A molten salt electrochemical method for preparing silver silicon nanowires based on silver mirror reaction

Through the molten salt electrochemical method based on silver mirror reaction, nanoscale silver particles were introduced into silica to prepare silver silicon nanowire structure, which solved the problem of volume expansion and poor conductivity of silicon battery materials when storing lithium, and significantly improved the Performance and stability of lithium-ion batteries.

CN115404498BActive Publication Date: 2024-11-29JIANGSU BAOLI TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211042798.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-29
Publication Date
2024-11-29
Estimated Expiration
2042-08-29

AI Technical Summary

Technical Problem

As the negative electrode material of lithium-ion batteries, silicon has huge volume expansion effects, material stress changes, continuous generation of SEI films and "dead lithium" problems when storing lithium, resulting in low efficiency of the battery for the first time and serious cycle life attenuation.

Method used

Through the molten salt electrochemical method based on silver mirror reaction, nanoscale silver particles were introduced into silica to prepare a silver-silicon nanowire structure with silver-silicon composite material. The method is easy to obtain raw materials and short process flow. Silver-silicon composite materials are prepared by adjusting electrolytic parameters.

Benefits of technology

This method effectively alleviates the volume changes of silver silicon nanowires during charging and discharging, significantly improves the stability and rate performance of lithium-ion batteries, and reduces production costs and process complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115404498B_ABST
    Figure CN115404498B_ABST
Patent Text Reader

Abstract

The present invention relates to a molten salt electrochemical method for preparing silver silicon nanowires based on silver mirror reaction, and belongs to the technical field of non-ferrous metal metallurgy. Ultrapure water and CTAB solution are added to monodisperse spherical silicon dioxide powder to obtain a hydrosol; a silver ammonia solution is prepared; the silver ammonia solution is added to the hydrosol, and after sufficient magnetic stirring, a glucose solution is added to react to obtain a SiO2 / Ag composite material; the SiO2 / Ag composite material is added with a binder polyvinyl alcohol, ground and mixed, and pressed to obtain an electrolytic raw material; the obtained electrolytic raw material is sintered in an argon atmosphere to obtain an electrolytic cathode; graphite is used as an anode, and is placed in a molten salt electrolyte for electrolysis. After the electrolysis is completed, an electrolytic product is obtained on the cathode, and the electrolytic product is soaked, pickled, filtered, and vacuum dried to obtain a silver silicon nanowire. The product prepared by the present invention is a silver silicon composite material with a one-dimensional nanowire structure. It can effectively alleviate the volume expansion effect when used as a negative electrode of a lithium ion battery, thereby obtaining better battery performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a molten salt electrochemical method for preparing silver silicon nanowires based on a silver mirror reaction, and belongs to the technical field of nonferrous metal metallurgy. Background Art

[0002] With the adjustment of the national energy strategic layout and the energy revolution led by the national strategic carbon reduction goals of "carbon peak" and "carbon neutrality", advanced energy storage technology has gradually become an important indicator for promoting structural reforms on the energy supply side, demonstrating national strength, and enhancing international competitiveness. Electrochemical energy storage is the most important means of energy storage, among which lithium-ion batteries have the highest share and are widely used in electronic products, new energy vehicles, power grids and other fields. The key to promoting the progress of high-energy, safe and long-life lithium-ion batteries lies in the preparation of high-performance battery materials. At present, due to its extremely high lithium storage capacity (3972 mAh / g, Li15Si4), suitable discharge platform (<0.5 V) and abundant reserves, silicon is considered to be the champion material for replacing commercial graphite anodes and effectively improving the energy density of lithium-ion battery cells. However, when storing lithium, silicon produces a huge volume expansion effect (>300%), which causes material stress changes and induces silicon core rupture, resulting in the continuous formation of SEI (Solid Electrolyte Interface) film and "dead lithium" that remains in the silicon lattice and cannot escape. The consumption of lithium in the above process is irreversible, resulting in low initial coulomb efficiency of silicon negative electrode and serious cycle life decay. The intrinsic conductivity of silicon at room temperature is low (about 10 -5 – 10 -3 S / cm) and the low diffusion rate of lithium in silicon (the diffusion coefficient is only 10 -14 – 10 -13 cm 2 / s), resulting in poor rate performance and cycle capacity of silicon negative electrode. Therefore, the defects of silicon itself induce short cycle life and low efficiency of batteries, which seriously restricts commercial applications and is a problem that must be faced and urgently solved.

[0003] In order to solve the problem of poor conductivity and volume expansion of silicon, and to overcome the problem of unstable material structure during lithium insertion and extraction, researchers have conducted extensive and in-depth modification research on silicon materials by nano-sizing, alloying, and compounding. One-dimensional linear nanomaterials can alleviate irreversible volume changes and provide a shorter lithium ion diffusion path. The addition of metals can increase the conductivity of silicon materials, which is beneficial to the improvement of battery performance. At present, the main methods for preparing silicon nanomaterials and alloying and compounding silicon materials are: chemical / physical vapor deposition, high-energy ball milling, spray drying, electrospinning, magnesium thermal reduction, sol-gel and other methods. However, the above methods have high equipment requirements, cumbersome processes, low yields, and purity and uniformity are difficult to control, which is not conducive to large-scale commercialization.

[0004] Chinese patent CN103447028B discloses a method for preparing a nano silver core / mesoporous silica shell structure with controllable morphology. The method uses a mixture of a silver trifluoroacetate solution and a tetraethyl orthosilicate solution, and successfully prepares a core-shell nanocomposite of a silver core / silicon dioxide shell structure by a polyol reduction method, but no further electrolysis exploration is conducted; Chinese patent CN110512223B discloses a molten salt electrochemical method for preparing silicon nanotubes without a template. When electrolyzing silicon precursors, metals and metal precursors, such as Au, Ag, Cu, Zn, Fe or one or more of their salts, are mechanically mixed in, and silicon nanotubes with an outer diameter of 80-600nm and a wall thickness of 5-200nm are successfully prepared; although the use of metal elements as electrolytic catalysts is the most effective method, precious metal materials such as Au powder and Ag powder increase the cost and are not conducive to large-scale production. Even if the corresponding metal salts are selected, many factors such as the electrolytic cell voltage and solubility in the molten salt need to be considered. Therefore, the present invention selects silver nitrate as the silver source, introduces silver into the silicon dioxide raw material through a simple silver mirror reaction, greatly reduces the production cost and the complexity of the process, and successfully prepares silver silicon nanowires. This structure is conducive to alleviating the volume change of the battery material during the charging and discharging process, and significantly improves the stability and rate performance of lithium-ion batteries. So far, there has been no relevant report on the molten salt electrochemical method for preparing silver silicon composite materials based on the silver mirror reaction. Summary of the invention

[0005] In view of the problems and shortcomings of the above-mentioned prior art, the present invention provides a molten salt electrochemical method for preparing silver silicon nanowires based on the silver mirror reaction. The method prepares a one-dimensional nano silicon wire with a silver silicon alloy droplet as the growth end, which is used as a negative electrode material for lithium ion batteries. The raw materials of the method are easy to obtain and the process flow is short. Nano-scale silver particles are mixed into SiO2 through a simple silver mirror reaction, and a silver silicon composite material is prepared by adjusting the electrolysis parameters (time, voltage, temperature, material ratio). The present invention is achieved by the following technology.

[0006] A molten salt electrochemical method for preparing silver silicon nanowires based on the silver mirror reaction, the specific steps of which are as follows:

[0007] Step 1, adding ultrapure water and CTAB solution to monodisperse spherical silica powder to form a hydrosol with good dispersibility;

[0008] Step 2, add ammonia water dropwise to the silver nitrate solution until a brown-yellow precipitate is formed, continue to add ammonia water dropwise until the precipitate disappears and the solution becomes transparent, and adjust the volume to prepare a silver ammonia solution with a percentage concentration of 2-5%;

[0009] Step 3, adding the silver ammonia solution obtained in step 2 to the hydrosol in step 1, after sufficient magnetic stirring, adding a glucose solution with a percentage concentration of 2-5%, reacting at 40-60°C, and after the reaction is completed, filtering the solution and vacuum drying to obtain a SiO2 / Ag composite material;

[0010] Step 4, adding the SiO2 / Ag composite material obtained in step 3 to the binder polyvinyl alcohol, grinding and mixing, and pressing and molding to obtain an electrolytic raw material;

[0011] Step 5, sintering the electrolytic raw material obtained in step 4 under an argon atmosphere to obtain an electrolytic cathode;

[0012] Step 6: Using the electrolytic cathode obtained in step 5 as the cathode and graphite as the anode, electrolysis is carried out in a molten salt electrolyte. After the electrolysis is completed, an electrolysis product is obtained on the cathode. The electrolysis product is soaked, pickled, filtered, and vacuum dried to obtain silver silicon nanowires (SiO2 / Ag composite material).

[0013] In the step 1, the diameter of the monodisperse spherical silica is 0.1-1 μm, the concentration of the CTAB solution is 0.03-10 mmol / L, and the solid-liquid ratio of the silica powder to ultrapure water is 1:10-100 g / mL.

[0014] In step 3, the volume ratio of the silver ammonia solution to the hydrosol is 0.2-1.6:1, magnetic stirring is performed for 4-8 hours, and then the reaction is carried out at 40-60° C. for 0.5-1 hour.

[0015] In step 3, the volume ratio of the silver ammonia solution to the glucose solution is 1:1-1:2; the vacuum drying temperature is 50-80°C, and the time is 5-8h.

[0016] In the step 4, the mass ratio of the binder polyvinyl alcohol to the SiO2 / Ag composite material is 30-70:70-30, the grinding and mixing time is 0.5-1h, and the pressing pressure is 10-20mpa.

[0017] In step 5, the sintering temperature is 700-900° C. and the sintering time is 2-5 hours.

[0018] The molten salt electrolyte in step 6 is a mono- or poly-salt mixture of LiCl, KCl, NaCl, CaCl2, and MgCl2 in any proportion; and the electrolysis voltage is 2.4-2.8V.

[0019] In step 6, 1-5 wt % HCl is used for pickling and the reaction is performed for 0.5-1 h; the vacuum drying temperature is 50-80° C.

[0020] The beneficial effects of the present invention are:

[0021] 1. The product prepared by the present invention is a silver-silicon composite material with a one-dimensional nanowire structure, which can effectively alleviate the volume expansion effect when used as a negative electrode of a lithium-ion battery, thereby obtaining better battery performance.

[0022] 2. This method uses the silver mirror reaction to obtain nano silver particles, which reduces the cost of selecting additives; and the nano silver particles increase the cathode conductive sites during the electrolysis process, improve the conductivity, and are conducive to increasing the yield.

[0023] 3. The present invention uses silicon dioxide, which is abundant in source and low in price, as raw material, has a short preparation process, low energy consumption, and the product morphology can be easily controlled by changing the electrolysis parameters. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The XRD diagrams are of the raw materials of the present invention and the prepared SiO2 / Ag and Si / Ag composite materials.

[0025] Figure 2 This is a FESEM image of the SiO2 / Ag composite material prepared in Example 1 of the present invention.

[0026] Figure 3 This is a SEM image of the Si / Ag composite material prepared in Example 1 of the present invention.

[0027] Figure 4 (a) is a TEM image of the Si / Ag composite material prepared in Example 1 of the present invention.

[0028] Figure 4 (b) is an EDS line scan image of the Si / Ag composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0029] The present invention will be further described below in conjunction with the accompanying drawings and specific implementation methods.

[0030] Example 1

[0031] The molten salt electrochemical method for preparing silver silicon nanowires based on the silver mirror reaction has the following specific steps:

[0032] Step 1, adding ultrapure water and 5 mL of CTAB solution to 1 g of monodisperse spherical silica powder to form a hydrosol with good dispersibility; the diameter of the monodisperse spherical silica is 0.2 μm, the concentration of the CTAB solution is 5 mmol / L, and the solid-liquid ratio of the silica powder to the ultrapure water is 1:30 g / mL;

[0033] Step 2, add ammonia water dropwise to the silver nitrate solution until a brown-yellow precipitate is formed, continue to add ammonia water dropwise until the precipitate disappears and the solution becomes transparent, and adjust the volume to prepare a silver ammonia solution with a percentage concentration of 2%;

[0034] Step 3, adding 24 ml of the silver ammonia solution obtained in step 2 to the hydrosol in step 1, after sufficient magnetic stirring, adding a glucose solution with a percentage concentration of 2%, reacting at 60°C, and after the reaction is completed, filtering the solution and vacuum drying to obtain a SiO2 / Ag composite material; the volume ratio of the silver ammonia solution to the hydrosol is 0.2:1, magnetic stirring is performed for 4 hours, and then reacting at 60°C for 0.5 hours, and magnetic stirring is performed at 600r / min; the vacuum drying temperature is 80°C, and the time is 8 hours; the volume ratio of the glucose solution to the silver ammonia solution is 1:1.5;

[0035] Step 4, adding the binder polyvinyl alcohol to the SiO2 / Ag composite material obtained in step 3, grinding and mixing, pressing and molding, and obtaining an electrolytic raw material with a diameter of 19 mm; the mass ratio of the binder polyvinyl alcohol to the SiO2 / Ag composite material is 60:40, the grinding and mixing time is 0.5 h, and the pressing pressure is 10 mpa;

[0036] Step 5, sintering the electrolytic raw material obtained in step 4 under an argon atmosphere to obtain an electrolytic cathode; sintering at 850° C. for 2 hours at a heating rate of 5° C. / min under an argon atmosphere to obtain an electrolytic cathode with a certain mechanical strength;

[0037] Step 6, using the electrolytic cathode obtained in step 5 as the cathode and graphite as the anode, electrolyzing in a CaCl2-NaCl molten salt electrolyte with a molar ratio of 1:1, the electrolysis temperature is 850°C, the electrolysis voltage is 2.8V, the electrolysis time is 6h, and after the electrolysis is completed, an electrolysis product is obtained on the cathode. The electrolysis product is soaked, pickled (5wt% HCl is used for pickling, and the reaction is 0.5h), filtered, and vacuum dried (dried at 80°C for 8h) to obtain silver silicon nanowires (Si / Ag composite materials).

[0038] The XRD patterns of the raw materials and the prepared SiO2 / Ag and Si / Ag composite materials of the present invention are as follows: Figure 1 As shown, from Figure 1 It can be seen that step 3 and step 6 of the present invention can indeed prepare SiO2 / Ag and Si / Ag composite materials.

[0039] The FESEM image of the SiO2 / Ag composite material prepared by the present invention is as follows: Figure 2 As shown, the tiny bright spots are silver particles with a size of 46±15.128 nm, and irregular Ag nanoparticles are dispersed in the SiO2 matrix.

[0040] The SEM image of the Si / Ag composite material prepared by the present invention is as follows: Figure 3 As shown in the TEM image Figure 4 As shown in (a), from Figure 3 and Figure 4It can be seen that the products show linear shapes with different aspect ratios and are cross-stacked. Some linear products have spherical growth ends (diameter 0.6±0.1μm). Figure 4 (b) EDS line scan shows that the spherical growth end is Ag-Si alloy, the main element of the linear product is silicon, and nano-silicon wire.

[0041] Example 2

[0042] The molten salt electrochemical method for preparing silver silicon nanowires based on the silver mirror reaction has the following specific steps:

[0043] Step 1, adding ultrapure water and 5 mL of CTAB solution to 1 g of monodisperse spherical silica powder to form a well-dispersed hydrosol; the diameter of the monodisperse spherical silica is 0.1 μm, the concentration of the CTAB solution is 0.03 mmol / L, and the solid-liquid ratio of the silica powder to the ultrapure water is 1:100 g / mL;

[0044] Step 2, add ammonia water dropwise to the silver nitrate solution until a brown-yellow precipitate is formed, continue to add ammonia water dropwise until the precipitate disappears and the solution becomes transparent, and adjust the volume to prepare a silver ammonia solution with a percentage concentration of 5%;

[0045] Step 3, adding the silver ammonia solution obtained in step 2 to the hydrosol in step 1, after sufficient magnetic stirring, adding a glucose solution with a percentage concentration of 5%, reacting at 50°C, and after the reaction is completed, filtering the solution and vacuum drying to obtain a SiO2 / Ag composite material; the volume ratio of the silver ammonia solution to the hydrosol is 1.6:1, magnetic stirring is performed for 8 hours, and then reacting at 50°C for 0.8 hours, and magnetic stirring is performed at 600r / min; the vacuum drying temperature is 50°C, and the time is 5 hours; the volume ratio of the glucose solution to the silver ammonia solution is 1:2;

[0046] Step 4, adding the binder polyvinyl alcohol to the SiO2 / Ag composite material obtained in step 3, grinding and mixing, pressing and molding, and obtaining an electrolytic raw material with a diameter of 19 mm; the mass ratio of the binder polyvinyl alcohol to the SiO2 / Ag composite material is 30:70, the grinding and mixing time is 1 hour, and the pressing pressure is 20 MPa;

[0047] Step 5, sintering the electrolytic raw material obtained in step 4 under an argon atmosphere to obtain an electrolytic cathode; sintering at 700° C. for 5 hours at a heating rate of 5° C. / min under an argon atmosphere to obtain an electrolytic cathode with a certain mechanical strength;

[0048] Step 6, using the electrolytic cathode obtained in step 5 as the cathode and graphite as the anode, electrolyzing in a LiCl-KCL-MgCl2 molten salt electrolyte with a molar ratio of 1:1:1, the electrolysis temperature is 800°C, the electrolysis voltage is 2.8V, the electrolysis time is 6h, and after the electrolysis is completed, an electrolysis product is obtained on the cathode. The electrolysis product is soaked, pickled (1wt% HCl is used for pickling, and the reaction is 0.5h), filtered, and vacuum dried (dried at 80°C for 8h) to obtain silver silicon nanowires (Si / Ag composite materials).

[0049] Example 3

[0050] The molten salt electrochemical method for preparing silver silicon nanowires based on the silver mirror reaction has the following specific steps:

[0051] Step 1, adding ultrapure water and 5 mL of CTAB solution to 1 g of monodisperse spherical silica powder to form a well-dispersed hydrosol; the diameter of the monodisperse spherical silica is 1 μm, the concentration of the CTAB solution is 10 mmol / L, and the solid-liquid ratio of the silica powder to the ultrapure water is 1:10 g / mL;

[0052] Step 2, add ammonia water dropwise to the silver nitrate solution until a brown-yellow precipitate is formed, continue to add ammonia water until the precipitate disappears and the solution becomes transparent, and adjust the volume to prepare a silver ammonia solution with a percentage concentration of 4%;

[0053] Step 3, adding the silver ammonia solution obtained in step 2 to the hydrosol in step 1, after sufficient magnetic stirring, adding a glucose solution with a percentage concentration of 3%, reacting at 40°C, and filtering the solution after the reaction, vacuum drying to obtain a SiO2 / Ag composite material; the volume ratio of the silver ammonia solution to the hydrosol is 1.0:1, magnetic stirring is performed for 8 hours, and then reacting at 40°C for 1 hour, and magnetic stirring is performed at 600r / min; the vacuum drying temperature is 70°C, and the time is 6 hours; the volume ratio of the glucose solution to the silver ammonia solution is 1:1;

[0054] Step 4, adding the binder polyvinyl alcohol to the SiO2 / Ag composite material obtained in step 3, grinding and mixing, pressing and molding, and obtaining an electrolytic raw material with a diameter of 19 mm; the mass ratio of the binder polyvinyl alcohol to the SiO2 / Ag composite material is 70:30, the grinding and mixing time is 0.8 h, and the pressing pressure is 18 MPa;

[0055] Step 5, sintering the electrolytic raw material obtained in step 4 under an argon atmosphere to obtain an electrolytic cathode; sintering at 900° C. for 4 hours at a heating rate of 5° C. / min under an argon atmosphere to obtain an electrolytic cathode with a certain mechanical strength;

[0056] Step 6, using the electrolytic cathode obtained in step 5 as the cathode and graphite as the anode, electrolyzing in a KCl-CaCl2 molten salt electrolyte with a molar ratio of 1:1, the electrolysis temperature is 700°C, the electrolysis voltage is 2.6V, and the electrolysis time is 6h. After the electrolysis is completed, an electrolysis product is obtained on the cathode. The electrolysis product is soaked, pickled (3wt% HCl is used for pickling, and the reaction is 0.8h), filtered, and vacuum dried (dried at 70°C for 8h) to obtain silver silicon nanowires (Si / Ag composite materials).

[0057] The specific implementation modes of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.

Claims

1. A molten salt electrochemical method for preparing silver silicon nanowires based on the silver mirror reaction, characterized in that The specific steps are as follows: Step 1, adding ultrapure water and CTAB solution to monodisperse spherical silica powder to form a hydrosol with good dispersibility; Step 2, add ammonia water dropwise to the silver nitrate solution until a brown-yellow precipitate is formed, continue to add ammonia water dropwise until the precipitate disappears and the solution becomes transparent, and adjust the volume to prepare a silver ammonia solution with a percentage concentration of 2-5%; Step 3, adding the silver ammonia solution obtained in step 2 to the hydrosol in step 1, after sufficient magnetic stirring, adding a glucose solution with a percentage concentration of 2-5%, reacting at 40-60° C., and after the reaction is completed, filtering the solution and vacuum drying to obtain a SiO2 / Ag composite material; Step 4, adding the SiO2 / Ag composite material obtained in step 3 to the binder polyvinyl alcohol, grinding and mixing, and pressing and molding to obtain an electrolytic raw material; Step 5, sintering the electrolytic raw material obtained in step 4 under an argon atmosphere to obtain an electrolytic cathode; Step 6, using the electrolytic cathode obtained in step 5 as the cathode and graphite as the anode, placing them in a molten salt electrolyte for electrolysis, obtaining an electrolysis product on the cathode after the electrolysis is completed, and soaking, acid washing, filtering, and vacuum drying the electrolysis product to obtain silver silicon nanowires; In the step 1, the diameter of the monodisperse spherical silica is 0.1-1 μm, the concentration of the CTAB solution is 0.03-10 mmol / L, and the solid-liquid ratio of the silica powder to ultrapure water is 1:10-100 g / mL.

2. The molten salt electrochemical method for preparing silver silicon nanowires based on the silver mirror reaction according to claim 1, characterized in that: In step 3, the volume ratio of the silver ammonia solution to the hydrosol is 0.2-1.6:1, magnetic stirring is performed for 4-8 hours, and then the reaction is performed at 40-60° C. for 0.5-1 hour.

3. The molten salt electrochemical method for preparing silver silicon nanowires based on the silver mirror reaction according to claim 1, characterized in that: In step 3, the volume ratio of the silver ammonia solution to the glucose solution is 1:1-1:2; the vacuum drying temperature is 50-80°C, and the time is 5-8h.

4. The molten salt electrochemical method for preparing silver silicon nanowires based on the silver mirror reaction according to claim 1, characterized in that: In the step 4, the mass ratio of the binder polyvinyl alcohol to the SiO2 / Ag composite material is 30-70:70-30, the grinding and mixing time is 0.5-1h, and the pressing pressure is 10-20mpa.

5. The molten salt electrochemical method for preparing silver silicon nanowires based on the silver mirror reaction according to claim 1, characterized in that: In step 5, the sintering temperature is 700-900° C. and the sintering time is 2-5 hours.

6. The molten salt electrochemical method for preparing silver silicon nanowires based on the silver mirror reaction according to claim 1, characterized in that: The molten salt electrolyte in step 6 is a mono- or poly-salt mixture of LiCl, KCl, NaCl, CaCl2, and MgCl2 in any proportion; and the electrolysis voltage is 2.4-2.8V.

7. The molten salt electrochemical method for preparing silver silicon nanowires based on the silver mirror reaction according to claim 1, characterized in that: In step 6, 1-5 wt % HCl is used for pickling and the reaction is performed for 0.5-1 h; the vacuum drying temperature is 50-80° C.

Citation Information

Patent Citations

  • Preparation method of shape-controllable nano silver core / mesoporous silicon dioxide shell structure

    CN103447028B

  • Template-free molten salt electrochemical method for preparing silicon nanotubes

    CN110512223B

  • Preparation method of silicon-silver composite anode material of lithium ion battery and reaction kettle

    CN102709537A

  • Electrochemical methods for making silicon nanopowder, silicon nanowires and silicon nanotubes

    US20110203938A1