A lanthanum molybdate surface-modified lithium-rich manganese-based positive electrode material and preparation method thereof
By inlaiding lanthanum molybdate nanoparticles and inducing spinel structure, the cycle and rate performance problems of lithium-rich manganese-based positive electrode materials are solved, which significantly improves its performance in lithium-ion batteries and achieves higher energy density and better Excellent electrochemical properties.
Patent Information
- Application Number
- CN202210866478.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-22
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-07-22
AI Technical Summary
Lithium-rich manganese-based positive electrode material has major defects in circulation and rate performance, resulting in poor performance in high-energy density lithium-ion battery applications, especially the poor conductivity of the Li2MnO3 component in the structure and the irreversible release of O2- Irreversible capacity loss and poor circulation performance.
By inlaid with inert lanthanum molybdate nanoparticles on the surface of lithium-rich manganese-based materials, a protective interface is formed and spinel structure is induced, which improves the diffusion rate of lithium ion and material stability, while reducing charge transfer using the oxygen vacancy of lanthanum molybdate oxide. impedance.
The cycle stability and rate performance of lithium-rich manganese-based materials are significantly improved, the deintercalation rate and charge transfer efficiency of lithium ions are enhanced, and the higher specific capacity and better cycle retention rate are achieved.
Smart Images

Figure CN115394974B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of positive electrode materials, and in particular to a method and application of a lanthanum molybdate surface-modified lithium-rich manganese-based positive electrode material. Background Art
[0002] In recent years, environmentally friendly rechargeable lithium-ion batteries have played an important role in the new energy industry. With the development of society and science and technology, the energy density requirements of lithium-ion batteries for hybrid vehicles and electric vehicles are constantly increasing. Commercial cathode materials such as LiCoO2 and LiFePO4 can no longer meet the high energy density requirements of lithium-ion batteries due to their defects in reversible capacity and low operating voltage. Lithium-rich manganese-based materials, with the general chemical formula of xLi2MnO3·(1-x)LiMO2 (0<x<1; M=Mn, Ni and Co, etc.), have higher specific capacity (>250mAh g -1 ) and a wider voltage range (2.0~4.8Vvs.Li + / Li), is expected to become the cathode material for the next generation of high energy density lithium-ion batteries. However, some inherent defects of this material currently seriously hinder its commercial application: (1) During the first charge, Li is released when the voltage exceeds 4.5V. + and O 2- The irreversible capacity loss caused by the Li-rich manganese-based materials leads to a low initial Coulombic efficiency; (3) 2- The irreversible release of Li2MnO3 makes it impossible to undergo redox reactions in subsequent cycles to provide additional high capacity, resulting in poor cycle performance of lithium-rich manganese-based materials; (3) The Li2MnO3 component present in the structure has poor conductivity, resulting in poor rate performance of lithium-rich manganese-based materials.
[0003] Surface modification has been proven to effectively improve the cycle performance of lithium-rich manganese-based positive electrode materials. Through surface modification, a protective interface can be formed on the surface of the lithium-rich manganese-based material to reduce the structural damage caused by HF corrosion, thereby achieving the purpose of improving the cycle stability of the lithium-rich manganese-based material. However, this method is difficult to solve the rate problem of lithium-rich manganese-based materials. The spinel structure has a three-dimensional lithium ion diffusion channel, which can effectively improve the lithium ion diffusion rate of the material and enhance the rate performance of the material. Therefore, it is particularly important to prepare a lithium-rich manganese-based positive electrode material with a protective layer on the surface and a built-in spinel structure through a simple method, while improving the cycle performance and rate performance of the material. Summary of the invention
[0004] In view of the poor cycle and rate performance of lithium-rich manganese-based positive electrode materials, the purpose of the present invention is to provide a method for surface-modified lithium-rich manganese-based positive electrode materials with lanthanum molybdate. Inert lanthanum molybdate nanoparticles are embedded on the surface of lithium-rich manganese-based materials, which can not only reduce the corrosion of electrolytes on active substances and enhance the cycle stability of lithium-rich manganese-based materials, but also induce ion rearrangement on the surface of the material to generate a spinel structure with a three-dimensional lithium ion diffusion channel, increase the lithium ion deintercalation rate, and enhance the rate performance of lithium-rich manganese-based materials.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A lanthanum molybdate surface-modified lithium-rich manganese-based positive electrode material, wherein the material matrix is a lithium-rich manganese-based oxide, and lanthanum molybdate composite oxide nanoparticles are embedded on the outside, wherein the mass ratio of the lanthanum molybdate composite oxide is 1-5wt% of the lithium-rich manganese-based oxide.
[0007] As a preferred solution, the general chemical formula of the lithium-rich manganese-based positive electrode material is: xLi2MnO3·(1-x)LiMO2, wherein 0<x<1, and M is one or more of Ni, Co, and Mn.
[0008] As a preferred solution, the lanthanum molybdate surface-modified lithium-rich manganese-based positive electrode material is a quadrangular prism-shaped structure with a porous surface.
[0009] The present invention provides a method for surface-modifying a lithium-rich manganese-based positive electrode material using lanthanum molybdate. The method has low raw material cost, simple conditions and equipment, simple operation steps, and can achieve large-scale preparation, comprising the following steps:
[0010] (1) Ultrasonic dispersion of lithium-rich manganese-based cathode materials in a mixed solution of deionized water and anhydrous ethanol to form a black suspension.
[0011] (2) Dissolve soluble molybdenum salt and lanthanum salt in deionized water to form a colorless transparent solution.
[0012] (3) Add the aqueous solutions of lanthanum salt and molybdenum salt to the suspension of lithium-rich material dropwise in sequence, and continue stirring to obtain a uniform suspension.
[0013] (4) The mixed suspension was transferred to a magnetic stirrer and heated at a constant temperature until it was evaporated to dryness to obtain a black powder.
[0014] (5) The collected black powder obtained above is heat-treated in an air atmosphere, and after natural cooling, a lithium-rich manganese-based positive electrode material with surface modification of lanthanum molybdate is obtained.
[0015] As a preferred solution, the mass ratio of lanthanum molybdate oxide accounts for 1.5% of the lithium-rich manganese-based positive electrode.
[0016] As a preferred solution, the ultrasonic dispersion time in step (1) is about 10 to 15 minutes.
[0017] As a preferred embodiment, the molybdenum salt in step (2) is ammonium heptamolybdate, and the lanthanum salt is lanthanum nitrate.
[0018] As a preferred solution, the stirring time in step (3) is 30 min.
[0019] As a preferred solution, the heating method in step (4) is water bath heating or oil bath heating; the temperature is 80-90°C,
[0020] As a preferred solution, the heat treatment temperature in step (5) is 600-650° C. and the time is 6-8 hours.
[0021] The invention provides a lanthanum molybdate surface-modified lithium-rich manganese-based positive electrode material, and applies the positive electrode material to a CR-2032 button-type lithium-ion battery.
[0022] Compared with the prior art, the advantages of the present invention are as follows:
[0023] (1) The method of surface-modifying lithium-rich manganese-based positive electrode materials with lanthanum molybdate provided by the present invention. Inert lanthanum molybdate nanoparticles are embedded on the surface of lithium-rich manganese-based materials, which can not only reduce the corrosion of the electrolyte on the active material and enhance the cycle stability of the lithium-rich manganese-based materials; it can also induce ion rearrangement on the surface of the material to generate a spinel structure with a three-dimensional lithium ion diffusion channel, thereby increasing the lithium ion deintercalation rate; at the same time, there are abundant oxygen vacancies inside the lanthanum molybdate oxide, which can reduce the charge transfer impedance of the material through the influence of the local electric field. The dual effects make the lithium-rich manganese-based materials have better rate performance.
[0024] (2) The present invention has the advantage of double modification without adding additional steps. The lithium-rich manganese-based material after surface modification of lanthanum molybdate is used as the positive electrode material to assemble into a CR-2032 button battery, and the electrochemical performance thereof is tested. The test results are as follows: 100 cycles of cycle test are carried out at a discharge rate of 1C, and the discharge specific capacity of the comparative example after 100 cycles is 171.5 mAh g -1 The cycle retention rate is 80.2%; the discharge capacity of the embodiment is increased to 191.4 mAh g -1 The cycle retention rate is 90.7%. In addition, the discharge specific capacities of the comparative example at 0.1C, 0.5C, 1C, 2C and 5C are 259.4 mAh g -1 , 224.4mAh g -1 , 193.2mAh g -1 , 168.8mAh g -1 and 134.4mAh g-1 The embodiments all showed higher specific capacities at different discharge rates, which were: 261.4 mAh g -1 , 226.3mAh g -1 , 204.8mAh g -1 、180.7mAh g -1 and 149.5mAh g -1 .
[0025] (3) The method for surface-modifying the lithium-rich manganese-based positive electrode material with lanthanum molybdate provided by the present invention has the advantages of simple preparation conditions, low raw material cost, simple operation steps, etc., and can achieve large-scale preparation. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 XRD images of the lithium-rich manganese-based positive electrode material before the surface modification of lanthanum molybdate (comparative example) and the lithium-rich manganese-based positive electrode material after the surface modification of lanthanum molybdate (example).
[0027] Figure 2 The SEM images are of the lithium-rich manganese-based positive electrode material before the surface modification of lanthanum molybdate (comparative example) and the lithium-rich manganese-based positive electrode material after the surface modification of lanthanum molybdate (example).
[0028] Figure 3 The graphs are the cycle performances of the lithium-rich manganese-based positive electrode material before the surface modification of lanthanum molybdate (comparative example) and the lithium-rich manganese-based positive electrode material after the surface modification of lanthanum molybdate (example).
[0029] Figure 4 It is a rate performance diagram of the lithium-rich manganese-based positive electrode material before the surface modification of lanthanum molybdate (comparative example) and the lithium-rich manganese-based positive electrode material after the surface modification of lanthanum molybdate (example). DETAILED DESCRIPTION
[0030] Comparative Example:
[0031] A specific preparation method of a lithium-rich manganese-based positive electrode material:
[0032] (1) Lithium salt, manganese salt, cobalt salt and nickel salt are dissolved in a mixed solution of deionized water and anhydrous ethanol (deionized water: anhydrous ethanol = 3:100, volume ratio) in a molar ratio, and stirred until a clear solution is obtained.
[0033] (2) Dissolve excess oxalic acid in a mixed solution of deionized water and anhydrous ethanol (deionized water: anhydrous ethanol = 2:3, volume ratio).
[0034] (3) The metal mixed solution is quickly poured into the oxalic acid solution and stirred continuously at room temperature for 6 to 8 hours at a speed of 450 to 550 r / min.
[0035] (4) The stirred solution is placed in a forced air drying oven to evaporate the solvent at a temperature of 80° C. to obtain a precursor powder.
[0036] (5) The precursor powder is calcined in two stages, at 450°C for 8 h and at 800°C for 20 h, with a heating rate of 2°C / min. After natural cooling, a lithium-rich manganese-based positive electrode material is obtained.
[0037] Example:
[0038] A specific preparation method of a lanthanum molybdate surface-modified lithium-rich manganese-based positive electrode material:
[0039] (1) Weigh an appropriate amount of the prepared lithium-rich manganese-based positive electrode material into a beaker containing a mixed solution (deionized water: anhydrous ethanol = 1:1). In order to make the material evenly dispersed, place it in an ultrasonic machine and continuously ultrasonicate it for 15 minutes to obtain a black suspension.
[0040] (2) Dissolve lanthanum nitrate and ammonium heptamolybdate in a stoichiometric ratio in an appropriate amount of deionized water to prepare aqueous solutions of lanthanum nitrate and ammonium heptamolybdate, and use a rubber-tipped dropper to drop the two aqueous solutions into the mixed solution of the lithium-rich manganese-based material at a uniform speed at a rate of about 1 drop / second.
[0041] (3) After the addition is complete, the mixed solution is placed in an oil bath at 90°C and stirred continuously until evaporated to dryness.
[0042] (4) After the black powder is collected and fully ground, it is heat treated at 600°C for 6 hours at a heating rate of 5°C / min. After natural cooling, a lithium-rich manganese-based positive electrode material with a surface modified by lanthanum molybdate is obtained.
[0043] The above-obtained materials are respectively used as positive electrode materials for button-type lithium-ion batteries. The specific implementation method is: the above-mentioned positive electrode materials are ground and mixed evenly with polyvinylidene fluoride and acetylene black in a mass ratio of 8:1:1, and an appropriate amount of N-methylpyrrolidone is added as a solvent, and the mixture is quickly ground to form a chocolate-like thick slurry. The obtained slurry is coated on the current collector, dried at a temperature of 120°C, and cut into small discs with a diameter of 14mm. A lithium sheet is used as the counter electrode, and the electrolyte is 1M LiPF6 dissolved in EC / DMC with a volume ratio of 1:1. It is assembled into a CR-2032 button cell in a glove box filled with argon. The electrochemical performance test is carried out using the Xinwei battery test system, and the test voltage range is 2.0~4.7V.
Claims
1. A lanthanum molybdate surface-modified lithium-rich manganese-based positive electrode material, characterized in that: The material matrix is lithium-rich manganese-based oxide, and lanthanum molybdate composite oxide nanoparticles are embedded on the outside, wherein the mass ratio of the lanthanum molybdate composite oxide is 1-5wt% of the lithium-rich manganese-based oxide.
2. The lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The general chemical formula is: xLi2MnO3·(1-x)LiMO2, wherein 0<x<1, and M is one or more of Ni, Co, and Mn.
3. The lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The lanthanum molybdate surface-modified lithium-rich manganese-based positive electrode material is a quadrangular prism-shaped structure with a porous surface.
4. The method for preparing the surface-modified lithium-rich manganese-based positive electrode material of lanthanum molybdate according to claim 1, characterized in that: The following steps are involved: (1) Ultrasonic dispersion of lithium-rich manganese-based cathode materials in a mixed solution of deionized water and anhydrous ethanol to form a black suspension. (2) dissolving soluble molybdenum salt and lanthanum salt in deionized water at a mass ratio of 1 to 5 wt % of lanthanum molybdate oxide to form a colorless transparent solution; (3) adding the aqueous solutions of lanthanum salt and molybdenum salt to the suspension of lithium-rich manganese-based material in sequence, and stirring continuously. (4) The mixed suspension is heated at a constant temperature until it is evaporated to dryness to obtain a black powder. (5) The collected black powder obtained above is heat-treated in an air atmosphere, and after natural cooling, a lithium-rich manganese-based positive electrode material after surface modification of lanthanum molybdate is obtained, wherein lanthanum molybdate nanoparticles are evenly embedded on the surface of the lithium-rich manganese-based positive electrode material.
5. The method for preparing the lanthanum molybdate surface-modified lithium-rich manganese-based positive electrode material according to claim 4, characterized in that: The molybdenum salt in step (2) is one or more of ammonium heptamolybdate, ammonium tetramolybdate, and ammonium dimolybdate, and the lanthanum salt is lanthanum nitrate or lanthanum acetate.
6. The method for preparing the lanthanum molybdate surface-modified lithium-rich manganese-based positive electrode material according to claim 4, characterized in that: The heating method in step (4) is water bath heating or oil bath heating; the temperature is 60-100°C.
7. The method for preparing the lanthanum molybdate surface-modified lithium-rich manganese-based positive electrode material according to claim 4, characterized in that: The heat treatment temperature in step (5) is 600-700° C. and the time is 6-8 hours.
8. The lanthanum molybdate surface-modified lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: It is used as the positive electrode material in CR-2032 button lithium-ion batteries.