A large spot laser and resistance heating wire composite welding method for thin plate fillet weld
Through the composite welding method of large spot laser thermal conductivity and resistance heating wire, the problems of uneven cladding and welding deformation in thin plate fillet welding are solved, efficient and uniform heat input and welding efficiency are achieved, and the mechanics of the welded joint are improved. Performance and density.
Patent Information
- Application Number
- CN202211185236.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-27
- Publication Date
- 2024-10-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the thin plate fillet welding process, a single laser heat source causes defects such as uneven cladding, thermal cracks and welding deformation, making it difficult to control heat input and filler metal cladding efficiency, and the arc hybrid welding method can cause welding deformation and plasma absorption. question.
Using the composite welding method of large spot laser thermal conductivity and resistance hot wire, by adjusting the angle and distance between the laser head and the wire feeding nozzle, and combining the computer master control module to control the laser power, hot wire current and wire feeding speed, low-power large spot heating is achieved. Guide welding ensures uniform filling of the welding wire and full fusion of the base metal, reducing welding deformation.
It improves the heat input controllability and efficiency of thin plate fillet welding, reduces welding deformation, enhances the mechanical properties of the welded joint, avoids pores and unfusion defects, and improves the density and cladding efficiency of the weld.
Smart Images

Figure CN115383312B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of laser welding methods, in particular to a large-spot laser thermal conduction and resistance heating wire composite welding process for a thin plate fillet weld. Background Art
[0002] T-joints are commonly used in aerospace, marine, pressure vessels, petrochemical and other fields, such as the wall panels of large aircraft and a large number of frame girder structures inside the hull. The reliability of such structures depends largely on the welding quality of the T-joint fillet welds. Due to the particularity of the T-joint structure, its fillet welds are more likely to have defects such as pores, cracks or local stress concentration during the welding process. Lasers and their composite heat sources have attracted widespread attention for their advantages of high forming accuracy, good mechanical properties, and high degree of automation. In particular, they have advantages that other welding technologies cannot match in the welding forming of fillet welds of thin plate structures. Compared with heat sources such as arcs, laser heat sources have higher energy density during the welding process and can achieve more precise heat input control. According to the different laser powers, laser welding can be divided into two modes: thermal conduction welding and deep fusion welding. Laser deep fusion welding requires a very high laser power density, which not only melts the metal, but also vaporizes the metal to form a keyhole. The weld formed has a large depth-to-width ratio and is suitable for the welding of fillet welds of medium and thick plates. The energy density of the laser thermal conduction welding beam is low. After the workpiece absorbs the laser, heat is transferred to the inside of the workpiece by heat conduction to form a molten pool. In this mode, the welding process is stable and does not produce spatter. The formed weld is smooth and free of porosity defects.
[0003] However, due to the small diameter of the spot of a single laser heat source, the temperature gradient in the weld area during welding is large, which not only places high requirements on the accuracy of workpiece assembly, but also easily causes defects such as uneven cladding and thermal cracks during the actual fillet welding process. It is difficult to resolve the contradiction between heat input control and filler metal cladding efficiency, and the process window is relatively narrow. Although the laser arc hybrid welding method can solve the contradiction between heat input and cladding efficiency during welding to a certain extent, due to the introduction of arc heat, the overall heat input increases, resulting in large welding deformation during welding of low-rigidity components such as thin plates. In addition, since plasma is formed during arc welding and plasma absorbs laser light, it is difficult to coordinate process parameters.
[0004] Based on the above research status, the present invention proposes a large spot laser thermal conduction and resistance heating wire composite welding method for the thin plate corner weld joint form. The method combines resistance heating wire and laser thermal conduction welding, and adjusts the angle and distance between the laser head and the rear wire feeding nozzle by an adjustable angle fixture to ensure that the filler wire can reach the center of the laser spot. The end of the rear wire feeding nozzle is connected to the DC TIG welder to provide hot wire current for the filler wire, which reduces the energy required for the laser heat source to melt the wire during the corner weld welding process, and ensures that most of the heat is used to melt the parent material to form a stable molten pool. By adjusting the focus and power of the laser, the output of the laser is kept as large spot thermal conduction welding. By combining with the resistance heating wire technology, while ensuring the overall cladding efficiency of the welding wire, the heat input to the parent material is further optimized by the large spot method, so that the heat input to the side wall of the web of the T-joint is more uniform, solving the problem of melt penetration or side wall unfusion that is easy to occur during the welding of thin plate corner welds. Summary of the invention
[0005] The present invention proposes a large-spot laser thermal conductivity and resistance heating wire composite welding method for thin plate corner welds. On the one hand, it solves the problems of poor cladding effect and difficulty in sufficient fusion of side wall structure that are easy to occur when welding corner welds with a single laser heat source; on the other hand, it reduces the heat input during the welding process of thin plate corner welds, improves the controllability of welding heat and welding efficiency, reduces the welding deformation of thin plate corner welds, and improves the mechanical properties of thin plate corner weld joints.
[0006] The object of the present invention is achieved in that the steps are as follows:
[0007] Step 1: Clean the surface oil of the thin plate to be welded, remove the oxide layer before pretreatment, spot-fix the T-joint of the thin plate to be welded and fix it on the welding walking platform with a clamp;
[0008] Step 2: Use a fixture to fix the laser head and the rear wire feeder, and adjust the positions of the laser and the rear wire feeder respectively, so that the angle between the laser beam axis and the vertical plate to be welded is within the set range and the angle between the laser beam axis and the welding wire axis is also within the set range, ensuring that the welding wire is accurately fed into the center of the laser spot and the extension length of the welding wire is controlled within the set range of 10 to 30 mm;
[0009] Step 3: Adjust the laser spot size of the laser beam acting on the workpiece to be welded to the set range, and fine-tune the position of the spot so that the center of the laser spot is on the side of the vertical plate to be welded, and control the area of the laser spot on the side of the vertical plate to account for 55% to 65% of the total spot area;
[0010] Step 4: Before starting welding, open the shielding gas nozzle and adjust the shielding gas flow rate to the set range, adjust the laser power to the minimum power of thermal conduction welding, maintain for 2 to 3 seconds, wait until the fillet weld area is fully preheated and the welding pool is initially formed, and then turn on the DC TIG welding power supply;
[0011] Step 5: The laser power, hot wire current, wire feeding speed and welding speed are uniformly regulated through the computer master control module to change the droplet transition state of the wire end, increase the droplet transition frequency, and improve the uniformity of droplet transition filling; at the same time, the precise and controllable characteristics of the laser heat source are used to reduce the heat input to the parent material and increase the melting area of the welding pool in the fillet weld area while ensuring that the thin plate fillet weld is fully melted, so as to prevent large welding deformation caused by excessive heat input or insufficient fusion of the side wall caused by too low heat input;
[0012] Step 6: When the laser beam reaches the end of the fillet weld, turn off the wire feeding mechanism, DC TIG welder, laser and travel mechanism, and then pass the protective gas for 5 to 10 seconds to prevent the weld metal from being oxidized.
[0013] The present invention also includes such structural features:
[0014] 1. In step 2: the setting range of the inclination angle between the laser beam axis and the vertical plate to be welded is 30° to 60°, and the setting range of the angle between the laser beam axis and the welding wire axis is 30° to 60°.
[0015] 2. In step 3: the laser spot size is set to 2-4 mm.
[0016] 3. In step 4: the setting range of the protective gas flow rate is 10L / min to 20L / min.
[0017] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention designs a large-spot laser thermal conductivity and resistance heating wire composite welding process for thin plate fillet welds. By introducing the resistance heating wire, on the one hand, the welding wire cladding efficiency and the uniformity of the welding wire filling are improved, and the weld formation is improved. On the other hand, the combination of the resistance heating wire and the large-spot laser effectively reduces the heat required by the laser heat source to melt the welding wire, so that the heat of the laser heat source can be mainly used to melt the parent material to form a molten pool, thereby reducing the power demand of the laser heat source in the thin plate welding process;
[0018] (2) Low-power large-spot laser is used as the heat source. Under the premise of ensuring the penetration depth of the thin plate fillet weld, the coverage area of the heat source and the uniformity of heat input during laser welding of the fillet weld are effectively improved, so that the side wall of the fillet weld vertical plate can be fully fused, the performance of the weld joint is improved, the welding deformation caused by heat input during welding is reduced, the practicality and application scope of the welding process are increased, and the laser thermal conduction method is used for welding to avoid defects such as pores and unfused joints, and the density of the weld joint is improved. Compared with laser wire welding, the depth-to-width ratio of the weld is reduced by 15%, the cladding efficiency is increased by 30%, and the welding deformation is reduced by 10%.
[0019] (3) The hot wire current, wire feeding speed, laser power and welding speed in the welding process are controlled by the computer master control module, and the heat between the welding wire and the base material is reasonably distributed. In addition, the forming heat source of the welding device and method is essentially an efficient improvement of laser wire welding. The equipment has strong flexibility and convenient process control. It is an economical and efficient thin plate fillet weld welding method. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 : Schematic diagram of laser hot wire welding method and spot position for large spot fillet weld;
[0021] Figure 2 : Schematic diagram of welding angle;
[0022] Figure 3 : The weld surface profile obtained by implementation;
[0023] The meaning of each figure mark in the figure: 1. laser beam; 2. vertical plate to be welded; 3. bottom plate to be welded; 4. welding molten pool; 5. fillet weld; 6. post-wire feeding nozzle; 7. welding wire; 8. laser spot; 9. shielding gas nozzle; α, post-welding wire incident angle; β, laser beam deviation angle. DETAILED DESCRIPTION
[0024] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0025] The present invention relates to a large-spot laser thermal conductivity and resistance hot wire composite welding device and process method for thin plate corner welds, which is mainly composed of a DC TIG welding power supply, a wire feeding mechanism, a laser, a computer master control module and other parts. First, the laser head and the rear wire feeding nozzle are fixed by a clamp, and the angle between the welding wire axis and the incident direction of the laser spot is adjusted within a set range of 30° to 60° according to the different types of welding wires and the requirements of spatial accessibility, so as to ensure that the welding wire can be delivered to the center of the laser spot and control the extension length of the welding wire within a set range of 10 to 30 mm. The rear wire feeding nozzle is arranged behind the laser heat source along the welding direction, so that the welding wire can be subjected to the composite action of the large-spot laser and the current hot wire before entering the molten pool of the laser heat source, and metal filling is performed after the laser heat source forms a stable molten pool. The rear wire feeding nozzle of the wire feeding mechanism is connected to the DC TIG welding power supply through a cable, and the control of the welding wire cladding state is achieved by adjusting the hot wire current, and the setting range of the hot wire current is 0 to 70A. The power density of the laser is adjusted to 10 5 W / cm 2 ~10 6 W / cm 2 , the laser power is 2000W~6000W, the laser spot size acting on the fillet weld is 2~4mm, the welding process is controlled in the form of laser thermal conduction welding, reducing the heat input to the thin plate fillet weld, which is conducive to reducing the welding deformation caused by heat input and large temperature gradient. Before welding, the inclination angle between the composite welding device and the vertical plate to be welded is adjusted to 30°~60°. During the welding process, the hot wire current of the DC TIG welding machine, the wire feeding speed of the wire feeding mechanism and the relevant parameters of the laser are adjusted by the computer master control module, so as to achieve the combination of low laser power and high cladding efficiency while ensuring the depth of fillet weld penetration.
[0026] The specific implementation steps of the large-spot laser thermal conductivity and resistance heating wire composite welding process method for a thin plate fillet weld according to the present invention are as follows in conjunction with the accompanying drawings and embodiments:
[0027] Step 1: Clean the surface oil and remove the oxide layer of the thin plate to be welded, and then spot-fix the T-joint of the thin plate to be welded and fix it on the welding walking platform with a clamp. The thickness of the thin plate is 1 to 4 mm.
[0028] Step 2: Use a fixture to fix the laser head and the rear wire feeder 6, and adjust the positions of the laser and the rear wire feeder 6 respectively, so that the angle between the axis of the laser beam 1 and the vertical plate 2 to be welded is within the set range and the angle between the axis of the laser beam 1 and the axis of the welding wire 7 is also within the set range, ensuring that the welding wire 7 can be accurately fed into the center of the laser spot 8 and the extended length of the welding wire 7 is controlled within the set range of 10 to 30 mm. The setting range of the inclination angle between the axis of the laser beam 1 and the vertical plate 2 to be welded is 30° to 60°, and the setting range of the angle between the axis of the laser beam 1 and the axis of the welding wire 7 is 30° to 60°.
[0029] Step 3: Adjust the size of the laser spot 8 of the laser beam 1 acting on the workpiece to be welded to the set range. The size of the laser spot 8 is set to 2-4 mm, and the position of the spot is fine-tuned so that the center position of the laser spot 8 is on the side of the vertical plate 2 to be welded. The area of the laser spot 8 on the vertical plate is controlled to account for 55%-65% of the total area of the spot to ensure that the side plate can be fully fused during the actual welding process.
[0030] Step 4: Before starting welding, open the shielding gas nozzle 9 and adjust the shielding gas flow rate to the set range, adjust the laser power to the minimum power of thermal conduction welding, maintain for 2 to 3 seconds, and turn on the DC TIG welding power supply after the fillet weld 5 area is fully preheated and the welding pool 4 is initially formed. The setting range of the shielding gas flow rate is 10L / min to 20L / min.
[0031] Step 5: The laser power, hot wire current, wire feeding speed and welding speed are uniformly regulated through the computer master control module to change the droplet transition state of the wire end, increase the droplet transition frequency, and improve the uniformity of droplet transition filling. At the same time, the precise and controllable characteristics of the laser heat source are used to reduce the heat input to the parent material 3 and increase the melting area of the welding pool 4 in the fillet weld 5 area while ensuring that the thin plate fillet weld 5 is fully melted, so as to prevent large welding deformation caused by excessive heat input or insufficient fusion of the side wall caused by too low heat input.
[0032] Step 6: When the laser beam reaches the end of fillet weld 5, turn off the wire feeding mechanism, DC TIG welder, laser and travel mechanism, and then pass the shielding gas for 5 to 10 seconds to prevent the weld metal from being oxidized.
[0033] In the specific embodiment, the welded specimen is selected to be a 6061 aluminum alloy with a 2mm vertical plate and a 3mm bottom plate, an ER4043 welding wire with a diameter of 1.2mm, and a fiber laser with a rated power of 6kW. A large spot is obtained by positive defocusing (the focus of the laser beam is above the welded specimen); the DC TIG welding machine adopts DC positive connection, constant wire feeding, and a welding wire extension length of 15mm. The shielding gas is argon with a purity of 99.99%. The angle between the laser beam 1 and the welded vertical plate is 30°, the angle between the axis of the laser beam 1 and the axis of the welding wire 7 is 50°, and the center of the laser spot 8 is on the welded vertical plate 2, and the area accounts for 60% of the total spot area.
[0034] The welding parameters used in the specific embodiment are shown in Table 1:
[0035] Table 1 Process parameters of large spot laser thermal conduction and bypass hot wire hybrid welding of thin plate fillet weld
[0036]
[0037] In the large-spot laser thermal conduction and resistance hot wire composite welding process of thin plate corner welds, without adding hot wire current, the laser spot 8 cannot achieve uniform, high-quality welding filling of the corner weld and coexistence with smaller base material heat input. The addition of hot wire current has a significant optimization effect on the melting transition state of the welding wire 7 and a significant weakening effect on the power requirement of the laser beam 1.
[0038] After the welding test, the weld obtained is as shown in the attached Figure 3 As shown, the weld has excellent formation. Metallographic and flaw detection tests were carried out on the weld. No defects such as pores, inclusions and cracks were found in the weld. The specimen did not undergo obvious deformation. Mechanical property tests were carried out on the weld. The tensile strength of the joint meets production requirements.
Claims
1. A large spot laser and resistance heating wire composite welding method for thin plate fillet welds, characterized in that: Here are the steps: Step 1: Clean the surface oil of the thin plate to be welded, remove the oxide layer before pretreatment, spot-fix the T-joint of the thin plate to be welded and fix it on the welding walking platform with a clamp; Step 2: Use a fixture to fix the laser head and the rear wire feeder, and adjust the positions of the laser and the rear wire feeder respectively, so that the angle between the laser beam axis and the vertical plate to be welded is within the set range and the angle between the laser beam axis and the welding wire axis is also within the set range, ensuring that the welding wire is accurately fed into the center of the laser spot and the extension length of the welding wire is controlled within the set range of 10 to 30 mm; Step 3: Adjust the laser spot size of the laser beam acting on the workpiece to be welded to the set range, and fine-tune the position of the spot so that the center of the laser spot is on the side of the vertical plate to be welded, and control the area of the laser spot on the side of the vertical plate to account for 55% to 65% of the total spot area; Step 4: Before starting welding, open the shielding gas nozzle and adjust the shielding gas flow rate to the set range, adjust the laser power to the minimum power of thermal conduction welding, maintain for 2 to 3 seconds, wait until the fillet weld area is fully preheated and the welding pool is initially formed, and then turn on the DC TIG welding power supply; Step 5: The laser power, hot wire current, wire feeding speed and welding speed are uniformly regulated through the computer master control module to change the droplet transition state of the wire end, increase the frequency of droplet transition, and improve the uniformity of droplet transition filling; at the same time, the precise and controllable characteristics of the laser heat source are used to reduce the heat input to the parent material and increase the melting area of the welding pool in the fillet weld area while ensuring that the thin plate fillet weld is fully penetrated, so as to prevent large welding deformation caused by excessive heat input or insufficient fusion of the side wall caused by too low heat input; Step 6: When the laser beam reaches the end of the fillet weld, turn off the wire feeding mechanism, DC TIG welder, laser and travel mechanism, and then pass the protective gas for 5 to 10 seconds to prevent the weld metal from being oxidized.
2. The large spot laser and resistance heating wire composite welding method for thin plate fillet weld according to claim 1 is characterized in that: In step 2: the setting range of the inclination angle between the laser beam axis and the vertical plate to be welded is 30° to 60°, and the setting range of the angle between the laser beam axis and the welding wire axis is 30° to 60°.
3. The large spot laser and resistance heating wire composite welding method for thin plate fillet weld according to claim 1 is characterized in that: In step 3: the laser spot size is set to 2-4 mm.