Preparation method of iron-doped nickel phosphide rich in phosphorus vacancies and its application in hydrogen production by electrolysis of seawater
Through the iron-doped nickel phosphide material with phosphorus-rich vacancies as a dual-function electrocatalyst, the electrochemical competition problem in the production of hydrogen by seawater electrolysis is solved, and the electrocatalytic effect is achieved with high efficiency, stability and low cost, and the high performance under industrial conditions is met. Current density and long cycle requirements.
Patent Information
- Application Number
- CN202210958698.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-10
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-08-10
Smart Images

Figure HDA0003790522740000011 
Figure HDA0003790522740000012 
Figure HDA0003790522740000021
Abstract
Description
Technical Field
[0001] The invention relates to the field of industrial electrolysis of seawater for hydrogen production, and specifically to a method for preparing iron-doped nickel phosphide rich in phosphorus vacancies and application of the method in electrolysis of seawater for hydrogen production. Background Art
[0002] Hydrogen production by water electrolysis (H 2 ) has 142MJ kg -1 With its high energy density and zero emissions, it is a promising alternative to traditional fossil fuels. Currently, conventional water electrolyzers using pure water as feedstock are not compatible. Therefore, direct seawater electrolysis to produce hydrogen is becoming increasingly attractive. Currently, the most challenging fundamental and technological barrier for direct seawater electrolysis is the electrochemical competition between the oxygen evolution reaction (OER) and the chlorine evolution reaction (ClER) at the anode. Therefore, it is crucial to design cost-effective, stable and efficient electrocatalysts that can deliver high current density at low applied voltages to avoid the CER side reaction in seawater.
[0003] Recently, extensive research activities have been devoted to the development of economical and practical alternatives based on 3d transition metal compounds. In particular, nickel-based phosphides are considered to be one of the best non-precious metal OER and hydrogen evolution reaction (HER) catalysts due to their excellent activity and durability. However, this system still suffers from inherent poor electrical conductivity and large overpotential. To address this problem, it is necessary to develop a bifunctional electrocatalyst that is simple to prepare, cost-effective, stable and efficient. Summary of the invention
[0004] 1. The purpose of the present invention is to provide a method for preparing iron-doped nickel phosphide rich in phosphorus vacancies, and to apply it to the electrolysis of seawater to produce hydrogen. Iron-doped nickel phosphide is grown on a current collector by a molten salt phosphating-assisted method, and phosphorus vacancies are introduced by a sodium borohydride etching method. Compared with the traditional method for preparing bifunctional electrocatalysts, the present invention can maintain catalytic stability under industrial conditions while ensuring efficient catalysis, and has important value in future practical applications.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The preparation method of the iron-doped nickel phosphide electrocatalyst rich in phosphorus vacancies provided by the present invention can be achieved through the following technical route:
[0007] (1) Pretreatment of the current collector: The current collector (nickel foam) was cut into appropriate sizes and immersed in acetone, ethanol, and deionized water for ultrasonic treatment, and then dried in a vacuum oven.
[0008] (2) Preparation of (Fe)NiOOH precursor: FeCl 3 6H 2O and Ni (NO 3 ) 2 6H 2 O is heated to 125-250°C in an oven, and nickel foam is placed therein to react for 1-60 minutes, and then cooled naturally. The nickel foam after the reaction is repeatedly rinsed with deionized water and ethanol and then dried in a vacuum oven.
[0009] (3)Fe-Ni 2 Preparation of P precursor: The reacted nickel foam is placed downstream of a tubular furnace, and the upstream sodium hypophosphite is kept at 300-400°C for 60-180 min, with a heating rate of 2-10°C / min.
[0010] (4)Fe-Ni 2 Preparation of Pv precursor: Soak the nickel foam after reaction in sodium borohydride solution for 30 to 180 minutes. Rinse the nickel foam after reaction repeatedly with deionized water and ethanol and dry it in a vacuum oven.
[0011] The preparation method according to the technical route is characterized in that: in the step (1), the nickel foam is cut into a size of 1 cm*2 cm, immersed in acetone, ethanol, and deionized water for ultrasonic treatment for 10 to 40 minutes respectively, and then dried to remove organic matter and oxides on the surface of the nickel foam.
[0012] The preparation method according to the technical route is characterized in that: in the step (2), FeCl 3 6H 2 O and Ni (NO 3 ) 2 6H 2 The mass ratio of O is (1~4:4~1) to synthesize a microneedle-shaped Fe-NiO(OH) precursor with relatively uniform morphology and size.
[0013] The preparation method according to the technical route is characterized in that the amount of sodium hypophosphite in the step (3) is 0.5 to 2 g.
[0014] The preparation method according to the technical route is characterized in that the concentration of sodium borohydride in step (4) is 0.1-5M.
[0015] The present invention also provides the use of the iron-doped nickel phosphide material rich in phosphorus vacancies described in the above technical route in industrial seawater electrolysis to produce hydrogen.
[0016] As a further feature of the present invention, the iron-doped nickel phosphide material rich in phosphorus vacancies prepared by the above preparation method has excellent electrochemical performance as a bifunctional electrocatalyst for industrial electrolysis of seawater. Under the conditions of industrial electrolysis of seawater (electrolyte: 6M KOH seawater, temperature: 60°C), only a working voltage of 1.77V is required to reach 3A / cm 2The current density can be stably cycled for 100 hours under industrial seawater conditions.
[0017] The present invention provides a method for preparing iron-doped nickel phosphide rich in phosphorus vacancies, and applies the method to electrolyze seawater to produce hydrogen. Iron-doped nickel phosphide is grown on a current collector by a molten salt phosphating-assisted method, and phosphorus vacancies are introduced by a sodium borohydride etching method, and finally an iron-doped nickel phosphide material with rich phosphorus vacancies is prepared. Compared with the traditional method for preparing bifunctional electrocatalysts, the present invention can maintain catalytic stability under industrial conditions while ensuring efficient catalysis, and has important value in future practical applications. DETAILED DESCRIPTION
[0018] The technical features of the present invention are described below in conjunction with specific experimental schemes and drawings, but the present invention is not limited thereto. The experimental methods described in the following examples are conventional methods unless otherwise specified; the instruments and materials described are commercially available unless otherwise specified.
[0019] Example 1
[0020] A phosphorus vacancy-rich iron-doped nickel phosphide material Fe-Ni for electrolysis of seawater to produce hydrogen 2 The synthesis method of Pv comprises the following steps:
[0021] (1) In this embodiment, the nickel foam is cut into 1 cm*2 cm pieces, and the nickel foam is placed in acetone, ethanol and deionized water for ultrasonic treatment for 30 min respectively, and then vacuum dried for later use.
[0022] (2) Weigh 3g Ni(NO 3 ) 2 6H 2 O and 2 g FeCl 3 6H 2 O was placed in a 25 mL glass bottle. The glass bottle was then placed in an oven at 150°C for 20 minutes until the salt melted. The pretreated nickel foam was immersed in the above molten salt for 5 minutes and then naturally cooled. It was rinsed with deionized water and ethanol for several times and then dried to obtain the Ni-FeO(OH) product. The X-ray diffraction (XRD) results of the material are shown in the figure ( Figure 1 ), proving that there is FeO(OH) phase in the material and Ni exists in doped form.
[0023] (3) Mix (Ni)FeOOH (downstream) with 1.5 g NaH 2 PO 2 (upstream) was placed in a tube furnace and heated to 350°C at a heating rate of 2°C / min and maintained at this temperature for 120 min to obtain Fe-Ni 2 P product, the X-ray diffraction (XRD) results of the material are shown in the figure ( Figure 2 ), proving that Ni exists in the material 2 P phase, Fe exists in doped form.
[0024] (4) By 2 P was placed in 0.1 M NaBH 4 The solution was immersed for 60 min to obtain Fe-Ni 2 Pv sample. Finally, Fe-Ni 2 The Pv samples were dried in a vacuum oven at 60 °C. 2 The X-ray diffraction (XRD) results of Pv materials are shown in the figure ( Figure 3 ), the material continues to maintain Fe-Ni 2 In the process of testing the bifunctional electrocatalyst, the conditions of industrial electrolysis of seawater (electrolyte: 6M KOH seawater, temperature: 60°C) were used in this example, and the prepared material was used as the cathode and anode of the two-electrode system electrolyzer. The bifunctional electrocatalyst prepared above only needs an operating voltage of 1.77V to reach 3A / cm 2 The current density ( Figure 4 ), and can circulate stably for 100h under industrial seawater conditions.
[0025] Example 2
[0026] A phosphorus vacancy-rich iron-doped nickel phosphide material Fe-Ni for electrolysis of seawater to produce hydrogen 2 The synthesis method of Pv comprises the following steps:
[0027] (1) In this embodiment, the nickel foam is cut into 1 cm*2 cm pieces, and the nickel foam is placed in acetone, ethanol and deionized water for ultrasonic treatment for 30 min respectively, and then vacuum dried for later use.
[0028] (2) The pretreated nickel foam was mixed with 3gNi(NO 3 ) 2 6H 2 O, 2g FeCl 3 6H 2 O was placed in a 25 mL glass bottle. The glass bottle was then placed in an oven at 150°C for 10 min until the salt melted. The pretreated nickel foam was immersed in the above molten salt for 10 min and then naturally cooled. It was rinsed with deionized water and ethanol for multiple times and then dried to obtain the (Ni)FeOOH product.
[0029] (3) Mix (Ni)FeOOH (downstream) with 1.5 g NaH 2 PO 2(upstream) was placed in a tube furnace and heated to 350°C at a heating rate of 5°C / min and maintained at this temperature for 120 min to obtain Fe-Ni 2 P product.
[0030] (4) By 2 P was placed in 0.3 M NaBH 4 The solution was immersed for 60 min to obtain Fe-Ni 2 Pv sample. Finally, Fe-Ni 2 The Pv sample was dried in a vacuum oven at 60°C. During the bifunctional electrocatalyst test, the material prepared in this example was used as both cathode and anode in a bifunctional electrolyzer. Under the conditions of industrial seawater electrolysis (electrolyte: 6M KOH seawater, temperature: 60°C), only 1.79V of working voltage was required to reach 3A / cm 2 The current density ( Figure 5 ), and can circulate stably for 100h under industrial seawater conditions.
[0031] Example 3
[0032] A phosphorus vacancy-rich iron-doped nickel phosphide material Fe-Ni for electrolysis of seawater to produce hydrogen 2 The synthesis method of Pv comprises the following steps:
[0033] (1) In this embodiment, the nickel foam is cut into 1 cm*2 cm pieces, and the nickel foam is placed in acetone, ethanol and deionized water for ultrasonic treatment for 30 min respectively, and then vacuum dried for later use.
[0034] (2) The pretreated nickel foam was mixed with 2gNi(NO 3 ) 2 6H 2 O, 3g FeCl 3 6H 2 O was placed in a 25 mL glass bottle. The glass bottle was then placed in an oven at 150°C for 10 min until the salt melted. The pretreated nickel foam was immersed in the above molten salt for 10 min and then naturally cooled. It was rinsed with deionized water and ethanol for multiple times and then dried to obtain the (Ni)FeOOH product.
[0035] (3) Mix (Ni)FeOOH (downstream) with 1.5 g NaH 2 PO 2 (upstream) was placed in a tube furnace and heated to 300°C at a heating rate of 5°C / min and maintained at this temperature for 120 min to obtain Fe-Ni 2 P product.
[0036] (4) By 2P was placed in 0.5 M NaBH 4 The solution was immersed for 30 min to obtain Fe-Ni 2 Pv sample. Finally, Fe-Ni 2 The Pv sample was dried in a vacuum oven at 60°C. During the bifunctional electrocatalyst test, the material prepared in this example was used as both cathode and anode in a bifunctional electrolyzer. Under the conditions of industrial seawater electrolysis (electrolyte: 6M KOH seawater, temperature: 60°C), only 1.81V of working voltage was required to reach 3A / cm 2 The current density can be stably cycled for 100h under industrial seawater conditions ( Figure 6 ). BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 : X-ray diffraction pattern of Ni-FeO(OH) obtained in Example 1;
[0038] Figure 2 : Fe-Ni obtained in Example 1 2 X-ray diffraction pattern of P;
[0039] Figure 3 : Fe-Ni obtained in Example 1 2 X-ray diffraction pattern of Pv;
[0040] Figure 4 : Linear sweep voltammetry curve of two electrodes of the dual-function alkaline seawater electrolyzer assembled in Example 1 of the present invention. The X-axis is the working potential (V), and the Y-axis is the current density (A / cm 2 ).
[0041] Figure 5 : Linear sweep voltammetry curve of two electrodes of the dual-function alkaline seawater electrolyzer assembled in Example 2 of the present invention. The X-axis is the working potential (V), and the Y-axis is the current density (A / cm 2 ).
[0042] Figure 6 : The two-electrode chronopotentiometric curve of the dual-function alkaline seawater electrolyzer assembled in Example 3 of the present invention, wherein the X-axis is time (h) and the Y-axis is working potential (V).
Claims
1. A method for preparing an iron-doped nickel phosphide electrocatalyst rich in phosphorus vacancies, characterized in that: The following steps are involved: Step (1): cutting the nickel foam into a size of 1 cm*2 cm, immersing it in acetone, ethanol, and deionized water for ultrasonic treatment for 10 to 40 minutes, and then drying it in a vacuum oven; Step (2): heating FeCl3·6H2O and Ni(NO3)2·6H2O in an oven to 125-250° C., placing nickel foam in the oven to react for 1-60 min, and cooling naturally; after the reaction, the nickel foam is repeatedly rinsed with deionized water and ethanol and dried in a vacuum oven to obtain Fe-NiO(OH); Step (3): placing the nickel foam after the reaction in step (2) at the downstream of a tube furnace, placing sodium hypophosphite at the upstream, heating the temperature to 300-400° C. at a heating rate of 2-10° C. / min, and keeping the temperature for 60-180 min to obtain Fe-Ni2P; Step (4): Soak the nickel foam after the reaction in step (3) in a sodium borohydride solution for 30 to 180 minutes, then rinse it repeatedly with deionized water and ethanol and dry it in a vacuum oven to obtain Fe-Ni2P v ; In the step (2), the mass ratio of FeCl3·6H2O to Ni(NO3)2·6H2O is (1-4:4-1); The amount of sodium hypophosphite in step (3) is 0.5 to 2 g; The concentration of sodium borohydride in step (4) is 0.1-5M.