Preparation method of modified organic adsorption resin and its application in preparation of hydrogen bromide
Through the preparation of modified organic adsorption resin and multi-layer processing technology, the problems of complex hydrogen bromide recovery process and low purity are solved, the preparation of high-purity hydrogen bromide is achieved, the process is simplified and safety risks are reduced, and the market demand is met.
Patent Information
- Application Number
- CN202211013258.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-23
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-08-23
AI Technical Summary
In the existing technology, the hydrogen bromide recovery process requires a large investment and is complex, and cannot improve the quality of the recovered products. There are safety risks and cannot meet the market demand for high-purity hydrogen bromide.
The preparation method of modified organic adsorption resin includes soaking the organic adsorption resin in an oxidizing solution, then blending it with polylactic acid and reacting in silicon tetrachloride gas to enhance the adsorption performance and apply it in the preparation of hydrogen bromide , through multi-layer treatment of bromine remover, adsorber and distillation tower, the impurities in the bromide tail gas are removed and high-purity hydrogen bromide is obtained.
It simplifies the process flow, improves the purity and quality of hydrogen bromide, is suitable for large-scale promotion and application, reduces safety risks, and meets the market demand for high-purity hydrogen bromide.
Smart Images

Figure CN115382516B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-purity gas preparation, and specifically relates to a preparation method of a modified organic adsorption resin and application of the modified organic adsorption resin in the preparation of hydrogen bromide. Background Art
[0002] In the production of organic bromides, liquid bromine is often used as a brominating agent to carry out bromination reactions with aromatic or aliphatic compounds. In the reaction, molecular bromine undergoes a substitution reaction with organic matter, and in addition to generating organic bromides, hydrogen bromide is also produced as a byproduct. The bromine utilization rate is only 50%. From both an economic and environmental perspective, the hydrogen bromide gas must be recovered.
[0003] At present, the main methods for recovering hydrogen bromide tail gas are: water absorption method to produce hydrobromic acid, alkali absorption method to extract liquid bromine from steam, reaction with methanol to produce bromomethanol, hydrogen peroxide oxidation to produce liquid bromine, etc. These methods have problems such as large investment and complex process, and introduce new safety risks and environmental risks. At the same time, high-purity hydrogen bromide can be used in etching processes in the semiconductor industry due to its strong corrosiveness. In the prior art, plasma hydrogen bromide etching technology can accurately control the etching depth and verticality, without destroying the ozone layer or producing greenhouse gases, and is a good substitute for fluorocarbon etching gases. At present, the market demand for high-purity hydrogen bromide products is growing.
[0004] Chinese patent document CN215506247U describes a hydrogen bromide tail gas absorption system, which uses water to absorb hydrogen bromide tail gas. Chinese patent document CN202179923U describes a hydrogen bromide tail gas absorption device, which uses a cooling process to recover hydrogen bromide. The above-mentioned systems are not suitable for recovering industrial tail gas in organic synthesis, and the absorbed items cannot be sold as products; moreover, the tail gas composition of bromide in organic synthesis is complex and requires high subsequent purification and cleansing. The device cannot improve the quality of the recovered hydrogen bromide product. Chinese patent document CN113501500A describes a synthesis process and synthesis furnace for high-purity hydrogen bromide. From the perspective of actual operation, this process will explode and there is a great safety risk.
[0005] Based on this, it is necessary to provide a preparation process of hydrogen bromide to solve the above technical problems. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a modified organic adsorption resin and its application in the preparation of hydrogen bromide, so as to solve the problems that the existing purification devices and processes cannot improve the quality of the recovered hydrogen bromide products, have relatively large investments, and have complex processes.
[0007] An object of the present invention is to provide a method for preparing a modified organic adsorption resin.
[0008] A method for preparing a modified organic adsorption resin comprises the following steps:
[0009] S1, adding the organic adsorption resin into the oxidation solution for immersion to obtain the oxidatively modified organic adsorption resin;
[0010] S2, adding the oxidatively modified organic adsorption resin and polylactic acid into a chloroform solution, stirring and dissolving and mixing evenly, and heating to volatilize the chloroform to obtain the oxidatively modified organic adsorption resin of polylactic acid;
[0011] S3, placing the polylactic acid oxidized modified organic adsorption resin into a device filled with silicon tetrachloride gas, and then introducing water vapor to react to obtain a modified organic adsorption resin.
[0012] Furthermore, in step S1, the organic adsorption resin is selected from at least one of polystyrene resin and polyacrylate resin, and the oxidizing liquid is selected from at least one of hydrogen peroxide, hypochlorous acid, periodic acid and sulfuric acid.
[0013] Furthermore, in step S1, the mass volume ratio of the organic adsorption resin to the oxidizing liquid is 1:(7-9), and the immersion time is 6-8 hours.
[0014] Furthermore, in step S2, the mass ratio of the oxidatively modified organic adsorption resin to the polylactic acid is (5-6):1, and the stirring, dissolving and mixing time is 2-3 hours.
[0015] Furthermore, in step S3, the reaction time is 5 to 6 hours.
[0016] Another object of the present invention is to provide the use of the modified organic adsorption resin prepared by the preparation method of the modified organic adsorption resin in the preparation of hydrogen bromide.
[0017] Furthermore, the method for preparing hydrogen bromide comprises the following steps:
[0018] 1) passing the bromide tail gas into a debrominator, wherein the debrominator is provided with activated carbon and is used to remove bromine in the bromide tail gas;
[0019] 2) cooling the bromide tail gas from which bromine is removed to room temperature, and then passing the bromide tail gas into a modified organic adsorption resin adsorber, wherein the modified organic adsorption resin adsorber is provided with a modified organic adsorption resin, and the modified organic adsorption resin adsorber is used to remove organic bromides in the bromide tail gas;
[0020] 3) The bromide tail gas from which the organic bromide is removed is passed into a light removal distillation tower for light removal treatment; then passed into a heavy removal distillation tower for heavy removal treatment, and finally a high-purity hydrogen bromide gas is obtained.
[0021] Furthermore, in step 1), the debrominator is controlled at a temperature of 200-350° C., and the activated carbon is selected from at least one of coal-based activated carbon, wood-based activated carbon, and synthetic activated carbon.
[0022] Furthermore, in step 1), the bromide tail gas is produced during the synthesis process by any one of bromobenzene, ethyl bromide, 1,2-dibromoethane, 2-bromopropane, 1,3-dibromopropane, bromobutylene, bromoisobutylene, 2-bromobutylene and 1,4-dibromobutylene.
[0023] Furthermore, in step 3), the light removal treatment is used to remove hydrogen, oxygen, nitrogen, argon, carbon monoxide, methane and carbon dioxide in the bromide tail gas; the heavy removal treatment is used to remove organic bromides, moisture and C2-C6 hydrocarbons in the bromide tail gas.
[0024] Compared with the prior art, the present invention has the following advantages:
[0025] In the present invention, firstly, the organic adsorption resin is modified, wherein the organic adsorption resin is immersed in an oxidizing liquid so that part of the double bonds in the organic adsorption resin are oxidized, and then the organic adsorption resin is blended with polylactic acid, and the carboxyl group or hydroxyl group in the polylactic acid is cross-linked with the oxidized double bonds in the organic adsorption resin, thereby greatly enhancing the adsorption performance of the organic adsorption resin. In addition, the polylactic acid oxidized modified organic adsorption resin is placed in a device filled with silicon tetrachloride gas, and then water vapor is introduced for reaction, and the generated silicon dioxide continues to cross-link with the polylactic acid oxidized modified organic adsorption resin, thereby further enhancing the adsorption performance of the organic adsorption resin. The present invention applies the modified organic adsorption resin to the preparation of hydrogen bromide, wherein the bromine in the bromide tail gas is removed by a debrominator, the modified organic adsorption resin adsorber is used to remove organic bromide in the bromide tail gas, the light removal distillation tower is used for light removal treatment, and the heavy removal distillation tower is used for heavy removal treatment, and finally high-purity hydrogen bromide gas is obtained. The whole synthesis process is simple and suitable for large-scale promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0027] Figure 1 This is a diagram of a hydrogen bromide preparation device according to the present invention;
[0028] Figure 2 This is a graph showing the adsorption capacity of bromobenzene by the modified organic adsorption resin prepared in Example 2 of the present invention;
[0029] The meanings of the reference numerals in the figure are as follows: 1: debrominator; 11: heater; 2: cooler; 3: modified organic adsorption resin adsorber; 4: light removal distillation tower; 5: heavy removal distillation tower; 6: buffer tank; 7: diaphragm compressor; 8: product gas cylinder. DETAILED DESCRIPTION
[0030] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] The conventional reagents and equipment used in the present invention, unless otherwise specified, are commercially available.
[0032] See also Figure 1 The bromide tail gas enters the debrominator 1 through a pipeline, and the heater 11 is started to make the temperature in the debrominator 1 reach 200-350°C. The bromide tail gas from which bromine is removed is cooled to room temperature through a cooler 2, and then passed into a modified organic adsorption resin adsorber 3 to remove organic bromides in the bromide tail gas. After that, the light components such as hydrogen, oxygen, nitrogen, argon, carbon monoxide, methane and carbon dioxide in the bromide tail gas are removed through a light removal distillation tower 4, and the heavy components such as organic bromides, moisture and C2-C6 hydrocarbon substances in the bromide tail gas are removed through a heavy removal distillation tower 5; finally, it passes through a buffer tank 6 and a diaphragm compressor 7 and enters a product gas cylinder 8.
[0033] The whole method for preparing hydrogen bromide will be introduced below in conjunction with specific embodiments.
[0034] Example 1
[0035] A method for preparing a modified organic adsorption resin comprises the following steps:
[0036] S1, adding polystyrene resin into hydrogen peroxide and soaking for 6 hours, wherein the mass volume ratio of the organic adsorption resin to the oxidizing solution is 1:9 to obtain an oxidatively modified organic adsorption resin;
[0037] S2, adding the oxidatively modified organic adsorption resin and polylactic acid into a chloroform solution, wherein the mass ratio of the oxidatively modified organic adsorption resin to the polylactic acid is 5:1, stirring and dissolving for 2 hours to mix evenly, and then heating to volatilize the chloroform to obtain the polylactic acid oxidatively modified organic adsorption resin;
[0038] S3, placing the polylactic acid oxidized modified organic adsorption resin into a device filled with silicon tetrachloride gas, and then introducing water vapor to react for 5 hours to obtain a modified organic adsorption resin.
[0039] The method for preparing hydrogen bromide comprises the following steps:
[0040] 1) passing the bromide tail gas generated in the synthesis process of 1,2-dibromoethane into a debrominator, wherein the debrominator is provided with activated carbon, the temperature of the debrominator is controlled at 200-350° C., the activated carbon is selected from at least one of coal-based activated carbon, wood-based activated carbon, and synthetic activated carbon, and the debrominator is used to remove bromine in the bromide tail gas;
[0041] 2) cooling the bromide tail gas from which bromine is removed to room temperature, and then passing the bromide tail gas into a modified organic adsorption resin adsorber, wherein the modified organic adsorption resin adsorber is provided with a modified organic adsorption resin, and the modified organic adsorption resin adsorber is used to remove organic bromides in the bromide tail gas;
[0042] 3) passing the bromide tail gas from which the organic bromide is removed into a light-removing distillation tower for light-removing treatment, wherein the light-removing treatment is used to remove hydrogen, oxygen, nitrogen, argon, carbon monoxide, methane and carbon dioxide in the bromide tail gas; and then passing the bromide tail gas into a heavy-removing distillation tower for heavy-removing treatment, wherein the heavy-removing treatment is used to remove organic bromide, water and C2-C6 hydrocarbon substances in the bromide tail gas, and finally obtaining high-purity hydrogen bromide gas.
[0043] Example 2
[0044] A method for preparing a modified organic adsorption resin comprises the following steps:
[0045] S1, adding polyacrylate resin to a mixed solution of hypochlorous acid and periodic acid and soaking for 7 hours, wherein the mass volume ratio of the organic adsorption resin to the oxidizing solution is 1:8 to obtain an oxidatively modified organic adsorption resin;
[0046] S2, adding the oxidatively modified organic adsorption resin and polylactic acid into a chloroform solution, wherein the mass ratio of the oxidatively modified organic adsorption resin to the polylactic acid is 5.5:1, stirring and dissolving for 2.5 hours to mix evenly, and then heating to volatilize the chloroform to obtain the polylactic acid oxidatively modified organic adsorption resin;
[0047] S3, placing the polylactic acid oxidized modified organic adsorption resin into a device filled with silicon tetrachloride gas, and then introducing water vapor to react for 5.5 hours to obtain a modified organic adsorption resin.
[0048] Take 100g of the prepared modified organic adsorption resin and use the intelligent weight adsorption instrument IGA-002 to measure the adsorption isotherms of bromobenzene at different temperatures. The results are as follows: Figure 2 As shown in the figure, it can be seen that the modified organic adsorption resin of the present invention has a large adsorption capacity for bromobenzene, and the equilibrium adsorption capacity for bromobenzene at 25°C is 2400 mg / g.
[0049] The method for preparing hydrogen bromide comprises the following steps:
[0050] 1) passing the bromide tail gas generated in the synthesis process of bromobenzene into a debrominator, wherein the debrominator is provided with activated carbon, the temperature of the debrominator is controlled at 200-350° C., the activated carbon is selected from at least one of coal-based activated carbon, wood-based activated carbon, and synthetic activated carbon, and the debrominator is used to remove bromine in the bromide tail gas;
[0051] 2) cooling the bromide tail gas from which bromine is removed to room temperature, and then passing the bromide tail gas into a modified organic adsorption resin adsorber, wherein the modified organic adsorption resin adsorber is provided with a modified organic adsorption resin, and the modified organic adsorption resin adsorber is used to remove organic bromides in the bromide tail gas;
[0052] 3) passing the bromide tail gas from which the organic bromide is removed into a light-removing distillation tower for light-removing treatment, wherein the light-removing treatment is used to remove hydrogen, oxygen, nitrogen, argon, carbon monoxide, methane and carbon dioxide in the bromide tail gas; and then passing the bromide tail gas into a heavy-removing distillation tower for heavy-removing treatment, wherein the heavy-removing treatment is used to remove organic bromide, water and C2-C6 hydrocarbon substances in the bromide tail gas, and finally obtaining high-purity hydrogen bromide gas.
[0053] Example 3
[0054] A method for preparing a modified organic adsorption resin comprises the following steps:
[0055] S1, adding polystyrene resin into sulfuric acid and soaking for 8 hours, wherein the mass volume ratio of the organic adsorption resin to the oxidizing solution is 1:7 to obtain an oxidatively modified organic adsorption resin;
[0056] S2, adding the oxidatively modified organic adsorption resin and polylactic acid into a chloroform solution, wherein the mass ratio of the oxidatively modified organic adsorption resin to the polylactic acid is 6:1, stirring and dissolving for 3 hours to mix evenly, and then heating to volatilize the chloroform to obtain the polylactic acid oxidatively modified organic adsorption resin;
[0057] S3, placing the polylactic acid oxidized modified organic adsorption resin into a device filled with silicon tetrachloride gas, and then introducing water vapor to react for 6 hours to obtain a modified organic adsorption resin.
[0058] The method for preparing hydrogen bromide comprises the following steps:
[0059] 1) passing the bromide tail gas generated in the synthesis process of isobutyl bromide into a debrominator, wherein the debrominator is provided with activated carbon, the temperature of the debrominator is controlled at 200-350° C., the activated carbon is selected from at least one of coal-based activated carbon, wood-based activated carbon, and synthetic activated carbon, and the debrominator is used to remove bromine in the bromide tail gas;
[0060] 2) cooling the bromide tail gas from which bromine is removed to room temperature, and then passing the bromide tail gas into a modified organic adsorption resin adsorber, wherein the modified organic adsorption resin adsorber is provided with a modified organic adsorption resin, and the modified organic adsorption resin adsorber is used to remove organic bromides in the bromide tail gas;
[0061] 3) passing the bromide tail gas from which the organic bromide is removed into a light-removing distillation tower for light-removing treatment, wherein the light-removing treatment is used to remove hydrogen, oxygen, nitrogen, argon, carbon monoxide, methane and carbon dioxide in the bromide tail gas; and then passing the bromide tail gas into a heavy-removing distillation tower for heavy-removing treatment, wherein the heavy-removing treatment is used to remove organic bromide, water and C2-C6 hydrocarbon substances in the bromide tail gas, and finally obtaining high-purity hydrogen bromide gas.
[0062] Comparative Example 1
[0063] The preparation method of the modified organic adsorption resin is basically the same as that of Example 2, except that in step S1, the polyacrylate resin is not soaked.
[0064] Comparative Example 2
[0065] The preparation method of the modified organic adsorption resin is basically the same as that of Example 2, except that in step S2, polylactic acid is not added.
[0066] Comparative Example 3
[0067] The preparation method of the modified organic adsorption resin is basically the same as that of Example 2, except that in step S3, silicon tetrachloride gas is not added.
[0068] Example 4 Purity Test of High Purity Hydrogen Bromide
[0069] The high-purity hydrogen bromide gas obtained in Examples 1 to 3 and Comparative Examples 1 to 3 was tested for purity by gas chromatography, and the results are shown in Table 1 below:
[0070] Table 1 Purity results of high purity hydrogen bromide
[0071]
[0072] It can be seen from the data in the table that the purity of the high-purity hydrogen bromide obtained in Examples 1 to 3 reaches the 5N level, while in Comparative Examples 1-3, the modified organic adsorption resin is not soaked, polylactic acid is not added, or silicon tetrachloride gas is not added. As a result, it is found that the content of impurities is relatively high, so that the obtained high-purity hydrogen bromide is only at the 4N level. The results show that the present invention efficiently removes impurities in the bromide tail gas by modifying the organic adsorption resin, so that the purity of the obtained high-purity hydrogen bromide reaches the 5N level.
[0073] The above embodiments are only specific implementation methods of the present invention, which are used to illustrate the technical solutions of the present invention rather than to limit them. The protection scope of the present invention is not limited thereto. Although the present invention has been described in detail with reference to the aforementioned embodiments, ordinary technicians in the field should understand that any technician familiar with the technical field can still modify the technical solutions recorded in the aforementioned embodiments within the technical scope disclosed by the present invention, or can easily think of changes, or make equivalent replacements for some of the technical features therein; and these modifications, changes or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention, and should all be covered within the protection scope of the present invention.
Claims
1. Application of modified organic adsorption resin in the preparation of hydrogen bromide, It is characterized in that The method for preparing hydrogen bromide comprises the following steps: 1) passing the bromide tail gas into a debrominator, wherein the debrominator is provided with activated carbon and is used to remove bromine in the bromide tail gas; the bromide tail gas is produced in a synthesis process by any one of bromobenzene, ethyl bromide, 1,2-dibromoethane, 2-bromopropane, 1,3-dibromopropane, bromobutylene, bromoisobutylene, 2-bromobutylene and 1,4-dibromobutylene; 2) cooling the bromide tail gas from which bromine is removed to room temperature, and then passing the bromide tail gas into a modified organic adsorption resin adsorber, wherein the modified organic adsorption resin adsorber is provided with a modified organic adsorption resin, and the modified organic adsorption resin adsorber is used to remove organic bromides in the bromide tail gas; 3) passing the bromide tail gas from which the organic bromide has been removed into a light-removing distillation tower for light-removing treatment; then passing the bromide tail gas into a heavy-removing distillation tower for heavy-removing treatment, and finally obtaining high-purity hydrogen bromide gas; the light-removing treatment is used to remove hydrogen, oxygen, nitrogen, argon, carbon monoxide, methane and carbon dioxide from the bromide tail gas; the heavy-removing treatment is used to remove organic bromide, moisture and C2-C6 hydrocarbon substances from the bromide tail gas; The preparation method of the modified organic adsorption resin comprises the following steps: S1, adding an organic adsorption resin into an oxidizing solution for immersion to obtain an oxidatively modified organic adsorption resin; the organic adsorption resin is selected from at least one of a polystyrene resin and a polyacrylate resin; S2, adding the oxidatively modified organic adsorption resin and polylactic acid into a chloroform solution, stirring and dissolving and mixing evenly, and heating to volatilize the chloroform to obtain the oxidatively modified organic adsorption resin of polylactic acid; S3, placing the polylactic acid oxidized modified organic adsorption resin into a device filled with silicon tetrachloride gas, and then introducing water vapor to react to obtain a modified organic adsorption resin.
2. The use according to claim 1, It is characterized in that In step S1, the oxidizing liquid is selected from at least one of hydrogen peroxide, hypochlorous acid, periodic acid and sulfuric acid.
3. The use according to claim 1, It is characterized in that In step S1, the mass volume ratio of the organic adsorption resin to the oxidizing liquid is 1:(7-9), and the soaking time is 6-8 hours.
4. The use according to claim 1, It is characterized in that In step S2, the mass ratio of the oxidatively modified organic adsorption resin to the polylactic acid is (5-6):1, and the stirring, dissolving and mixing time is 2-3 hours.
5. The use according to claim 1, It is characterized in that In step S3, the reaction time is 5 to 6 hours.
6. The use according to claim 1, It is characterized in that In step 1), the debrominator is controlled at a temperature of 200-350° C., and the activated carbon is selected from at least one of coal-based activated carbon, wood-based activated carbon, and synthetic activated carbon.
Citation Information
Patent Citations
Synthesis process and synthesis furnace of high-purity hydrogen bromide
CN113501500A
Hydrogen bromide tail gas absorption device
CN202179923U
Hydrogen bromide tail gas absorption system
CN215506247U
Immobilized tannin adsorbent resin, and preparation method and application thereof
CN106732433A
Blood purification adsorbent for uremia and preparation method of adsorbent
CN107876031A