Light emitting diode and method for preparing the same

By setting a barrier area with an energy gap higher than the well layer in the well layer in the stress relief layer of the light emitting diode, the carriers are blocked horizontally, and the problem of non-radiative recombination of the carriers in the dislocation position is solved, and the internal content of the light emitting diode is improved Quantum efficiency.

CN115398653BActive Publication Date: 2024-11-22ANHUI SANAN OPTOELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080004960.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-14
Publication Date
2024-11-22
Estimated Expiration
2040-09-14

AI Technical Summary

Technical Problem

The existing light emitting diodes have dislocations due to the mismatch between the heterogeneous substrate and the N-type semiconductor layer material, and non-radiative recombination occurs at the dislocation position, reducing the luminous efficiency.

Method used

A barrier region is provided in the well layer of the stress relief layer. The energy gap of the barrier region is higher than that of the well layer, which prevents the lateral expansion of carriers and reduces non-radiative recombination.

Benefits of technology

The internal quantum efficiency of the light emitting diode is improved, the non-radiative recombination of carriers at dislocation positions is reduced, and the luminous efficiency is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115398653B_ABST
    Figure CN115398653B_ABST
Patent Text Reader

Abstract

A light-emitting diode and a method for preparing the same, comprising a substrate (10), a first conductive semiconductor layer (20), a stress release layer (30), a light-emitting layer (40), and a second conductive semiconductor layer (50), wherein the stress release layer comprises alternately stacked well layers (31) and barrier layers (32), at least one well layer having at least one blocking region (311) distributed inside, the energy gap of the blocking region being higher than the energy gap of the well layer. The blocking region is arranged inside the well layer, and the blocking region can block carriers in the well layer from lateral expansion to the dislocation region to cause non-radiative recombination, thereby improving the light-emitting efficiency of the light-emitting diode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of semiconductor technology, and in particular relates to a light-emitting diode with a stress release layer and a preparation method thereof. By setting a blocking area that can block the lateral diffusion of carriers in a well layer of the stress release layer, the non-radiative recombination of carriers at dislocation positions is reduced, thereby improving the internal quantum efficiency of the light-emitting diode. Background Art

[0002] See attached Figure 1 Conventional light-emitting diodes are usually grown on a foreign substrate 10' by MOCVD in sequence by using an N-type semiconductor layer 20', a stress release layer 30', a light-emitting layer 40' and a P-type semiconductor layer 50'. Since there is a considerable lattice mismatch between the foreign substrate 10' (such as a sapphire substrate) and the N-type semiconductor layer 20' (such as an N-type GaN layer), a large number of dislocations D' are also formed during the epitaxial growth process. Carriers (such as electrons or holes) can undergo non-radiative recombination at the dislocation position, thereby reducing the luminous efficiency of the light-emitting layer. This is the main reason for the low internal quantum efficiency of the light-emitting diode.

[0003] Therefore, how to reduce the non-radiative recombination of carriers is an important issue that needs to be solved at present. Summary of the invention

[0004] In order to solve the above technical problems, the present invention focuses on the stress release layer, and increases the internal quantum efficiency of the light-emitting diode by reducing the non-radiative recombination of carriers in the stress release layer. The specific technical solution is as follows:

[0005] According to a first aspect of the present invention, a light-emitting diode is provided, comprising: a first conductive semiconductor layer and a second conductive semiconductor layer with opposite electrical properties; a light-emitting layer sandwiched between the first conductive semiconductor layer and the second conductive semiconductor layer; a stress release layer sandwiched between the first conductive semiconductor layer and the light-emitting layer, comprising alternating well layers and barrier layers; and characterized in that at least one blocking region is distributed in at least one of the well layers, and the energy gap of the blocking region is greater than the energy gap of the well layer.

[0006] Among them, since there are a large number of dislocations in the well layer, and carriers can undergo non-radiative recombination by lateral expansion to the dislocation position, the present invention mainly forms a blocking zone at the dislocation position inside the well layer, that is, the blocking zone corresponds to the position of the region with dislocations inside the well layer. Since the energy gap of the blocking zone is higher than that of the well layer, carriers usually migrate from high energy gap positions to low energy gap positions. Therefore, the blocking zone can block the lateral expansion of carriers, thereby blocking the non-radiative recombination of carriers at the dislocation position, that is, the blocking zone blocks the lateral expansion of carriers in the well layer, reducing the non-radiative recombination of carriers at the dislocation position.

[0007] Furthermore, the energy gap of the blocking region is smaller than or equal to the energy gap of the barrier layer. In the present invention, the energy gap of the blocking region is preferably the same as the energy gap of the barrier layer.

[0008] Furthermore, the barrier regions are regularly or irregularly distributed inside the well layer. In the present invention, the barrier regions are preferably randomly distributed inside the well layer in a dotted shape. Since the position of the dislocation inside the well layer is random, the position of the barrier region corresponding thereto is also random. And the area size of the barrier region is also random, and the area size is the same or different.

[0009] Further, the upper surface of the barrier region is flush with the upper surface of the well layer, and the lower surface of the barrier region is located inside the well layer or flush with the lower surface of the well layer. Therefore, the thickness of the barrier region is less than or equal to the thickness of the well layer. In the present invention, the upper surface of the barrier region is preferably flush with the upper surface of the well layer, and the lower surface is located inside the well layer, and the thickness ratio of the barrier region to the well layer is less than or equal to 1 / 2.

[0010] Furthermore, the well layer is a material layer containing In, the barrier region is a material layer containing or not containing In, and the In content of the barrier region is lower than the In content of the well layer. In the present invention, the well layer material is preferably Inx1Ga1-x1N, and the barrier layer is Inx2Ga1-x2N, wherein 0 <x1<1,0≤x2<1,x1> x2. More preferably, the well layer is InGaN, the barrier layer is GaN, and the blocking region is GaN.

[0011] Furthermore, the cross-sectional shape of the blocking area is an inverted triangle, a square, or an irregular shape.

[0012] According to a second aspect of the present invention, there is provided a method for preparing the above-mentioned light emitting diode, comprising the following steps:

[0013] (1) Providing a substrate;

[0014] (2) depositing a first conductive type semiconductor layer on the substrate;

[0015] (3) depositing a stress release layer on the first conductive semiconductor layer, wherein the stress release layer comprises alternately stacked well layers and barrier layers;

[0016] (4) depositing a light-emitting layer on the stress release layer;

[0017] (5) depositing a second conductive semiconductor layer on the light-emitting layer;

[0018] The invention is characterized in that at least one barrier region is distributed in at least one of the well layers, and the energy gap of the barrier region is greater than the energy gap of the well layer.

[0019] In one embodiment, the barrier region is formed by subjecting the well layer to high temperature treatment to precipitate In from at least part of the dislocation region inside the well layer to form the barrier region. Further, the temperature at which the well layer is treated is higher than the growth temperature of the well layer and less than or equal to the growth temperature of the barrier layer. Furthermore, the well layer is treated at high temperature in an ammonia atmosphere.

[0020] In another embodiment, the barrier region is formed by first treating the well layer with an etching gas to form a depression in at least part of the dislocation region inside the well layer, and then growing a barrier layer on the surface of the well layer, the barrier layer filling the depression and forming the barrier region in the depression. Further, the etching gas includes hydrogen.

[0021] Furthermore, the method for preparing the light emitting diode further includes the steps of depositing a first electrode on the first conductive semiconductor layer, and sequentially depositing a current blocking layer, a transparent conductive layer and a second electrode on the second conductive semiconductor layer.

[0022] The present invention forms a barrier region with a higher energy gap than the well layer in the well layer of the stress release layer, especially forms a barrier region in the dislocation region inside the well layer, so as to block the carriers in the well layer from extending laterally to the dislocation position to cause non-radiative recombination, thereby increasing the internal quantum efficiency of the light-emitting diode. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram of the cross-sectional structure of a light emitting diode in the prior art.

[0024] Figure 1 FIG. 4 is a schematic diagram of a cross-sectional structure of a light emitting diode according to one embodiment of the present invention.

[0025] Figure 2 It is a schematic diagram of a top view structure of a well layer according to one embodiment of the present invention.

[0026] Figure 3 FIG. 4 is a schematic diagram of a cross-sectional structure of a light emitting diode according to another embodiment of the present invention. DETAILED DESCRIPTION

[0027] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that the drawings of the present invention are all simplified and non-precisely proportioned, and are only used to conveniently and clearly assist in explaining the present invention.

[0028] The light-emitting diode proposed by the present invention has a barrier region for blocking the lateral expansion of carriers at a position corresponding to the dislocation in the well layer of the stress release layer, thereby preventing the non-radiative recombination of carriers at the dislocation position and reducing the internal quantum efficiency of the light-emitting diode. When forming the barrier region, the formed well layer structure is annealed in nitrogen to sublimate or decompose In in a part of the well layer. Specifically, In in the well layer located on the dislocation inside the well layer is easily decomposed and precipitated. Alternatively, the formed well layer structure is subjected to surface corrosion treatment in hydrogen to form a groove in a part of the well layer, and then the groove is filled with a material having a higher energy gap than the well layer.

[0029] Figure 2 It is a cross-sectional view of a light emitting diode according to one embodiment of the present invention.

[0030] See attached Figure 2 The light emitting diode of the present invention comprises: a substrate 10; a first conductive semiconductor layer 20 and a second conductive semiconductor layer 50 having opposite electrical properties; a light emitting layer 40 sandwiched between the first conductive semiconductor layer 20 and the second conductive semiconductor layer 50; a stress release layer 30 sandwiched between the first conductive semiconductor layer 20 and the light emitting layer 40, comprising alternately stacked well layers 31 and barrier layers 32, wherein at least one well layer 31 is distributed with at least one blocking region 311, and the energy gap of the blocking region 311 is greater than the energy gap of the well layer 31.

[0031] The material of the substrate 10 may include sapphire, silicon carbide, silicon nitride, silicon, etc. The substrate 10 may be further patterned to form a concave-convex structure 11 on its surface that is conducive to light extraction, thereby increasing the light extraction efficiency of the light-emitting diode. The present invention does not impose any particular limitation on this. With regard to the material and structure of the above-mentioned substrate 10, the present embodiment preferably uses a patterned sapphire substrate 10, but this preferred structure does not constitute a limitation on the present invention.

[0032] The first conductive semiconductor layer 20 is a gallium nitride-based semiconductor layer, which can be doped with n-type impurities to provide electrons. The second conductive semiconductor layer 50 is a gallium nitride-based semiconductor layer, which can be doped with p-type impurities to provide holes. Electrons and holes undergo radiation recombination in the light-emitting layer 40, making the light-emitting diode emit light. The stress release layer 30 is used to release the stress inside the light-emitting diode. The constituent materials of the first conductive semiconductor layer 20, the stress release layer 30, the light-emitting layer 40 and the second conductive semiconductor layer 50 can be represented by the molecular formula AlxInyGa1-x-yN, where 0≤x<1, 0≤y<1, and 0≤x+y<1.

[0033] The gallium nitride-based compound semiconductor layer is deposited on a foreign substrate 10 such as sapphire or silicon carbide. Due to the lattice mismatch of each material layer, a large number of dislocations D are generated. In the subsequent epitaxial growth process, the dislocations D extend along the thickness direction of the epitaxial growth. When they extend into the light-emitting layer 40, carriers are prone to non-radiative recombination in the dislocation D region, reducing the luminous efficiency.

[0034] The light-emitting layer 40 usually includes a single quantum well structure or a multi-quantum well structure, and Japanese Patent Application Publication No. 2001-68733 discloses that a quantum box structure is manufactured by forming a conventional quantum well structure and annealing the structure in hydrogen, thereby decomposing the InGaN crystal disposed on the dislocation D. However, annealing the quantum well structure in hydrogen causes In to be released from the part that serves as the quantum box structure, which will cause the emission wavelength to shift blue. However, the present application provides a barrier region 311 similar to the quantum box structure in the well layer 31 of the stress release layer 30, which neither causes the emission wavelength to shift blue, nor reduces non-radiative recombination, thereby increasing the luminous efficiency.

[0035] The light emitting layer 40 is formed by alternately stacking a quantum well layer 41 and a quantum barrier layer 42, wherein the energy gap of the quantum barrier layer 42 is higher than that of the quantum well layer 41. Because the gallium nitride compound semiconductor including In can emit high-intensity light in the blue light wavelength region, the quantum well layer 41 is a nitride compound semiconductor material layer including In, for example, it can be represented by the molecular formula Inx1Ga1-x1N, where 0<x1<1. The quantum barrier layer 42 is a gallium nitride-based material layer, for example, it can be represented by the molecular formula Aly2Inx2Ga1-x2-y2N, where 0≤x2≤1, 0≤y2≤1, x2<x1, and preferably the quantum barrier layer 42 is GaN or AlGaN, etc.

[0036] It should be noted that when the substrate 10, especially a larger substrate 10, such as a 4-12 inch substrate 10, grows the bottom layer (the semiconductor layer before the light emitting layer 40), the higher growth temperature of the bottom layer will cause the epitaxial wafer to slowly become concave before the light emitting layer 40. At this time, if the light emitting layer 40 is directly grown, the epitaxial wafer will become convex, the stress cannot be well released, and the warpage of the epitaxial wafer is large, causing breakage. Therefore, in this embodiment, a stress release layer 30 is provided between the first conductive semiconductor layer 20 and the light emitting layer 40 to release stress and prevent breakage.

[0037] The stress release layer 30 includes alternately stacked well layers 31 and barrier layers 32, wherein a large number of dislocations D and defects exist inside the well layer 31, which can release the stress caused by the mismatch between the sapphire and the gallium nitride-based compound semiconductor layer, and can alleviate the defects caused by the lattice mismatch between the sapphire and the gallium nitride-based semiconductor layer. The well layer 31 and the barrier layer 32 of the stress release layer 30 are alternately stacked 3 times or more, preferably 6 times.

[0038] Since there are a large number of dislocations D in the well layer 31, the carriers in the stress release layer 30 can move to the dislocation D position through lateral expansion and undergo non-radiative recombination. Therefore, in order to reduce the occurrence of non-radiative recombination, it is necessary to block the lateral expansion of the carriers to the dislocation D position. In this embodiment, a blocking region 311 is set at the dislocation D position in the well layer 31 to block the lateral expansion of the carriers. Since the carriers usually migrate from the high energy gap position to the low energy gap position, in order to block the lateral expansion of the carriers, the energy gap of the blocking region 311 must be higher than the energy gap of the well layer 31.

[0039] The dislocations D in the well layer 31 are irregularly and randomly distributed, and the barrier regions 311 are mainly formed at the dislocation D positions, so the barrier regions 311 are also irregularly and randomly distributed. Of course, in other embodiments, the barrier regions 311 may also be arranged to be regularly distributed.

[0040] Figure 3 FIG. 3 is a schematic diagram showing a top view of the well layer 31 in one embodiment.

[0041] See attached Figure 3 It can be seen from the top view that the barrier regions 311 are randomly distributed in the well layer 31 in the form of dots, and the sizes of the barrier regions 311 are also random, and can be the same or different.

[0042] Figure 4 The TEM cross-sectional view of the stress release layer 30 in one embodiment is shown, wherein the light-colored area is the well layer 31 , the dark-colored area is the barrier layer 32 , and the dark-colored area indicated by the arrow is the blocking region 311 .

[0043] It can be seen from the TEM cross-sectional view that, macroscopically, relative to the lighter-colored well layer 31 , the barrier region 311 is a darker-colored strip, and microscopically, the cross-sectional shape of the barrier region 311 may be an inverted triangle, a square, or an irregular shape.

[0044] The well layer 31 of the stress relaxation layer 30 is generally a material layer containing In, the blocking region 311 is a material layer without In or containing In, and the In content of the blocking region 311 is lower than that of the well layer 31, so as to achieve the purpose that the energy gap of the blocking region 311 is higher than that of the well layer 31. The In content of the well layer 31 of the stress relaxation layer 30 is less than the In content in the quantum well layer 41 of the light-emitting layer 40, and the light-emitting layer 40 is the main light-emitting region. The energy gap of the barrier layer 32 in the stress relaxation layer 30 is greater than that of the well layer 31, and the energy gap of the blocking region 311 is greater than that of the well layer 31. In this embodiment, the energy gap of the blocking region 311 is less than or equal to the energy gap of the barrier layer 32, and preferably the energy gap of the blocking region 311 is the same as the energy gap of the barrier layer 32. In this embodiment, preferably the material of the well layer 31 is Inx3Ga1-x3N, and the blocking region 311 is A1y4Inx4Ga1-x4N, where 0 < x3 < 1, 0 ≤ x4 < 1, 0 ≤ y4 < 1, and x4 < x3. Since the greater the difference in energy gap between the blocking region 311 and the well layer 31 is, the better, it is preferred that the blocking region 311 does not contain In, and its blocking effect on carriers is better. For example, the well layer 31 is InGaN, the barrier layer 32 is GaN, and the blocking region 311 is GaN. At this time, the energy gap of the blocking region 311 is the same as that of the barrier layer 32, and both are greater than the energy gap of the well layer 31.

[0045] Continue to refer to the appendix Figure 2 , the upper surface of the blocking region 311 is flush with the upper surface of the well layer 31, and the lower surface of the blocking region 311 is located inside the well layer 31 or flush with the lower surface of the well layer 31 (as Figure 2 and 4 shown), that is, the well layer 31 is in a continuous state or is intermittently blocked by the blocking region 311. Therefore, the thickness of the blocking region 311 is less than or equal to the thickness of the well layer 31. In this embodiment, preferably the upper surface of the blocking region 311 is flush with the upper surface of the well layer 31, and the lower surface is located inside the well layer 31, and the thickness ratio of the blocking region 311 to the well layer 31 is less than or equal to 1 / 2. Specifically, the thickness of the well layer 31 is between 10 Å and 50 Å, and the thickness of the blocking region 311 is not greater than 25 Å.

[0046] The thickness of the barrier layer 32 is between 30 Å and 200 Å. When the barrier layer 32 is too thin, the flattening of the upper surface of the barrier layer 32 cannot be obtained, resulting in the blocking region 311 not being filled up and the blocking effect being poor; on the contrary, when the barrier layer 32 is too thick, the stress relaxation effect is limited. Further, the thickness of the barrier layer 32 is preferably between 60 Å and 80 Å.

[0047] In another embodiment of the present invention, a method for manufacturing the above light-emitting diode is provided, including the following steps:

[0048] First, provide a substrate 10, the substrate 10 is a patterned sapphire substrate 10. After the substrate 10 is cleaned, it is placed in an MOCVD machine for epitaxial growth.

[0049] Next, a first conductive semiconductor layer 20 is deposited on the substrate 10 by using the MOCVD method. The first conductive semiconductor layer 20 is GaN doped with Si impurities.

[0050] Again, a stress release layer 30 is deposited on the first conductive semiconductor layer 20 by MOCVD method. The stress release layer 30 includes alternately stacked well layers 31 and barrier layers 32. The well layers 31 are InGaN, the barrier layers 32 are GaN, and the well layers 31 and the barrier layers 32 are repeatedly grown 6 to 8 times.

[0051] At least one barrier region 311 is distributed in at least one well layer 31, and the energy gap of the barrier region 311 is greater than the energy gap of the well layer 31. The well layer 31 is InGaN, and the barrier region 311 is GaN.

[0052] In one embodiment, the barrier region 311 is formed by the following method: after the growth of the well layer 31 is completed, the well layer 31 is treated at high temperature. At this time, the material layer having at least part of the dislocation D region inside the well layer 31 is unstable, especially the In therein is easy to precipitate or decompose, so that a barrier region 311 containing no In or having an In content less than that of the well layer 31 is formed at this position. When the material of the well layer 31 is InGaN, after the In therein is precipitated or decomposed, the barrier region 311 formed is GaN. The temperature for treating the well layer 31 is higher than the growth temperature of the well layer 31 and lower than or equal to the growth temperature of the barrier layer 32. The gas atmosphere during the treatment can be an ammonia atmosphere. The upper and lower surfaces of the well layer 31 are flat, and the upper and lower surfaces of the barrier layer 32 are also flat.

[0053] The high temperature for processing the well layer 31 is between 800 and 900 degrees. When the temperature is lower than 800 degrees, the InGaN corrosion rate is slower and the processing time is longer; when the temperature is higher than 900 degrees, the InGaN corrosion is faster and the time is shorter, which is not easy to control.

[0054] In another embodiment, the barrier region 311 can also be formed by the following method: after the growth of the well layer 31 is completed, the surface of the well layer 31 is corroded by a corrosive gas. At this time, the material layer of at least part of the well layer 31 having the dislocation D region is unstable, and this position is easily corroded by the gas to form a recessed region, and then a barrier layer 32 is grown on the surface of the well layer 31. The barrier layer 32 fills the recess and forms the barrier region 311 in the recess. At this time, the material of the barrier region 311 is the material of the barrier layer 32. Among them, the corrosive gas includes hydrogen. The upper and lower surfaces of the well layer 31 are flat, and the upper and lower surfaces of the barrier layer 32 are also flat. The growth temperature of the well layer 31 is lower than the growth temperature of the barrier layer 32. The treatment time of hydrogen is between 10 seconds and 60 seconds, the flow rate is 7slm~20slm, and the treatment temperature is about 830 degrees.

[0055] In the light-emitting layer 40, if hydrogen is used to treat the quantum well layer 41, it will cause quantum well damage, reduce the area of ​​the quantum well light-emitting region, and reduce the light efficiency. In the present application, hydrogen is used to treat the well layer 31 of the stress release layer 30, and the well layer 31 does not belong to the light-emitting region, so the light-emitting area and light-emitting efficiency will not be reduced.

[0056] Any of the above methods uses the MOCVD method to grow the barrier region 311 without taking the epitaxial wafer out of the MOCVD machine for other operations. The process is easy to operate and more conducive to mass production.

[0057] Next, the light emitting layer 40 is deposited on the stress release layer 30 by MOCVD method. The light emitting layer 40 includes quantum well layers 41 and quantum barrier layers 42 which are alternately stacked. The quantum well layers 41 are InGaN, and the In content thereof is higher than that of the well layers 31 of the stress release layer 30. The quantum barrier layers 42 are GaN. The quantum well layers 41 and the quantum barrier layers 42 are repeatedly grown 6 to 8 times.

[0058] Next, a second conductive semiconductor layer 50 is deposited on the light emitting layer 40 by using the MOCVD method. The second conductive semiconductor layer 50 is GaN doped with Mg impurities.

[0059] Then, the second conductive semiconductor layer 50 is etched to the first conductive semiconductor layer 20 to expose a portion of the first conductive semiconductor layer 20, and a first metal electrode is formed on the surface of the exposed first conductive semiconductor layer 20, and at the same time, a metal electrode and a second metal electrode are formed on the surface of the second conductive semiconductor layer 50. The etching method includes dry etching and wet etching.

[0060] Finally, the semiconductor stack is split to form independent light-emitting crystal grains. The splitting step includes firstly scribing the semiconductor stack and then splitting it.

[0061] The first conductive semiconductor layer 20, the stress release layer 30, the light emitting layer 40 and the second conductive semiconductor layer 50 are all gallium nitride compound semiconductor layers. The present application has no specific restrictions on their growth methods. For example, conventional MBE, MOCVD and HVPE methods can be used, among which MOCVD is preferred.

[0062] It should be understood that the above specific implementation scheme is a preferred embodiment of the present invention, and the scope of the present invention is not limited to this embodiment. Any changes made according to the present invention are within the protection scope of the present invention.

Claims

1. Light emitting diodes, including: A first conductive type semiconductor layer and a second conductive type semiconductor layer with opposite electrical properties; A light-emitting layer is sandwiched between the first conductive semiconductor layer and the second conductive semiconductor layer; A stress release layer, sandwiched between the first conductive semiconductor layer and the light emitting layer, comprising alternately stacked well layers and barrier layers; The invention is characterized in that at least one barrier region is distributed in at least one of the well layers, and the energy gap of the barrier region is greater than the energy gap of the well layer.

2. The light emitting diode according to claim 1, characterized in that: The well layer of the stress release layer has dislocations in it, and at least part of the barrier region is disposed in the dislocation region.

3. The light emitting diode according to claim 1, characterized in that: The blocking region blocks the lateral expansion of carriers in the well layer, thereby reducing the non-radiative recombination of carriers at dislocation positions.

4. The light emitting diode according to claim 1, characterized in that: The energy gap of the blocking region is smaller than or equal to the energy gap of the barrier layer.

5. The light emitting diode according to claim 1, characterized in that: The barrier regions are regularly or irregularly distributed inside the well layer.

6. The light emitting diode according to claim 1, characterized in that: The barrier regions are randomly distributed in the well layer in a dot-like shape.

7. The light emitting diode according to claim 1, characterized in that: The upper surface of the barrier region is flush with the upper surface of the well layer, and the lower surface of the barrier region is located inside the well layer or is flush with the lower surface of the well layer.

8. The light emitting diode according to claim 7, characterized in that: The thickness of the barrier region is less than or equal to the thickness of the well layer.

9. The light emitting diode according to claim 8, characterized in that: The thickness ratio of the barrier region to the well layer is less than or equal to 1 / 2.

10. The light emitting diode according to claim 1, characterized in that: The well layer is a material layer containing In, the barrier region is a material layer containing no In or containing In, and the In content of the barrier region is lower than the In content of the well layer.

11. The light emitting diode according to claim 10, characterized in that: The well layer material is Inx1Ga1-x1N, and the barrier region is Inx2Ga1-x2N, wherein 0 <x1<1,0≤x2<1,x1> x2.

12. The light emitting diode according to claim 11, characterized in that: The well layer is InGaN, the barrier layer is GaN, and the blocking region is GaN.

13. The light emitting diode according to claim 1, characterized in that: The cross-sectional shape of the blocking area is an inverted triangle, a square, or an irregular shape.

14. A method for preparing a light emitting diode, comprising the following steps: (1) Providing a substrate; (2) depositing a first conductive type semiconductor layer on the substrate; (3) depositing a stress release layer on the first conductive semiconductor layer, wherein the stress release layer comprises alternately stacked well layers and barrier layers; (4) depositing a light-emitting layer on the stress release layer; (5) depositing a second conductive semiconductor layer on the light-emitting layer; Features: At least one barrier region is distributed in at least one of the well layers, and the energy gap of the barrier region is greater than the energy gap of the well layer.

15. The method for preparing a light emitting diode according to claim 14, characterized in that: The barrier region is formed by subjecting the well layer to high temperature treatment to precipitate In from at least a portion of the dislocation region inside the well layer to form the barrier region.

16. The method for preparing a light emitting diode according to claim 15, characterized in that: The temperature for processing the well layer is higher than the growth temperature of the well layer and lower than or equal to the growth temperature of the barrier layer.

17. The method for preparing a light emitting diode according to claim 16, characterized in that: The well layer is subjected to high temperature treatment in an ammonia atmosphere.

18. The method for preparing a light emitting diode according to claim 14, characterized in that: The barrier region is formed by first treating the well layer with an etching gas to form a depression in at least part of the dislocation region inside the well layer, and then growing a barrier layer on the surface of the well layer to fill the depression and form a barrier region in the depression.

19. The method for preparing a light emitting diode according to claim 18, characterized in that: The etching gas includes hydrogen.