In addition, Patent Document 2 discloses a polyoxyalkylene polymer having two or more hydrolyzable silyl groups at one terminal portion, and as a method for producing the polymer, the following method is described: first, after converting the terminal hydroxyl group of the polymer into an alkoxide group, an epoxy compound having a carbon-carbon double bond is reacted, and further an organic halide having a carbon-carbon double bond such as allyl chloride is reacted, thereby introducing two or more carbon-carbon double bonds into one terminal portion, and then a hydrosilane is subjected to an addition reaction.
[0006] On the other hand, in recent years, the construction market has been seeking sealing materials that are less likely to leak out. Therefore, a method has been studied in which a reactive diluent having a hydrolyzable silyl group introduced only at one end of a polymer molecular chain is added to replace the existing phthalate plasticizers and PPG plasticizers in a curable composition for sealing materials.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 52-73998
[0010] Patent Document 2: International Publication No. 2013 / 180203 Summary of the invention
[0011] Problems to be solved by the invention
[0012] If such a reactive diluent is combined with a curable composition containing a hydrolyzable silyl polyoxyalkylene polymer, although exudation can be suppressed, there is a tendency that the resilience of the cured product (the ability to return to the original shape after a given deformation) is reduced. In order to cope with this tendency, a method for improving resilience by increasing the modulus of the cured product containing a hydrolyzable silyl polyoxyalkylene polymer as a base polymer (the stress required for a given deformation, in this case, the stress during elongation of a dumbbell-shaped test body) is considered. However, if the modulus increases, it will lead to a decrease in flexibility, and therefore, it is desirable to keep the modulus at a low level.
[0013] In view of the above-mentioned current situation, an object of the present invention is to provide a mixture of a hydrolyzable silyl group-containing polyoxyalkylene polymer capable of forming a cured product having improved restorability despite having a low modulus, and a curable composition containing the mixture.
[0014] Solutions to the problem
[0015] The present inventors have conducted intensive studies to solve the above-mentioned problems and have found that a mixture of a polymer having an average of 1.5 or more terminal structures per polymer molecule (or the number is 2 or more) and a polymer having an average of 1.2 or less terminal structures per polymer molecule (or the number is 1), wherein the polymers are polyoxyalkylene polymers having a hydrolyzable silyl group and a terminal olefin group and / or an internal olefin group in the terminal structure, the total number of the hydrolyzable silyl group, the terminal olefin group and the internal olefin group in each polymer is more than 1.0 per terminal structure, and the ratio of the number of moles of the hydrolyzable silyl group to the total number of moles of the hydrolyzable silyl group, the terminal olefin group and the internal olefin group in the entire mixture is set to a low level of 40 to 75%, thereby being able to form a mixture of hydrolyzable silyl group-containing polyoxyalkylene polymers that exhibits a low modulus (i.e., high flexibility) but a high recovery property. The present invention has been completed.
[0016] That is, the first aspect of the present invention relates to a mixture, which is a mixture of polyoxyalkylene polymers (A) and (B), each of which has a main chain structure of polyoxyalkylene and a terminal structure bonded to the terminal of the main chain structure,
[0017] The terminal structure has a hydrolyzable silyl group and a terminal olefin group and / or an internal olefin group.
[0018] The number of the terminal structures per molecule of the polyoxyalkylene polymer (A) is 1.5 or more,
[0019] The number of the terminal structures per molecule of the polyoxyalkylene polymer (B) is 1.2 or less,
[0020] In each of the polyoxyalkylene polymers (A) and (B), the total number of the hydrolyzable silyl group, the terminal olefin group and the internal olefin group in the terminal structure is more than 1.0 per terminal structure.
[0021] In the entire mixture, the ratio of the number of moles of the hydrolyzable silyl group to the total number of moles of the hydrolyzable silyl group, the terminal olefin group and the internal olefin group is 40 to 75%.
[0022] It is preferred that the polyoxyalkylene polymer (A) has two or more terminal structures in one molecule, and the polyoxyalkylene polymer (B) has one terminal structure in one molecule.
[0023] A second aspect of the present invention relates to a mixture comprising a polyoxyalkylene polymer (A) and a polyoxyalkylene polymer (B), each of which has a main chain structure of polyoxyalkylene and a terminal structure bonded to a terminal of the main chain structure.
[0024] The terminal structure has a hydrolyzable silyl group and a terminal olefin group and / or an internal olefin group.
[0025] The polyoxyalkylene polymer (A) has two or more terminal structures in one molecule.
[0026] The polyoxyalkylene polymer (B) has one terminal structure in one molecule.
[0027] In each of the polyoxyalkylene polymers (A) and (B), the total number of the hydrolyzable silyl group, the terminal olefin group and the internal olefin group in the terminal structure is more than 1.0 per terminal structure.
[0028] In the entire mixture, the ratio of the number of moles of the hydrolyzable silyl group to the total number of moles of the hydrolyzable silyl group, the terminal olefin group and the internal olefin group is 40 to 75%.
[0029] The polyoxyalkylene polymer (A) preferably has two terminal structures in one molecule.
[0030] In the first aspect and the second aspect, it is preferred that the cured product of the mixture has a stress at 100% elongation of 0.30 MPa or less.
[0031] It is preferred that the ratio of the number of moles of the hydrolyzable silyl group to the total number of moles of the hydrolyzable silyl group, the terminal olefin group and the internal olefin group in the entire mixture is 40 to 70%.
[0032] It is preferred that the terminal structure include a site derived from an epoxy compound having a terminal olefin group.
[0033] It is preferred that in the entire mixture, the total number of the hydrolyzable silyl group, the terminal olefin group, and the internal olefin group in the terminal structure is more than 2.0 per terminal structure.
[0034] Preferably, the hydrolyzable silyl group is represented by the general formula (3):
[0035] -SiR 2 Y2(3)
[0036] (Where R 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, or a triorganosiloxy group represented by (R')3SiO-. R' represents the same or different substituted or unsubstituted monovalent hydrocarbon groups having 1 to 20 carbon atoms. Y represents the same or different hydroxyl groups or hydrolyzable groups.)
[0037] It is preferred that the number of the hydrolyzable silyl groups is 1.0 or more per terminal structure in the entire mixture.
[0038] Furthermore, the present invention relates to a curable composition comprising the above mixture.
[0039] Preferably, the curable composition further contains a reactive diluent (D), which is a polymer having 0.5 or more and less than 1.2 hydrolyzable silyl groups per molecule and having a viscosity at 23° C. lower than that of the mixture.
[0040] It is preferred that the curable composition further contains a (meth)acrylate polymer (C) having a hydrolyzable silyl group.
[0041] Furthermore, the present invention also relates to a cured product of the above curable composition.
[0042] In addition, the present invention also relates to a method for producing the above-mentioned mixture in a first embodiment, the method comprising: a step of forming the main chain structure of the above-mentioned polyoxyalkylene by polymerizing a mixture of an initiator having an average of 1.5 or more hydroxyl groups per molecule and an initiator having an average of 1.2 or less hydroxyl groups per molecule with an epoxy compound; and a step of forming the above-mentioned terminal structure at the terminal of the above-mentioned main chain structure. Preferably, the initiator having an average of 1.5 or more hydroxyl groups per molecule has 2 or more hydroxyl groups per molecule, and the initiator having an average of 1.2 or less hydroxyl groups per molecule has 1 hydroxyl group per molecule.
[0043] In addition, the present invention also relates to a second method for producing the above-mentioned mixture, which method includes: a process of forming the main chain structure of the above-mentioned polyoxyalkylene by polymerizing a mixture of an initiator having more than two hydroxyl groups in one molecule and an initiator having one hydroxyl group in one molecule with an epoxy compound; and a process of forming the above-mentioned terminal structure at the end of the above-mentioned main chain structure.
[0044] Effects of the Invention
[0045] According to the present invention, there can be provided a mixture of a hydrolyzable silyl group-containing polyoxyalkylene polymer capable of forming a cured product having improved restorability despite having a low modulus, and a curable composition containing the mixture. DETAILED DESCRIPTION
[0046] Hereinafter, embodiments of the present invention will be described in detail.
[0047] <Mixture of polyoxyalkylene polymers (A) and (B)>
[0048] The polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B) contained in the mixture of the present invention respectively have a main chain structure of polyoxyalkylene and a terminal structure bonded to the terminal of the main chain structure. It should be noted that the mixture of the present invention refers to a mixture substantially containing only the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B).
[0049] The main chain structure is a polymer main chain composed of oxyalkylene repeating units. The main chain structure may be a linear structure or a branched structure. The main chain structure is preferably a polymer main chain composed only of oxyalkylene repeating units, or a polymer main chain composed only of structures derived from an initiator used in polymerization in addition to oxyalkylene repeating units. Here, oxyalkylene repeating units refer to repeating units constituting polyethers, for example, oxyalkylene units having 2 to 6 carbon atoms, preferably 2 to 4 carbon atoms.
[0050] The main chain structure of polyoxyalkylene is not particularly limited, and examples thereof include polyoxyethylene, polyoxypropylene, polyoxybutylene, polytetrahydrofuran, polyoxyethylene-polyoxypropylene copolymer, polyoxypropylene-polyoxybutylene copolymer, etc. Polyoxypropylene is preferred. As the main chain structure, only one type can be used, or two or more types can be used in combination. In addition, the main chain structure of the polyoxyalkylene polymer (A) can be the same as or different from the main chain structure of the polyoxyalkylene polymer (B).
[0051] The terminal structure refers to a site that does not contain the oxyalkylene repeating unit constituting the main chain structure, and the site is bonded to the terminal of the main chain structure. The terminal structure has a hydrolyzable silyl group, and a terminal olefin group and / or an internal olefin group. A terminal group that does not contain any of the hydrolyzable silyl group, the terminal olefin group, and the internal olefin group (for example, a butyl group bonded to the terminal of the main chain structure) does not belong to the terminal structure.
[0052] For example, when the main chain structure of the polyoxyalkylene polymer (A) is linear, the terminal structure may be present in a maximum of 2 per molecule of the polymer (A) on average. When the main chain structure of the polymer (A) is branched, for example, when the branch is tri-branched, the terminal structure may be present in a maximum of 3 per molecule of the polymer (A) on average, and may be present in more than 3 depending on the branch structure. In addition, when the main chain structure of the polymer (A) is a mixture of linear and branched structures, the number of terminal structures per molecule of the polymer may be a value between 2 and 3 on average. The terminal structure may be bonded to the oxyalkylene unit located at the end of the main chain structure via an oxygen atom.
[0053] The polyoxyalkylene polymers (A) and (B) each have a terminal structure having a hydrolyzable silyl group, and either or both of a terminal olefin group and an internal olefin group. The terminal structure having a hydrolyzable silyl group, and either or both of a terminal olefin group and an internal olefin group does not mean that all the terminal structures contained in the polymer have a hydrolyzable silyl group, and either or both of a terminal olefin group and an internal olefin group, but means that in the polymer (A) or (B) as a whole including a plurality of polymer molecules, the terminal structure has a hydrolyzable silyl group, and either or both of a terminal olefin group and an internal olefin group. That is, the terminal structure in a certain molecule contained in the polymer (A) or (B) may have only a hydrolyzable silyl group but not a terminal olefin group or an internal olefin group, or may have either or both of a terminal olefin group and an internal olefin group but not a hydrolyzable silyl group.
[0054] According to the first embodiment of the present invention, for the polyoxyalkylene polymer (A), the number of the above-mentioned terminal structures per molecule of the polymer is 1.5 or more, preferably 1.7 or more, and more preferably 1.9 or more. In addition, the upper limit of the number of the above-mentioned terminal structures per molecule of the polymer (A) is not particularly limited, and is preferably 4 or less on average, more preferably 3 or less on average, and particularly preferably 2 or less on average. In the first embodiment, the polymer (A) is preferably a polymer having two or more of the above-mentioned terminal structures in one molecule, and more preferably a polymer having two of the above-mentioned terminal structures in one molecule.
[0055] According to the second embodiment of the present invention, the polyoxyalkylene polymer (A) is a polymer having two or more of the above-mentioned terminal structures in one molecule. The upper limit of the number of the above-mentioned terminal structures in one molecule of the polymer (A) is not particularly limited, and is preferably 4 or less, and more preferably 3 or less. The polyoxyalkylene polymer (A) is particularly preferably a polymer having two of the above-mentioned terminal structures in one molecule. It should be noted that in the second embodiment, the number of terminal structures in one molecule of the polymer is not an average value.
[0056] When the polyoxyalkylene polymer (A) has a linear main chain structure, there are two molecular chain ends, and both of the two molecular chain ends include the above terminal structure, so that the polyoxyalkylene polymer (A) has two of the above terminal structures in one molecule. The polyoxyalkylene polymer (A) having such a linear main chain structure can be produced, for example, by performing one or more steps of reaction, wherein an epoxy compound is polymerized in the presence of an initiator having two hydroxyl groups in one molecule, followed by a reaction of introducing a hydrolyzable silyl group.
[0057] In addition, when the polyoxyalkylene polymer (A) has a branched main chain structure, there are three or more molecular chain ends, and at least two of the molecular chain ends (preferably all of the molecular chain ends) contain the above-mentioned terminal structure, so that the polyoxyalkylene polymer (A) has two or more of the above-mentioned terminal structures in one molecule. The polyoxyalkylene polymer (A) having such a branched main chain structure can be produced, for example, by performing one or more steps of reaction, wherein an epoxy compound is polymerized in the presence of an initiator having three or more hydroxyl groups in one molecule, followed by a reaction of introducing a hydrolyzable silyl group.
[0058] The polyoxyalkylene polymer (A) is preferably a polymer having a linear main chain structure. However, as the polyoxyalkylene polymer (A), a polymer having a branched main chain structure may be used, or a polymer having a linear main chain structure and a polymer having a branched main chain structure may be used in combination.
[0059] According to the first embodiment of the present invention, for the polyoxyalkylene polymer (B), the number of the above-mentioned terminal structures per 1 molecule of the polymer is 1.2 or less, preferably 1.1 or less, and more preferably 1.0 or less. In addition, the lower limit of the number of the above-mentioned terminal structures per 1 molecule of the polymer (B) is not particularly limited, and is preferably 0.5 or more, more preferably 0.6 or more, and particularly preferably 0.7 or more. The main chain structure of the polyoxyalkylene polymer (B) is preferably linear. In addition, the above-mentioned terminal structure possessed by the polymer (B) is more preferably present only at one of the two ends of the linear polymer (B). In the case where the above-mentioned terminal structure is present only at one end of the linear polymer (B), the above-mentioned terminal structure exists at most 1 per 1 molecule of the polymer (B). In the first embodiment, the polymer (B) is preferably a polymer having only 1 of the above-mentioned terminal structures in 1 molecule.
[0060] According to the second embodiment of the present invention, the polyoxyalkylene polymer (B) is a polymer having only one of the above-mentioned terminal structures in one molecule. Such a polyoxyalkylene polymer (B) can be manufactured, for example, by performing one or more steps of reaction, wherein the one or more steps of reaction are a reaction in which an epoxy compound is polymerized in the presence of an initiator having only one hydroxyl group in one molecule and a hydrolyzable silyl group is introduced. The polyoxyalkylene polymer thus obtained contains a structure derived from the above-mentioned initiator at one molecular chain end. For example, when butanol is used as an initiator, the obtained polyoxyalkylene polymer contains a butyl group at one molecular chain end. The structure derived from such an initiator belongs to the above-mentioned terminal group that does not contain any of the hydrolyzable silyl group, the terminal olefin group, and the internal olefin group.
[0061] It should be noted that, in addition to the terminal structure comprising a hydrolyzable silyl group, and a terminal olefin group and / or an internal olefin group, the polyoxyalkylene polymer (A) may also have the terminal group not containing any of the hydrolyzable silyl group, the terminal olefin group, and the internal olefin group, or may not have the terminal group. On the other hand, the polyoxyalkylene polymer (B) has both the terminal structure and the terminal group.
[0062] The hydrolyzable silyl group is a silyl group that forms a siloxane bond by hydrolysis and dehydration condensation and can bond with each other. The polyoxyalkylene polymers (A) and (B) each have the hydrolyzable silyl group, thereby showing curability based on the dehydration condensation reaction. The hydrolyzable silyl group of the polyoxyalkylene polymer (A) and the hydrolyzable silyl group of the polyoxyalkylene polymer (B) may be the same or different.
[0063] The hydrolyzable silyl group can be specifically represented by the following general formula (1):
[0064] -(Si(R 1 2-b )(Y′ b )O) m S i 2 3-a Y a (1).
[0065] In formula (1), R 1 and R 2 represents the same or different substituted or unsubstituted monovalent hydrocarbon groups having 1 to 20 carbon atoms, or a triorganosiloxy group represented by (R′)3SiO-. R′ represents the same or different substituted or unsubstituted monovalent hydrocarbon groups having 1 to 20 carbon atoms. Y and Y′ represent the same or different hydroxyl groups or hydrolyzable groups. a represents 0, 1, 2 or 3. b represents 0, 1 or 2, and when m is 2 or more, different numbers may coexist as b. m represents an integer from 0 to 19. wherein a+m×b represents an integer greater than 1.
[0066] In R 1 or R 2 In the substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, the carbon number is preferably 1 to 10, more preferably 1 to 8, further preferably 1 to 6, further preferably 1 to 3, and particularly preferably 1 or 2. When the hydrocarbon group has a substituent, the substituent is not particularly limited, and examples thereof include halogen groups such as chloro, alkoxy groups such as methoxy, and amino groups such as N,N-diethylamino.
[0067] R' in the triorganosiloxy group represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. The carbon number is preferably 1 to 10, more preferably 1 to 8, further preferably 1 to 6, further preferably 1 to 3, and particularly preferably 1 or 2. When the hydrocarbon group has a substituent, the substituent is not particularly limited, and examples thereof include halogen groups such as chloro, alkoxy groups such as methoxy, and amino groups such as N,N-diethylamino. The three R's may be the same or different from each other.
[0068] As R 1 and R 2, for example, unsubstituted alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-hexyl, 2-ethylhexyl, and n-dodecyl; substituted alkyl groups such as chloromethyl, methoxymethyl, and N,N-diethylaminomethyl; unsaturated hydrocarbon groups such as vinyl, isopropenyl, and allyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl, tolyl, and 1-naphthyl; aralkyl groups such as benzyl; triorganosiloxy groups represented by (R′)3SiO- in which R′ is methyl, phenyl, etc. Preferably, it is a substituted or unsubstituted alkyl group, more preferably methyl, ethyl, chloromethyl, and methoxymethyl, further preferably methyl and ethyl, and particularly preferably methyl. As R 1 and R 2 Only one group may be used, or two or more groups may be used in combination.
[0069] As Y and Y', for example, hydroxyl, hydrogen, halogen, alkoxy, acyloxy, oxime ester, amino, amide, acid amide, aminooxy, mercapto, alkenyloxy, etc. can be mentioned. The above-mentioned alkoxy and the like may have a substituent. Since the hydrolysis is stable and easy to handle, an alkoxy group is preferred, and a methoxy group, an ethoxy group, a n-propoxy group, an isopropoxy group is more preferred, a methoxy group, an ethoxy group is further preferred, and a methoxy group is particularly preferred. As Y and Y', only one group may be used, or two or more groups may be used in combination.
[0070] As described above, m represents an integer of 0 to 19, and preferably represents 0. When m is 0, the above general formula (1) is represented by the following general formula (2):
[0071] -SiR 2 3-a Y a (2).
[0072] In the general formula (2), a represents 1, 2 or 3.
[0073] Examples of the hydrolyzable silyl group represented by the general formula (2) include a trimethoxysilyl group, a triethoxysilyl group, a tri(2-propenyloxy)silyl group, a triacetoxysilyl group, a methyldimethoxysilyl group, a methyldiethoxysilyl group, a dimethoxyethylsilyl group, a (chloromethyl)dimethoxysilyl group, a (chloromethyl)diethoxysilyl group, a (methoxymethyl)dimethoxysilyl group, a (methoxymethyl)diethoxysilyl group, a (N,N-diethylaminomethyl)dimethoxysilyl group, and a (N,N-diethylaminomethyl)diethoxysilyl group. Among them, methyldimethoxysilyl, trimethoxysilyl, triethoxysilyl, (chloromethyl) dimethoxysilyl, (methoxymethyl) dimethoxysilyl, (methoxymethyl) diethoxysilyl, (N, N- diethylaminomethyl) dimethoxysilyl are preferred because they show high reactivity and can obtain a cured product with good mechanical properties. From the viewpoint of reactivity, trimethoxysilyl, (chloromethyl) dimethoxysilyl, (methoxymethyl) dimethoxysilyl are more preferred. From the viewpoint of stability, methyldimethoxysilyl, methyldiethoxysilyl, triethoxysilyl are preferred, and methyldiethoxysilyl and triethoxysilyl are further preferred. In addition, trimethoxysilyl, triethoxysilyl, and methyldimethoxysilyl are more preferred because they are easy to manufacture. Among them, methyldimethoxysilyl is most preferred.
[0074] In the above general formula (2), in order to achieve both storage stability and reactivity of the polymer and flexibility of the cured product, a is preferably 2. When a is 2, the above general formula (2) is represented by the following general formula (3):
[0075] -SiR 2 Y2(3).
[0076] In the formula, R 2 and Y have the same meanings as above. In the above general formula (1) or (2), two or more hydrolyzable silyl groups having different a's may be used in combination.
[0077] The terminal olefin group refers to a carbon-carbon double bond having a methylene group (H2C=), and specifically, can be represented by the following general formula (4):
[0078] H2C=C(R 3 )-CH2- (4).
[0079] In formula (4), R 3represents hydrogen, or a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, a substituted or unsubstituted aryl group having 6 to 10 carbon atoms, or a substituted or unsubstituted aralkyl group having 7 to 10 carbon atoms. The number of carbon atoms of the alkyl group is preferably 1 to 8, more preferably 1 to 6, further preferably 1 to 3, and particularly preferably 1 or 2. The number of carbon atoms of the aryl group is preferably 6 to 8, more preferably 6 to 7. The number of carbon atoms of the aralkyl group is more preferably 7 to 8. When the alkyl group, aryl group, or aralkyl group has a substituent, the substituent is not particularly limited, and examples thereof include halogen groups such as chloro, alkoxy groups such as methoxy, and amino groups such as N,N-diethylamino.
[0080] As R 3 Examples of R include hydrogen, alkyl groups such as methyl, ethyl, propyl, and butyl, aryl groups such as phenyl, and aralkyl groups such as benzyl. 3 , preferably hydrogen or alkyl, more preferably hydrogen, methyl or ethyl, and still more preferably hydrogen or methyl. 3 They can be the same or different.
[0081] The internal olefin group is a carbon-carbon double bond without a methylene group (H2C=), and specifically, can be represented by the following general formula (5):
[0082] H3C-C(R 3 )=CH- (5).
[0083] R in formula (5) 3 Usually represents the same as R in the above formula (4) 3 The same group, in R 3 Within the definition range, it can be expressed as R in formula (4) 3 In addition, the presence of multiple R 3 They can be the same or different.
[0084] As described later, the internal olefin group is a group that can be generated by the internal conversion reaction of the terminal olefin group. 3 =H), the internal olefin group generated by the internal conversion reaction is a 1-propenyl group.
[0085] The polyoxyalkylene polymers (A) and (B) each have a hydrolyzable silyl group, and a terminal olefin group and / or an internal olefin group in their terminal structures. In each of the polyoxyalkylene polymers (A) and (B), the total number of the hydrolyzable silyl group, the terminal olefin group and the internal olefin group in the terminal structure is more than 1.0 per terminal structure on average. Thus, the cured product of the mixture of the polyoxyalkylene polymers (A) and (B) can show a lower modulus when the amount of hydrolyzable silyl group introduced is the same as that of the cured product of the polyoxyalkylene polymer having the total number being less than 1.0 per terminal structure. The total number in each of the polymers (A) and (B) is preferably 1.1 or more, more preferably 1.3 or more, further preferably 1.5 or more, and further preferably 2.0 or more. Furthermore, it is particularly preferably greater than 2.0, and most preferably 2.5 or more. The upper limit of the total number is not limited, but is preferably 10 or less, more preferably 8 or less, further preferably 6 or less, and particularly preferably 5 or less. In addition, the said total number in a polyoxyalkylene type polymer (A) and the said total number in a polyoxyalkylene type polymer (B) may be the same or different.
[0086] The total number of hydrolyzable silyl groups, terminal olefin groups and internal olefin groups per one of the terminal structures can be appropriately determined by a person skilled in the art. As an example, as described later, when a polyoxyalkylene polymer (A) or (B), or a mixture of (A) and (B), is produced by reacting a hydroxyl-terminated polyoxyalkylene polymer (E) with an epoxy compound having a terminal olefin group and then reacting the polymer with an organic halide having a terminal olefin group, the total number can be calculated by adding 1 (the number of olefin groups introduced by the organic halide) to the equivalent number of hydroxyl groups of the epoxy compound relative to the hydroxyl-terminated polyoxyalkylene polymer (E). In addition, the total number can also be calculated by using the polyoxyalkylene polymer (A) and / or (B) and its precursor intermediate of the present invention. 1 The content of the iodine value can be calculated by analyzing H NMR, iodine value / hydroxyl value obtained by titration, etc.
[0087] According to the present invention, for the mixture of polyoxyalkylene polymers (A) and (B), the proportion of hydrolyzable silyl groups relative to the total of hydrolyzable silyl groups, terminal olefin groups and internal olefin groups in the mixture as a whole is reduced to a relatively low level, thereby forming a cured product having improved resilience while maintaining a low modulus. That is, in the mixture of polyoxyalkylene polymers (A) and (B), the proportion of the number of moles of hydrolyzable silyl groups relative to the total number of moles of hydrolyzable silyl groups, terminal olefin groups and internal olefin groups is an average of 40% or more and 75% or less. By setting this ratio to 40% or more and 75% or less, the cured product containing the mixture of polyoxyalkylene polymers (A) and (B) of the present invention can have both low modulus and good resilience.
[0088] In order to further reduce the modulus of the above-mentioned cured product, the above-mentioned ratio in the overall mixture of polymers (A) and (B) is preferably 74% or less, more preferably 72% or less, further preferably 70% or less, further preferably 65% or less, and particularly preferably 59% or less. In addition, in order to further improve the recovery of the above-mentioned cured product, the above-mentioned ratio in the overall mixture of polymers (A) and (B) is preferably 50% or more, more preferably 55% or more, further preferably 60% or more, and particularly preferably 65% or more. In order to take into account both the modulus and the recovery of the above-mentioned cured product, the above-mentioned ratio in the overall mixture of polymers (A) and (B) is preferably in the range of 55% or more and 70% or less.
[0089] In addition, in each of the polyoxyalkylene polymers (A) and (B), the ratio of the number of moles of hydrolyzable silyl groups to the total number of moles of hydrolyzable silyl groups, terminal olefin groups and internal olefin groups is preferably 30% or more and 80% or less on average. The above ratio in each of the polymers (A) and (B) is more preferably 75% or less, more preferably 70% or less, still more preferably 65% or less, and particularly preferably 60% or less. In addition, the above ratio in each of the polymers (A) and (B) is more preferably 35% or more, more preferably 40% or more, still more preferably 45% or more, and particularly preferably 50% or more. It should be noted that the above ratio in the polyoxyalkylene polymer (A) and the above ratio in the polyoxyalkylene polymer (B) may be the same as or different from that in the polyoxyalkylene polymer (B).
[0090] In addition, "the ratio of the number of moles of hydrolyzable silyl groups to the total number of moles of hydrolyzable silyl groups, terminal olefin groups and internal olefin groups" can also be expressed by "the introduction rate of hydrolyzable silyl groups".
[0091] The ratio of the molar number of the hydrolyzable silyl group to the total molar number of the hydrolyzable silyl group, the terminal olefin group and the internal olefin group can be calculated by1 For example, when the terminal olefin group is an allyl group and a hydrolyzable silyl group is introduced into the terminal structure by hydrosilylation of a hydrosilane compound having a hydrolyzable silyl group as described below, calculation can be performed using the integral values of the following signals.
[0092] ·Hydrolyzable silyl group: CH2 bonded to the silyl group (around 0.6 ppm, 2H)
[0093] Terminal olefin group: CH2 of methylene group (around 5.2ppm, 2H)
[0094] Internal olefin group: CH bonded to the terminal CH3 group (total of near 4.3ppm and near 4.8ppm, 1H)
[0095] It should be noted that, when other signals are superimposed, the integral value of the signal is removed for calculation.
[0096] The mixture of polyoxyalkylene polymers (A) and (B) has hydrolyzable silyl groups within the range satisfying the above-mentioned total number of hydrolyzable silyl groups, terminal olefin groups and internal olefin groups; and the ratio of the molar number of hydrolyzable silyl groups to the total molar number of hydrolyzable silyl groups, terminal olefin groups and internal olefin groups. In the above-mentioned mixture as a whole, the number of hydrolyzable silyl groups is preferably 0.7 or more per terminal structure, more preferably 0.9 or more, further preferably 1.0 or more, further preferably 1.2 or more, particularly preferably 1.4 or more, and most preferably 1.5 or more. Thus, the mixture of polyoxyalkylene polymers (A) and (B) can show good curability. The upper limit of the above-mentioned number of hydrolyzable silyl groups is not particularly limited, and is preferably 10 or less per terminal structure, more preferably 5 or less, further preferably 3 or less, and particularly preferably 2.5 or less.
[0097] The number of hydrolyzable silyl groups per terminal structure can be calculated by multiplying the above-mentioned "total number of hydrolyzable silyl groups, terminal olefin groups and internal olefin groups per terminal structure" by the above-mentioned "ratio of the molar number of hydrolyzable silyl groups to the total molar number of hydrolyzable silyl groups, terminal olefin groups and internal olefin groups".
[0098] The specific structure of the terminal structure having a hydrolyzable silyl group and a terminal olefin group and / or an internal olefin group possessed by the polyoxyalkylene polymers (A) and (B) is not particularly limited. As an example of the terminal structure having a hydrolyzable silyl group and a terminal olefin group, the following general formula (6) can be shown:
[0099] [Chemical formula 1]
[0100]
[0101] In addition, as another example, the following general formula (7) can be shown:
[0102] [Chemical formula 2]
[0103]
[0104] The oxygen atom on the left end in the general formulae (6) and (7) represents the oxygen in the oxyalkylene unit located at the end of the main chain structure of the polyoxyalkylene. In the general formulae (6) and (7), the group represented by the general formula (2) is shown as the hydrolyzable silyl group, but the present invention is not limited thereto.
[0105] In the general formulae (6) and (7), d and e each represent an integer greater than 0, and the sum of d and e is greater than 0 per terminal structure. The sum of d and e is preferably greater than 0.1, more preferably greater than 0.3, further preferably greater than 0.5, and further preferably greater than 1.0. It is particularly preferably greater than 1.0, and most preferably greater than 1.5. In addition, the sum of d and e is preferably less than 9, more preferably less than 7, further preferably less than 5, and particularly preferably less than 4.
[0106] R 2 and R 3 The multiple R in each formula has the same meaning as above. 2 or R 3 They can be the same or different.
[0107] In the general formulas (6) and (7), R 4 represents a divalent organic group having 1 to 6 carbon atoms which is directly bonded or optionally has an oxygen atom. The number of carbon atoms in the organic group is preferably 1 to 4, more preferably 1 to 2, and even more preferably 2. 4 , preferably a divalent organic group having 1 to 6 carbon atoms optionally having an oxygen atom, more preferably -CH2-, -CH2O-, -CH2OCH2-, -C(=O)-O-CH2-, and further preferably -CH2OCH2-. 4 They can be the same or different.
[0108] In the general formulas (6) and (7), R 5 represents a divalent organic group having 1 to 6 carbon atoms which is directly bonded or optionally has an oxygen atom. The number of carbon atoms in the organic group is preferably 1 to 4, more preferably 1 to 2, and even more preferably 1. 5 , preferably a direct bond, a divalent hydrocarbon group having 1 to 6 carbon atoms, more preferably a direct bond, -CH2-, or -CH2CH2-, further preferably a direct bond, -CH2-, and particularly preferably -CH2-.
[0109] The terminal structure represented by the general formula (6) has (e+1) hydrolyzable silyl groups and d terminal olefin groups. The terminal structure represented by the general formula (7) has e hydrolyzable silyl groups and (d+1) terminal olefin groups. The d terminal olefin group-containing units and the e hydrolyzable silyl group-containing units shown in the general formula (6) or (7) correspond to the sites derived from the epoxy compound having a terminal olefin group described later.
[0110] The terminal structure represented by the general formula (6) or (7) represents one terminal structure bonded to one end of the main chain structure. In the formula (6) or (7), a plurality of hydrolyzable silyl groups and / or terminal olefin groups are shown, but the formula (6) or (7) respectively represents one terminal structure instead of two or more terminal structures, indicating that a plurality of hydrolyzable silyl groups and / or terminal olefin groups exist in one terminal structure. In addition, the oxyalkylene repeating unit constituting the main chain structure is not shown in the formula (6) or (7). That is, the structures in brackets that exist in d or e numbers in the formula (6) or (7) do not belong to the oxyalkylene repeating units constituting the main chain structure.
[0111] These general formulae are merely examples for illustration, and the terminal structures in the present invention are not limited to these chemical structures. The terminal olefin groups contained in the general formulae (6) and (7) may also be internal olefin groups. In particular, a portion of the multiple terminal olefin groups present may also be internal olefin groups. In addition, the bonding order of the d terminal olefin group-containing units and the e hydrolyzable silyl group-containing units is not limited to the order shown in the general formulae (6) and (7). The specific structural formula of the terminal structure possessed by the polyoxyalkylene polymers (A) and (B) is not limited to a single structural formula, and generally various structural formulas may coexist. The terminal structure represented by the general formula (6) may coexist with the terminal structure represented by the general formula (7). In addition, the terminal structure possessed by the polyoxyalkylene polymer (A) may be the same as or different from the terminal structure possessed by the polyoxyalkylene polymer (B).
[0112] The ratio of the polyoxyalkylene polymer (A) to (B) in the mixture of the present invention is not particularly limited, but is preferably 95:5 to 20:80, more preferably 90:10 to 30:70, further preferably 80:20 to 40:60, and particularly preferably 75:25 to 50:50 by weight. It should be noted that the polyoxyalkylene polymers (A) and (B) of the present invention may be used alone or in combination of two or more.
[0113] The number average molecular weight of each of the polyoxyalkylene polymers (A) and (B) is not particularly limited, but from the viewpoint of achieving a balance between production cost and polymer handleability, the polystyrene equivalent molecular weight determined by GPC is preferably 3,000 to 100,000, more preferably 3,000 to 50,000, and even more preferably 3,000 to 30,000.
[0114] The molecular weight distribution (Mw / Mn) of each polyoxyalkylene polymer (A) and (B) is not particularly limited, but preferably narrow. Specifically, it is preferably less than 2.0, more preferably less than 1.6, further preferably less than 1.5, and particularly preferably less than 1.4. In addition, from the viewpoint of improving the durability, elongation, etc. of the cured product and improving various mechanical properties, it is preferably less than 1.2. The molecular weight distribution (Mw / Mn) can be calculated based on the number average molecular weight and weight average molecular weight determined by GPC.
[0115] From the perspective of being able to maintain the flexibility of the cured product of the curable composition containing the mixture, for the mixture of polyoxyalkylene polymers (A) and (B), the stress at 100% elongation (100% modulus) of the cured product of the mixture is preferably 0.30 MPa or less, more preferably 0.25 MPa or less, and further preferably 0.20 MPa or less. On the other hand, in order to maintain the mechanical properties of the cured product, the stress at 100% elongation of the cured product of the above-mentioned mixture is preferably 0.10 MPa or more, more preferably 0.12 MPa or more, and further preferably 0.15 MPa or more. Here, the stress at 100% elongation of the cured product of the above-mentioned mixture is defined as a value measured under the following conditions.
[0116] <Method for measuring stress at 100% elongation of cured product of mixture>
[0117] A mixture of polymer (A) and (B) / tin (II) octylate / laurylamine / distilled water = 40 / 1.2 / 0.2 / 0.24 (weight ratio) was filled into a 3 mm thick sheet mold frame, stored at 23°C and 50% relative humidity for more than 1 hour, and then aged in a 70°C dryer for 20 hours to obtain a sheet-like cured product.
[0118] The obtained cured product was punched into a No. 3 dumbbell shape to obtain a test piece according to JIS K 6251. The obtained test piece was subjected to a tensile test (tensile speed 200 mm / min) at 23°C and 50% relative humidity using an Autograph to measure the stress at 100% elongation.
[0119] <Method for producing polyoxyalkylene polymer (A) or (B), or a mixture of polymers (A) and (B)>
[0120] Next, a method for producing a polyoxyalkylene polymer (A) or (B), or a mixture of polymers (A) and (B) is described. It should be noted that when producing the above-mentioned mixture, the polyoxyalkylene polymers (A) and (B) can be synthesized independently and then mixed, or the polyoxyalkylene polymers (A) and (B) can be synthesized simultaneously in one system.
[0121] When the polyoxyalkylene polymer (A) or (B) is synthesized individually or when the polyoxyalkylene polymer (A) and (B) are synthesized simultaneously in one system, a mixture of the polymers (A) and (B) can be produced by introducing more than 1.0 terminal olefin groups per terminal structure into a hydroxyl-terminated polyoxyalkylene polymer (E) by utilizing the reactivity of the hydroxyl group, and then reacting the mixture with a hydrolyzable silyl group-containing compound reactive with the terminal olefin group to introduce a hydrolyzable silyl group.
[0122] The following is a specific description of the method for producing a polyoxyalkylene polymer (A) or (B), or a mixture of polymers (A) and (B). However, the method is not limited to the following description. First, a hydroxyl-terminated polyoxyalkylene polymer (E) is reacted with an epoxy compound (8) having a terminal olefin group, and further reacted with an organic halide (10) having a terminal olefin group, thereby introducing more than 1.0 terminal olefin groups per terminal structure of the polymer. Next, a hydrosilane compound (12) having a hydrolyzable silyl group is subjected to a hydrosilylation reaction with the terminal olefin group, thereby introducing a hydrolyzable silyl group into the terminal structure to obtain a polyoxyalkylene polymer (A) or (B), or a mixture of polymers (A) and (B). In the above production method, the reaction of the terminal structure of the polymer can be represented by the following reaction formula, for example. It should be noted that, in the formula, X represents a halogen and M represents an alkali metal.
[0123] [Chemical formula 3]
[0124]
[0125] In the present invention, when the hydrolyzable silyl group is introduced, not all the reactive terminal olefin groups are reacted with the above-mentioned hydrosilane compound, but the reaction rate is suppressed so that a part of the terminal olefin groups remain in an unreacted state, thereby obtaining a polyoxyalkylene polymer (A) or (B) in which the ratio of the molar number of the hydrolyzable silyl group to the total molar number of the hydrolyzable silyl group, the terminal olefin group and the internal olefin group satisfies the range of 40 to 75%, or a mixture of the polymers (A) and (B).
[0126] The internal olefin group can be generated by an internal conversion reaction (isomerization) of the terminal olefin group as a side reaction during the hydrosilylation reaction. The generated internal olefin group has a low hydrosilylation activity and therefore does not react with the hydrosilane compound during the hydrosilylation reaction and remains in the polyoxyalkylene polymer (A) and / or (B).
[0127] Hereinafter, one embodiment of a method for producing a polyoxyalkylene polymer (A) or (B), or a mixture of polymers (A) and (B) will be described in detail, but the method for producing a polyoxyalkylene polymer (A) or (B), or a mixture of polymers (A) and (B) is not limited to the following description.
[0128] (polymerization)
[0129] The main chain structure of the polyoxyalkylene polymer can be formed by polymerizing an epoxy compound and an initiator having a hydroxyl group by a conventionally known method, thereby obtaining a hydroxyl-terminated polyoxyalkylene polymer (E). The specific polymerization method is not particularly limited, but a polymerization method using a composite metal cyanide complex catalyst such as a zinc hexacyanocobaltate glyme complex is preferred because a hydroxyl-terminated polymer having a small molecular weight distribution (Mw / Mn) can be obtained.
[0130] The initiator having a hydroxyl group is not particularly limited, and examples thereof include organic compounds having one or more hydroxyl groups, such as ethylene glycol, propylene glycol, glycerin, pentaerythritol, low molecular weight polyoxypropylene glycol, low molecular weight polyoxypropylene triol, butanol, allyl alcohol, low molecular weight polyoxypropylene monoallyl ether, and low molecular weight polyoxypropylene monoalkyl ether.
[0131] According to the first embodiment of the present invention, as an initiator having a hydroxyl group, a mixture of an initiator having an average of more than 1.5 hydroxyl groups in one molecule and an initiator having an average of less than 1.2 hydroxyl groups in one molecule is used. In the presence of the mixture, an epoxy compound is polymerized to form a main chain structure, thereby obtaining a hydroxyl-terminated polyoxyalkylene polymer (E) in the form of a mixture of two polymers. The polymer (E) is subjected to the later-described terminal olefin group introduction step and the hydrolyzable silyl group introduction step to form a terminal structure, thereby synthesizing a mixture of polymers (A) and (B) of the first embodiment of the present invention in one system. The initiator having an average of more than 1.5 hydroxyl groups in one molecule is preferably an initiator having more than 2 hydroxyl groups in one molecule, and more preferably an initiator having 2 hydroxyl groups in one molecule. In addition, the initiator having an average of less than 1.2 hydroxyl groups in one molecule is preferably an initiator having 1 hydroxyl group in one molecule.
[0132] According to the second embodiment of the present invention, as an initiator having a hydroxyl group, a mixture of an initiator having more than two hydroxyl groups in one molecule and an initiator having one hydroxyl group in one molecule is used, and an epoxy compound is polymerized to form a main chain structure under the condition of the presence of the mixture, thereby obtaining a hydroxyl-terminated polyoxyalkylene polymer (E) in the form of a mixture of two polymers. The initiator having more than two hydroxyl groups in the above-mentioned 1 molecule is preferably an initiator having two hydroxyl groups in one molecule. For example, in the case of using an initiator having two hydroxyl groups in one molecule and a mixture of an initiator having one hydroxyl group in one molecule such as butanol, the obtained hydroxyl-terminated polyoxyalkylene polymer (E) becomes a mixture of a polyoxyalkylene polymer having a hydroxyl group at both ends and a polyoxyalkylene polymer having a hydroxyl group at a single end. Then, the introduction process of the terminal olefin group and the introduction process of the hydrolyzable silyl group described later are implemented to form a terminal structure, thereby a mixture of the polymer (A) and (B) of the second embodiment of the present invention can be synthesized in one system.
[0133] When only an organic compound having two or more hydroxyl groups is used as the initiator having a hydroxyl group, the polymer (A) can be synthesized, and when only an organic compound having one hydroxyl group is used, the polymer (B) can be synthesized.
[0134] The epoxy compound is not particularly limited, and examples thereof include alkylene oxides such as ethylene oxide and propylene oxide, and glycidyl ethers such as methyl glycidyl ether and butyl glycidyl ether. Propylene oxide is preferred.
[0135] (Introduction of terminal olefin group)
[0136] As a method for introducing more than 1.0 terminal olefin groups per terminal structure, a method is preferably used in which an alkali metal salt is allowed to act on a hydroxyl-terminated polyoxyalkylene polymer (E) to convert the terminal hydroxyl group into an alkoxide group, and then the alkali metal salt is reacted with an epoxy compound (8) having a terminal olefin group, and then the alkali metal salt is reacted with an organic halide (10) having a terminal olefin group. Alternatively, a composite metal cyanide complex catalyst may be used instead of the alkali metal salt.
[0137] The alkali metal salt is not particularly limited, and examples thereof include sodium hydroxide, sodium alkoxide, potassium hydroxide, potassium alkoxide, lithium hydroxide, lithium alkoxide, cesium hydroxide, cesium alkoxide, etc. For ease of handling and solubility, sodium hydroxide, sodium methoxide, sodium ethoxide, potassium hydroxide, potassium methoxide, potassium ethoxide, and more preferably sodium methoxide and potassium methoxide. From the perspective of availability, sodium methoxide is particularly preferred. The alkali metal salt can also be provided for the reaction in a state dissolved in a solvent.
[0138] The amount of the alkali metal salt used is not particularly limited, but is preferably 0.5 or more, more preferably 0.6 or more, further preferably 0.7 or more, and further preferably 0.8 or more in terms of the molar ratio relative to the hydroxyl group of the hydroxyl-terminated polyoxyalkylene polymer (E). The molar ratio is preferably 1.2 or less, and more preferably 1.1 or less.
[0139] The alkali metal salt is used to convert the hydroxyl group of the hydroxyl-terminated polyoxyalkylene polymer (E) into an alkoxide group. In order to efficiently carry out the conversion reaction, it is preferred to remove water and substances having hydroxyl groups other than the polyoxyalkylene polymer from the reaction system in advance. The removal can be carried out by a known method, for example, heating evaporation, reduced pressure devolatilization, spray gasification, thin film evaporation, azeotropic devolatilization, etc.
[0140] The temperature for allowing the alkali metal salt to act can be appropriately set by those skilled in the art, and is preferably 50° C. to 150° C., more preferably 110° C. to 145° C. The time for allowing the alkali metal salt to act is preferably 10 minutes to 5 hours, more preferably 30 minutes to 3 hours.
[0141] Next, by subjecting the epoxy compound (8) having a terminal olefin group to a ring-opening addition reaction with the polyoxyalkylene polymer, a terminal structure (9) including a site derived from the epoxy compound having a terminal olefin group can be formed.
[0142] The above-mentioned epoxide compound having a terminal olefin group can be represented by the chemical formula (8) in the above-mentioned reaction formula, but is not limited thereto. Specific examples of the epoxide compound include allyl glycidyl ether, methallyl glycidyl ether, glycidyl acrylate, glycidyl methacrylate, butylene oxide, 1,4-cyclopentadiene monoepoxide, etc., and allyl glycidyl ether is particularly preferred.
[0143] The amount of the epoxy compound (8) having a terminal olefin group is not particularly limited and may be appropriately set in consideration of the total number of hydrolyzable silyl groups, terminal olefin groups and internal olefin groups in the target terminal structure and the reactivity of the epoxy compound used. Specifically, the molar ratio of the epoxy compound (8) to the hydroxyl group of the hydroxyl-terminated polyoxyalkylene polymer (E) is preferably 0.1 or more, more preferably 0.3 or more, further preferably 0.5 or more, and further preferably 1.0 or more. It is particularly preferably greater than 1.0, and most preferably 1.5 or more. In addition, the molar ratio is preferably 9 or less, more preferably 7 or less, further preferably 5 or less, and particularly preferably 4 or less.
[0144] The reaction temperature when subjecting the epoxide compound (8) having a terminal olefin group to a ring-opening addition reaction can be appropriately set by a person skilled in the art, and is preferably 60° C. to 150° C., more preferably 110° C. to 145° C. The reaction time is preferably 10 minutes to 5 hours, more preferably 1 hour to 4 hours.
[0145] Next, an organic halide (10) having a terminal olefin group is reacted with a polyoxyalkylene polymer having a terminal structure (9) containing a site derived from an epoxy compound having a terminal olefin group, thereby forming an ether bond by a halogen substitution reaction and converting the alkoxide group at the polymer terminal into a terminal olefin group. Thus, a terminal structure (11) having more than 1.0 terminal olefin groups per terminal structure can be formed.
[0146] The organic halide having a terminal olefin group can be represented by the chemical formula (10) in the above reaction formula, but is not limited thereto. Specific examples of the organic halide include vinyl chloride, allyl chloride, methallyl chloride, vinyl bromide, allyl bromide, methallyl bromide, vinyl iodide, allyl iodide, methallyl iodide, etc. For ease of handling, allyl chloride and methallyl chloride are preferred.
[0147] The amount of the organic halide (10) having a terminal olefin group is not particularly limited, but is preferably 0.7 or more, more preferably 1.0 or more, in terms of molar ratio relative to the hydroxyl group of the hydroxyl-terminated polyoxyalkylene polymer (E). The molar ratio is preferably 5.0 or less, more preferably 2.0 or less.
[0148] The temperature at which the organic halide (10) having a terminal olefin group is reacted can be appropriately set by a person skilled in the art, and is preferably 50° C. to 150° C., more preferably 110° C. to 140° C. The reaction time is preferably 10 minutes to 5 hours, more preferably 20 minutes to 2 hours.
[0149] (Introduction of Hydrolyzable Silyl Group)
[0150] A hydrosilane compound (12) having a hydrolyzable silyl group is subjected to a hydrosilylation reaction with a polyoxyalkylene polymer having a terminal structure (11) in which the number of terminal olefin groups per terminal structure is greater than 1.0 on average, thereby introducing a hydrolyzable silyl group into a portion of the terminal olefin groups. At this time, the remaining portion of the terminal olefin groups does not react with the hydrosilane compound (12) and remains in the polymer. In addition, in the hydrosilylation reaction, as described above, a portion of the terminal olefin groups may be isomerized into internal olefin groups by a side reaction. By the above operation, a polyoxyalkylene polymer (A) or (B) having terminal structures (6) and / or (7) having a hydrolyzable silyl group and terminal olefin groups and / or internal olefin groups, or a mixture of polymers (A) and (B) can be produced. In addition to being easy to carry out, the hydrosilylation reaction also allows easy adjustment of the amount of hydrolyzable silyl groups introduced, and has the advantage that the physical properties of the resulting polymer are stable.
[0151] The above-mentioned hydrolyzable silyl group-containing hydrosilane compound can be represented by the chemical formula (12) in the above-mentioned reaction formula, but is not limited thereto. Specific examples of the above-mentioned hydrosilane compound include halogenated silanes such as trichlorosilane, dichloromethylsilane, chlorodimethylsilane, dichlorophenylsilane, (chloromethyl)dichlorosilane, (dichloromethyl)dichlorosilane, bis(chloromethyl)chlorosilane, (methoxymethyl)dichlorosilane, (dimethoxymethyl)dichlorosilane, and bis(methoxymethyl)chlorosilane; trimethoxysilane, triethoxysilane, dimethoxymethylsilane, diethoxymethylsilane, dimethoxyphenylsilane, Ethyldimethoxysilane, methoxydimethylsilane, ethoxydimethylsilane, (chloromethyl)methylmethoxysilane, (chloromethyl)dimethoxysilane, (chloromethyl)diethoxysilane, bis(chloromethyl)methoxysilane, (methoxymethyl)methylmethoxysilane, (methoxymethyl)dimethoxysilane, bis(methoxymethyl)methoxysilane, (methoxymethyl)diethoxysilane, (ethoxymethyl)diethoxysilane, (3,3,3-trifluoropropyl)dimethoxysilane, Methoxysilane, (N,N-diethylaminomethyl)dimethoxysilane, (N,N-diethylaminomethyl)diethoxysilane, [(chloromethyl)dimethoxysilyloxy]dimethylsilane, [(chloromethyl)diethoxysilyloxy]dimethylsilane, [(methoxymethyl)dimethoxysilyloxy]dimethylsilane, [(methoxymethyl)diethoxysilyloxy]dimethylsilane, [(diethylaminomethyl)dimethoxysilyloxy]dimethyl Alkoxysilanes such as [(3,3,3-trifluoropropyl)dimethoxysilyloxy]dimethylsilane; acyloxysilanes such as diacetoxymethylsilane and diacetoxyphenylsilane; ketoximate silanes such as bis(dimethylketoxime)methylsilane and bis(cyclohexylketoxime)methylsilane; isopropenoxysilanes (deacetone type) such as triisopropenoxysilane, (chloromethyl)diisopropenoxysilane and (methoxymethyl)diisopropenoxysilane.
[0152] The amount of the hydrosilane compound (12) having a hydrolyzable silyl group may be appropriately set in consideration of the amount of terminal olefin groups in the polyoxyalkylene polymer before the hydrosilylation reaction so that the ratio of the number of moles of the hydrolyzable silyl group to the total number of moles of the hydrolyzable silyl group, the terminal olefin group and the internal olefin group is in the range of 40 to 75%. Specifically, the molar ratio of the hydrosilane compound to the terminal olefin group in the polyoxyalkylene polymer before the hydrosilylation reaction is preferably 40 to 75%.
[0153] In order to promote the reaction, the hydrosilylation reaction is preferably carried out in the presence of a hydrosilylation catalyst. As hydrosilylation catalysts, metals such as cobalt, nickel, iridium, platinum, palladium, rhodium, ruthenium, and their complexes are known, and these hydrosilylation catalysts can be used. Specifically, there can be mentioned: a catalyst in which platinum is supported on a carrier such as alumina, silica, carbon black, etc.; chloroplatinic acid; a chloroplatinic acid complex containing chloroplatinic acid and an alcohol, aldehyde, ketone, etc.; a platinum-olefin complex [e.g., Pt(CH2=CH2)2(PPh3), Pt(CH2=CH2)2Cl2]; a platinum-vinylsiloxane complex [e.g., Pt{(vinyl)Me2SiOSiMe2(vinyl)}, Pt{Me(vinyl)SiO}4]; a platinum-phosphine complex [e.g., Ph(PPh3)4, Pt(PBu3)4]; a platinum-phosphite complex [e.g., Pt{P(OPh)3}4], etc. From the viewpoint of reaction efficiency, platinum catalysts such as chloroplatinic acid and vinylsiloxane platinum complexes are preferred.
[0154] The temperature conditions of the hydrosilylation reaction are not particularly limited, and those skilled in the art can set them appropriately. For the purpose of reducing the viscosity of the reaction system and improving reactivity, it is preferred to react under heating conditions, specifically, more preferably at 50°C to 150°C, and further preferably at 70°C to 120°C. The reaction time can also be appropriately set, and in order to prevent the condensation reaction of the unexpected polymer, it is preferred to adjust the reaction time together with the temperature conditions. Specifically, it is preferably 30 minutes or more and 5 hours or less, and more preferably 3 hours or less.
[0155] The hydrosilylation reaction may be carried out in the presence of a trialkyl orthocarboxylate, which can suppress the viscosity increase during the hydrosilylation reaction and improve the storage stability of the obtained polymer.
[0156] Examples of the trialkyl orthocarboxylate include trimethyl orthoformate, triethyl orthoformate, trimethyl orthoacetate, triethyl orthoacetate, etc. Preferred are trimethyl orthoformate and trimethyl orthoacetate.
[0157] When a trialkyl orthocarboxylate is used, its amount is not particularly limited, but is preferably about 0.1 to 10 parts by weight, more preferably about 0.1 to 3 parts by weight, relative to 100 parts by weight of the polyoxyalkylene polymer (A) or (B), or a mixture of the polymers (A) and (B).
[0158] <Curable composition>
[0159] The present invention can provide a curable composition comprising a mixture of the polyoxyalkylene polymers (A) and (B).
[0160] (Silanol condensation catalyst)
[0161] The curable composition of the present invention preferably contains a silanol condensation catalyst for the purpose of accelerating the hydrolysis / condensation reaction of the hydrolyzable silyl groups of the polyoxyalkylene polymers (A) and (B), that is, accelerating the curing reaction.
[0162] As the silanol condensation catalyst, a conventionally known silanol condensation catalyst can be used, and specifically, an organic tin compound, a carboxylic acid metal salt, an amine compound, a carboxylic acid, a metal alkoxide, an inorganic acid, etc. can be used.
[0163] Specific examples of the organotin compound include dibutyltin dilaurate, dibutyltin dioctoate, dibutyltin bis(butylmaleate), dibutyltin diacetate, dibutyltin oxide, dibutyltin bis(acetylacetonate), a reaction product of dibutyltin oxide and a silicate compound, a reaction product of dibutyltin oxide and a phthalate, dioctyltin diacetate, dioctyltin dilaurate, dioctyltin bis(ethylmaleate), dioctyltin bis(octylmaleate), dioctyltin bis(acetylacetonate), a reaction product of dioctyltin oxide and a silicate compound, etc. Due to the increasing concern for the environment in recent years, dioctyltin compounds are preferred.
[0164] Specific examples of the carboxylic acid metal salt include tin carboxylate, bismuth carboxylate, titanium carboxylate, zirconium carboxylate, iron carboxylate, etc. As the carboxylic acid group, the following carboxylic acids can be combined with various metals.
[0165] Specific examples of amine compounds include: amines such as octylamine, 2-ethylhexylamine, laurylamine, and stearylamine; nitrogen-containing heterocyclic compounds such as pyridine, 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), and 1,5-diazabicyclo[4.3.0]nonene-5 (DBN); guanidines such as guanidine, phenylguanidine, and diphenylguanidine; biguanides such as butylbiguanidine, 1-o-tolylbiguanidine, and 1-phenylbiguanidine; amino-containing silane coupling agents; ketimine compounds, etc.
[0166] Specific examples of the carboxylic acid include acetic acid, propionic acid, butyric acid, 2-ethylhexanoic acid, lauric acid, stearic acid, oleic acid, linoleic acid, neodecanoic acid, and versatic acid.
[0167] Specific examples of the metal alkoxide include titanium compounds such as tetrabutyl titanate, titanium tetrakis(acetylacetonate), and diisopropoxytitanium bis(ethyl acetylacetonate); aluminum compounds such as aluminum tris(acetylacetonate), and diisopropyl ethylaluminum acetylacetate; and zirconium compounds such as zirconium tetrakis(acetylacetonate).
[0168] As other silanol condensation catalysts, compounds containing fluorine anions, photoacid generators, and photobase generators may also be used.
[0169] The silanol condensation catalyst may be used in combination of two or more different catalysts. For example, by using the above-mentioned amine compound and carboxylic acid in combination, there is a possibility that the effect of improving the reactivity can be obtained.
[0170] As the amount of the silanol condensation catalyst, from the viewpoint of both improving the condensation reaction rate and the operability during curing, it is preferably 0.001 to 20 parts by weight, more preferably 0.01 to 15 parts by weight, and particularly preferably 0.01 to 10 parts by weight relative to 100 parts by weight of the mixture of the polyoxyalkylene polymer (A) and (B) of the present invention. In addition, in the silanol condensation catalyst, after the curable composition is cured, there is a situation where it oozes out to the surface of the cured product or contaminates the surface of the cured product. In such a case, by setting the amount of the silanol condensation catalyst to 0.01 to 3.0 parts by weight, the surface state of the cured product can be well maintained while ensuring the curability.
[0171] (Reactive diluent (D))
[0172] The curable composition of the present invention preferably has 0.5 or more and less than 1.2 hydrolyzable silyl groups per molecule, and further contains a reactive diluent (D), which is a polymer having a viscosity measured at 23°C lower than that of the mixture of the polyoxyalkylene polymers (A) and (B) of the present invention. In the present invention, when such a reactive diluent (D) is added, the viscosity of the composition can be reduced while maintaining high resilience, thereby suppressing bleeding. However, the reactive diluent (D) does not belong to any of the above-mentioned polyoxyalkylene polymers (A) and (B).
[0173] Examples of the main chain skeleton of the reactive diluent (D) include polyoxyalkylene polymers, saturated hydrocarbon polymers, (meth)acrylate polymers, polyorganosiloxane polymers, etc. Among these, polyoxyalkylene polymers are also preferred as the main chain skeleton of the reactive diluent (D) from the viewpoint of compatibility of the mixture of the polyoxyalkylene polymers (A) and (B) of the present invention.
[0174] The hydrolyzable silyl group in the reactive diluent (D) may be located at the molecular chain end, the side chain, or any of the two positions. In particular, when the hydrolyzable silyl group is located at the molecular chain end, the molecular weight between the crosslinking points becomes longer, and it is easy to obtain a rubber-like cured product with good mechanical properties, which is more preferred. The number of hydrolyzable silyl groups is an average of 0.5 or more and less than 1.2 per molecule. From the perspective of mechanical properties during curing, the lower limit is preferably 0.6 or more. In addition, in order to effectively reduce the modulus of the cured product, it is preferably less than 1.0.
[0175] In addition, the reactive diluent (D) may or may not have a terminal olefin group and / or an internal olefin group in addition to the hydrolyzable silyl group, and the total number of the hydrolyzable silyl group, the terminal olefin group and the internal olefin group may be 1.0 or less per terminal structure.
[0176] From the viewpoint of obtaining a viscosity-lowering effect while ensuring good mechanical properties of the cured product, the polymer as the reactive diluent (D) preferably has a number average molecular weight of 3,000 or more and less than 15,000 as measured by polystyrene conversion using GPC.
[0177] The molecular weight distribution of the reactive diluent (D) is not particularly limited, but is preferably less than 2.0, more preferably 1.6 or less, particularly preferably 1.4 or less. In order to enhance the dilution effect of the curable composition, it is preferably 1.2 or less.
[0178] The main chain structure of the reactive diluent (D) can be any structure in a straight chain or branched structure, preferably a straight chain. In addition, the hydrolyzable silyl group possessed by the reactive diluent (D) is more preferably present only at one of the two ends of the linear reactive diluent (D). The reactive diluent (D) is preferably a polymer having only one of the above-mentioned hydrolyzable silyl groups in one molecule. In addition, the main chain structure can be a single structure, and each polymer can mix the polymers manufactured separately, or can be manufactured simultaneously in a manner to obtain any polymer.
[0179] The hydrolyzable silyl group of the reactive diluent (D) can be arbitrarily selected, and preferably has the same hydrolyzable silyl group as the polyoxyalkylene polymer (A) and / or (B) because it is easy to adjust the physical properties of the cured product. A methyldimethoxysilyl group is particularly preferred.
[0180] From the viewpoint of obtaining a viscosity reducing effect while ensuring good mechanical properties of the cured product, the amount of the reactive diluent (D) added is preferably from 1 part by weight to 200 parts by weight, more preferably from 10 parts by weight to 100 parts by weight, relative to 100 parts by weight of the mixture of the polyoxyalkylene polymers (A) and (B) of the present invention.
[0181] ((Meth)acrylate polymer (C))
[0182] The curable composition of the present invention preferably further contains a (meth)acrylate polymer (C) having a hydrolyzable silyl group. By further containing a (meth)acrylate polymer (C), there is a tendency for the weather resistance of the cured product to be improved. The position of the hydrolyzable silyl group in the (meth)acrylate polymer (C) may be at the end of the polymer main chain or near the middle of the main chain.
[0183] The (meth)acrylate monomer constituting the main chain of the (meth)acrylate polymer (C) is not particularly limited, and various (meth)acrylate monomers can be used. Specifically, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, phenyl (meth)acrylate, toluyl (meth)acrylate, benzyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, stearyl (meth)acrylate, glycidyl (meth)acrylate, (3-trimethoxysilyl)propyl (meth)acrylate , (meth)acrylic acid monomers such as (3-dimethoxymethylsilyl)propyl (meth)acrylate, (2-trimethoxysilyl)ethyl (meth)acrylate, (2-dimethoxymethylsilyl)ethyl (meth)acrylate, trimethoxysilylmethyl (meth)acrylate, (dimethoxymethylsilyl)methyl (meth)acrylate, ethylene oxide adduct of (meth)acrylic acid, trifluoromethylmethyl (meth)acrylate, 2-trifluoromethylethyl (meth)acrylate, 2-perfluoroethylethyl (meth)acrylate, 2-perfluoroethyl-2-perfluorobutylethyl (meth)acrylate, perfluoroethyl (meth)acrylate, trifluoromethyl (meth)acrylate, bis(trifluoromethyl)methyl (meth)acrylate, 2-trifluoromethyl-2-perfluoroethylethyl (meth)acrylate, 2-perfluorohexylethyl (meth)acrylate, 2-perfluorodecylethyl (meth)acrylate, and 2-perfluorohexadecylethyl (meth)acrylate.
[0184] Examples of monomer units other than those mentioned above include acrylic acid such as acrylic acid and methacrylic acid; amide groups such as N-hydroxymethyl acrylamide and N-hydroxymethyl methacrylamide; monomers containing epoxy groups such as glycidyl acrylate and glycidyl methacrylate; and monomers containing nitrogen groups such as diethylaminoethyl acrylate and diethylaminoethyl methacrylate.
[0185] As the (meth)acrylate polymer (C), a polymer obtained by copolymerizing a (meth)acrylate monomer and a vinyl monomer copolymerizable therewith can be used. The vinyl monomer is not particularly limited, and examples thereof include: styrene monomers such as styrene, vinyltoluene, α-methylstyrene, chlorostyrene, styrenesulfonic acid and its salts; fluorine-containing vinyl monomers such as perfluoroethylene, perfluoropropylene, and vinylidene fluoride; silicon-containing vinyl monomers such as vinyltrimethoxysilane and vinyltriethoxysilane; maleic anhydride, maleic acid, monoalkyl esters and dialkyl esters of maleic acid; fumaric acid, monoalkyl esters and dialkyl esters of fumaric acid; maleimide, methylmaleimide, ethylmaleimide, propylmaleimide, butylmaleimide, hexylmaleimide, Maleimide monomers such as octylmaleimide, dodecylmaleimide, stearylmaleimide, phenylmaleimide, and cyclohexylmaleimide; cyano group-containing vinyl monomers such as acrylonitrile and methacrylonitrile; amide group-containing vinyl monomers such as acrylamide and methacrylamide; vinyl ester monomers such as vinyl acetate, vinyl propionate, vinyl pivalate, vinyl benzoate, and vinyl cinnamate; alkenyl monomers such as ethylene and propylene; conjugated diene monomers such as butadiene and isobutylene; vinyl chloride, vinylidene chloride, allyl chloride, allyl alcohol, etc., and multiple of them can also be used as copolymer components.
[0186] The number of hydrolyzable silyl groups per molecule of the (meth)acrylate polymer (C) is preferably 0.5 to 5.0, more preferably 1.0 or more from the viewpoint of mechanical properties of the curable composition during curing, and more preferably 3.0 or less from the viewpoint of stability of the (meth)acrylate polymer (C).
[0187] The method for introducing a hydrolyzable silyl group into a (meth)acrylate polymer is not particularly limited, and for example, the following method can be used.
[0188] (iv) A method of copolymerizing a compound having a polymerizable unsaturated group and a hydrolyzable silyl group with the above-mentioned monomers. According to this method, the hydrolyzable silyl group tends to be randomly introduced into the main chain of the polymer.
[0189] (v) A method of polymerizing a (meth)acrylate polymer using a mercaptosilane compound having a hydrolyzable silyl group as a chain transfer agent. According to this method, a hydrolyzable silyl group can be introduced into a polymer terminal.
[0190] (vi) A method of copolymerizing a compound having a polymerizable unsaturated group and a reactive functional group (V group) and then reacting a compound having a hydrolyzable silyl group and a functional group reactive with the V group. Specifically, a method of copolymerizing 2-hydroxyethyl acrylate and then reacting an isocyanate silane having the hydroxyl group and a hydrolyzable silyl group; a method of copolymerizing a glycidyl acrylate and then reacting an aminosilane compound having an epoxy group and a hydrolyzable silyl group.
[0191] (vii) A method of introducing a hydrolyzable silyl group by modifying the terminal functional group of a (meth)acrylate polymer synthesized by a living radical polymerization method. A (meth)acrylate polymer obtained by a living radical polymerization method can easily introduce a functional group to the polymer terminal, and by modifying the (meth)acrylate polymer, a hydrolyzable silyl group can be introduced to the polymer terminal.
[0192] As silicon compounds that can be used to introduce a hydrolyzable silyl group into a (meth)acrylate polymer by the above method, the following compounds can be exemplified. As compounds having a polymerizable unsaturated group and a hydrolyzable silyl group used in method (iv), 3-(trimethoxysilyl)propyl (meth)acrylate, 3-(dimethoxymethylsilyl)propyl (meth)acrylate, 3-(triethoxysilyl)propyl (meth)acrylate, (trimethoxysilyl)methyl (meth)acrylate, (dimethoxymethylsilyl)methyl (meth)acrylate, (triethoxysilyl)methyl (meth)acrylate, (diethoxymethylsilyl)methyl (meth)acrylate, 3-((methoxymethyl)dimethoxysilyl)propyl (meth)acrylate, etc. can be cited. From the viewpoint of availability, 3-trimethoxysilylpropyl (meth)acrylate and 3-(dimethoxymethylsilyl)propyl (meth)acrylate are particularly preferred.
[0193] Examples of the mercaptosilane compound having a hydrolyzable silyl group used in method (v) include 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyldimethoxymethylsilane, 3-mercaptopropyltriethoxysilane, mercaptomethyltrimethoxysilane, (mercaptomethyl)dimethoxymethylsilane, and mercaptomethyltriethoxysilane.
[0194] Examples of the compound having a hydrolyzable silyl group and a functional group reactive with the V group used in the method (vi) include isocyanate silane compounds such as 3-isocyanate propyl trimethoxysilane, 3-isocyanate propyl dimethoxymethyl silane, 3-isocyanate propyl triethoxysilane, isocyanate methyl trimethoxysilane, isocyanate methyl triethoxysilane, isocyanate methyl dimethoxymethyl silane, and isocyanate methyl diethoxymethyl silane; 3-glycidoxypropyl trimethoxysilane, 3-glycidoxypropyl triethoxysilane, 3-glycidoxypropyl dimethoxymethyl silane, glycidoxymethyl trimethoxysilane, and glycidoxymethyl Epoxysilane compounds such as triethoxysilane, glycidoxymethyldimethoxymethylsilane, and glycidoxymethyldiethoxymethylsilane; aminosilane compounds such as 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyldimethoxymethylsilane, aminomethyltrimethoxysilane, aminomethyltriethoxysilane, aminomethyldimethoxymethylsilane, N-cyclohexylaminomethyltriethoxysilane, N-cyclohexylaminomethyldiethoxymethylsilane, N-phenylaminomethyltrimethoxysilane, N-(2-aminoethyl)aminomethyltrimethoxysilane, and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane.
[0195] In the above method (vii), any modification reaction can be utilized, for example, the following methods can be utilized: a method of using a compound having a functional group capable of reacting with a terminal reactive group obtained by polymerization and a hydrolyzable silyl group; a method of introducing a double bond into the polymer terminal by using a compound having a functional group capable of reacting with a terminal reactive group and a double bond, and introducing a hydrolyzable silyl group thereto by hydrosilylation, etc.
[0196] It should be noted that these methods may be used in any combination. For example, when the method (vi) and the method (v) are combined, a (meth)acrylate polymer having a hydrolyzable silyl group at both the molecular chain terminal and / or the side chain can be obtained.
[0197] The hydrolyzable silyl group contained in the (meth)acrylate polymer (C) can be represented by the following general formula (8), similar to the hydrolyzable silyl group contained in the polyoxyalkylene polymer (A) and / or (B):
[0198] -(Si(R 1 2-b )(Y′ b )O) m S i 2 3-a Y a (8).
[0199] About R1 , R 2 , Y, Y', a, b, m are the same as those in general formula (1). When m is 0, the general formula (8) is represented by the following general formula (9):
[0200] -SiR 2 3-a Y a (9).
[0201] In the general formula (9), a represents 1, 2 or 3. Specifically, the hydrolyzable silyl group possessed by the (meth)acrylate polymer (C) is preferably a methyldimethoxysilyl group, a methyldiethoxysilyl group, a trimethoxysilyl group, or a triethoxysilyl group. In addition, from the viewpoint of achieving both storage stability and curability of the curable composition containing the (meth)acrylate polymer (C), a methyldimethoxysilyl group is more preferred, and from the viewpoint of being able to improve the recovery of the cured product of the composition, a trimethoxysilyl group is more preferred.
[0202] For those skilled in the art, the monomer composition of the (meth)acrylate polymer (C) can be generally selected according to the application and purpose, but in applications requiring flexibility such as sealing materials, the glass transition temperature (Tg) is preferably relatively low, preferably having a Tg of -100°C or higher and 100°C or lower, and more preferably having a Tg of -60°C or higher and 0°C or lower. It should be noted that Tg is obtained by the following Fox formula.
[0203] Fox formula: 1 / (Tg(K))=Σ(Mi / Tgi)
[0204] (where Mi represents the weight fraction of the monomer i component constituting the polymer, and Tgi represents the glass transition temperature (K) of the homopolymer of monomer i.)
[0205] The number average molecular weight of the (meth)acrylate polymer (C) is not particularly limited, but the polystyrene equivalent molecular weight measured by GPC is preferably 500 to 100,000, more preferably 1,500 to 50,000, and particularly preferably 5,000 to 30,000.
[0206] A method of mixing a polyoxyalkylene polymer with a (meth)acrylate polymer is proposed in Japanese Patent Publication No. 59-122541, Japanese Patent Publication No. 63-112642, Japanese Patent Publication No. 6-172631, Japanese Patent Publication No. 11-116763, etc. In addition, a method of polymerizing a (meth)acrylate monomer in the presence of a polyoxypropylene polymer having a hydrolyzable silyl group can also be used. The manufacturing method is specifically disclosed in Japanese Patent Publication No. 59-78223, Japanese Patent Publication No. 60-228516, Japanese Patent Publication No. 60-228517, etc. The mixture of the polyoxyalkylene polymer (A) and (B) of the present invention can also be mixed by the same method as the (meth)acrylate polymer (C), but is not limited thereto.
[0207] The ratio of the mixture of the polyoxyalkylene polymers (A) and (B) to the (meth)acrylate polymer (C) of the present invention is not particularly limited, but is preferably 95:5 to 10:90, more preferably 90:10 to 20:80, and particularly preferably 80:20 to 40:60 by weight. It should be noted that the mixture of the polyoxyalkylene polymers (A) and (B) and the (meth)acrylate polymer (C) of the present invention may be used alone or in combination of two or more.
[0208] (Other additives)
[0209] Silicon compounds, tackifiers, plasticizers, solvents, diluents, silicates, fillers, anti-dripping agents, antioxidants, light stabilizers, ultraviolet light absorbers, physical property adjusters, tackifying resins, compounds containing epoxy groups, photocurable substances, oxygen-curable substances, surface improvers, epoxy resins, other resins, flame retardants, and foaming agents can be added to the curable composition of the present invention as other additives. In addition, for the purpose of adjusting the various physical properties of the curable composition or the cured product, various additives can also be added to the curable composition of the present invention as required. As examples of such additives, for example, curing adjusters, free radical inhibitors, metal deactivators, ozone degradation inhibitors, phosphorus peroxide decomposers, lubricants, pigments, mildew inhibitors, etc. can be cited.
[0210] <Filling agent>
[0211] Various fillers can be incorporated into the composition of the present invention. As fillers, heavy calcium carbonate, colloidal calcium carbonate, magnesium carbonate, diatomaceous earth, clay, talc, titanium oxide, fumed silica, precipitated silica, crystalline silica, fused silica, silicic anhydride, hydrous silicic acid, carbon black, iron oxide, aluminum powder, zinc oxide, active zinc flower, PVC powder, PMMA powder, glass fiber and filaments, etc. The above-mentioned fillers can be used alone or in combination of two or more.
[0212] The amount of the filler used is preferably 1 to 300 parts by weight, more preferably 10 to 250 parts by weight, based on 100 parts by weight of the mixture of the polyoxyalkylene polymers (A) and (B) of the present invention.
[0213] For the purpose of lightening the composition (lowering specific gravity), organic hollow spheres and inorganic hollow spheres may be added. The hollow spheres are spherical fillers, the interior of which is hollow. The materials of the hollow spheres include inorganic materials such as glass, white sand, and silica, and organic materials such as phenolic resin, urea-formaldehyde resin, polystyrene, and saran. The above-mentioned hollow spheres may be used alone or in combination of two or more.
[0214] The amount of the hollow spheres used is preferably 0.1 to 100 parts by weight, more preferably 1 to 20 parts by weight, based on 100 parts by weight of the mixture of the polyoxyalkylene polymers (A) and (B) of the present invention.
[0215] <Thickener>
[0216] A tackifier may be added to the composition of the present invention. As the tackifier, a silane coupling agent or a reaction product of a silane coupling agent may be added.
[0217] Specific examples of the silane coupling agent include amino-containing silanes such as γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldimethoxysilane, N-β-aminoethyl-γ-aminopropyltrimethoxysilane, N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, and (2-aminoethyl)aminomethyltrimethoxysilane; γ-isocyanatepropyltrimethoxysilane, γ-isocyanatepropyltrimethoxysilane, and the like. Ethoxysilane, γ-isocyanate propyl methyl dimethoxysilane, α-isocyanate methyl trimethoxysilane, α-isocyanate methyl dimethoxymethyl silane and other isocyanate group-containing silanes; γ-mercaptopropyl trimethoxysilane, γ-mercaptopropyl triethoxysilane, γ-mercaptopropyl methyl dimethoxysilane and other mercapto group-containing silanes; γ-glycidoxypropyl trimethoxysilane, β-(3,4-epoxycyclohexyl)ethyl trimethoxysilane and other epoxy group-containing silanes. In addition, various reactants of silane coupling agents can also be used. The above-mentioned thickeners can be used alone or in combination of two or more.
[0218] The amount of the tackifier used is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the mixture of the polyoxyalkylene polymers (A) and (B) of the present invention.
[0219] <Plasticizer>
[0220] A plasticizer may be added to the composition of the present invention. Specific examples of the plasticizer include phthalate compounds such as dibutyl phthalate, diisononyl phthalate (DINP), diheptyl phthalate, di(2-ethylhexyl) phthalate, diisodecyl phthalate (DIDP), and butyl benzyl phthalate; terephthalate compounds such as bis(2-ethylhexyl)-1,4-benzenedicarboxylate; and non-phthalate compounds such as diisononyl 1,2-cyclohexanedicarboxylate. compounds; aliphatic polycarboxylic acid ester compounds such as dioctyl adipate, dioctyl sebacate, dibutyl sebacate, diisodecyl succinate, and acetyl tributyl citrate; unsaturated fatty acid ester compounds such as butyl oleate and acetyl ricinoleic acid methyl ester; alkyl phenyl sulfonate; phosphate compounds; trimellitate compounds; chlorinated paraffin; hydrocarbon oils such as alkyl biphenyl and partially hydrogenated terphenyl; process oil; epoxidized soybean oil, epoxy stearate benzyl and other epoxy plasticizers, etc.
[0221] In addition, a polymer plasticizer may be used. Specific examples of polymer plasticizers include vinyl polymers; polyester plasticizers; polyether polyols such as polyethylene glycol and polypropylene glycol having a number average molecular weight of 500 or more, and polyether derivatives such as derivatives obtained by converting the hydroxyl groups of these polyether polyols into ester groups, ether groups, etc.; polystyrenes; polybutadiene, polybutylene, polyisobutylene, butadiene-acrylonitrile, polychloroprene, etc.
[0222] The amount of the plasticizer used is preferably 5 to 150 parts by weight, more preferably 10 to 120 parts by weight, and even more preferably 20 to 100 parts by weight, based on 100 parts by weight of the mixture of the polyoxyalkylene polymers (A) and (B) of the present invention. The plasticizer may be used alone or in combination of two or more.
[0223] <Solvents and diluents>
[0224] A solvent or a diluent may be added to the composition of the present invention. The solvent and the diluent are not particularly limited, and aliphatic hydrocarbons, aromatic hydrocarbons, alicyclic hydrocarbons, halogenated hydrocarbons, alcohols, esters, ketones, ethers, etc. may be used. When a solvent or a diluent is used, the boiling point of the solvent is preferably 150° C. or more, more preferably 200° C. or more, and further preferably 250° C. or more, due to the problem of air pollution when the composition is used indoors. The above-mentioned solvents or diluents may be used alone or in combination of two or more.
[0225] <Anti-sagging agent>
[0226] If necessary, in order to prevent sagging and improve workability, an anti-sagging agent may be added to the composition of the present invention. In addition, the anti-sagging agent is not particularly limited, and examples thereof include: polyamide waxes; hydrogenated castor oil derivatives; metal soaps such as calcium stearate, aluminum stearate, and barium stearate. These anti-sagging agents may be used alone or in combination of two or more.
[0227] The amount of the anti-sagging agent used is preferably 0.1 to 20 parts by weight based on 100 parts by weight of the mixture of the polyoxyalkylene polymers (A) and (B) of the present invention.
[0228] <Antioxidants>
[0229] An antioxidant (anti-aging agent) may be used in the composition of the present invention. If an antioxidant is used, the weather resistance of the cured product can be improved. Examples of antioxidants include hindered phenols, monophenols, bisphenols, and polyphenols. Specific examples of antioxidants are also described in Japanese Patent Application Publication No. 4-283259 and Japanese Patent Application Publication No. 9-194731.
[0230] The amount of the antioxidant used is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, based on 100 parts by weight of the mixture of the polyoxyalkylene polymers (A) and (B) of the present invention.
[0231] <Light stabilizer>
[0232] A light stabilizer may be used in the composition of the present invention. If a light stabilizer is used, photo-oxidative degradation of the cured product can be prevented. Examples of the light stabilizer include benzotriazoles, hindered amines, and benzoate compounds, and hindered amines are particularly preferred.
[0233] The amount of the light stabilizer used is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, based on 100 parts by weight of the mixture of the polyoxyalkylene polymers (A) and (B) of the present invention.
[0234] <Ultraviolet light absorber>
[0235] An ultraviolet light absorber can be used in the composition of the present invention. If an ultraviolet light absorber is used, the surface weather resistance of the cured product can be improved. Examples of ultraviolet light absorbers include benzophenones, benzotriazoles, salicylates, substituted tolyls, and metal chelate compounds, among which benzotriazoles are particularly preferred, and commercially available products include Tinuvin P, Tinuvin 213, Tinuvin 234, Tinuvin 326, Tinuvin 327, Tinuvin 328, Tinuvin 329, and Tinuvin 571 (all manufactured by BASF).
[0236] The amount of the ultraviolet absorber used is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, based on 100 parts by weight of the mixture of the polyoxyalkylene polymers (A) and (B) of the present invention.
[0237] <Physical property adjuster>
[0238] As needed, a physical property adjuster for adjusting the tensile properties of the generated cured product can be added to the curable composition of the present invention. As a physical property adjuster, there is no particular limitation, for example, alkyl alkoxy silanes such as phenoxytrimethylsilane, methyltrimethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, and n-propyltrimethoxysilane; aryl alkoxy silanes such as diphenyldimethoxysilane and phenyltrimethoxysilane; alkyl isopropenoxy silanes such as dimethyldiisopropenoxysilane, methyltriisopropenoxysilane, and γ-glycidoxypropylmethyldiisopropenoxysilane; trialkylsilyl borate such as tris(trimethylsilyl)borate and tris(triethylsilyl)borate; silicone varnish; polysiloxanes, etc. By using the above-mentioned physical property adjuster, the hardness of the composition of the present invention can be increased when it is cured, or conversely, the hardness can be reduced and the elongation at break can be increased. The above-mentioned physical property adjusters can be used alone or in combination of two or more.
[0239] In particular, the compound having a univalent silanol group in the molecule generated by hydrolysis has the effect of not causing the viscosity of the cured product surface to deteriorate and reducing the modulus of the cured product. Particularly preferably, the compound generating trimethylsilanol. As the compound having a univalent silanol group in the molecule generated by hydrolysis, the derivatives of alcohols such as hexanol, octanol, phenol, trimethylolpropane, glycerine, pentaerythritol, sorbitol, etc., and the silicon compound that can generate silane monoalcohol by hydrolysis can be cited.
[0240] The amount of the property adjuster used is preferably 0.1 to 10 parts by weight, more preferably 0.5 to 5 parts by weight, based on 100 parts by weight of the mixture of the polyoxyalkylene polymers (A) and (B) of the present invention.
[0241] <Tackifying resin>
[0242] In the present invention, a tackifier resin is added for the purpose of improving the adhesiveness and adhesion to the substrate or according to other needs. As the tackifier resin, a commonly used tackifier resin can be used without particular limitation.
[0243] As specific examples, terpene resins, aromatic modified terpene resins, hydrogenated terpene resins, terpene-phenolic resins, phenolic resins, modified phenolic resins, xylene-phenolic resins, cyclopentadiene-phenolic resins, coumarone-indene resins, rosin resins, rosin ester resins, hydrogenated rosin ester resins, xylene resins, low molecular weight polystyrene resins, styrene copolymer resins, styrene block copolymers and hydrides thereof, petroleum resins (e.g., C5 hydrocarbon resins, C9 hydrocarbon resins, C5C9 hydrocarbon copolymer resins, etc.), hydrogenated petroleum resins, DCPD resins, etc. can be enumerated. These resins can be used alone or in combination of two or more.
[0244] The amount of the tackifier resin used is preferably 2 to 100 parts by weight, more preferably 5 to 50 parts by weight, and even more preferably 5 to 30 parts by weight, based on 100 parts by weight of the mixture of the polyoxyalkylene polymers (A) and (B) of the present invention.
[0245] <Compounds containing epoxy groups>
[0246] An epoxy group-containing compound can be used in the composition of the present invention. If an epoxy group-containing compound is used, the recovery of the cured product can be improved. Examples of epoxy group-containing compounds include epoxidized unsaturated oils and fats, epoxidized unsaturated fatty acid esters, alicyclic epoxy compounds, compounds represented by epichlorohydrin derivatives, and mixtures thereof. Specifically, epoxidized soybean oil, epoxidized linseed oil, bis(2-ethylhexyl)-4,5-epoxycyclohexane-1,2-dicarboxylate (E-PS), octyl epoxystearate, butyl epoxystearate, and the like can be cited. The epoxy compound can be used in the range of 0.5 to 50 parts by weight relative to 100 parts by weight of the mixture of the polyoxyalkylene polymers (A) and (B) of the present invention.
[0247] <Photocurable substances>
[0248] Photocurable substances can be used in the composition of the present invention. If photocurable substances are used, a film of the photocurable substance can be formed on the surface of the cured product, which can improve the stickiness and weather resistance of the cured product. Among such compounds, many substances such as organic monomers, oligomers, resins or compositions containing these compounds are known. As representative compounds, monomers having one or more acrylic or methacrylic unsaturated groups, unsaturated acrylic compounds as oligomers or mixtures thereof, polyvinyl cinnamate or azidized resins can be used.
[0249] The photocurable substance is preferably used in an amount of 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, based on 100 parts by weight of the mixture of the polyoxyalkylene polymers (A) and (B) of the present invention.
[0250] <Oxygen-curable substances>
[0251] Oxygen-curing substances can be used in the composition of the present invention. Examples of oxygen-curing substances include unsaturated compounds that react with oxygen in the air, which react with oxygen in the air to form a cured film near the surface of the cured product, thereby preventing the surface from becoming sticky and dirt and dust from adhering to the surface of the cured product. Specific examples of oxygen-curing substances include drying oils represented by tung oil, linseed oil, and the like, various alkyd resins obtained by modifying the compounds; acrylic polymers, epoxy resins, and silicone resins modified by drying oils; liquid polymers such as 1,2-polybutadiene, 1,4-polybutadiene, and polymers of C5 to C8 dienes obtained by polymerizing or copolymerizing diene compounds such as butadiene, chloroprene, isoprene, and 1,3-pentadiene. They can be used alone or in combination of two or more.
[0252] The amount of the oxygen-curable substance used is preferably in the range of 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, relative to 100 parts by weight of the mixture of the polyoxyalkylene polymers (A) and (B) of the present invention. As described in Japanese Patent Application Laid-Open No. 3-160053, the oxygen-curable substance is preferably used in combination with a photocurable substance.
[0253] <Epoxy resin>
[0254] An epoxy resin may be used in combination with the composition of the present invention. The composition to which the epoxy resin is added is particularly preferably used as an adhesive, especially an adhesive for exterior wall tiles. Examples of the epoxy resin include bisphenol A type epoxy resins and novolac type epoxy resins.
[0255] The usage ratio of these epoxy resins and the mixture of the polyoxyalkylene polymers (A) and (B) of the present invention is preferably in the range of mixture of polyoxyalkylene polymers (A) and (B) / epoxy resin=100 / 1 to 1 / 100 in terms of weight ratio.
[0256] When an epoxy resin is added, a curing agent for curing the epoxy resin may be used in combination with the composition of the present invention. As the epoxy resin curing agent that can be used, generally used epoxy resin curing agents may be used without particular limitation.
[0257] When using a curing agent for epoxy resin, the amount used is preferably in the range of 0.1 to 300 parts by weight based on 100 parts by weight of the epoxy resin.
[0258] <<Preparation of curable composition>>
[0259] The curable composition of the present invention can be prepared in the form of a one-component type in which all the ingredients are pre-blended and sealed and cured by moisture in the air after construction, or in the form of a two-component type in which a silanol condensation catalyst, a filler, a plasticizer, water and other ingredients are pre-blended as a curing agent and the blended materials are mixed with the organic polymer composition before use. From the perspective of operability, the one-component type is preferred.
[0260] In the case where the curable composition is a one-component type, since all the ingredients are prepared in advance, it is preferred that the ingredients containing water are dehydrated and dried in advance before use, or dehydrated by reduced pressure during mixing. In addition, in addition to the dehydration and drying method, the storage stability is further improved by adding alkoxysilane compounds such as n-propyltrimethoxysilane, vinyltrimethoxysilane, vinylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, γ-mercaptopropylmethyldiethoxysilane, and γ-glycidoxypropyltrimethoxysilane.
[0261] The amount of the dehydrating agent, especially the silicon compound capable of reacting with water such as vinyltrimethoxysilane, is preferably used in the range of 0.1 to 20 parts by weight, more preferably in the range of 0.5 to 10 parts by weight, relative to 100 parts by weight of the mixture of the polyoxyalkylene polymers (A) and (B) of the present invention.
[0262] <Application>
[0263] The curable composition of the present invention can be used as an adhesive, a sealing material for buildings / ships / cars / roads, etc., an adhesive, a waterproof material, a coating waterproof material, a mold-forming agent, a shockproof material, a shock-absorbing material, a sound-insulating material, a foaming material, a coating, and a spray material. The cured product obtained by curing the curable composition of the present invention can be suitably used as a sealing material or an adhesive because it has excellent flexibility and adhesiveness.
[0264] In addition, the curable composition of the present invention can be used for electrical / electronic component materials such as solar cell back sealing materials, electrical / electronic components such as wire / cable insulation coating materials, electrical insulating materials for devices, acoustic insulating materials, elastic adhesives, adhesives, contact adhesives, spray-type sealing materials, crack repair materials, adhesives for tile bonding, adhesives for asphalt waterproofing materials, powder coatings, injection molding materials, medical rubber materials, medical adhesives, medical adhesive sheets, medical device sealing materials, dental impression materials, food packaging materials, adhesive boards and other external materials. The present invention can be used in various applications such as sealing materials for joints of packaging materials, coating materials, anti-skid coating materials, cushioning materials, primers, conductive materials for electromagnetic wave shielding, thermal conductive materials, hot melt materials, potting agents for electrical and electronic products, films, gaskets, concrete reinforcing materials, adhesives for temporary bonding, various molding materials, and rust-proofing / waterproofing sealing materials for the end faces (cut portions) of mesh glass and laminated glass, automobile parts, large vehicle parts such as trucks and buses, train vehicle parts, aircraft parts, ship parts, motor parts, various mechanical parts, etc. Liquid sealants. Taking automobiles as an example, it can be used for various applications such as bonding and mounting of plastic covers, decorative objects, rims, shock absorbers, window installations, interior components, exterior components, etc. In addition, it can be closely attached to a wide range of substrates such as glass, porcelain, wood, metal, and resin moldings, either alone or with the help of a primer, and therefore can also be used as various types of sealing compositions and adhesive compositions. In addition, the curable composition of the present invention can also be used as an adhesive for interior panels, an adhesive for exterior panels, an adhesive for pasting tiles, an adhesive for pasting stones, an adhesive for ceiling processing, an adhesive for floor processing, an adhesive for wall processing, an adhesive for vehicle panels, an adhesive for electrical / electronic / precision equipment assembly, an adhesive for bonding leather, fiber products, cloth, paper, board and rubber, a reactive post-crosslinking pressure-sensitive adhesive, a sealant for window frame installation (direct glazing), a sealant for multi-layer glass, a sealant for SSG process, or a sealant for construction joints of buildings, civil engineering, and bridge materials. In addition, it can also be used as an adhesive material such as an adhesive tape and an adhesive sheet.
[0265] Example
[0266] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.
[0267] The "terminal components" mentioned below refer to polyoxypropylene having reactive silyl groups and / or reactive silyl groups (hydroxyl groups, allyl groups, etc.) that can be introduced into both ends of the linear polyoxypropylene. The "terminal components" have two of the above terminal structures in one polymer molecule.
[0268] The "single-terminal component" refers to a polyoxypropylene having a reactive silyl group and / or a group into which a reactive silyl group can be introduced only at one of the two terminals of a linear polyoxypropylene, and having no group into which a reactive silyl group and a group into which a reactive silyl group can be introduced at the other terminal. The "single-terminal component" has one of the above terminal structures in one molecule of the polymer.
[0269] The components at both terminals belong to the polyoxyalkylene polymer (A) of the first embodiment and the second embodiment, and the component at one terminal belongs to the polyoxyalkylene polymer (B) of the first embodiment and the second embodiment.
[0270] (Synthesis example 1)
[0271] A mixture of polyoxypropylene glycol and n-butanol having a number average molecular weight of about 4500 was used as an initiator, and propylene oxide was polymerized by a zinc hexacyanocobaltate glyme complex catalyst until the molecular weight reached the following value, thereby obtaining a hydroxyl-terminated polyoxypropylene mixture (E-1) having a number average molecular weight of about 17000, which contained both terminal components and one terminal component. The weight ratio of both terminal components / one terminal component in the polyoxypropylene mixture (E-1) was about 7 / 3.
[0272] (Synthesis Examples 2 to 10)
[0273] As shown in Table 1, hydroxyl-terminated polyoxypropylene or hydroxyl-terminated polyoxypropylene mixtures (E-2) to (E-10) were obtained by the same method as in Synthesis Example 1 using polyoxypropylene glycol and / or n-butanol having a number average molecular weight of about 4500 as initiators.
[0274]
[0275] (Example 1)
[0276] 1.0 equivalent of a methanol solution of sodium methoxide was added to the hydroxyl group of the above-mentioned hydroxyl-terminated polyoxypropylene mixture (E-1), and the methanol was distilled off at 140°C. Next, 2.0 equivalents of allyl glycidyl ether were added at 140°C, reacted for 2 hours, unsaturated bonds were introduced, and 1.5 equivalents of 3-chloro-1-propylene (allyl chloride) were further added to convert the terminal hydroxyl group into an allyl group. After removing impurities such as residual metal salts, 50 ppm of a divinyldisiloxane platinum complex (3% by mass isopropanol solution in terms of platinum) and 2.1 parts by weight of methyldimethoxysilane were added to 100 parts by weight of the obtained allyl-terminated polyoxypropylene mixture, and reacted at 90°C for 2 hours, thereby obtaining a polyoxypropylene mixture (AB-1) having a methyldimethoxysilyl group at the terminal and containing both terminal components and a single terminal component and having a number average molecular weight of 17,000.
[0277] In the polyoxypropylene mixture (AB-1), the total number of hydrolyzable silyl groups, terminal olefin groups and internal olefin groups per terminal structure (hereinafter referred to as the total number of groups per terminal structure) was 3.0, the ratio of the number of moles of hydrolyzable silyl groups to the total number of moles of hydrolyzable silyl groups, terminal olefin groups and internal olefin groups (hereinafter referred to as the hydrolyzable silyl group introduction rate) was 55%, the number of hydrolyzable silyl groups per terminal structure was 1.7, and the viscosity at 23° C. was 11 Pa·s. The weight ratio of the two-terminal components / one-terminal component in the polyoxypropylene mixture (AB-1) was about 7 / 3. This polyoxypropylene mixture (AB-1) was used in Example 21.
[0278] It should be noted that the polyoxypropylene mixture (AB-1) contains both a polyoxyalkylene polymer (A) as a dual-terminal component having two terminal structures in one molecule, and a polyoxyalkylene polymer (B) as a single-terminal component having one terminal structure in one molecule. Each polymer may be referred to as (A-1) and (B-1), respectively, but since they are produced simultaneously, for convenience, the mixture of the two polymers is referred to as (AB-1).
[0279] In addition, since the polyoxyalkylene polymers (A) and (B) contained in the polyoxypropylene mixture (AB-1) are simultaneously terminal-modified, it is considered that the total number of groups per terminal structure and the hydrolyzable silyl group introduction rate in each polymer are respectively the same as the total number of groups per terminal structure and the hydrolyzable silyl group introduction rate in the entire mixture.
[0280] The above also applies to each mixture (AB-2 to 9, AB-11 to 14) shown below.
[0281] (Examples 2 to 4, 6 to 10, Comparative Examples 1 to 4, Synthesis Examples 11 to 20)
[0282] Using the hydroxyl-terminated polymers (E) shown in Tables 2-1 and 2-2, and according to the amounts of the raw materials shown in Table 2, polyoxypropylene or a mixture thereof having a methyldimethoxysilyl group at the end (AB-1 to 9, AB-11 to 14, A-31 to 37, B-21 to 22, D-1) was obtained by the same method as in Example 1.
[0283]
[0284]
[0285] (Synthesis Example 21)
[0286] 52.1 parts by weight of isobutyl alcohol was added to a four-necked flask equipped with a stirrer, and the temperature was raised to 90° C. in a nitrogen atmosphere. A mixed solution obtained by dissolving 14.5 parts by weight of methyl methacrylate, 68.2 parts by weight of butyl acrylate, 14.9 parts by weight of stearyl methacrylate, 2.4 parts by weight of 3-(dimethoxymethylsilyl)propyl methacrylate, and 0.3 parts by weight of 2,2'-bis(2-methylbutyronitrile) in 12.4 parts by weight of isobutyl alcohol was added dropwise thereto over 7 hours. Polymerization was further performed at 90° C. for 2 hours to obtain an isobutyl alcohol solution (solid content 60% by weight) of a (meth)acrylate polymer (C-1) having an average of 1.8 methyldimethoxysilyl groups per molecule, a number average molecular weight of 17,000, and a weight average molecular weight of 48,000.
[0287] (Example 5)
[0288] 70 parts by weight of the polymer mixture (AB-1) obtained in Example 1 and 50 parts by weight of the isobutyl alcohol solution of the polymer (C-1) obtained in Synthesis Example 21 were mixed, and the isobutyl alcohol was distilled off under reduced pressure to obtain a polymer mixture having a weight ratio of polymer (AB-1) / polymer (C-1) of 70 / 30 and a viscosity of 25 Pa.sD at 23° C. The obtained polymer mixture was used in Example 25.
[0289] (Comparative Example 5)
[0290] 70 parts by weight of the polymer mixture (A-31) obtained in Synthesis Example 11 and 50 parts by weight of the isobutyl alcohol solution of the polymer (C-1) obtained in Synthesis Example 21 were mixed, and the isobutyl alcohol was distilled off under reduced pressure to obtain a polymer mixture having a weight ratio of polymer (A-31) / polymer (C-1) of 70 / 30 and a viscosity of 34 Pa.s at 23° C. The obtained polymer mixture was used in Comparative Example 25.
[0291] (Example 11)
[0292] 70 parts by weight of the polyoxyalkylene polymer (A-35) obtained in Synthesis Example 15 and 30 parts by weight of the polyoxyalkylene polymer (B-21) obtained in Synthesis Example 19 were mixed well to obtain a polyoxyalkylene mixture.
[0293] The polyoxypropylene mixture had a total number of 2.6 groups per terminal structure, a hydrolyzable silyl group introduction rate of 64%, an average number of 1.7 hydrolyzable silyl groups per terminal structure, and a viscosity of 9 Pa·s at 23° C. In Example 31, the polyoxypropylene mixture was used.
[0294] (Examples 12 to 13, Comparative Examples 11 to 13)
[0295] Using each polymer (A) and each polymer (B) or (D) shown in Table 3 and each raw material amount shown in Table 3, a polyoxypropylene mixture having a methyldimethoxysilyl group at the terminal was obtained in the same manner as in Example 11.
[0296] [Table 3]
[0297] (Examples 21 to 33 and Comparative Examples 21 to 33)
[0298] The following evaluations were performed using each polymer mixture or each polymer produced in each of the above-mentioned Examples, Comparative Examples, or Synthesis Examples.
[0299] <Method for measuring stress at 100% elongation of each polymer mixture or cured product of each polymer>
[0300] The stress at 100% elongation of each polymer mixture or a cured product of each polymer is measured by the above-mentioned measurement method.
[0301] <Evaluation method of composition properties>
[0302] After each polymer mixture or each polymer, the filler, titanium oxide, anti-sagging agent, light stabilizer, and ultraviolet absorber among the various additives shown below were fully mixed, the mixture was dispersed through three paint rollers three times to prepare a main agent. Then, a dehydrating agent, a tackifier, and a silanol condensation catalyst were added and fully mixed, and the mixture was uniformly kneaded and degassed using a rotation and revolution mixer to prepare each curable composition. Using each of the prepared curable compositions, various test bodies were prepared in a constant temperature and humidity atmosphere of 23°C and a relative humidity of 50%, and various evaluations were performed.
[0303] (Various Additives Used in Examples and Comparative Examples Related to Evaluation of Composition Properties)
[0304] The following additives were used in the evaluation of the physical properties of the compositions of Examples 21 to 33 and Comparative Examples 21 to 33. The amounts added are parts by weight relative to 100 parts by weight of each polymer mixture or each polymer as a base polymer.
[0305] Reactive diluent (D): Reactive diluent (D-1) prepared in Synthesis Example 18, 76 parts by weight
[0306] Fillers:
[0307] (i) Fatty acid treated precipitated calcium carbonate (HAKUENKA CCR, manufactured by Shiraishi Industries, Ltd.), 120 parts by weight
[0308] (ii) Heavy calcium carbonate (Whiten SB red, manufactured by Shiraishi Calcium Co., Ltd.), 40 parts by weight
[0309] Titanium oxide: TIPAQUE R-820, manufactured by Ishihara Sangyo Co., Ltd., 10 parts by weight
[0310] Anti-sagging agent: fatty acid amide wax (Disparon #6500, Kusumoto Chemicals Co., Ltd.), 2 parts by weight
[0311] Light stabilizer: bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate (Tinuvin 770, manufactured by BASF), 1 part by weight
[0312] Ultraviolet absorber: 2-(5-chloro-2H-benzotriazol-2-yl)-4-methyl-6-tert-butylphenol (Tinuvin 326, manufactured by BASF), 1 part by weight
[0313] Dehydrating agent: vinyltrimethoxysilane (A-171, manufactured by Momentive Corporation), 2 parts by weight
[0314] Thickener: 3-(N-2-aminoethylamino)propyltrimethoxysilane (A-1120, manufactured by Momentive Corporation), 3 parts by weight
[0315] Silanol condensation catalyst: dioctyltin dilaurate (U-810, manufactured by Nitto Kasei Co., Ltd.), 2 parts by weight
[0316] (Dumbbell properties)
[0317] At 23°C and 50% relative humidity, the curable composition was filled into a 3mm thick sheet mold frame. After curing for 3 days at 23°C and 50% relative humidity, it was aged in a 50°C dryer for 4 days to obtain a sheet-like cured product. The obtained cured product was punched into a No. 3 dumbbell shape according to JIS K6251 to obtain a test piece. Using the obtained test piece, a tensile test (tensile speed 200mm / min) was performed using Autograph at 23°C and 50% relative humidity, and the stress at 100% elongation, the stress at break, and the elongation at break were measured.
[0318] (Resilience)
[0319] The above-mentioned sheet-like solidified material was punched into a dumbbell shape No. 7 to obtain a dumbbell test piece. Two marking lines were drawn at intervals of 10 mm with the contracted portion of the dumbbell test piece as the center. The dumbbell test piece was stretched so that the interval between the marking lines was 20 mm, and fixed in this state and placed in a dryer at 50°C. After 24 hours, the fixing was released, and the interval between the marking lines after 24 hours was measured under the conditions of 23°C and relative humidity of 50%, thereby calculating the recovery rate.
[0320] The results obtained by the above operations are shown in Tables 4 to 8.
[0321]
[0322] From the results shown in Table 4, it can be seen that the cured products of the compositions of each Example comprising a mixture of polyoxyalkylene polymers (A) and (B) satisfying the requirements of the present invention exhibited equivalent or higher viscosity, had equivalent total number of groups per terminal structure, and exhibited higher recovery than the cured products of the compositions of each Comparative Example not satisfying the requirements of the present invention even when exhibiting equivalent stress during elongation, since the polyoxyalkylene polymer (B) was not contained. In addition, no significant difference was observed in dumbbell physical properties.
[0323] Furthermore, it can be seen from Example 25 that even if a (meth)acrylate polymer (C) having a hydrolyzable silyl group is further contained, the same effect is exhibited.
[0324] [Table 5-1]
[0325]
[0326] (*1) Not broken before elongation reaches 100%
[0327] [Table 5-2]
[0328]
[0329] From the results shown in Tables 5-1 and 5-2, it can be seen that the cured products of the compositions of each embodiment comprising a mixture of polyoxyalkylene polymers (A) and (B) satisfying the requirements of the present invention have a better balance between flexibility and recovery properties than the cured products of the compositions of each comparative example whose hydrolyzable silyl group introduction rate does not satisfy the requirements of the present invention even if they have the same main chain structure and the same total number of groups per terminal structure.
[0330] [Table 6]
[0331]
[0332] From the results shown in Table 6, it can be seen that the cured product of the composition of Example 28, which comprises a mixture of polyoxyalkylene polymers (A) and (B) that meet the requirements of the present invention, has the same main chain structure and shows significantly superior recovery properties compared to the cured product of the composition of Comparative Example 29 in which the total number of groups per terminal structure does not meet the requirements of the present invention even when showing the same stress during elongation.
[0333] [Table 7]
[0334]
[0335] (*2) Not broken before elongation to 100%
[0336] The mixture of Examples 31 and 32 shown in Table 7 is a mixture of polyoxyalkylene polymers (A) and (B) prepared by respectively preparing polymers (A) and (B) that meet the requirements of the present invention and then mixing them. It can be seen that the cured products of the compositions of Examples 31 and 32 contain the same polymer (A), but since they do not contain polymer (B), compared with the cured product of the composition of Comparative Example 30 that does not meet the requirements of the present invention, the flexibility is significantly improved while maintaining the resilience to a certain extent. In addition, it can be seen that the cured products of the compositions of Examples 31 and 32 are excellent in the balance between flexibility and resilience compared with the cured products of the compositions of the comparative examples that do not meet the requirements of the present invention in terms of the hydrolyzable silyl group introduction rate (Comparative Examples 31 and 32) and the total number of groups per terminal structure of the polymer (B) (Comparative Example 31).
[0337] In addition, Example 21 is shown again for reference. Example 21 uses a polymer (AB-1) that meets the requirements of the present invention and has the same viscosity, total number of groups per terminal structure, hydrolyzable silyl group introduction rate, and number of hydrolyzable silyl groups per terminal structure as the polymer (A-35) used in Comparative Example 30. It can be seen that although the recovery property of Example 21 is slightly reduced compared with Comparative Example 30, the stress during elongation of the cured product is greatly reduced, the elongation is also improved, and the flexibility is greatly improved.
[0338] [Table 8]
[0339]
[0340] From the results shown in Table 8, it can be seen that the cured product of the composition of Example 33 comprising a mixture of polyoxyalkylene polymers (A) and (B) that meet the requirements of the present invention is excellent in the balance between flexibility and resilience, even if it is a mixture of polyoxyalkylene polymers having the same main chain structure, compared with the cured product of the composition of Comparative Example 33 in which the total number of groups per terminal structure of the polymer (B) and the introduction rate of hydrolyzable silyl groups do not meet the requirements of the present invention.
[0341] Based on the above results, it can be seen that for the mixture of polyoxyalkylene polymers (A) and (B) of the present invention, the cured product of the curable composition containing the mixture shows a low modulus but high resilience, and other various physical properties are also equivalent to those of existing products. Therefore, it can be appropriately used as a low-viscosity base polymer for a highly resilient sealing material that is not prone to leakage.
Claims
1. A mixture comprising a polyoxyalkylene polymer (A) and a polyoxyalkylene polymer (B), wherein each of the polyoxyalkylene polymers (A) and (B) has a main chain structure of polyoxyalkylene and a terminal structure bonded to a terminal of the main chain structure, The terminal structure has a hydrolyzable silyl group and a terminal olefin group and / or an internal olefin group, The number of the terminal structures per molecule of the polyoxyalkylene polymer (A) is 1.5 or more, The number of the terminal structures per molecule of the polyoxyalkylene polymer (B) is 1.2 or less, In each of the polyoxyalkylene polymers (A) and (B), the total number of the hydrolyzable silyl group, the terminal olefin group and the internal olefin group in the terminal structure is more than 1.0 per terminal structure, In the entire mixture, the ratio of the number of moles of the hydrolyzable silyl group to the total number of moles of the hydrolyzable silyl group, the terminal olefin group and the internal olefin group is 40 to 75%.
2. The mixture according to claim 1, wherein The polyoxyalkylene polymer (A) has two or more terminal structures in one molecule, and the polyoxyalkylene polymer (B) has one terminal structure in one molecule.
3. A mixture comprising a polyoxyalkylene polymer (A) and a polyoxyalkylene polymer (B), wherein each of the polyoxyalkylene polymers (A) and (B) has a main chain structure of polyoxyalkylene and a terminal structure bonded to a terminal of the main chain structure, The terminal structure has a hydrolyzable silyl group and a terminal olefin group and / or an internal olefin group, The polyoxyalkylene polymer (A) has two or more terminal structures in one molecule. The polyoxyalkylene polymer (B) has one terminal structure in one molecule. In each of the polyoxyalkylene polymers (A) and (B), the total number of the hydrolyzable silyl group, the terminal olefin group and the internal olefin group in the terminal structure is more than 1.0 per terminal structure, In the entire mixture, the ratio of the number of moles of the hydrolyzable silyl group to the total number of moles of the hydrolyzable silyl group, the terminal olefin group and the internal olefin group is 40 to 75%.
4. The mixture according to claim 3, wherein The polyoxyalkylene polymer (A) has two terminal structures in one molecule.
5. The mixture according to any one of claims 1 to 4, wherein The cured product of the mixture has a stress at 100% elongation of 0.30 MPa or less.
6. The mixture according to any one of claims 1 to 4, wherein In the entire mixture, the ratio of the number of moles of the hydrolyzable silyl group to the total number of moles of the hydrolyzable silyl group, the terminal olefin group and the internal olefin group is 40 to 70%.
7. The mixture according to any one of claims 1 to 4, wherein The terminal structure includes a site derived from an epoxy compound having a terminal olefin group.
8. The mixture according to any one of claims 1 to 4, wherein In each of the polyoxyalkylene polymers (A) and (B), the total number of the hydrolyzable silyl group, the terminal olefin group, and the internal olefin group in the terminal structure is more than 2.0 per terminal structure.
9. The mixture according to any one of claims 1 to 4, wherein The hydrolyzable silyl group is represented by the general formula (3): -SiR 2 Y2(3) In the formula, R 2 represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms, or a triorganosiloxy group represented by (R′)3SiO-, R′ represents the same or different substituted or unsubstituted monovalent hydrocarbon groups having 1 to 20 carbon atoms, and Y represents the same or different hydroxyl groups or hydrolyzable groups.
10. The mixture according to any one of claims 1 to 4, wherein In the entire mixture, the number of the hydrolyzable silyl groups is 1.0 or more per terminal structure. 11 . A curable composition comprising the mixture according to claim 1 .
12. The curable composition according to claim 11, further comprising a reactive diluent (D), wherein the reactive diluent (D) is a polymer having an average of 0.5 or more and less than 1.2 hydrolyzable silyl groups per molecule and having a viscosity at 23°C lower than that of the mixture. 13 . The curable composition according to claim 11 , further comprising a (meth)acrylate polymer (C) having a hydrolyzable silyl group. 14 . A cured product, which is a cured product of the curable composition according to claim 11 .
15. A method for producing a mixture according to any one of claims 1, 2, 5 to 10, comprising: A step of forming the main chain structure of the polyoxyalkylene by polymerizing a mixture of an initiator having an average of 1.5 or more hydroxyl groups per molecule and an initiator having an average of 1.2 or less hydroxyl groups per molecule with an epoxy compound; and A step of forming the terminal structure at the terminal of the main chain structure.
16. The manufacturing method according to claim 15, wherein: The initiator having an average of 1.5 or more hydroxyl groups in one molecule has two or more hydroxyl groups in one molecule, and the initiator having an average of 1.2 or less hydroxyl groups in one molecule has one hydroxyl group in one molecule.
17. A method for producing a mixture according to any one of claims 3 to 10, comprising: A step of forming the main chain structure of the polyoxyalkylene by polymerizing a mixture of an initiator having two or more hydroxyl groups in one molecule and an initiator having one hydroxyl group in one molecule with an epoxy compound; and A step of forming the terminal structure at the terminal of the main chain structure.