Copper-aluminum particle powder containing coating layer, preparation method and application thereof
By forming a dense protective film of copper-aluminum paste on the surface of copper-aluminum particle powder, the bypass problem between conductors caused by silver ion migration in the heterojunction battery is solved, reducing costs and improving stability in high temperature and high humidity environments. , achieving low resistance and high reliability.
Patent Information
- Application Number
- CN202210916203.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-01
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-08-01
AI Technical Summary
In traditional silver paste, during the power generation process of heterojunction cells, the migration of silver ions causes bypass paths between conductors, causing insulation degradation and even short circuits, and the cost is high.
Using copper-aluminum particle powder containing a coating layer, a dense protective film is formed on the surface of the copper-aluminum particle powder, and copper-aluminum paste is used instead of silver paste to reduce line resistance and improve stability against high-temperature and high-humidity environments.
The copper-aluminum paste has low contact resistance and low line resistance, and the cost is only 1/10 of that of silver paste. The resistance change rate is ≤8% at 85°C and 85% RH, and the long-term reliability is good.
Smart Images

Figure SMS_2 
Figure SMS_4 
Figure SMS_5
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of solar cell metallization, and in particular to a copper-aluminum particle powder containing a coating layer, a preparation method and an application thereof. Background Art
[0002] HJT (Heterojunction with Intrinsic Thin Layer) batteries use low-temperature silver paste on both sides. The consumption of silver paste is huge and the price is expensive, which is one of the reasons for the high cost of HJT. According to CPIA, the consumption of low-temperature silver paste on both sides of HJT batteries in 2020 was about 223.3 mg / piece, a year-on-year decrease of 25.6%. Although the consumption of silver paste is still large, it has been greatly improved in 2020 compared with 2019. At present, various technical reforms are being used to reduce the consumption of low-temperature silver paste to reduce the production cost of HJT batteries. It is expected that by 2030, the consumption of HJT low-temperature silver paste will drop to 135 mg / piece, a decrease of 39.5% from 2020. Silicon wafers are the core material of HJT batteries and account for about 45% of the cost structure of HJT. Excluding the cost of silicon wafers, among non-silicon materials, silver paste, as a core auxiliary material, accounts for about 59%. The quality of heterojunction electrodes affects the transmission of holes and electrons, which has a great impact on the conversion efficiency of batteries. On this basis, heterojunction low-temperature curing slurry has become a key material.
[0003] Using base metals to replace silver can greatly reduce the electrode cost in non-silicon materials to 7-8%, and the cost per watt can be reduced by 0.15 yuan, which is basically the same as the PERC cost.
[0004] Among the existing metals, copper has the closest conductivity to silver. The advantages and disadvantages of copper electroplating technology are very obvious. The biggest advantage is that copper replaces part or all of the silver metal. The material cost is low, and double-sided metallization can be completed at the same time. The disadvantage is that the process is longer than the traditional screen printing process, requiring more equipment and labor costs, and copper is easily oxidized at high temperatures, and its chemical properties are difficult to control. There are many harmful chemicals in the electroplating solution, which are difficult to handle and lead to high environmental protection costs.
[0005] In addition, when traditional silver paste is used in heterojunction batteries, in a high humidity environment, water molecules penetrate deeply into the surface of the silver conductor and electrolyze to form hydrogen ions and hydroxide ions. Under the action of the electric field and hydroxide ions, silver dissociates to produce silver ions. The migration of silver ions will cause a bypass between conductors without electrical connections, resulting in reduced insulation and even short circuits. In severe cases, it may cause component fires. In addition, the cost of silver is 5,000+ yuan / kg, which is relatively high. Summary of the invention
[0006] In order to solve the problems in the prior art that the migration of silver ions in the power generation process of heterojunction batteries used for traditional silver paste causes bypass formation between conductors without electrical connections, resulting in reduced insulation and even short circuit, as well as high silver costs, the present application provides a copper-aluminum particle powder containing a coating layer, a preparation method and an application thereof. The copper-aluminum particle powder containing a coating layer is used in copper-aluminum paste, has low contact resistance, low line resistance, and is resistant to high temperature and high humidity environments, with a resistance attenuation rate of ≤8%, good long-term reliability, and a cost of 1 / 10 of that of silver paste.
[0007] The specific technical solutions of this application are as follows:
[0008] 1. A copper-aluminum particle powder containing a coating layer, wherein the internal region of the particles of the copper-aluminum particle powder containing a coating layer is a copper-aluminum particle, the surface layer is a coating layer, and the coating layer contains a coating agent and a corrosion inhibitor.
[0009] 2. The copper-aluminum particle powder containing a coating layer according to item 1, wherein the particles of the copper-aluminum particle powder containing a coating layer sequentially comprise copper-aluminum particles, a corrosion inhibitor and a coating agent from the inside to the outside.
[0010] 3. The copper-aluminum particle powder containing a coating layer according to item 1 or 2, wherein the specific surface area of the particles of the copper-aluminum particle powder containing a coating layer is 0.7-1.8 m 2 / g, preferably, the tap density is ≥3.2g / ml.
[0011] 4. The copper-aluminum particle powder containing a coating layer according to any one of items 1 to 3, wherein the average particle size D of the particles of the copper-aluminum particle powder containing a coating layer is 50 1.2-1.8μm;
[0012] Preferably, the average particle size D of the copper-aluminum particle powder containing the coating layer is 10 0.5-0.8μm;
[0013] Preferably, the average particle size D of the copper-aluminum particle powder containing the coating layer is 90 3.4-4.2μm;
[0014] Preferably, the average particle size D of the copper-aluminum particle powder containing the coating layer is 97 ≤10μm.
[0015] 5. The copper-aluminum particle powder containing a coating layer according to any one of items 1 to 4, wherein the coating agent is stearic acid, oleic acid and / or lauric acid.
[0016] 6. The copper-aluminum particle powder containing a coating layer according to any one of items 1 to 5, wherein the corrosion inhibitor is La(NO3)3, NdCl3 and / or Ce(NO3)3.
[0017] 7. The copper-aluminum particle powder containing a coating layer according to any one of items 1 to 6, wherein the coating layer has a thickness of 3-5 nm.
[0018] 8. A method for preparing a copper-aluminum particle powder containing a coating layer, comprising:
[0019] Ball-milling and filtering the copper-aluminum particle powder to obtain a slurry containing the copper-aluminum particle powder;
[0020] The slurry containing copper-aluminum particle powder is mixed with a solution containing a coating agent and a corrosion inhibitor, and then dried to obtain copper-aluminum particle powder containing a coating layer.
[0021] 9. The method according to item 8, wherein the copper-aluminum particle powder is ball-milled in the presence of a low-boiling point organic solvent and zirconium balls, and preferably, the mass ratio of the copper-aluminum particle powder, the low-boiling point organic solvent and the zirconium balls is 0.9-1.2: 0.7-1.0:2.3-2.7.
[0022] 10. The method according to claim 9, wherein the low boiling point organic solvent is petroleum ether, ethanol, n-butanol, isobutanol, ethyl acetate and / or tetrahydrofuran.
[0023] 11. The method according to any one of items 8 to 10, wherein, in terms of mass percentage in the copper-aluminum particle powder, copper accounts for 65-80% and aluminum accounts for 20-35%.
[0024] 12. The method according to any one of items 8 to 11, wherein the specific surface area of the particles in the copper-aluminum particle powder is 0.8-1.5 m 2 / g, tap density ≥3.2g / ml, the average particle size D 50 0.9-1.5μm.
[0025] 13. The method according to any one of items 8 to 12, wherein the mass ratio of the slurry containing the copper and aluminum particle powder to the solution containing the coating agent and the corrosion inhibitor is 1:0.5-1.2.
[0026] 14. The method according to any one of items 8 to 13, wherein the coating agent is stearic acid, oleic acid and / or lauric acid;
[0027] Preferably, the corrosion inhibitor is La(NO3)3, NdCl3 and / or Ce(NO3)3.
[0028] 15. The method according to any one of items 8 to 14, wherein the solution containing the coating agent and the corrosion inhibitor is an aqueous solution containing the coating agent, the corrosion inhibitor and a low-boiling point organic solvent; preferably, the mass ratio of the coating agent, the low-boiling point organic solvent, the corrosion inhibitor and water is 0.01-0.2:0.3-0.8:0.01-0.8:1.
[0029] 16. A copper-aluminum paste, comprising the copper-aluminum particle powder containing a coating layer as described in any one of items 1 to 7 or the copper-aluminum particle powder containing a coating layer prepared by the method described in any one of items 8 to 15.
[0030] 17. The copper-aluminum paste according to item 16, wherein the copper-aluminum paste further comprises epoxy resin, reactive diluent, surfactant, epoxy accelerator, curing agent, silicone oil, thixotropic agent and solvent;
[0031] Preferably, in parts by weight, the copper-aluminum particle powder containing the coating layer is 80-88 parts, the epoxy resin is 2-5 parts, the reactive diluent is 2-6 parts, the surfactant is 0.1-1 parts, the epoxy accelerator is 0.2-3 parts, the curing agent is 0.3-4 parts, the silicone oil is 0.2-1 parts, the thixotropic agent is 0.3-2 parts, and the solvent is 0.5-5 parts.
[0032] 18. The copper-aluminum paste according to item 17, wherein the epoxy resin is selected from one or more of bisphenol A, bisphenol F, hydrogenated bisphenol A and polyurethane-modified epoxy resin;
[0033] Preferably, the reactive diluent is selected from two or three of n-butyl glycidyl ether, glycidyl methacrylate and polypropylene glycol glycidyl ether;
[0034] Preferably, the surfactant is selected from one or more of BYK204, BYK110, TEGO Wet270 and TEGO Dispers 740W;
[0035] Preferably, the epoxy accelerator is selected from one or more of 1-aminoethyl-2-methylimidazole, triethanolamine, dimethylbenzylamine and DMP-30;
[0036] Preferably, the curing agent is N,N-dimethylaniline, dicyandiamide and / or blocked isocyanate;
[0037] Preferably, the silicone oil is PMX200-50CS, PMX200-500CS and / or PMX200-1000CS;
[0038] Preferably, the thixotropic agent is selected from one or more of THIXATROL PLUS, BYK 410, THIXCIN R and ST;
[0039] Preferably, the solvent is butyl carbitol acetate, butyl carbitol and / or terpineol.
[0040] 19. An electrode comprising the copper-aluminum paste according to any one of items 16 to 18.
[0041] 20. A battery comprising the electrode according to item 19.
[0042] Effects of the Invention
[0043] The copper-aluminum particle powder containing a coating layer described in the present application forms a dense protective film on the surface of the copper-aluminum particle powder. The copper-aluminum paste formed using the copper-aluminum particle powder containing a coating layer has a resistance change rate of ≤8% at 85° C. and 85% rh (relative humidity).
[0044] The copper-aluminum paste formed by using the copper-aluminum particle powder containing a coating layer as described in the present application has low contact resistance, low line resistance, and low cost, which is only 1 / 10 of that of silver paste.
[0045] 1. The corrosion inhibitors used in this application are La(NO3)3, NdCl3 and / or Ce(NO3)3, which inhibit corrosion by forming a layer of metal oxides and hydroxides on the surface of copper and aluminum particle powders. Since the cathode reaction of metal corrosion is an oxygen reduction reaction, the pH value of the cathode area increases, and rare earth metal ions are deposited in the cathode area in the form of hydroxides or oxides, hindering the corrosion reaction.
[0046] 2. The conductive powder used in the present invention is copper-aluminum particle powder. In the air, the activity of aluminum is greater than that of copper powder, and the oxidation process of aluminum powder can form dense aluminum oxide, which hinders further corrosion reaction.
[0047] 3. The coating agent used in the present invention is mainly lauric acid and stearic acid, which mainly wraps the surface of the copper powder to prevent the copper powder from agglomerating during the vacuum drying process, so that the copper-aluminum particle powder containing the coating layer is prepared into a slurry with good dispersibility. At the same time, the coating can isolate oxygen and prevent the copper powder from contacting with the air, further preventing the copper powder from oxidation.
[0048] 4. The epoxy resin used in the present invention is bisphenol A, bisphenol F, hydrogenated bisphenol A, and polyurethane modified epoxy resin. After curing, it can form a good and dense film with the copper and aluminum particle powder containing the coating layer to protect the copper and aluminum particle powder containing the coating layer from corrosion, because it has weather resistance, solvent resistance, and good film-forming performance. The working principle is: the resin contains a large number of FC bonds with a bond energy of 485KJ / mol. Under the action of heat, light, etc., the FC bonds are difficult to break, forming a good protective film. DETAILED DESCRIPTION
[0049] In the prior art, silver-coated copper powder is used to replace silver powder in the preparation of heterojunction batteries to reduce costs. However, since the coverage rate of silver-coated copper powder is 70-80%, the silver-coated copper powder is coated by surface modification to prevent oxidation during the curing process. Generally, the coating agent is an oil-soluble substance that can be dissolved in the organic solvent in the slurry, resulting in coating failure and unstable curing resistance under air. In addition, since the silver content of silver-coated copper powder is generally 20-50%, silver ion migration cannot be avoided in essence, and because the silver content in silver-coated copper is high and the manufacturing process is complicated, the cost reduction is not as large as that of pure base metals. In view of this, the present application provides a copper-aluminum particle powder containing a coating layer, wherein the particles of the copper-aluminum particle powder containing a coating layer are copper-aluminum particles inside, and the surface layer is a coating layer, and the coating layer contains a coating agent and a corrosion inhibitor.
[0050] The particles in the copper-aluminum particle powder containing a coating layer described in the present application form a dense protective film on the surface of the copper-aluminum particles, which can inhibit corrosion.
[0051] In addition, the present application uses copper-aluminum particle powder as the conductive powder. Since the copper-aluminum alloy particle powder is in the air, the activity of aluminum is greater than that of copper, and the aluminum oxidation process can form dense aluminum oxide, which hinders further corrosion reactions.
[0052] The present application uses a coating agent and a corrosion inhibitor as a coating layer, and the coating agent is wrapped on the surface of the copper-aluminum particles to prevent the copper-aluminum particle powder from agglomerating during the vacuum drying process, so that the copper-aluminum slurry prepared from the copper-aluminum particle powder containing the coating layer has good dispersibility. At the same time, the coating layer can isolate oxygen, prevent the copper-aluminum particle powder containing the coating layer from contacting with the air, and further prevent the copper-aluminum particle powder from being oxidized. In addition, since the cathode reaction of metal corrosion is an oxygen reduction reaction, which leads to an increase in the pH value of the cathode area, the rare earth metal ions in the slow-release agent are deposited in the cathode part in the form of hydroxides or oxides, which can hinder the progress of the corrosion reaction.
[0053] In some embodiments, the particles of the copper-aluminum particle powder containing a coating layer sequentially comprise copper-aluminum particles, a corrosion inhibitor, and a coating agent from the inside to the outside.
[0054] In some embodiments, the specific surface area of the copper-aluminum particle powder containing the coating layer is 0.7-1.8 m 2 / g, preferably, the tap density is ≥3.2g / ml, preferably 3.2-7g / ml.
[0055] For example, the specific surface area of the copper-aluminum particle powder containing the coating layer can be 0.7 m 2 / g, 0.8m 2 / g, 0.9m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.3m 2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.7m 2 / g, 1.8m 2 / g, etc.
[0056] The tap density can be 3.2 g / ml, 4 g / ml, 5 g / ml, 6 g / ml, 7 g / ml, etc.
[0057] In the present application, the specific surface area of the particles of the copper-aluminum particle powder containing a coating layer can be determined by conventional methods in the art. For example, the specific surface area of the particles of the copper-aluminum particle powder containing a coating layer can be determined by a specific surface area tester commonly used in the art.
[0058] In the present application, the tap density can be measured by conventional methods in the art, for example, the tap density of the copper-aluminum particle powder containing the coating layer can be measured by a tap density meter commonly used in the art.
[0059] In some embodiments, the average particle size D of the copper-aluminum particle powder containing the coating layer is 50 1.2-1.8μm;
[0060] Preferably, the average particle size D of the copper-aluminum particle powder containing the coating layer is 10 0.5-0.8μm;
[0061] Preferably, the average particle size D of the copper-aluminum particle powder containing the coating layer is 90 3.4-4.2μm;
[0062] Preferably, the average particle size D of the copper-aluminum particle powder containing the coating layer is 97 ≤10μm, preferably 4.2-10μm.
[0063] For example, the average particle size D of the copper-aluminum particle powder containing the coating layer is 50 It can be 1.2μm, 1.3μm, 1.4μm, 1.5μm, 1.6μm, 1.7μm, 1.8μm, etc.
[0064] The average particle size D of the copper-aluminum particle powder containing the coating layer is 10 It can be 0.5μm, 0.6μm, 0.7μm, 0.8μm, etc.
[0065] The average particle size D of the copper-aluminum particle powder containing the coating layer is 90 It can be 3.4μm, 3.5μm, 3.6μm, 3.7μm, 3.8μm, 3.9μm, 4.0μm, 4.1μm, 4.2μm, etc.;
[0066] The average particle size D of the copper-aluminum particle powder containing the coating layer is 90 It can be 10μm, 9μm, 8μm, 7μm, 6μm, 5μm, 4μm, etc.
[0067] In this application, the average particle size D 10 Refers to the particle size of 10% of the particles in the copper-aluminum particle powder containing the coating layer;
[0068] Similarly, the average particle size D 50 , D 90 and D 97 The average particle size D of the particles of the copper-aluminum particle powder containing the coating layer refers to the particle size of 50% of the particles, the particle size of 90% of the particles, and the particle size of 97% of the particles, respectively. For example, in the present application, the average particle size D of the particles of the copper-aluminum particle powder containing the coating layer is 50 The particle size of 50% of the particles in the copper-aluminum particle powder containing the coating layer is 1.2-1.8 μm.
[0069] In the present application, there is no limitation on the method for determining the average particle size, which can be determined by conventional methods in the art. For example, a conventional laser particle size analyzer in the art can be used to test the average particle size of the copper-aluminum particle powder containing a coating layer.
[0070] In some embodiments, the coating agent is stearic acid, oleic acid and / or lauric acid.
[0071] The present application uses a coating agent to coat the particles in the copper-aluminum particle powder, which can prevent the copper powder in the copper-aluminum particle powder from agglomerating during the vacuum drying process, so that the copper-aluminum slurry prepared from the copper-aluminum particle powder containing the coating layer has good dispersibility. By using the coating agent, oxygen can be isolated, and the copper powder in the copper-aluminum particle powder can be prevented from contacting with the air, thereby further preventing the copper powder in the copper-aluminum particle powder from oxidizing.
[0072] In some embodiments, the corrosion inhibitor is La(NO3)3, NdCl3 and / or Ce(NO3)3
[0073] The present application coats the surface of the copper-aluminum particle powder with a corrosion inhibitor, and can inhibit corrosion by forming a layer of metal oxide and hydroxide on the surface of the copper-aluminum particle powder.
[0074] In some embodiments, the coating layer has a thickness of 3-5 nm.
[0075] For example, the thickness of the coating layer may be 3 nm, 4 nm, 5 nm, etc.
[0076] In some embodiments, the inner region of the copper-aluminum particle powder containing a coating layer is a copper-aluminum particle, and the surface layer is a coating layer, and the coating layer contains a coating agent and a corrosion inhibitor. In some embodiments, the particles of the copper-aluminum particle powder containing a coating layer contain copper-aluminum particles, a corrosion inhibitor, and a coating agent in order from the inside to the outside. In some embodiments, the specific surface area of the particles of the copper-aluminum particle powder containing a coating layer is 0.7-1.8 m 2 / g, preferably, the tap density is ≥3.2g / ml. In some embodiments, the average particle size D of the copper-aluminum particle powder containing the coating layer is 50 Preferably, the average particle size D of the copper-aluminum particle powder containing the coating layer is 10 Preferably, the average particle size D of the copper-aluminum particle powder containing the coating layer is 90 Preferably, the average particle size D of the copper-aluminum particle powder containing the coating layer is 97 ≤10μm. In some embodiments, the coating agent is stearic acid, oleic acid and / or lauric acid. In some embodiments, the corrosion inhibitor is La(NO3)3, NdCl3 and / or Ce(NO3)3. In some embodiments, the thickness of the coating layer is 3-5nm.
[0077] The copper-aluminum particle powder containing a coating layer described in the present application has a coating layer formed on its surface, which can prevent the copper powder of the copper-aluminum particle powder from contacting with the air and preventing the oxidation of the copper powder. The obtained copper-aluminum particle powder containing a coating layer is used in copper-aluminum slurry, has low contact resistance, low line resistance, and is resistant to high temperature and high humidity environments. The resistance attenuation rate is ≤8% and has good long-term reliability.
[0078] The present application provides a method for preparing a copper-aluminum particle powder containing a coating layer, which comprises:
[0079] Ball-milling and filtering the copper-aluminum particle powder to obtain a slurry containing the copper-aluminum particle powder;
[0080] The slurry containing copper-aluminum particle powder is mixed with a solvent containing a coating agent and a corrosion inhibitor, and then dried to obtain copper-aluminum particle powder containing a coating layer.
[0081] In some embodiments, the copper-aluminum particle powder is ball-milled in the presence of a low-boiling point organic solvent and zirconium balls. Preferably, the mass ratio of the copper-aluminum particle powder, the low-boiling point organic solvent and the zirconium balls is 0.9-1.2:0.7-1.0:2.3-2.7, preferably 1:0.8:2.5. In some embodiments, a ball milling aid is added for ball milling. Preferably, the amount of the ball milling aid added is 0.01-1% of the total amount of the copper-aluminum particle powder, the low-boiling point solvent and the zirconium balls. For example, the amount of the ball milling aid added can be 0.01%, 0.05%, 0.1%, 0.5%, 0.1% and the like of the total amount of the copper-aluminum particle powder, the low-boiling point solvent and the zirconium balls; preferably, the ball milling aid is ethylene glycol, propylene glycol and / or polyacrylic acid.
[0082] In some embodiments, the copper-aluminum particle powder is placed in a ball mill in the presence of a low boiling point organic solvent and zirconium balls for ball milling.
[0083] In the present application, there is no limitation on the ball milling device, which can be conventionally selected as needed. For example, the ball milling can be performed in a ball mill commonly used in the art, preferably in a horizontal ball mill.
[0084] Preferably, the ball milling speed is 15-35 rpm / min;
[0085] Preferably, the ball milling time is 6-8 h.
[0086] In some embodiments, the low boiling point solvent is petroleum ether, ethanol and / or n-butanol; preferably, the low boiling point solvent is added during the ball milling process to disperse the copper and aluminum particle powder so that the copper and aluminum particle powder can be fully ball milled.
[0087] In some embodiments, ball-milling and filtering the copper-aluminum particle powder to obtain a slurry containing the copper-aluminum particle powder also includes centrifugally stirring the filtrate obtained after filtration using a low-boiling point solvent, and then filtering to obtain a slurry containing the copper-aluminum particle powder; preferably, the low-boiling point solvent is used to wash the ball milling aid to remove the ball milling aid.
[0088] In some embodiments, the rotation speed of the centrifugal stirring is 600-1000 rpm / min, and preferably, the stirring time is 5-20 min. Preferably, the above steps are repeated 3-5 times to make the pH value of the obtained slurry containing copper and aluminum particle powder 5-7.
[0089] In some embodiments, based on the mass percentage of the copper and aluminum particle powder, the copper is 65-80% and the aluminum is 20-35%.
[0090] For example, in terms of mass percentage in the copper-aluminum particle powder, copper can be 65%, 70%, 75%, 80%, etc.;
[0091] Aluminum can be 20%, 25%, 30%, 35%, etc.
[0092] In some embodiments, the copper-aluminum particle powder has a specific surface area of 0.8-1.5 m 2 / g, tap density ≥3.2g / ml, and the average particle size D50 of the copper-aluminum particle powder is 0.9-1.5μm.
[0093] For example, the specific surface area of the copper-aluminum particle powder can be 0.8 m 2 / g, 0.9m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.3m 2 / g, 1.4m 2 / g, 1.5m 2 / g, etc.
[0094] The average particle size D of the copper-aluminum particle powder is 50 The thickness may be 0.9 μm, 1.0 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, or the like.
[0095] In some embodiments, the average particle size D of the copper-aluminum particle powder is 10 0.3-0.5μm;
[0096] Preferably, the average particle size D of the copper-aluminum particle powder is 90 2.5~3.2μm;
[0097] Preferably, the average particle size D of the copper-aluminum particle powder is 97 ≤6μm.
[0098] For example, the average particle size D of the copper-aluminum particle powder is 10 It can be 0.3μm, 0.4μm, 0.5μm, etc.
[0099] The average particle size D of the copper-aluminum particle powder is 90 The thickness may be 2.5 μm, 2.6 μm, 2.7 μm, 2.8 μm, 2.9 μm, 3.0 μm, 3.1 μm, 3.2 μm, or the like.
[0100] In some embodiments, the solvent containing the capping agent and the buffer is an aqueous solution containing the capping agent, a low boiling point solvent and a corrosion inhibitor. Preferably, the mass ratio of the capping agent, the low boiling point organic solvent, the corrosion inhibitor and water is 0.01-0.2:0.3-0.8:0.01-0.8:1.
[0101] For example, the mass ratio (m 包覆剂 :m 低沸点溶剂 :m 缓蚀剂 :m 水 ) can be 0.01:0.3:0.01:1, 0.01:0.5:0.01:1, 0.01:0.8:0.01:1, 0.01:0.3:0.05:1, 0.01:0.3:0.1:1, 0.01:0.3:0.5:1, 0.01:0.3:0.8:1, 0.05:0.3:0.01 :1, 0.05:0.5:0.01:1, 0.05:0.8:0.01:1, 0.05:0.3:0.05:1, 0.05:0.3:0.1:1, 0.05:0.3:0.5:1, 0.05:0.3:0.8:1, 0.1:0.3:0.01:1, 0.1:0.5:0.01:1, 0.1:0.8:0.01:1, 0.1:0.3:0.05:1, 0.1:0.3:0.1:1, 0.1:0.3:0.5:1, 0.1:0.3:0.8:1, 0.2:0.3:0.01:1, 0.2:0.5:0.01:1, 0.2:0.8:0.01:1, 0.2:0.3:0.05:1, 0.2:0.3:0.1:1, 0.2:0.3:0.5:1, 0.2:0.3:0.8:1, etc.
[0102] The aqueous solution containing the coating agent, the low boiling point solvent and the corrosion inhibitor is a solution obtained by adding the coating agent, the low boiling point solvent and the corrosion inhibitor into water and stirring. Preferably, the stirring speed is 300-900 rpm / min, preferably, the stirring time is 10-60 min, and preferably, the stirring is carried out at a temperature of 60-80°C.
[0103] In some embodiments, the coating agent is stearic acid, oleic acid and / or lauric acid;
[0104] Preferably, the corrosion inhibitor is La(NO3)3, NdCl3 and / or Ce(NO3)3.
[0105] In some embodiments, the mass ratio of the slurry containing the copper and aluminum particle powder to the solution containing the coating agent and the corrosion inhibitor is 1:0.5-1.2.
[0106] For example, the mass ratio (m 含有铜铝颗粒粉末的浆料 :m 含有包覆剂和缓蚀剂的溶液 ) can be 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1.0, 1:1.1, 1:1.2, etc.
[0107] In some cases, a slurry containing copper-aluminum particle powder is mixed with a solution containing a coating agent and a corrosion inhibitor, and then dried to obtain copper-aluminum particle powder containing a coating layer, which includes stirring and mixing the slurry containing copper-aluminum particle powder with a solution containing a coating agent and a corrosion inhibitor, and then drying to obtain copper-aluminum particle powder containing a coating layer. Preferably, the stirring speed is 600-1000rpm / min; preferably, the stirring time is 1-3h.
[0108] In some embodiments, the slurry containing copper and aluminum particle powder is stirred and mixed with a solution containing a coating agent and a corrosion inhibitor at a temperature of ≤ 40°C, preferably at 20-40°C.
[0109] In some embodiments, the drying is vacuum drying, preferably drying at 40-80° C. for 9-24 hours to obtain the copper-aluminum particle powder containing the coating layer.
[0110] The present application provides a copper-aluminum paste, which comprises the copper-aluminum particle powder containing a coating layer as described above or the copper-aluminum particle powder containing a coating layer prepared by the method described above.
[0111] In some embodiments, the copper-aluminum paste comprises epoxy resin, reactive diluent, surfactant, epoxy accelerator, curing agent, silicone oil, thixotropic agent and solvent;
[0112] The epoxy resin coated powder is bonded to the ITO substrate and the copper-aluminum particle powder containing the coating layer to provide adhesion;
[0113] The curing agent is used to cause the epoxy resin to undergo condensation, polymerization, addition, catalysis and other reactions to form a network-like three-dimensional polymer.
[0114] The reactive diluent is a low molecular weight epoxy compound containing epoxy groups, which mainly reduces viscosity and increases resin toughness.
[0115] The epoxy accelerator is used to accelerate the curing of epoxy resin at low temperature.
[0116] The silicone oil is used to increase the mesh passing performance of the copper-aluminum paste and prevent false printing and broken grid from occurring during the printing process.
[0117] The thixotropic agent is used to increase the thixotropic property of the copper-aluminum paste, increase the storage time of the copper-aluminum paste, and maintain good linearity under narrow line width.
[0118] The solvent is used to reduce the viscosity of the copper-aluminum paste.
[0119] Preferably, in parts by weight, the copper-aluminum particle powder containing the coating layer is 80-88 parts, the epoxy resin is 2-5 parts, the reactive diluent is 2-6 parts, the surfactant is 0.1-1 parts, the epoxy accelerator is 0.2-3 parts, the curing agent is 0.3-4 parts, the silicone oil is 0.2-1 parts, the thixotropic agent is 0.3-2 parts, and the solvent is 0.5-5 parts.
[0120] For example, in parts by weight, the copper-aluminum particle powder containing the coating layer can be 80 parts, 81 parts, 82 parts, 83 parts, 84 parts, 85 parts, 86 parts, 87 parts, 88 parts, etc.;
[0121] The epoxy resin can be 2 parts, 3 parts, 4 parts, 5 parts, etc.;
[0122] The active diluent may be 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, etc.;
[0123] The surfactant can be 0.1 part, 0.2 part, 0.3 part, 0.4 part, 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part, 1.0 part, etc.;
[0124] The epoxy accelerator can be 0.2 parts, 0.5 parts, 0.8 parts, 1.0 parts, 1.5 parts, 2.0 parts, 2.5 parts, 3.0 parts, etc.;
[0125] The curing agent can be 0.3, 0.5, 0.8, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, etc.;
[0126] The silicone oil can be 0.2 parts, 0.5 parts, 0.8 parts, 1.0 parts, etc.;
[0127] The thixotropic agent may be 0.3, 0.5, 0.8, 1.0, 1.5, 2.0, etc.;
[0128] The solvent may be 0.5 parts, 0.8 parts, 1.0 parts, 1.5 parts, 2.0 parts, 2.5 parts, 3.0 parts, 3.5 parts, 4.0 parts, 4.5 parts, 5.0 parts, etc.
[0129] In some embodiments, the epoxy resin is selected from one or more of bisphenol A, bisphenol F, hydrogenated bisphenol A and polyurethane modified epoxy resin;
[0130] Preferably, the reactive diluent is selected from two or three of n-butyl glycidyl ether, glycidyl methacrylate and polypropylene glycol glycidyl ether;
[0131] Preferably, the surfactant is selected from one or more of BYK204, BYK110, TEGO Wet270 and TEGO Dispers 740W;
[0132] Preferably, the epoxy accelerator is selected from one or more of 1-aminoethyl-2-methylimidazole, triethanolamine, dimethylbenzylamine and 2,4,6-tris(dimethylaminomethyl)phenol (DMP-30);
[0133] Preferably, the curing agent is N,N-dimethylaniline, dicyandiamide and / or blocked isocyanate;
[0134] Preferably, the silicone oil is PMX200-50CS, PMX200-500CS and / or PMX200-1000CS;
[0135] The PMX200-50CS means that the viscosity of PMX-200 is 50CS. Similarly, PMX200-500CS and PMX200-1000CS have the same meaning.
[0136] Preferably, the thixotropic agent is selected from One or more of BYK 410, THIXCIN R and ST;
[0137] Preferably, the solvent is butyl carbitol acetate, butyl carbitol and / or terpineol.
[0138] The epoxy value of the bisphenol A is 0.38-0.54, and the epoxy value refers to the amount of epoxy groups contained in 100g of epoxy resin.
[0139] The epoxy value of the bisphenol F is 0.55-0.625;
[0140] The epoxy value of hydrogenated bisphenol A is 0.42-0.47;
[0141] The epoxy value of polyurethane modified epoxy resin is 0.47-0.56
[0142] The blocked isocyanate refers to an isocyanate whose terminal group is temporarily blocked by reaction, and when used, isocyanate can be released at a certain temperature to play a bonding role.
[0143] The copper-aluminum paste described in the present application contains epoxy resin and copper-aluminum particle powder containing a coating layer. After curing, the epoxy resin forms a good and dense film with the copper-aluminum particle powder containing the coating layer, protecting the copper-aluminum particle powder containing the coating layer from corrosion, and has weather resistance, solvent resistance, and good film-forming properties. Preferably, its mechanism of action is: the epoxy resin contains a large amount of FC bonds with a bond energy of 485KJ / mol. Under the action of heat, light, etc., the FC bonds are difficult to break, thereby forming a good protective film with the copper-aluminum particle powder containing the coating layer.
[0144] In the present application, there is no limitation on the preparation method of the copper-aluminum paste, which can be conventionally selected according to needs, for example, copper-aluminum particle powder containing a coating layer, epoxy resin, active diluent, surfactant, epoxy accelerator, curing agent, silicone oil, thixotropic agent and solvent are mixed, stirred and rolled to obtain the paste.
[0145] In some embodiments, the mixture is first stirred at a rotation speed of 20-40 rpm / min for 20-30 min, and then stirred at a rotation speed of 30-60 rpm / min for 30-80 min. Preferably, vacuum is drawn during stirring to a vacuum degree of ≥-0.6 Mpa.
[0146] In some embodiments, rolling is performed by conventional methods in the art, for example, rolling is performed by the following method:
[0147] Table 1 Parameters of rolling method
[0148] Number of rolls Roller gate clearance Rolling speed (rpm / min) 1 0.1 200 2 0.15 300 3 0.19 400 4 0.45 400 5 0.65 400 6 0.65 400 7 0.3 400
[0149] In some embodiments, the copper-aluminum paste is obtained by measuring the fineness after rolling. Preferably, the fineness of the copper-aluminum paste is ≤6 μm.
[0150] The present application does not impose any limitation on the determination of fineness, and it can be conventionally selected according to needs, for example, a scraper fineness meter can be used for measurement.
[0151] In some embodiments, after rolling, a filtering step is further included to remove foreign matter or bright pieces in the copper-aluminum paste. Preferably, the copper-aluminum paste is obtained by filtering using a 300-mesh sieve.
[0152] Example
[0153] The present application provides a general and / or specific description of the materials and test methods used in the experiments. In the following examples, unless otherwise specified, % means wt%, i.e., weight percentage. The reagents or instruments used without indicating the manufacturer are all conventional reagent products that can be obtained commercially.
[0154] Example 1-1 Preparation of copper-aluminum particle powder containing a coating layer
[0155] (1) Take a copper-aluminum particle powder with a content of 70% copper and 30% aluminum (D10: 0.37 μm, D50: 1.12 μm, D90: 2.98 μm, D97: 5.35 μm, and a specific surface area of 0.91 m 2 / g, tap density: 3.6g / ml): ethanol: zirconium ball ratio of 1:0.8:2.5 was weighed, and then 0.15% of ethylene glycol was added. Put it into a ball milling jar, use a horizontal ball mill with a ball milling speed of 25rpm / min, ball mill for 7h, then remove the floating matter in the slurry, and filter the clear liquid with filter paper.
[0156] (2) removing the floating matter on the surface of the copper-aluminum particle powder slurry prepared in step (2), filtering the clear liquid with filter paper, then adding petroleum ether to the clear liquid at a ratio of 1:1, and then placing it in a centrifuge tube, stirring it with a magnetic stirrer at a speed of 800 rpm / min for 8 minutes, filtering the clear liquid with filter paper, repeating the operation 4 times, and obtaining a slurry containing copper-aluminum particle powder at a pH value of 6.3;
[0157] (3) Mixing stearic acid: ethanol: LaNO3: water in a mass ratio of 0.06: 0.5: 0.3: 1, and using a magnetic stirrer to stir at a speed of 600 rpm / min, the temperature is 70°C, and stirring for 15 minutes to obtain an aqueous solution containing stearic acid, ethanol and LaNO3; then mixing the copper-aluminum particle powder slurry obtained in step (2) and the aqueous solution containing stearic acid, ethanol and LaNO3 in a mass ratio of 1: 1, and using a magnetic stirrer at a speed of 800 rpm / min, stirring for 2 hours, the temperature is 25°C, using filter paper to filter the clear liquid, and then placing it in a vacuum drying oven, drying at 65°C for 14 hours to a dry state to obtain a copper-aluminum particle powder containing a coating layer, wherein the copper-aluminum particle powder containing a coating layer is tested by a laser particle size analyzer with an index of D 10 :0.63μm,D 50 :1.52μm,D 90 :3.83μm,D97 : 6.42μm, the specific surface area measured by the specific surface area tester is 1.2m 2 / g, and the tap density was measured using a tap density meter: 3.5g / ml.
[0158] Example 1-2 Preparation of Copper-Aluminum Particle Powder Containing a Coating Layer
[0159] (1) Take copper-aluminum particle powder with a ratio of 75% copper and 25% aluminum (wherein D10: 0.42 μm, D50: 0.93 μm, D90: 3.07 μm, D97: 4.78 μm, and a specific surface area of 1.15 m 2 / g, tap density: 3.9g / ml): ethanol: zirconium ball ratio of 1:0.8:2.5 was weighed, and then 0.1% of propylene glycol was added. Put it into a ball milling jar, use a horizontal ball mill with a ball milling speed of 17rpm / min, ball mill for 7h, then remove the floating matter in the slurry, and filter the clear liquid with filter paper.
[0160] (2) removing the floating matter on the surface of the copper-aluminum particle powder slurry prepared in step (2), filtering the clear liquid with filter paper, then adding n-butanol to the clear liquid at a ratio of 1:1, and then placing it in a centrifuge tube, stirring for 10 minutes with a magnetic stirrer at a speed of 800 rpm / min, filtering the clear liquid with filter paper, repeating the operation 4 times, and obtaining a slurry containing copper-aluminum particle powder at a pH value of 6.6;
[0161] (3) Mix oleic acid: ethanol: NdCl: water in a mass ratio of 0.1: 0.5: 0.25: 1, and use a magnetic stirrer to stir at a speed of 600 rpm / min, the temperature is 70°C, and stir for 20 minutes to obtain an aqueous solution containing stearic acid, ethanol and LaNO3; then mix the slurry containing copper-aluminum particle powder obtained in step (2) and the aqueous solution containing stearic acid, ethanol and NdCl in a mass ratio of 1: 1, and use a magnetic stirrer at a speed of 800 rpm / min, stir for 2 hours, the temperature is 25°C, filter the clear liquid with filter paper, then put it into a vacuum drying oven, and dry it at 65°C for 12 hours to a dry state to obtain a copper-aluminum particle powder containing a coating layer, and measure it according to the method described in Example 1-1. The index of the copper-aluminum particle powder containing a coating layer is D 10 :0.68μm,D 50 :1.35μm,D 90 :4.24μm,D 97 :5.42μm, specific surface area is 1.35m 2 / g, and the tap density is 3.7g / ml.
[0162] Example 1-3 Preparation of Copper-Aluminum Particle Powder Containing a Coating Layer
[0163] The difference between Example 1-3 and Example 2 is that the mass ratio of the slurry containing copper-aluminum particle powder and the solution containing the coating agent and the corrosion inhibitor is different. The obtained copper-aluminum particle powder containing the coating layer is measured in the same way as in Example 1-1, and its index is D 10 :0.40μm,D 50 :0.89μm,D 90 :2.98μm,D 97 :4.56μm, specific surface area is 1.27m 2 / g, and the tap density is 3.8g / ml.
[0164] Example 1-4 Preparation of Copper-Aluminum Particle Powder Containing a Coating Layer
[0165] The difference between Example 1-4 and Example 2 is that the mass ratio of the slurry containing copper-aluminum particle powder and the solution containing the coating agent and the corrosion inhibitor is different. The obtained copper-aluminum particle powder containing the coating layer is measured in the same way as in Example 1-1, and its index is D 10 :0.38μm,D 50 :0.85μm,D 90 :2.85μm,D 97 :4.32μm, specific surface area is 1.36m 2 / g, and the tap density is 3.5g / ml.
[0166] Example 1-5 Preparation of Copper-Aluminum Particle Powder Containing a Coating Layer
[0167] The difference between Example 1-5 and Example 2 is that the mass ratios of the coating agent, the low boiling point organic solvent, the corrosion inhibitor and water are different. The obtained copper-aluminum particle powder containing the coating layer is measured in the same way as in Example 1-1, and its index is D 10 :0.35μm,D 50 :0.82μm,D 90 :2.80μm,D 97 :4.28μm, specific surface area is 1.48m 2 / g, and the tap density is 3.9g / ml.
[0168] Example 1-6 Preparation of Copper-Aluminum Particle Powder Containing a Coating Layer
[0169] The difference between Example 1-6 and Example 2 is that the mass ratios of the coating agent, the low boiling point organic solvent, the corrosion inhibitor and water are different. The obtained copper-aluminum particle powder containing the coating layer is measured in the same way as in Example 1-1, and its index is D 10 :0.37μm,D 50 :0.85μm,D 90 :2.86μm,D97 :4.32μm, specific surface area is 1.45m 2 / g, and the tap density is 4.1g / ml.
[0170] Example 1-7 Preparation of Copper-Aluminum Particle Powder Containing a Coating Layer
[0171] The difference between Example 1-7 and Example 2 is that the mass ratios of the coating agent, the low boiling point organic solvent, the corrosion inhibitor and water are different. The obtained copper-aluminum particle powder containing the coating layer is measured in the same way as in Example 1-1, and its index is D 10 :0.32μm,D 50 :0.79μm,D 90 :2.78μm,D 97 :4.15μm, specific surface area is 1.62m 2 / g, and the tap density is 4.2g / ml.
[0172] Example 1-8 Preparation of Copper-Aluminum Particle Powder Containing a Coating Layer
[0173] The difference between Example 1-8 and Example 2 is that the mass ratios of the coating agent, the low boiling point organic solvent, the corrosion inhibitor and water are different. The obtained copper-aluminum particle powder containing the coating layer is measured in the same way as in Example 1-1, and its index is D 10 :0.45μm,D 50 :0.96μm,D 90 :3.05μm,D 97 :4.62μm, specific surface area is 1.18m 2 / g, and the tap density is 3.8g / ml.
[0174] Example 1-9 Preparation of Copper-Aluminum Particle Powder Containing a Coating Layer
[0175] The difference between Example 1-9 and Example 2 is that the mass ratios of the coating agent, the low boiling point organic solvent, the corrosion inhibitor and water are different. The obtained copper-aluminum particle powder containing the coating layer is measured in the same way as in Example 1-1, and its index is D 10 :0.41μm,D 50 :0.90μm,D 90 :2.99μm,D 97 :4.60μm, specific surface area is 1.21m 2 / g, and the tap density is 3.4g / ml.
[0176] Example 1-10 Preparation of Copper-Aluminum Particle Powder Containing a Coating Layer
[0177] The difference between Example 1-10 and Example 2 is that the mass ratios of the coating agent, the low boiling point organic solvent, the corrosion inhibitor and water are different. The obtained copper-aluminum particle powder containing the coating layer is measured in the same way as in Example 1-1, and its index is D 10 :0.38μm,D 50 :0.88μm,D 90 :2.95μm,D 97 :4.45μm, specific surface area is 1.31m 2 / g, and the tap density is 3.6g / ml.
[0178] Example 1-11 Preparation of Copper-Aluminum Particle Powder Containing a Coating Layer
[0179] The difference between Example 1-11 and Example 2 is that the mass ratio of the coating agent, the low boiling point organic solvent, the corrosion inhibitor and water is different. The obtained copper-aluminum particle powder containing the coating layer is measured in the same way as in Example 1-1, and its index is D 10 :0.40μm,D 50 :0.91μm,D 90 :2.95μm,D 97 :4.55μm, specific surface area is 1.25m 2 / g, and the tap density is 3.4g / ml.
[0180] Comparative Example 1 Preparation of Copper-Aluminum Powder
[0181] The preparation was carried out in the same manner as in Example 1, except that no coating agent was used. The obtained copper-aluminum particle powder was measured according to the method described in Example 1, and the index of the obtained copper-aluminum particle powder was: D 10 :0.38μm, D 50 :0.87μm,D 90 :2.88μm,D 97 :4.40μm, specific surface area is 1.42m 2 / g, and the tap density is 3.3g / ml.
[0182] Table 2 Ratios of various components in different embodiments and comparative examples
[0183]
[0184] Example 2-1 Preparation of copper-aluminum paste
[0185] (1) 86 g of the copper-aluminum particle powder containing a coating layer obtained in Example 1-1, 2.8 g of hydrogenated bisphenol A, 0.5 g of bisphenol A E51, 2 g of polypropylene glycol glycidyl ether, 3 g of n-butyl glycidyl ether, 0.5 g of a surfactant (BYK204), 1.5 g of an epoxy accelerator (DMP-30), 1.2 g of a curing agent (dicyandiamide), 0.5 g of a silicone oil (PMX200-50CS), and 0.8 g of a thixotropic agent were added. and 1.2 g of solvent (butyl carbitol) were put into a blender for stirring at a speed of 35 rpm / min for 20 min. The blender was then stopped to scrape the stirring paddle clean, and then stirred at a speed of 45 rpm / min for 60 min to obtain the material. Vacuum was drawn during stirring, and the vacuum degree was -0.8 MPa.
[0186] (2) Roll the stirred material according to the rolling process in Table 1, and filter the rolled slurry to remove foreign matter or sequins using a 300-mesh sieve to obtain a copper-aluminum slurry with a fineness of 3 μm.
[0187] Example 2-2 Preparation of copper-aluminum paste
[0188] (1) 86 g of the copper-aluminum particle powder containing a coating layer obtained in Example 1-2, 2.3 g of bisphenol F epoxy resin, 1 g of polyurethane-modified epoxy resin, 3 g of glycidyl methacrylate, 2 g of n-butyl glycidyl ether, 0.3 g of surfactant (TEGO Wet270), 1.5 g of epoxy accelerator (dimethylbenzylamine), 1.8 g of curing agent (blocked isocyanate), 0.5 g of silicone oil (PMX200-500CS), 0.8 g of thixotropic agent (BYK410) and 0.8 g of solvent (butyl carbitol) were placed in a stirrer and stirred at a speed of 35 rpm / min for 20 min. The stirring blade was then stopped and scraped clean. The material was stirred at a speed of 45 rpm / min for 60 min to obtain a material. Vacuum was evacuated during stirring, and the vacuum degree was -0.8 MPa.
[0189] (2) Roll the stirred material according to the rolling process in Table 1, and filter the rolled slurry to remove foreign matter or sequins using a 300-mesh sieve to obtain a copper-aluminum slurry with a fineness of 4 μm.
[0190] Example 2-3 Preparation of copper-aluminum paste
[0191] The difference between Example 2-3 and Example 2-2 is that the copper-aluminum particle powder containing a coating layer prepared in Example 1-3 is used to prepare the copper-aluminum paste.
[0192] Example 2-4 Preparation of copper-aluminum paste
[0193] The difference between Example 2-4 and Example 2-2 is that the copper-aluminum particle powder containing a coating layer prepared in Example 1-4 is used to prepare the copper-aluminum paste.
[0194] Example 2-5 Preparation of copper-aluminum paste
[0195] The difference between Example 2-5 and Example 2-2 is that the copper-aluminum particle powder containing a coating layer prepared in Example 1-5 is used to prepare the copper-aluminum paste.
[0196] Example 2-6 Preparation of copper-aluminum paste
[0197] The difference between Example 2-6 and Example 2-2 is that the copper-aluminum particle powder containing a coating layer prepared in Example 1-6 is used to prepare the copper-aluminum paste.
[0198] Example 2-7 Preparation of copper-aluminum paste
[0199] The difference between Example 2-7 and Example 2-2 is that the copper-aluminum particle powder containing a coating layer prepared in Example 1-7 is used to prepare the copper-aluminum paste.
[0200] Example 2-8 Preparation of copper-aluminum paste
[0201] The difference between Example 2-8 and Example 2-2 is that the copper-aluminum particle powder containing a coating layer prepared in Example 1-8 is used to prepare the copper-aluminum paste.
[0202] Example 2-9 Preparation of copper-aluminum paste
[0203] The difference between Example 2-9 and Example 2-2 is that the copper-aluminum particle powder containing a coating layer prepared in Example 1-9 is used to prepare the copper-aluminum paste.
[0204] Example 2-10 Preparation of copper-aluminum paste
[0205] The difference between Example 2-10 and Example 2-2 is that the copper-aluminum particle powder containing a coating layer prepared in Example 1-10 is used to prepare the copper-aluminum paste.
[0206] Example 2-11 Preparation of copper-aluminum paste
[0207] The difference between Example 2-11 and Example 2-2 is that the copper-aluminum particle powder containing a coating layer prepared in Example 1-11 is used to prepare the copper-aluminum paste.
[0208] Example 2-12 Preparation of copper-aluminum paste
[0209] The difference between Example 2-12 and Example 2-2 is that different amounts of epoxy resin are used to prepare copper-aluminum paste.
[0210] Example 2-13 Preparation of copper-aluminum paste
[0211] The difference between Example 2-13 and Example 2-2 is that different amounts of epoxy resin are used to prepare copper-aluminum paste.
[0212] Example 2-14 Preparation of copper-aluminum paste
[0213] The difference between Example 2-14 and Example 2-2 is that different amounts of copper-aluminum particle powder containing a coating layer are used to prepare the copper-aluminum paste.
[0214] Comparative Example 2 Preparation of Copper-Aluminum Paste
[0215] The preparation was carried out in the same manner as in Example 2-1, except that the copper-aluminum particle powder obtained in Comparative Example 1 was used.
[0216] Comparative Example 3 Preparation of Copper-Aluminum Paste
[0217] The preparation was carried out in the same manner as in Example 2-1, except that the copper-aluminum alloy powder before treatment in Example 1-2 was used.
[0218] Table 3 Composition table of copper-aluminum pastes of different embodiments and comparative examples
[0219]
[0220]
[0221] The copper-aluminum pastes obtained in Examples 2-1 to 2-14 and the copper-aluminum pastes obtained in Comparative Examples 2 and 3 were printed on silicon wafers by screen printing. The sheet resistance was measured by four-probe at 85° C. and 85% RH. The results are shown in Table 4:
[0222] Table 4 Sheet resistance table of copper-aluminum paste obtained in different embodiments and comparative examples
[0223]
[0224] As can be seen from the table, the square resistance of the copper-aluminum paste prepared using the copper-aluminum particle powder containing a coating layer prepared using Examples 1-1 to 1-11 is relatively low. After 56 days, the square resistance is below 13.7 mΩ / □, while the square resistance of the copper-aluminum paste prepared in the comparative example is above 32.5 mΩ / □, indicating that the copper-aluminum particle powder containing a coating layer prepared in the present application forms a dense protective film on the surface of the copper-aluminum alloy powder, which can hinder the progress of corrosion.
[0225] The above is only the preferred embodiment of the present application, and does not limit the present application in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present application without departing from the technical solution of the present application still falls within the protection scope of the technical solution of the present application.
Claims
1. A copper-aluminum particle powder containing a coating layer, wherein: The inner region of the particles of the copper-aluminum particle powder containing a coating layer is a copper-aluminum particle, and the surface layer is a coating layer, wherein the coating layer contains a coating agent and a corrosion inhibitor; The corrosion inhibitor is La(NO3)3, NdCl3 and / or Ce(NO3)3.
2. The copper-aluminum particle powder containing a coating layer according to claim 1, wherein The particles of the copper-aluminum particle powder containing a coating layer sequentially comprise copper-aluminum particles, a corrosion inhibitor and a coating agent from the inside to the outside.
3. The copper-aluminum particle powder containing a coating layer according to claim 1, wherein The specific surface area of the copper-aluminum particle powder containing the coating layer is 0.7-1.8 m 2 / g.
4. The copper-aluminum particle powder containing a coating layer according to claim 1, wherein The tap density of the copper-aluminum particle powder containing the coating layer is ≥3.2 g / ml.
5. The copper-aluminum particle powder containing a coating layer according to claim 1, wherein The average particle size D of the copper-aluminum particle powder containing the coating layer is 50 1.2-1.8μm.
6. The copper-aluminum particle powder containing a coating layer according to claim 1, wherein The average particle size D of the copper-aluminum particle powder containing the coating layer is 10 0.5-0.8μm.
7. The copper-aluminum particle powder containing a coating layer according to claim 1, wherein The average particle size D of the copper-aluminum particle powder containing the coating layer is 90 3.4-4.2μm.
8. The copper-aluminum particle powder containing a coating layer according to claim 1, wherein The average particle size D of the copper-aluminum particle powder containing the coating layer is 97 ≤10μm.
9. The copper-aluminum particle powder containing a coating layer according to any one of claims 1 to 8, wherein The coating agent is stearic acid, oleic acid and / or lauric acid.
10. The copper-aluminum particle powder containing a coating layer according to any one of claims 1 to 8, wherein: The coating layer has a thickness of 3-5 nm.
11. A method for preparing a copper-aluminum particle powder containing a coating layer, comprising: Ball-milling and filtering the copper-aluminum particle powder to obtain a slurry containing the copper-aluminum particle powder; The slurry containing copper-aluminum particle powder is mixed with a solution containing a coating agent and a corrosion inhibitor, and then dried to obtain copper-aluminum particle powder containing a coating layer; The corrosion inhibitor is La(NO3)3, NdCl3 and / or Ce(NO3)3.
12. The method according to claim 11, wherein: The copper-aluminum particle powder is ball-milled in the presence of a low boiling point organic solvent and zirconium balls.
13. The method according to claim 12, wherein: The mass ratio of the copper-aluminum particle powder, the low-boiling point organic solvent and the zirconium ball is (0.9-1.2:0.7-1.0:2.3-2.7).
14. The method according to claim 12, wherein: The low boiling point organic solvent is petroleum ether, ethanol, n-butanol, isobutanol, ethyl acetate and / or tetrahydrofuran.
15. The method according to claim 11, wherein: Calculated by mass percentage in the copper-aluminum particle powder, copper accounts for 65-80% and aluminum accounts for 20-35%.
16. The method according to claim 11, wherein: The specific surface area of the particles in the copper-aluminum particle powder is 0.8-1.5m 2 / g, tap density ≥3.2g / ml, the average particle size D 50 0.9-1.5μm.
17. The method according to claim 11, wherein: The mass ratio of the slurry containing copper and aluminum particle powder to the solution containing coating agent and corrosion inhibitor is 1:0.5-1.
2.
18. The method according to claim 11, wherein: The coating agent is stearic acid, oleic acid and / or lauric acid.
19. The method according to any one of claims 11 to 18, wherein: The solution containing the coating agent and the corrosion inhibitor is an aqueous solution containing the coating agent, the corrosion inhibitor and a low-boiling-point organic solvent.
20. The method according to claim 19, wherein: The mass ratio of the coating agent, the low boiling point organic solvent, the corrosion inhibitor and water is 0.01-0.2:0.3-0.8:0.01-0.8:
1.
21. A copper-aluminum paste comprising copper-aluminum particle powder containing a coating layer and epoxy resin; The coating layer comprises a coating agent and a corrosion inhibitor; The epoxy resin includes one or more selected from bisphenol A, bisphenol F, hydrogenated bisphenol A and polyurethane modified epoxy resin; The epoxy value of the bisphenol A is 0.38-0.54; The epoxy value of the bisphenol F is 0.55-0.625; The epoxy value of hydrogenated bisphenol A is 0.42-0.47; The epoxy value of polyurethane modified epoxy resin is 0.47-0.56; The epoxy value refers to the amount of epoxy groups contained in 100 g of epoxy resin.
22. The copper-aluminum paste according to claim 21, wherein: The copper-aluminum paste further comprises a reactive diluent, a surfactant, an epoxy accelerator, a curing agent, silicone oil, a thixotropic agent and a solvent.
23. The copper-aluminum paste according to claim 22, wherein: In parts by weight, the copper-aluminum particle powder containing the coating layer is 80-88 parts, the epoxy resin is 2-5 parts, the active diluent is 2-6 parts, the surfactant is 0.1-1 parts, the epoxy accelerator is 0.2-3 parts, the curing agent is 0.3-4 parts, the silicone oil is 0.2-1 parts, the thixotropic agent is 0.3-2 parts, and the solvent is 0.5-5 parts.
24. The copper-aluminum paste according to claim 22, wherein: The active diluent is selected from two or three of n-butyl glycidyl ether, glycidyl methacrylate and polypropylene glycol glycidyl ether.
25. The copper-aluminum paste according to claim 22, wherein: The surfactant is selected from one or more of BYK204, BYK110, TEGOWet270 and TEGO Dispers 740W.
26. The copper-aluminum paste according to claim 22, wherein: The epoxy accelerator is selected from one or more of 1-aminoethyl-2-methylimidazole, triethanolamine, dimethylbenzylamine and DMP-30.
27. The copper-aluminum paste according to claim 22, wherein: The curing agent is N,N-dimethylaniline, dicyandiamide and / or blocked isocyanate.
28. The copper-aluminum paste according to claim 22, wherein: The silicone oil is PMX200-50CS, PMX200-500CS and / or PMX200-1000CS.
29. The copper-aluminum paste according to claim 22, wherein: The thixotropic agent is selected from one or more of THIXATROL PLUS, BYK 410, THIXCIN R and ST.
30. The copper-aluminum paste according to claim 22, wherein: The solvent is butyl carbitol acetate, butyl carbitol and / or terpineol.
31. An electrode comprising the copper-aluminum paste according to any one of claims 21 to 30.
32. A battery comprising the electrode according to claim 31.