A compound with anthracenebenzofuran as the core and its application

By introducing fused ring group modification and deuteration treatment into the anthracene benzofuran core compound, new compounds are formed, which solves the problem of insufficient efficiency, life and color purity of existing organic electroluminescent devices, and achieves high efficiency and long life and high color purity luminous performance, suitable for OLED devices and display devices.

CN115417842BActive Publication Date: 2024-11-05SHAANXI PUCHENG HI-TECH NEW MATERIALS IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211222829.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-08
Publication Date
2024-11-05
Estimated Expiration
2042-10-08

AI Technical Summary

Technical Problem

Existing organic electroluminescent devices have shortcomings in efficiency, life and color purity, and it is difficult to meet the requirements of industrial applications.

Method used

By introducing specific fused ring group modification and deuteration treatment into the anthracene benzofuran core compound, a new compound is formed as the host material of the luminescent layer, improving the overall stability and performance of the device.

Benefits of technology

It significantly improves the luminous efficiency, service life and color purity of organic electroluminescent devices, and is suitable for OLED light emitting devices and display devices, showing excellent performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115417842B_ABST
    Figure CN115417842B_ABST
Patent Text Reader

Abstract

The present invention discloses a compound with anthracenebenzofuran as the core, which exhibits excellent performance when used as a main material in the light-emitting layer of an organic electroluminescent device. Specifically, the compound with anthracenebenzofuran as the core provided by the present invention is modified by introducing a specific group or deuterated at a specific position, and the new compound has good rigidity and performance. It has been verified that the compound with anthracenebenzofuran as the core provided by the present invention can significantly improve the performance of the light-emitting device, achieve high efficiency, long life, and excellent color purity, and is widely applicable to use as a light-emitting material in OLED light-emitting devices and display devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic electroluminescent materials, and relates to a compound with anthracenebenzofuran as a core and application thereof in an organic electroluminescent device. Background Art

[0002] Organic electroluminescent elements are developing rapidly as a new type of solid-state light-emitting technology and have gradually been industrialized. Organic electroluminescent elements usually have a structure including an anode, a hole injection layer, a hole transport layer, an electron blocking layer, a light-emitting layer, a hole blocking layer, an electron transport layer, an electron injection layer and a cathode. For such a device structure, holes are usually injected from the anode into the organic layer under the action of an external electric field, and electrons are injected from the cathode into the organic layer. When the injected holes and electrons meet in the light-emitting layer, excitons are formed. When the excitons re-transition to the ground state, they release energy and emit light. In order to improve the efficiency, brightness, life and other optoelectronic properties of the device, it is necessary to continuously improve the organic functional layer materials as described above.

[0003] Anthracenebenzofuran has high thermal stability due to its unique molecular conjugated structure. The material constructed after modification with electron-donating groups can obtain a more appropriate frontier orbital energy level and achieve blue light emission. The device has high efficiency, long life, narrow half-width, and excellent color purity, and is expected to be applied industrially. Summary of the invention

[0004] The purpose of the present invention is to provide a compound with anthracenebenzofuran as the core and its application, which makes full use of its conjugation and the electron-donating property of furan, and is further modified with fused ring groups such as anthracene and naphthalene or deuterated at specific substitution positions. This type of compound can be used as a main material of the light-emitting layer in an organic electroluminescent device, which can significantly improve the device performance of the organic electroluminescent device and achieve high efficiency, long life and excellent color purity.

[0005] Based on the above objectives, the present application solves this need in the field by providing a compound with anthracenebenzofuran as the core and its application.

[0006] In one aspect, the present invention relates to a compound with anthracenebenzofuran as the core, which has a chemical structure as shown in formula (I):

[0007]

[0008] Among them, L 1 is a single bond, a substituted or unsubstituted aryl group, an aryl group with partially deuterated hydrogen atoms or a aryl group with completely deuterated hydrogen atoms or a aryl group with completely deuterated hydrogen atoms or a aryl group with completely deuterated hydrogen atoms;

[0009] Ar 1is substituted or unsubstituted aryl, substituted or unsubstituted heteroaryl, substituted or unsubstituted aryl with partial deuteration of hydrogen atoms, substituted or unsubstituted aryl with complete deuteration of hydrogen atoms, substituted or unsubstituted heteroaryl with partial deuteration of hydrogen atoms, substituted or unsubstituted heteroaryl with complete deuteration of hydrogen atoms;

[0010] (Ar 1 ) m is selected from Ar 1 A substituent group, m is an integer of 1-5;

[0011] R 1 -R 11 Each of the groups shown in each independently represents hydrogen or deuterium. Specifically, when m=2, 3, 4 or 5, each selected from Ar 1 The substituents may be the same or different.

[0012] Furthermore, in the compound with anthracenebenzofuran as the core provided by the present invention, the aryl group is one of phenyl, naphthyl, anthracene and pyrene.

[0013] Furthermore, in the compound with anthracenebenzofuran as the core provided by the present invention, the heteroaryl group is a heteroaryl group containing N, O, and S.

[0014] Furthermore, in the compound with anthracenebenzofuran as the core provided by the present invention, the L 1 is a single bond or is selected from one of the following structural formulas:

[0015]

[0016] Here, Dn means that n hydrogen atoms are replaced by deuterium.

[0017] Furthermore, in the compound with anthracenebenzofuran as the core provided by the present invention, the compound is selected from the chemical structure shown in any one of compounds 1-54:

[0018]

[0019]

[0020]

[0021]

[0022]

[0023]

[0024] Here, D means that a hydrogen atom is replaced by deuterium, and Dn means that n hydrogen atoms are replaced by deuterium.

[0025] It has been verified that the compound with anthracenebenzofuran as the core provided by the present invention can significantly improve the performance of the light-emitting device, achieve high efficiency, long life, and excellent color purity, and is widely applicable to OLED light-emitting devices and display devices as a light-emitting material. Therefore, the present invention further requests protection for the use of the above-mentioned compound with anthracenebenzofuran as the core in an organic electroluminescent device; an organic electroluminescent device, including a light-emitting layer, the main material of the light-emitting layer including any of the above-mentioned compounds with anthracenebenzofuran as the core; and the use of the above-mentioned organic electroluminescent device in an organic electroluminescent display device.

[0026] Compared with the prior art, the present invention has the following beneficial effects or advantages:

[0027] The present invention introduces a specific condensed ring group to modify anthracenebenzofuran at a specific position to form a new deuterated or non-deuterated compound, thereby improving the overall stability of the organic electroluminescent material. The compound with anthracenebenzofuran as the core provided by the present invention is used as the main material of the light-emitting layer, which can significantly improve the performance of the light-emitting device, achieve high efficiency, long life, and excellent color purity, and is widely applicable to use as a light-emitting material in OLED light-emitting devices and display devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The figure is a schematic diagram of the structure of an organic electroluminescent element provided in an embodiment of the present invention.

[0029] Explanation of the reference numerals: 1 is a substrate, 2 is an anode layer, 3 is a hole injection layer, 4 is a first hole transport layer, 5 is a second hole transport layer, 6 is a light-emitting layer, 7 is a hole blocking layer, 8 is an electron transport layer, 9 is an electron injection layer, and 10 is a cathode layer. DETAILED DESCRIPTION

[0030] The technical solution of the present invention is described below in conjunction with embodiments; however, the present invention is not limited to the following embodiments.

[0031] In order to enable those skilled in the art to better understand and implement the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments and drawings, but the embodiments are not intended to limit the present invention.

[0032] The experimental methods and detection methods described in the following embodiments are conventional methods unless otherwise specified; the reagents and materials are commercially available unless otherwise specified.

[0033] Example 1

[0034] This example provides a synthesis process of an intermediate for synthesizing a compound with anthracenebenzofuran as the core.

[0035]

[0036] In a three-necked flask, 200 g of intermediate 1-1, 246.4 g of potassium carbonate, and 2 L of N,N-dimethylformamide were added. Nitrogen was introduced to replace the air in the system, and then 152.1 g of methyl iodide was added dropwise. The temperature was raised to 50 °C and stirred for reaction for 6 hours, then cooled to room temperature. The reaction solution was poured into 6 L of water under stirring to precipitate solids. The filter cake obtained after filtration was dissolved in toluene and washed with water until neutral. The organic phase was dried over anhydrous sodium sulfate and purified on a silica gel column to obtain 189.8 g of intermediate 1-2 with a yield of 89.3%.

[0037]

[0038] 180 g of intermediate 1-2 and 2 L of tetrahydrofuran were added to a three-necked flask, and 86.4 g of sodium borohydride was added in batches under stirring at 0°C. The reaction was kept at this temperature for 1 hour, and then the temperature was naturally raised to room temperature and the reaction was continued for 4 hours with stirring. After TLC detection showed that the raw materials had reacted completely, 1 N hydrochloric acid solution was added to adjust the pH to neutral. The organic phase was dried over anhydrous sodium sulfate and concentrated, and the crude product was purified by silica gel column to obtain 114.2 g of intermediate 1-3 with a yield of 72.6%.

[0039]

[0040] Add 110g of intermediate 1-3 and 1.2L of tetrahydrofuran to a three-necked flask, introduce nitrogen to replace the air in the system, cool to 0°C, drop 73.7g of N,N,N',N'-tetramethylethylenediamine and 330mL of n-butyllithium (1.6M in hexane), keep the reaction at this temperature for 2h, then drop 196.5g of dibromoethane, naturally warm to room temperature and stir to react for 8h. After TLC detection, wash with water to neutrality after the raw material is completely reacted, dry the organic phase with anhydrous sodium sulfate and purify it on a silica gel column to obtain 115.0g of intermediate 1-3, with a yield of 76.1%.

[0041]

[0042] In a three-necked flask, add 110g of intermediate 1-5, 107.6g of intermediate 1-6, 75.4g of potassium acetate, and 1.2L of toluene. After nitrogen is introduced to replace the air in the system, add 8.4g of (1,1'-bis(diphenylphosphino)ferrocene) palladium dichloride, raise the temperature to reflux and stir to react for 6h. After TLC detection, the raw materials are completely reacted and cooled to room temperature. The reaction solution is washed with water until neutral, and the organic phase is dried with anhydrous sodium sulfate and purified by a silica gel column to obtain 112.7g of intermediate 1-7 with a yield of 87.7%.

[0043]

[0044] In a three-necked flask, add 110g of intermediate 1-7, 118.4g of intermediate 1-8, 90.8g of potassium carbonate, 21.2g of tetrabutylammonium bromide, 1.2L of toluene, 400mL of ethanol, and 200mL of water. After nitrogen is introduced to replace the air in the system, add 19.0g of tetrakis(triphenylphosphine)palladium, raise the temperature to reflux and stir to react for 6h. After TLC detection, the raw materials are completely reacted and cooled to room temperature. The reaction solution is washed with water until neutral, and the organic phase is dried with anhydrous sodium sulfate and purified by a silica gel column to obtain 91.9g of intermediate 1-9, with a yield of 73.5%.

[0045]

[0046] Add 90g of intermediate 1-9 and 800mL of dichloromethane to a three-necked flask, cool to 0°C, drop 88.0g of boron tribromide (1M dichloromethane solution), naturally warm to room temperature and stir to react for 4h. After TLC detection, pour into ice water to quench the reaction, wash the organic phase with water until neutral, and then dry over anhydrous sodium sulfate. Concentrate the obtained crude product and purify it on a silica gel column to obtain 80.3g of intermediate 1-10, with a yield of 92.6%.

[0047]

[0048] Add 80g of intermediate 1-10, 5.8g of sodium hydride (60% dispersed in paraffin oil), and 1L of N,N-dimethylformamide to a three-necked flask, raise the temperature to reflux and stir to react for 8h. After TLC detection, cool to room temperature, pour the reaction solution into 3L of water, stir to precipitate solids, and filter. The filter cake is completely dissolved in toluene, washed with water until neutral, dried over anhydrous sodium sulfate, and concentrated. The crude product is purified by silica gel column and recrystallization to obtain 64.7g of intermediate 1, with a yield of 85.6%.

[0049] Example 2

[0050] This example provides the preparation process of Compound 1, Compound 3, Compound 4, Compound 5, Compound 12, Compound 27, Compound 39, Compound 40, Compound 48, and Compound 49.

[0051] (1) Preparation of Compound 1

[0052]

[0053] In a three-necked flask, 5g of intermediate 1, 4.7g of compound 1-1, 4.0g of potassium carbonate, 0.9g of tetrabutylammonium bromide, 50mL of toluene, 16mL of ethanol, and 8mL of water were added. After nitrogen was introduced to replace the air in the system, 0.8g of tetrakis(triphenylphosphine)palladium was added, and the temperature was raised to reflux and stirred for 6h. After TLC detection, the raw material was completely reacted and cooled to room temperature. The reaction solution was washed with water until neutral. The organic phase was dried over anhydrous sodium sulfate and concentrated. The crude product was purified by silica gel column and recrystallized to obtain 5.2g of compound 1, with a yield of 69.5%. The NMR data are as follows: 1 H NMR(400MHz)δ8.59(s,1H),8.55(s,1H),8.42(s,1H),8.02(d,J=7.2,2H),7.98(d,J=7.2,2H),7.93(s,1H),7.81 -7.85(m,4H),7.61(d,J=7.2,1H),7.48(d,J=6.4,2H),7.38-7.43(m,4H),7.29(d,J=6.4,1H),7.17-7.23(m,4H).

[0054] (2) Preparation of Compound 3

[0055]

[0056] In a three-necked flask, 5g of intermediate 1, 5.5g of compound 3-1, 4.0g of potassium carbonate, 0.9g of tetrabutylammonium bromide, 50mL of toluene, 16mL of ethanol, and 8mL of water were added. After nitrogen was introduced to replace the air in the system, 0.8g of tetrakis(triphenylphosphine)palladium was added, and the temperature was raised to reflux and stirred for 6h. After TLC detection, the raw materials were completely reacted and cooled to room temperature. The reaction solution was washed with water until neutral. The organic phase was dried over anhydrous sodium sulfate and concentrated. The crude product was purified by silica gel column and recrystallized to obtain 5.5g of compound 3, with a yield of 67.2%. The NMR data are as follows: 1 H NMR(400MHz)δ8.59(s,1H),8.53(s,1H),8.41(s,1H),8.21-8.25(m,3H),7.96-8.02(m,6H),7. 81-7.85(m,4H),7.58-7.61(m,2H),7.38-7.43(m,4H),7.30(d,J=7.2,2H),7.27(d,J=7.2,2H).

[0057] (3) Preparation of Compound 4

[0058]

[0059] In a three-necked flask, 5g of intermediate 1, 5.5g of compound 4-1, 4.0g of potassium carbonate, 0.9g of tetrabutylammonium bromide, 50mL of toluene, 16mL of ethanol, and 8mL of water were added. After nitrogen was introduced to replace the air in the system, 0.8g of tetrakis(triphenylphosphine)palladium was added, and the temperature was raised to reflux and stirred for 6h. After TLC detection, the raw material was completely reacted and cooled to room temperature. The reaction solution was washed with water until neutral. The organic phase was dried over anhydrous sodium sulfate and concentrated to obtain a crude product. Purification and recrystallization of the obtained silica gel column gave 5.9g of compound 4, with a yield of 71.2%. The NMR data are as follows: 1 H NMR(400MHz)δ8.59(s,1H),8.53(s,1H),8.41(s,1H),8.05(d,J=7.2,2H),8 .01(d,J=7.2,2H),7.95(s,1H),7.79-7.86(m,7H),7.63(d,J=7.2,1H),7.47 -7.50(m,2H),7.42(d,J=7.2,2H),7.37(d,J=6.4,2H),7.31(d,J=7.2,2H),7.28(d,J=7.2,2H).

[0060] (4) Preparation of Compound 5

[0061]

[0062] In a three-necked flask, 5g of intermediate 1, 5.9g of compound 5-1, 4.0g of potassium carbonate, 0.9g of tetrabutylammonium bromide, 50mL of toluene, 16mL of ethanol, and 8mL of water were added. After nitrogen was introduced to replace the air in the system, 0.8g of tetrakis(triphenylphosphine)palladium was added, and the temperature was raised to reflux and stirred for 6h. After TLC detection, the raw materials were completely reacted and cooled to room temperature. The reaction solution was washed with water until neutral. The organic phase was dried over anhydrous sodium sulfate and concentrated to obtain a crude product. Purification and recrystallization of the obtained product on a silica gel column gave 5.7g of compound 5, with a yield of 66.1%. The NMR data are as follows: 1 H NMR(400MHz)δ8.59(s,1H),8.54(s,1H),8.42(s,1H),8.07(d,J=7.2,2H ),8.03(d,J=7.2,2H),7.95(s,1H),7.82-7.86(m,4H),7.57-7.62(m,3H ),7.42(d,J=7.2,2H),7.38(d,J=6.4,2H),7.33(t,J=6.4,1H),7.31(d, J=7.2,2H),7.28(d,J=7.2,2H),7.11(d,J=6.4,2H),7.08(d,J=6.4,2H).

[0063] (5) Preparation of Compound 12

[0064]

[0065] In a three-necked flask, 5g of intermediate 1, 3.9g of compound 12-1, 4.0g of potassium carbonate, 0.9g of tetrabutylammonium bromide, 50mL of toluene, 16mL of ethanol, and 8mL of water were added. After nitrogen was introduced to replace the air in the system, 0.8g of tetrakis(triphenylphosphine)palladium was added, and the temperature was raised to reflux and stirred for 6h. After TLC detection, the raw material was completely reacted and cooled to room temperature. The reaction solution was washed with water until neutral. The organic phase was dried over anhydrous sodium sulfate and concentrated to obtain a crude product. Purification and recrystallization on a silica gel column gave 4.1g of compound 12, with a yield of 61.3%. The NMR data are as follows: 1 H NMR(400MHz)δ8.59(s,1H),8.54(s,1H),8.43(s,1H),8.33(d,J=7.2,1H),8.16(d,J=7.2,1H),8.03(d,J=7 .2,1H),7.82-7.93(m,8H),7.71-7.73(m,2H),7.67(d,J=7.2,1H),7.47(d,J=7.2,1H),7.42(d,J=7.2,2H).

[0066] (6) Preparation of Compound 27

[0067]

[0068] In a three-necked flask, 5g of intermediate 1, 5.9g of compound 27-1, 4.0g of potassium carbonate, 0.9g of tetrabutylammonium bromide, 50mL of toluene, 16mL of ethanol, and 8mL of water were added. After nitrogen was introduced to replace the air in the system, 0.8g of tetrakis(triphenylphosphine)palladium was added, and the temperature was raised to reflux and stirred for 6h. After TLC detection, the raw materials were completely reacted and cooled to room temperature. The reaction solution was washed with water until neutral. The organic phase was dried over anhydrous sodium sulfate and concentrated to obtain a crude product. Purification and recrystallization on a silica gel column gave 6.6g of compound 27, with a yield of 76.2%. The NMR data are as follows: 1 H NMR(400MHz)δ8.59(s,1H),8.53(s,1H),8.43(s,1H),8.01(d,J=7.2,4H),7.94(s,1H),7.82-7.86(m,4H),7.64(d,J=7.2,1 H),7.47(d,J=6.4,2H),7.39-7.43(m,4H),7.32(t,J=6.4,1H),7.25(d,J=7.2,4H),7.15(d,J=6.4,2H),7.12(d,J=6.4,2H).

[0069] (7) Preparation of Compound 39

[0070]

[0071] In a three-necked flask, add 8g of intermediate 1, 10.8g of compound 39-1, 6.4g of potassium carbonate, 1.5g of tetrabutylammonium bromide, 50mL of toluene, 16mL of ethanol, and 8mL of water. After nitrogen is introduced to replace the air in the system, add 1.3g of tetrakis(triphenylphosphine)palladium, raise the temperature to reflux and stir to react for 6h. After TLC detection, the raw material is completely reacted and cooled to room temperature. The reaction solution is washed with water until neutral. The organic phase is dried over anhydrous sodium sulfate and concentrated to obtain a crude product. Purify and recrystallize the obtained compound 39-2 with a yield of 73.7%. The NMR data are as follows: 1 H NMR(400MHz)δ8.59(s,1H),8.53(s,1H),8.42(s,1H),8.01(d,J=7.2,2H),7 .97(d,J=7.2,2H),7.93(s,1H),7.79-7.86(m,7H),7.63(d,J=7.2,1H),7.47 -7.50(m,2H),7.42(d,J=7.2,2H),7.37(d,J=6.4,2H),7.30(d,J=7.2,2H),7.27(d,J=7.2,2H),7.15(d,J=6.4,2H),7.12(d,J=6.4,2H).

[0072]

[0073] Add 10g of compound 39-2, 1.0g of aluminum chloride, and 200mL of deuterated benzene to the reaction flask, and stir at room temperature for 4h. After the reaction is completed, add deuterated water and stir for 10min before separation. The organic phase is dried over anhydrous sodium sulfate and concentrated, and recrystallized to obtain 6.9g of compound 39, with a yield of 65.8%. MS: [M+H]+=677.

[0074] (8) Preparation of Compound 40

[0075]

[0076] In a three-necked flask, add 8g of intermediate 1, 8.2g of compound 40-1, 6.4g of potassium carbonate, 1.5g of tetrabutylammonium bromide, 50mL of toluene, 16mL of ethanol, and 8mL of water. After nitrogen is introduced to replace the air in the system, add 1.3g of tetrakis(triphenylphosphine)palladium, raise the temperature to reflux and stir to react for 6h. After TLC detection, the raw material is completely reacted and cooled to room temperature. The reaction solution is washed with water until neutral. The organic phase is dried over anhydrous sodium sulfate and concentrated to obtain a crude product. Purification and recrystallization on a silica gel column give 8.3g of compound 40-2, with a yield of 65.9%. The NMR data are as follows: 1H NMR(400MHz)δ8.59(s,1H),8.54(s,1H),8.41(s,1H),8.27(d,J=7.2,1H),8.09(d,J=7.2,1H),7.93(s,1H),7.79-7.86(m,8H ), 7.73 (d, J = 7.2, 1H), 7.67 (d, J = 7.2, 2H), 7.55 (d, J = 7.2, 1H), 7.42 (d, J = 6.4, 2H), 7.18 (d, J = 6.4, 2H), 7.15 (d, J = 6.4, 2H).

[0077]

[0078] 8 g of compound 40-2, 1.0 g of aluminum chloride, and 160 mL of deuterated benzene were added to the reaction flask and stirred at room temperature for 4 h. After the reaction was completed, deuterated water was added and stirred for 10 min before separation. The organic phase was dried over anhydrous sodium sulfate and concentrated, and recrystallized to obtain 5.6 g of compound 40 with a yield of 67.2%. MS: [M+H]+=569.

[0079] (9) Preparation of Compound 48

[0080]

[0081] In a three-necked flask, add 8g of intermediate 1, 10.8g of compound 48-1, 6.4g of potassium carbonate, 1.5g of tetrabutylammonium bromide, 50mL of toluene, 16mL of ethanol, and 8mL of water. After nitrogen is introduced to replace the air in the system, add 1.3g of tetrakis(triphenylphosphine)palladium, raise the temperature to reflux and stir to react for 6h. After TLC detection, the raw material is completely reacted and cooled to room temperature. The reaction solution is washed with water until neutral. The organic phase is dried over anhydrous sodium sulfate and concentrated to obtain a crude product. Purification and recrystallization on a silica gel column give 11.4g of compound 48-2, with a yield of 76.2%. The NMR data are as follows: 1 H NMR(400MHz)δ8.59(s,1H),8.53(s,1H),8.49(d,J=7.2,1H),8.42(s,1H),8.23(d,J=7.2,1H),8.05(d,J=7.2,1H),8 .02(d,J=7.2,2H),7.97(d,J=7.2,2H),7.93(s,1H),7.79-7.85(m,5H),7.63(d,J=7.2,1H),7.57(d,J=7.2,1H),7.47 -7.50(m,4H),7.30(d,J=7.2,2H),7.26(d,J=7.2,2H),7.15(d,J=6.4,2H),7.12(d,J=6.4,2H).

[0082]

[0083] Add 10g of compound 48-2, 1.0g of aluminum chloride, and 200mL of deuterated benzene to the reaction flask, and stir at room temperature for 4h. After the reaction is completed, add deuterated water and stir for 10min before separation. The organic phase is dried over anhydrous sodium sulfate and concentrated, and recrystallized to obtain 6.5g of compound 48, with a yield of 62.2%. MS: [M+H]+=677.

[0084] (10) Preparation of Compound 49

[0085]

[0086] In a three-necked flask, add 8g of intermediate 1, 11.8g of compound 49-1, 6.4g of potassium carbonate, 1.5g of tetrabutylammonium bromide, 50mL of toluene, 16mL of ethanol, and 8mL of water. After nitrogen is introduced to replace the air in the system, add 1.3g of tetrakis(triphenylphosphine)palladium, raise the temperature to reflux and stir to react for 6h. After TLC detection, the raw material is completely reacted and cooled to room temperature. The reaction solution is washed with water until neutral. The organic phase is dried over anhydrous sodium sulfate and concentrated to obtain a crude product. Purify and recrystallize the obtained compound 49-2 on a silica gel column, and the yield is 70.9%. The NMR data are as follows: 1 H NMR(400MHz)δ8.59(s,1H),8.53(s,1H),8.43(s,1H),8.05(d,J=7.2,2H),7 .98(d,J=7.2,2H),7.93(s,1H),7.76-7.88(m,7H),7.63(d,J=7.2,1H),7.47 -7.50(m,4H),7.35(t,J=7.2,1H),7.32(d,J=7.2,2H),7.26(d,J=7.2,2H),7.21(d,J=7.2,1H),7.16(d,J=7.2,2H),7.12(d,J=7.2,2H).

[0087]

[0088] Add 10g of compound 39-2, 1.0g of aluminum chloride, and 200mL of deuterated benzene to the reaction flask, and stir at room temperature for 4h. After the reaction is completed, add deuterated water and stir for 10min before separation. The organic phase is dried over anhydrous sodium sulfate and concentrated, and recrystallized to obtain 7.1g of compound 39 with a yield of 68.3%. MS: [M+H]+=717.

[0089] Except for Compound 1, Compound 3, Compound 4, Compound 5, Compound 12, Compound 27, Compound 39, Compound 40, Compound 48 and Compound 49 disclosed in the present invention, other compounds can be prepared by referring to the above preparation method.

[0090] Example 3

[0091] This embodiment provides compounds 1, 3, 4, 5, 12, 27, 39, 40, 48, 49 and the existing light-emitting layer host material BH1 in T 1 Simulation calculations of energy levels and HOMO and LUMO indicators.

[0092] Compound 1, compound 3, compound 4, compound 5, compound 12, compound 27, compound 39, compound 40, compound 48, compound 49 and the existing light-emitting layer host material BH1 were subjected to T 1 Energy level and HOMO, LUMO simulation calculation. The highest occupied molecular orbital (HOMO) and the lowest unoccupied molecular orbital (LUMO) are the data obtained by simulation calculation. The calculation method adopts B3LYP hybrid functional and basis set 6-31g (d, P). The results are shown in Table 1.

[0093] Table 1, T 1 Energy level and HOMO, LUMO simulation results

[0094]

[0095]

[0096] As shown in Table 1, the compounds disclosed in the present invention have suitable HOMO / LUMO, and are suitable for use as the main material of the light-emitting layer. The compounds with anthracenebenzofuran as the core of the present invention can effectively improve the luminous efficiency and service life of the device when applied to OLED devices.

[0097] Device Application Examples

[0098] Taking some compounds provided by the present invention as examples, the compounds are applied as luminescent materials to organic electroluminescent devices to verify the excellent effects achieved.

[0099] The excellent effect of the OLED material of the present invention in the device is specifically described in detail through the device performance of device embodiments 1-10 and comparative example 1. The structure and manufacturing process of the device embodiments 1-10 of the present invention and comparative example 1 are exactly the same, and the same glass substrate and electrode material are used, and the film thickness of the electrode material is also consistent. The difference is that the main material of the light-emitting layer is adjusted, as follows.

[0100] Device Example 1

[0101] This embodiment provides an organic electroluminescent device, the structure of which is as follows: Figure 1As shown, it includes a substrate 1, an anode layer 2, a hole injection layer 3, a first hole transport layer 4, a second hole transport layer 5, a light emitting layer 6, a hole blocking layer 7, an electron transport layer 8, an electron injection layer 9 and a cathode layer 10 which are stacked in sequence.

[0102] Among them, the material of the anode layer 2 is indium tin oxide (ITO) with a high work function, the material of the hole injection layer 3 is HAT-CN with a thickness of 5nm; the material of the first hole transport layer 4 is HT-1 with a thickness of 60nm; the material of the second hole transport layer 5 is HT-2 with a thickness of 15nm; the light-emitting layer 6 uses BH1 as the main material and BD01 as the light-emitting material, with a doping mass ratio of 5% and a thickness of 30nm; the material of the hole blocking layer 7 is HB-1 with a thickness of 10nm; the material of the electron transport layer 8 is ET-1 with a thickness of 30nm; the material of the electron injection layer 9 is Liq with a thickness of 2nm; the material of the cathode layer is Al with a thickness of 100nm.

[0103] The basic material structure used in each functional layer of the device is as follows:

[0104]

[0105] The specific preparation steps of the above organic electroluminescent device are as follows:

[0106] 1) Clean the ITO anode on the transparent glass or plastic substrate by ultrasonic cleaning with deionized water, acetone, and ethanol for 20 minutes each, and then perform plasma treatment in an oxygen atmosphere for 5 minutes;

[0107] 2) On the ITO anode layer, a hole injection layer material HAT-CN is deposited by vacuum evaporation with a thickness of 5 nm, which serves as a hole injection layer;

[0108] 3) Vacuum evaporation of hole transport material HT-1 on the hole injection layer with a thickness of 60 nm, which serves as the first hole transport layer;

[0109] 4) Vacuum evaporation of a hole transport material HT-2 with a thickness of 15 nm is performed on the first hole transport layer HT-1, and this layer serves as the second hole transport layer;

[0110] 5) On the second hole transport layer, a light-emitting layer was co-deposited by vacuum evaporation, using compound 1 as the main material and BD01 as the light-emitting material, with a doping mass ratio of 5% and a thickness of 30 nm;

[0111] 6) On the light-emitting layer, a hole blocking material HB-1 is deposited by vacuum evaporation with a thickness of 10 nm, and this layer serves as a hole blocking layer;

[0112] 7) On the hole blocking layer, the electron transport material ET-1 is evaporated by vacuum evaporation with a thickness of 30 nm, and this layer serves as the electron transport layer;

[0113] 8) On the electron transport layer, the electron injection material Liq is evaporated by vacuum evaporation with a thickness of 2 nm, and this layer serves as the electron injection layer;

[0114] 9) On the electron injection layer, cathode Al is deposited by vacuum evaporation with a thickness of 100 nm. This layer is used as a cathode conductive electrode.

[0115] The implementation process of device examples 2 to 10 is the same as that of device example 1, except that the main material of the light-emitting layer is replaced by other developed compounds instead of compound 1.

[0116] Comparative Example 1

[0117] The same as device embodiment 1, except that BH1 is used as the main material of the light-emitting layer instead of compound 1.

[0118] The components of different devices prepared in device embodiments 1 to 10 and comparative example 1 of the present invention are shown in Table 2:

[0119] Table 2. Comparison of organic electroluminescent device components of various device embodiments

[0120]

[0121] The cathode and anode of each group of organic electroluminescent devices were connected by a known driving circuit, and the voltage-efficiency-current density relationship of the OLED device was tested by a standard method using a Keithley 2400 power supply combined with a PR670 photometer; the life of the device was tested by a constant current method under the test condition of a constant current density of 10 mA / cm 2 The time it takes for the brightness to decay to 90% of the initial brightness is the LT90 life of the device. The test results are shown in Table 3.

[0122] Table 3, Performance results of organic electroluminescent devices in each group

[0123]

[0124]

[0125] As shown in Table 3, the compounds provided by the present invention are applied as the main material of the light-emitting layer to the OLED device, and have excellent performance. For example, the compound 4 in the device embodiment 4 is used as the main material of the blue light, and compared with BH1 in the comparative example 1, the luminous efficiency and service life are significantly improved, the luminous efficiency is increased by 20.9%, and the device life is increased by 46.1%; the deuterated material compound 39 is compared with the comparative material BH1, the device luminous efficiency is increased by 33.3%, and the device life is increased by 67.3%. It can be seen that the compounds of the present invention are selected as the main material of the light-emitting layer, and compared with the existing materials applied to the OLED light-emitting device, the luminous efficiency and life performance of the device are good, and it has great application value in the application of OLED devices and has good industrialization prospects.

[0126] The present invention obtains a new compound by connecting anthracene, naphthalene and other fused ring groups to the existing anthracene benzofuran core skeleton at a fixed substitution position, and further deuterates the compound. The compound modified with a specific group has a suitable frontier orbital energy level, and the innovative series of compounds exhibit excellent performance as the main material of the light-emitting layer in an organic electroluminescent (OLED) device.

[0127] As described above, the present invention can be well implemented. The above embodiments are only descriptions of the preferred implementation modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various changes and improvements made to the technical solutions of the present invention by ordinary technicians in this field should fall within the protection scope determined by the present invention.

Claims

1. A compound with anthracenebenzofuran as the core, It is characterized in that The compound is selected from the chemical structure shown in any one of compounds 1-54: Here, D means that a hydrogen atom is replaced by deuterium, and Dn means that n hydrogen atoms are replaced by deuterium.

2. Use of the compound with anthracenebenzofuran as the core according to any one of claim 1 in an organic electroluminescent device.

3. An organic electroluminescent device comprising a light-emitting layer, It is characterized in that The light-emitting layer comprises the compound with anthracenebenzofuran as the core as claimed in any one of claims 1.