A shrinkage reducing agent and its preparation method and application
By introducing alcohol shrinkage-reducing functional monomers and modified calcium sulfate fibers into the polycarboxylate water-reducing agent, a synergistic shrinkage-reducing agent is prepared, which solves the problems of concrete shrinkage and cracks and improves the crack resistance and compatibility.
Patent Information
- Application Number
- CN202211217936.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-30
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-09-30
AI Technical Summary
Existing concrete shrinkage and cracking problems exist in transportation construction and construction projects. The use of expansion agents is harsh and uneven, and the fiber distribution is messy. Simply adding shrinkage reducing agents has problems of poor compatibility and high cost.
The alcohol shrinkage-reducing functional monomer and fiber are introduced into the structure of the polycarboxylate water-reducing agent, and the calcium sulfate fiber is modified through esterification reaction and silane coupling to prepare a shrinkage-reducing membrane with the synergistic effect of alcohol shrinkage-reducing functional monomer and calcium sulfate fiber. agent to inhibit concrete shrinkage.
It effectively prevents water evaporation, reduces the formation of capillary pores, controls and inhibits cracks, improves the crack resistance of concrete, and evenly distributes fibers to solve the problem of poor compatibility.
Smart Images

Figure GDA0004991353180000031 
Figure GDA0004991353180000032 
Figure GDA0004991353180000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cement or concrete admixtures, and specifically relates to a shrinkage reducing agent and a preparation method and application thereof. Background Art
[0002] Concrete has the advantages of excellent working performance and durability, wide sources of raw materials, and low cost. However, the brittleness and shrinkage of concrete lead to cracks inside it, which not only reduces the strength of concrete, but also affects the durability of concrete. Relevant surveys have found that the problem of concrete cracking is widely present in transportation construction projects such as bridge decks and highways, as well as in port engineering structures, civil buildings and commercial buildings. Therefore, studying how to reduce concrete shrinkage and improve concrete durability is of great significance to the development of concrete engineering.
[0003] At present, measures such as adding expansion agents, fibers, and shrinkage reducers are often used to solve concrete shrinkage cracking. Expansion agents have strict requirements on curing conditions and the expansion rate is difficult to control; the distribution of fibers in concrete is disorderly and uneven, the compatibility with concrete is poor, and the construction operation is cumbersome. Shrinkage reducers are considered to be one of the most effective measures to control concrete shrinkage cracking. However, simply adding shrinkage reducers also has problems such as poor compatibility with water reducers, low strength, and high engineering application costs.
[0004] Polycarboxylic acid-based water reducers are the third generation of water reducers after lignin and naphthalene-based water reducers, and are gaining more and more attention. Their molecular structure is designable, and by adjusting the main chain polymerization degree, branch chain length, and carboxyl ratio, they can achieve functionalization including shrinkage reduction performance. Currently, there have been reports on the synthesis and performance research of shrinkage-reducing polycarboxylic acid-based water reducers, but they still have defects such as high dosage and poor shrinkage reduction effect. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a shrinkage reducing agent and a preparation method and application thereof. The shrinkage reducing agent is prepared by introducing alcohol shrinkage reducing functional monomers and fibers into the structure of a polycarboxylic acid water-reducing agent. The shrinkage of concrete is inhibited by the synergistic effect of the alcohol shrinkage reducing functional monomers and the fibers.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] A method for preparing a shrinkage reducing agent, the preparation method comprising the following steps:
[0008] (1) subjecting an alcohol-based shrinkage-reducing functional monomer to an esterification reaction with acrylic acid or maleic anhydride to obtain an esterification functional monomer;
[0009] (2) Modifying calcium sulfate fiber with a silane coupling agent containing double bonds to obtain calcium sulfate fiber modified with a silane coupling agent;
[0010] (3) The polyether macromonomer, initiator, solvent, and calcium sulfate fiber solution modified by silane coupling agent are mixed, and the reaction temperature is controlled to be 10-40° C. Then, an aqueous solution A containing unsaturated acid, sodium methyl methacrylate sulfonate, the esterification functional monomer in step (1), and an aqueous solution B containing a reducing agent and a chain transfer agent are added dropwise thereto respectively. After the addition is completed, the mixture is reacted at a constant temperature for 1-2.0 hours, and then the pH is adjusted to 6-7 to obtain the shrinkage reducing agent.
[0011] The step (1) specifically comprises the following steps: under the protection of an inert gas, mixing an alcohol-based shrinkage-reducing functional monomer with acrylic acid or maleic anhydride and stirring for 0.5 to 1.0 h, adding p-aminobenzenesulfonic acid and p-hydroxyanisole, refluxing at 80 to 160° C. for 3 to 15 h, and then performing reduced pressure distillation.
[0012] In step (1), the alcohol shrinkage-reducing functional monomer is any one or more of diethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, and diethylene glycol dipropylene glycol monobutyl ether.
[0013] The esterification reaction of acrylic acid with diethylene glycol dipropylene glycol monobutyl ether is as follows:
[0014]
[0015] The esterification reaction of maleic anhydride and diethylene glycol dipropylene glycol monobutyl ether is as follows:
[0016]
[0017] In step (1), the molar ratio of the alcohol shrinkage-reducing functional monomer and acrylic acid or maleic anhydride is 1.5-5:1; the masses of p-aminobenzenesulfonic acid and p-hydroxyanisole are 1.5-3% and 0.8-1.5% of the sum of the masses of the alcohol shrinkage-reducing functional monomer and acrylic acid or maleic anhydride, respectively.
[0018] The step (2) specifically comprises the following steps: ultrasonically dispersing the calcium sulfate fibers in ethanol, then adding deionized water and a silane coupling agent thereto, stirring and reacting at 50-90° C. for 12-24 hours, and then filtering, washing, drying and crushing.
[0019] In step (2), the ethanol is anhydrous ethanol.
[0020] In step (2), the double bond-containing silane coupling agent is any one or more of γ-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane, and triethoxyvinylsilane.
[0021] In step (2), the calcium sulfate fiber is 30-150 μm long and 500 nm in diameter; the weight of the silane coupling agent is 3-8% of the weight of the calcium sulfate fiber.
[0022] In step (3), the weight parts of the raw materials are: 360-600 parts of polyether macromonomer, 3-8 parts of initiator, 85-160 parts of calcium sulfate fiber solution modified by silane coupling agent, 15-50 parts of unsaturated acid, 20-60 parts of sodium methyl propylene sulfonate, 33-56 parts of esterification functional monomer in step (1), 0.5-2 parts of reducing agent and 1.8-4 parts of chain transfer agent.
[0023] In step (3), the calcium sulfate fiber solution modified by the silane coupling agent is obtained by ultrasonically dispersing the calcium sulfate fiber modified by the silane coupling agent in deionized water; the mass ratio of the calcium sulfate fiber modified by the silane coupling agent to the deionized water is 1:10 to 20, preferably 1:16.
[0024] In step (3), the polyether macromonomer is any one or more of ethylene glycol monovinyl polyethylene glycol ether with a number average molecular weight of 5000-6000, methyl allyl polyoxyethylene ether with a number average molecular weight of 3000-4000, and allyl polyoxyethylene ether with a number average molecular weight of 2000-3000.
[0025] In step (3), the initiator is hydrogen peroxide or ammonium persulfate; the unsaturated acid is acrylic acid; the reducing agent is ascorbic acid; and the chain transfer agent is 3-mercaptopropionic acid.
[0026] In step (3), the aqueous solution A is added dropwise for 1 to 4 hours, and the aqueous solution B is added dropwise for 1 to 4 hours.
[0027] The shrinkage reducing agent prepared by the preparation method of the present invention has a structure in which alcohol shrinkage reducing functional monomers and calcium sulfate fibers are grafted simultaneously.
[0028] The invention also provides application of the shrinkage reducing agent in concrete, which inhibits the shrinkage of concrete through the synergistic effect of the alcohol shrinkage reducing functional monomer and the fiber.
[0029] In the preparation method of the shrinkage reducing agent provided by the present invention, firstly, an alcohol shrinkage reducing functional monomer is subjected to an esterification reaction with acrylic acid or maleic anhydride to obtain an esterified functional monomer. After such monomer is used as a shrinkage reducing agent prepared by a raw material, the hydrophilic group in the alcohol shrinkage reducing functional monomer can firmly fix water molecules on the surface of the hydration product, thereby preventing water evaporation and making it difficult for the capillary meniscus in the cement-based material to form, thereby eliminating or delaying the generation of self-shrinkage; then, calcium sulfate fiber is modified with a silane coupling agent containing a double bond to obtain calcium sulfate fiber modified with a silane coupling agent, so that double bonds can be introduced into the calcium sulfate fiber through modification with a silane coupling agent; finally, after the copolymerization reaction in step (3), a shrinkage reducing agent having both the alcohol shrinkage reducing functional monomer and the calcium sulfate fiber grafted in the structure is obtained, and the shrinkage of concrete is inhibited by the synergistic effect of the alcohol shrinkage reducing functional monomer and the fiber.
[0030] Compared with the prior art, the present invention has the following beneficial effects: the shrinkage reducer provided by the present invention has a shrinkage reducing functional monomer such as the hydrophilic group in the molecule of diethylene glycol dipropylene glycol monobutyl ether, which can firmly fix water molecules on the surface of the hydration product, prevent water evaporation, and make it difficult for the capillary meniscus in the cement-based material to form, thereby eliminating or delaying the generation of self-shrinkage. The incorporation of calcium sulfate fiber can produce a bridging overlap effect in the cracks, play a role in controlling and inhibiting the generation and development of cracks, or reduce the size of the cracks, thereby improving the crack resistance of concrete. At the same time, the present invention grafts calcium sulfate fiber into the structure of polycarboxylate water-reducing agent through a silane coupling agent, so that the calcium sulfate fiber is evenly distributed in the water-reducing agent solution, and evenly distributed in the concrete during the use of the water-reducing agent, solving the problem of disorderly and uneven distribution in concrete and poor compatibility with concrete. DETAILED DESCRIPTION
[0031] The present invention is described in detail below with reference to the embodiments.
[0032] Example 1
[0033] A method for preparing a shrinkage reducing agent comprises the following steps:
[0034] (1) Preparation of esterification functional monomer: In a three-necked flask equipped with a thermometer, a magnetic stirrer and a reflux condenser, a certain amount of maleic anhydride and diethylene glycol dipropylene glycol monobutyl ether were added in a molar ratio of 3:1, and nitrogen was introduced while stirring for 0.5 h. Then, 2% of p-aminobenzenesulfonic acid and 1% of p-hydroxyanisole were added, and the mixture was heated to 80° C. and refluxed with stirring. The mixture was reacted for 15 h until no water was produced, and the reaction was stopped. Then, the mixture was distilled under reduced pressure at 45° C. and cooled to obtain a light yellow viscous liquid, which was the esterification functional monomer.
[0035] (2) Preparation of calcium sulfate fiber modified by silane coupling agent: 5 g of calcium sulfate fiber was weighed and placed in a 300 mL beaker, and 180 mL of anhydrous ethanol was added to the beaker at the same time. The calcium sulfate fiber-ethanol solution in the beaker was ultrasonicated for 30 min to make the calcium sulfate fiber evenly dispersed in the ethanol. Then 20 mL of deionized water and KH-570 with a mass ratio of 3% of the calcium sulfate fiber were added to the calcium sulfate fiber-ethanol solution. The mixed suspension was placed on a heat-collecting magnetic stirrer and magnetically stirred for 24 h in a water bath at 50° C. After the reaction, the solution was filtered with a circulating water vacuum pump, and the filter cake was repeatedly rinsed with anhydrous ethanol and dried at 40° C. for 8 h to obtain calcium sulfate fiber modified with KH-570. Finally, the obtained KH-570-modified calcium sulfate fiber was ground with a mortar, passed through a 250-mesh sieve, and sealed for storage. Before use, 5 g of The KH-570 modified calcium sulfate fiber was placed in 80 g of water and ultrasonicated for 30 min to make it evenly distributed in the aqueous solution to obtain a KH-570 modified calcium sulfate fiber solution;
[0036] (3) Copolymerization: 15 parts of acrylic acid, 45 parts of sodium methacrylic acid, and 35 parts of the esterification functional monomer in step (1) were added to 105 parts of deionized water to prepare a mixed solution A; 0.8 parts of ascorbic acid and 1.8 parts of 3-mercaptopropionic acid were added to 56 parts of deionized water to prepare a mixed solution B. 400 parts of methyl allyl polyoxyethylene ether with a number average molecular weight of 3000-4000, 7 parts of hydrogen peroxide, 350 parts of water, and 85 parts of KH-570 modified calcium sulfate fiber solution were added to a four-necked bottle equipped with a stirrer and a thermometer, and the reaction temperature was controlled to be 25°C. At the same time, the mixed solution A and the mixed solution B were added dropwise, and the dropping time of the mixed solution A was 2.5 hours, and the dropping time of the mixed solution B was 3 hours. After the dropping was completed, the reaction was carried out at a constant temperature for 2 hours; after the reaction was completed, the reaction product was cooled to room temperature, and a 30% mass concentration of sodium hydroxide solution was added to adjust the pH value to 6-7, and the shrinkage reducing agent was obtained.
[0037] Example 2
[0038] A method for preparing a shrinkage reducing agent comprises the following steps:
[0039] (1) Preparation of esterification functional monomer: In a three-necked flask equipped with a thermometer, a magnetic stirrer and a reflux condenser, a certain amount of maleic anhydride and diethylene glycol dipropylene glycol monobutyl ether were added in a molar ratio of 3:1, and stirred for 0.5 h while introducing nitrogen, and then 2% of p-aminobenzenesulfonic acid and 1% of p-hydroxyanisole were added to the total mass of maleic anhydride and diethylene glycol dipropylene glycol monobutyl ether, and the mixture was heated to 100° C. and refluxed with stirring, and reacted for 12 h until no water was produced, and then the reaction was stopped, and then vacuum distillation was carried out at 45° C., and the material was cooled and discharged to obtain a light yellow viscous liquid, which is the esterification functional monomer;
[0040] (2) Preparation of calcium sulfate fiber modified by silane coupling agent: 5 g of calcium sulfate fiber was weighed and placed in a 300 mL beaker, and 180 mL of anhydrous ethanol was added to the beaker at the same time. The calcium sulfate fiber-ethanol solution in the beaker was ultrasonicated for 30 min to make the calcium sulfate fiber evenly dispersed in the ethanol. Then 20 mL of deionized water and KH-570, which accounted for 5% of the mass of calcium sulfate fiber, were added to the calcium sulfate fiber-ethanol solution. The mixed suspension was placed on a heat-collecting magnetic stirrer and magnetically stirred for 21 h in a water bath at 60° C. After the reaction, the solution was filtered with a circulating water vacuum pump, and the filter cake was repeatedly rinsed with anhydrous ethanol and dried at 40° C. for 8 h to obtain calcium sulfate fiber modified with KH-570. Finally, the obtained KH-570-modified calcium sulfate fiber was ground with a mortar, passed through a 250-mesh sieve, and sealed for storage. Before use, 5 g of The KH-570 modified calcium sulfate fiber was placed in 80 g of water and ultrasonicated for 30 min to make it evenly distributed in the aqueous solution to obtain a KH-570 modified calcium sulfate fiber solution;
[0041] (3) Copolymerization: 20 parts of acrylic acid, 33 parts of sodium methacrylic acid, and 35 parts of the esterification functional monomer in step (1) were added to 105 parts of deionized water to prepare a mixed solution A; 0.8 parts of ascorbic acid and 1.8 parts of 3-mercaptopropionic acid were added to 56 parts of deionized water to prepare a mixed solution B. 360 parts of ethylene glycol monovinyl polyglycol ether with a number average molecular weight of 5000-6000, 5 parts of hydrogen peroxide, 300 parts of water and 85 parts of KH-570 modified calcium sulfate fiber solution were added to a four-necked bottle equipped with a stirrer and a thermometer, and the reaction temperature was controlled to be 30°C. At the same time, the mixed solution A and the mixed solution B were added dropwise, the dropping time of the mixed solution A was 1.0h, and the dropping time of the mixed solution B was 1.5h. After the dropping was completed, the reaction was carried out at a constant temperature for 2h; after the reaction was completed, the reaction product was cooled to room temperature, and a 30% mass concentration of sodium hydroxide solution was added to adjust the pH value to 6-7, so as to obtain a shrinkage reducing agent.
[0042] Example 3
[0043] A method for preparing a shrinkage reducing agent comprises the following steps:
[0044] (1) Preparation of esterification functional monomer: In a three-necked flask equipped with a thermometer, a magnetic stirrer and a reflux condenser, a certain amount of maleic anhydride and diethylene glycol monobutyl ether were added in a molar ratio of 3:1, and stirred for 0.5 h while passing nitrogen gas. Then, 2% of p-aminobenzenesulfonic acid and 1% of p-hydroxyanisole were added, and the mixture was heated to 120° C. and refluxed with stirring. The reaction was continued for 9 h until no water was produced, and the reaction was stopped. Then, the mixture was distilled under reduced pressure at 45° C., cooled and discharged to obtain a light yellow viscous liquid, which was the esterification functional monomer;
[0045] (2) Preparation of calcium sulfate fiber modified by silane coupling agent: 5 g of calcium sulfate fiber was weighed and placed in a 300 mL beaker, and 180 mL of anhydrous ethanol was added to the beaker at the same time. The calcium sulfate fiber-ethanol solution in the beaker was ultrasonicated for 30 min to make the calcium sulfate fiber evenly dispersed in the ethanol. Then 20 mL of deionized water and KH-570, which accounted for 8% of the mass of calcium sulfate fiber, were added to the calcium sulfate fiber-ethanol solution. The mixed suspension was placed on a heat-collecting magnetic stirrer and magnetically stirred for 18 h in a water bath at 70° C. After the reaction, the solution was filtered with a circulating water vacuum pump, and the filter cake was repeatedly rinsed with anhydrous ethanol and dried at 40° C. for 8 h to obtain calcium sulfate fiber modified with KH-570. Finally, the obtained KH-570-modified calcium sulfate fiber was ground with a mortar, passed through a 250-mesh sieve, and sealed for storage. Before use, 5 g of The KH-570 modified calcium sulfate fiber was placed in 80 g of water and ultrasonicated for 30 min to make it evenly distributed in the aqueous solution to obtain a KH-570 modified calcium sulfate fiber solution;
[0046] (3) Copolymerization: 25 parts of acrylic acid, 45 parts of sodium methacrylic acid, and 56 parts of the esterification functional monomer in step (1) were added to 105 parts of deionized water to prepare a mixed solution A; 1.5 parts of ascorbic acid and 2.5 parts of 3-mercaptopropionic acid were added to 75 parts of deionized water to prepare a mixed solution B. 380 parts of allyl polyoxyethylene ether with a number average molecular weight of 2000-3000, 4 parts of ammonium persulfate, 400 parts of water and 85 parts of KH-570 modified calcium sulfate fiber solution were added to a four-necked bottle equipped with a stirrer and a thermometer, and the reaction temperature was controlled to be 40°C. Mixed solution A and mixed solution B were added dropwise at the same time. The dropping time of mixed solution A was 3.5 hours, and the dropping time of mixed solution B was 4 hours. After the dropping was completed, the reaction was carried out at a constant temperature for 2 hours. After the reaction was completed, the reaction product was cooled to room temperature, and a 30% mass concentration of sodium hydroxide solution was added to adjust the pH value to 6-7 to obtain a shrinkage reducing agent.
[0047] Example 4
[0048] A method for preparing a shrinkage reducing agent comprises the following steps:
[0049] (1) Preparation of esterification functional monomer: A certain amount of maleic anhydride and tetraethylene glycol monomethyl ether in a molar ratio of 3:2 were added to a three-necked flask equipped with a thermometer, a magnetic stirrer and a reflux condenser, and nitrogen was introduced while stirring for 0.5 h. Then, 2% of p-aminobenzenesulfonic acid and 1% of p-hydroxyanisole were added, and the mixture was heated to 140° C. and refluxed with stirring. The mixture was reacted for 6 h until no water was produced, and the reaction was stopped. Then, the mixture was distilled under reduced pressure at 45° C., cooled and discharged to obtain a light yellow viscous liquid, which was the esterification functional monomer;
[0050] (2) Preparation of calcium sulfate fiber modified by silane coupling agent: 10 g of calcium sulfate fiber was weighed and placed in a 300 mL beaker, and 180 mL of anhydrous ethanol was added to the beaker. The calcium sulfate fiber-ethanol solution in the beaker was ultrasonicated for 30 min to make the calcium sulfate fiber evenly dispersed in the ethanol. Then, 20 mL of deionized water and KH-570 (5% by weight of the calcium sulfate fiber) were added to the calcium sulfate fiber-ethanol solution. The mixed suspension was placed on a heat-collecting magnetic stirrer, placed in a water bath at 80°C, and magnetically stirred for 15 hours. After the reaction, the solution was filtered with a circulating water vacuum pump, the filter cake was repeatedly washed with anhydrous ethanol, and dried at 40°C for 8 hours to obtain calcium sulfate fiber modified with KH-570. Finally, the obtained KH-570 modified calcium sulfate fiber was ground with a mortar, passed through a 250-mesh sieve, and sealed for storage. Before use, 5g of KH-570 modified calcium sulfate fiber was placed in 80g of water and ultrasonicated for 30 minutes to make it evenly distributed in the aqueous solution to obtain a KH-570 modified calcium sulfate fiber solution;
[0051] (3) Copolymerization: 20 parts of acrylic acid, 33 parts of sodium methacrylic acid, 35 parts of the alcohol shrinkage-reducing functional monomer synthesized by esterification in step (1) are added to 120 parts of water to prepare mixed solution A, and 0.8 parts of ascorbic acid and 1.8 parts of 3-mercaptopropionic acid are added to 56 parts of water to prepare mixed solution B. 360 parts of ethylene glycol monovinyl polyglycol ether with a number average molecular weight of 5000-6000, 5 parts of hydrogen peroxide, 300 parts of deionized water and 85 parts of KH-570 modified calcium sulfate fiber solution are added to a four-necked bottle equipped with a stirrer and a thermometer; the reaction temperature is controlled to be 10°C, and mixed solution A and mixed solution B are added dropwise at the same time, the dropwise addition time of mixed solution A is 1 hour, and the dropwise addition time of mixed solution B is 1.5 hours. After the dropwise addition is completed, the reaction is carried out at a constant temperature for 1 hour; after the reaction is completed, the reaction product is cooled to room temperature, and a concentrated sodium hydroxide solution is added to adjust the pH value to 6-7 to obtain a shrinkage-reducing agent.
[0052] Example 5
[0053] A method for preparing a shrinkage reducing agent comprises the following steps:
[0054] (1) Preparation of esterification functional monomer: In a three-necked flask equipped with a thermometer, a magnetic stirrer and a reflux condenser, a certain amount of acrylic acid and tetraethylene glycol monomethyl ether were added in a molar ratio of 3:2, and nitrogen was introduced while stirring for 0.5 h. Then, 2% of p-aminobenzenesulfonic acid and 1% of p-hydroxyanisole were added based on the total mass of acrylic acid and tetraethylene glycol monomethyl ether. The mixture was heated to 140° C. and refluxed with stirring. The reaction was continued for 3 h until no water was produced. The reaction was stopped, and then vacuum distillation was performed at 45° C. The material was cooled and discharged to obtain a light yellow viscous liquid, which was the esterification functional monomer;
[0055] (2) Preparation of calcium sulfate fiber modified by silane coupling agent: 10 g of calcium sulfate fiber was weighed and placed in a 300 mL beaker, and 180 mL of anhydrous ethanol was added to the beaker at the same time. The calcium sulfate fiber-ethanol solution in the beaker was ultrasonicated for 30 min to make the calcium sulfate fiber evenly dispersed in the ethanol. Then 20 mL of deionized water and KH-570, which accounted for 8% of the mass of calcium sulfate fiber, were added to the calcium sulfate fiber-ethanol solution. The mixed suspension was placed on a heat-collecting magnetic stirrer and magnetically stirred for 12 h in a water bath at 90° C. After the reaction, the solution was filtered with a circulating water vacuum pump, and the filter cake was repeatedly rinsed with anhydrous ethanol and dried at 40° C. for 8 h to obtain calcium sulfate fiber modified with KH-570. Finally, the obtained KH-570-modified calcium sulfate fiber was ground with a mortar, passed through a 250-mesh sieve, and sealed for storage. Before use, 5 g of The KH-570 modified calcium sulfate fiber was placed in 80 g of water and ultrasonicated for 30 min to make it evenly distributed in the aqueous solution to obtain a KH-570 modified calcium sulfate fiber solution;
[0056] (3) Copolymerization: 20 parts of acrylic acid, 33 parts of sodium methacrylic acid, 35 parts of alcohol shrinkage-reducing functional monomer synthesized by esterification in step (1) were added to 120 parts of water to prepare mixed solution A, and 0.8 parts of ascorbic acid and 1.8 parts of 3-mercaptopropionic acid were added to 56 parts of water to prepare mixed solution B. 360 parts of ethylene glycol monovinyl polyglycol ether with a number average molecular weight of 5000-6000, 5 parts of hydrogen peroxide, 300 parts of water and 85 parts of KH-570 modified calcium sulfate fiber solution were added to a four-necked bottle equipped with a stirrer and a thermometer; the reaction temperature was controlled to be 15°C, and mixed solution A and mixed solution B were added dropwise at the same time, the dropping time of mixed solution A was 1 hour, and the dropping time of mixed solution B was 1.5 hours. After the dropping was completed, the reaction was carried out at a constant temperature for 1 hour; after the reaction was completed, the reaction product was cooled to room temperature, and a concentrated sodium hydroxide solution was added to adjust the pH value to 6-7, thereby obtaining a shrinkage-reducing agent.
[0057] Comparative Example 1
[0058] The rest is the same as Example 1, except that step (2) is omitted and the KH-570 modified calcium sulfate fiber solution in step (3) is replaced by an equal amount of calcium sulfate whisker solution, wherein the calcium sulfate whisker solution is obtained by placing 5 g of calcium sulfate whisker in 80 g of water and ultrasonicating for 30 min.
[0059] Comparative Example 2
[0060] The other steps are the same as those in Example 1, except that step (1) is omitted and the unesterified alcohol shrinkage-reducing functional monomer is directly added to step (3). The alcohol shrinkage-reducing functional monomer is only used as a shrinkage-reducing material in this comparative example and does not participate in the polymerization reaction of the water reducer.
[0061] Standard cement was used to test the shrinkage ratio and other properties of C50 concrete according to the standard GB8076-2008 "Concrete Admixtures". The results are shown in Table 1.
[0062] Table 1
[0063]
[0064]
[0065] It can be seen from the table that the synthetic shrinkage-reducing agent of the present invention has good dispersibility when applied in concrete, can significantly reduce the drying shrinkage rate of concrete, reduce the surface tension of the solution, and improve the compressive strength of concrete.
[0066] The detailed description of a shrinkage reducing agent and its preparation method and application with reference to the above-mentioned embodiments is illustrative rather than restrictive, and several embodiments can be listed according to the limited scope. Therefore, changes and modifications without departing from the overall concept of the present invention should fall within the scope of protection of the present invention.
Claims
1. A method for preparing a shrinkage reducing agent, characterized in that: The preparation method comprises the following steps: (1) subjecting an alcohol-based shrinkage-reducing functional monomer to an esterification reaction with acrylic acid or maleic anhydride to obtain an esterification functional monomer; (2) Modifying calcium sulfate fiber with a silane coupling agent containing double bonds to obtain calcium sulfate fiber modified with a silane coupling agent; (3) mixing a polyether macromonomer, an initiator, a solvent, and a calcium sulfate fiber solution modified by a silane coupling agent, controlling the reaction temperature to be 10 to 40° C., and then simultaneously adding dropwise the unsaturated acid, sodium methyl methacrylate sulfonate, an aqueous solution A of the esterification functional monomer in step (1), and an aqueous solution B containing a reducing agent and a chain transfer agent, and reacting at a constant temperature for 1 to 2.0 hours after the addition is complete, and then adjusting the pH to 6 to 7, to obtain the shrinkage reducing agent; In step (1), the alcohol shrinkage-reducing functional monomer is any one or more of diethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, and diethylene glycol dipropylene glycol monobutyl ether.
2. The preparation method according to claim 1, characterized in that: The step (1) specifically comprises the following steps: under the protection of an inert gas, mixing an alcohol-based shrinkage-reducing functional monomer with acrylic acid or maleic anhydride and stirring for 0.5 to 1.0 h, adding p-aminobenzenesulfonic acid and p-hydroxyanisole, refluxing at 80 to 160° C. for 3 to 15 h, and then performing reduced pressure distillation.
3. The preparation method according to claim 1, characterized in that: The step (2) specifically comprises the following steps: ultrasonically dispersing the calcium sulfate fibers in ethanol, then adding deionized water and a silane coupling agent thereto, stirring and reacting at 50-90° C. for 12-24 hours, and then filtering, washing, drying and crushing.
4. The preparation method according to claim 1 or 3, characterized in that: In step (2), the double bond-containing silane coupling agent is any one or more of γ-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane, and triethoxyvinylsilane.
5. The preparation method according to claim 1 or 3, characterized in that: In step (2), the calcium sulfate fiber is 30-150 μm long and 500 nm in diameter; the weight of the silane coupling agent is 3-8% of the weight of the calcium sulfate fiber.
6. The preparation method according to claim 1, 2 or 3, characterized in that: In step (3), the weight parts of the raw materials are: 360-600 parts of polyether macromonomer, 3-8 parts of initiator, 85-160 parts of calcium sulfate fiber solution modified by silane coupling agent, 15-50 parts of unsaturated acid, 20-60 parts of sodium methyl propylene sulfonate, 33-56 parts of esterification functional monomer in step (1), 0.5-2 parts of reducing agent and 1.8-4 parts of chain transfer agent.
7. The preparation method according to claim 1, characterized in that: In step (3), the polyether macromonomer is any one or more of ethylene glycol monovinyl polyethylene glycol ether with a number average molecular weight of 5000-6000, methyl allyl polyoxyethylene ether with a number average molecular weight of 3000-4000, and allyl polyoxyethylene ether with a number average molecular weight of 2000-3000.
8. The shrinkage reducing agent prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the shrinkage reducing agent as claimed in claim 8 in concrete.